Preparation method of ferroferric oxide nanoparticles with controllable morphology and particle size

By dissolving the iron salt in polyol and adding a structural guide agent for high-temperature reaction, the problems of low mass preparation efficiency and difficult to control the particle size of iron tetraoxide nanoparticles in the prior art are solved, and the morphology and particle size are achieved. Adjustable and suitable for biochemical applications.

CN119018939AActive Publication Date: 2024-11-26JIMEI UNIV

Patent Information

Application Number
CN202411161548.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26
Estimated Expiration
2044-08-22

AI Technical Summary

Technical Problem

It is difficult to prepare iron tetraoxide nanoparticles with controllable morphology and particle size in large batches, especially in large-scale industrial production, and the existing solvent-thermal preparation efficiency is low and it is difficult to prepare uniform nanoparticles less than 100 nm.

Method used

The iron salt is dissolved in polyol and then stirred ultrasonicly, and then added a structural guide agent to carry out a high-temperature reaction, followed by natural cooling and washing with deionized water and ethanol to obtain iron tetraoxide nanoparticles with adjustable morphology and particle size. The method includes the use of iron salts such as ferric acetylacetonate, potassium ferrocyanide, iron sulfate, and structural guides such as glycol and urea to control reaction conditions such as temperature and time to achieve the preparation of different morphology and particle sizes.

Benefits of technology

Achieve efficient mass production of iron tetroxide nanoparticles with adjustable morphology and particle size. It is simple to operate and has high yield. It obtains spherical, rod-shaped, polyhedral nanoparticles with different morphology, and has different magnetic responsiveness and is applicable. in the field of biochemistry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018939A_ABST
    Figure CN119018939A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of ferroferric oxide nanoparticles with controllable morphology and particle size. Comprising the following steps: S1, dissolving ferric salt in polyhydric alcohol, performing ultrasonic treatment, and stirring until the ferric salt is not dissolved any more; s2, adding a structure guiding agent, continuously stirring, transferring the obtained liquid into a reaction kettle, sealing, and carrying out high-temperature reaction; and S3, after the reaction is completed, naturally cooling to room temperature, and respectively washing an obtained black product with deionized water and ethanol for multiple times to obtain the ferroferric oxide nanoparticles. The method disclosed by the invention is simple in process operation and high in yield, and the morphology and the particle size of the prepared Fe3O4 microspheres can be regulated and controlled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of methods for preparing ferroferric oxide nanoparticles, and in particular to a method for preparing ferroferric oxide nanoparticles with controllable morphology and particle size. Background Art

[0002] Fe3O4 magnetic nanoparticles have the characteristics of simple preparation, high stability, low cost, good biocompatibility, good magnetic responsiveness, and easy surface modification. They are widely used in biochemical fields such as nucleic acid extraction, cell sorting, protein purification, nuclear magnetic resonance imaging, drug targeting, and magnetic hyperthermia.

[0003] At present, magnetic Fe3O4 nanoparticles can be prepared by chemical coprecipitation, hydrothermal method, thermal decomposition method and solvothermal method. Among them, the reaction temperature of the coprecipitation method is low, the monodispersity of the obtained nanoparticles is poor, and the particles are prone to agglomeration or oxidation during the washing process of the nanoparticles, and monodisperse Fe3O4 nanoparticles cannot be effectively prepared. The hydrothermal method is based on the preparation of monodisperse nanoparticles by metal ion crystallization under harsh experimental conditions such as high temperature and high pressure, but the subsequent treatment process will still cause the oxidation of nanoparticles in the air and affect their chemical composition. The ferroferric oxide nanoparticles synthesized by the thermal decomposition method have high purity and are not easy to agglomerate, but the conditions are harsh and the cost is high. The solvothermal method is one of the most commonly used methods for preparing magnetic ferroferric oxide nanoparticles. The heating reaction is carried out in a closed high-pressure hydrothermal reactor. The prepared ferroferric oxide nanoparticles have the advantages of uniform morphology, good dispersibility, and controllable size, and have attracted widespread attention from scientific researchers. However, this method requires the reaction to be carried out in a high-pressure closed container, and the preparation efficiency is extremely low, which is not conducive to large-scale industrial production. For example, CN113636601A discloses a method for preparing magnetic ferroferric oxide nanoparticles by solvent method, in which the mass ratio of hexahydrated ferric chloride, ethylene glycol, sodium citrate and anhydrous sodium acetate is 15:555:36:24, and the ratio of ferric chloride is only 2.7%; CN116332240A discloses a method for preparing magnetic ferroferric oxide nanoparticles by solvent method, in which the ratio of ferric chloride to solvent is only 12.7% at most; CN110615483A discloses a method for preparing magnetic Fe3O4 microspheres by solvent method, in which the ratio of ferric chloride to solvent is only 10% at most; CN117566807A discloses a method for preparing magnetic ferroferric oxide nanoparticles by solvent method, in which the concentration of trivalent iron ion compound is 0.005-0.5 mol / L. In addition, the particle size prepared by this method is relatively large, and it is difficult to prepare ferroferric oxide nanoparticles with uniform size below 100 nm.

[0004] Therefore, there is an urgent need to develop a method for preparing ferroferric oxide nanoparticles that can achieve large-scale preparation and have controllable morphology and particle size. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing ferroferric oxide nanoparticles which can be mass-produced and have adjustable morphology and particle size.

[0006] To achieve the above object, the present invention provides a method for preparing ferroferric oxide nanoparticles with controllable morphology and particle size, which is characterized by comprising the following steps:

[0007] S1. Dissolve the iron salt in the polyol, and stir under ultrasonication until the iron salt is no longer soluble.

[0008] S2, adding a structure directing agent, continuing to stir, transferring the resulting liquid to a reaction kettle, sealing, and reacting at high temperature;

[0009] S3. After the reaction is completed, the product is naturally cooled to room temperature, and the obtained black product is washed several times with deionized water and ethanol to obtain ferrosoferric oxide nanoparticles.

[0010] Furthermore, in S1, the iron salt is at least one of ferric acetylacetonate, potassium ferrocyanide, ferrocene, ferric sulfate, ferric nitrate, and ferric chloride.

[0011] Furthermore, in S1, the polyol as the solvent is at least one of ethylene glycol, 1,2-propylene glycol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol and glycerol.

[0012] Furthermore, in S1, the concentration of the iron salt after the iron salt is dissolved in the polyol is 50 w / v% to 100 w / v%.

[0013] Further, in S2, the structure directing agent is at least one of sodium citrate, anhydrous sodium acetate, urea, polyethyleneimine, potassium nitrate, polyethylene glycol, potassium permanganate, sodium hydroxide, ethylenediamine, and polyvinyl pyrrolidone;

[0014] Optionally, the structure directing agent is added in an amount of 6 w / v% to 180 w / v%.

[0015] Furthermore, in S3, the high temperature reaction is carried out at 180-220° C. for 8-24 hours.

[0016] Furthermore, the morphology of the ferroferric oxide nanoparticles obtained in S3 is spherical, rod-shaped, polyhedral, hollow sphere, pine cone-shaped, honeycomb-shaped, and the ferroferric oxide particles have a size of 30 to 400 nm.

[0017] Different morphologies of ferroferric oxide nanoparticles have different magnetic responsiveness, that is, different magnetic separation times. Magnetic beads with different morphologies have different numbers of silanol groups after being embedded with silica, and the extraction rates of nucleic acids are also different.

[0018] The present invention uses different structural directing agents to produce different shapes of ferroferric oxide nanoparticles. For example, when urea is added, urea and H2O generate CO2 and NH3 under a higher vapor pressure, and these microbubbles are retained in the reaction medium. With the assistance of the reaction medium, crystals are formed, and these microbubbles serve as aggregation centers to guide the crystals to aggregate around the gas-liquid interface. As the crystals grow and the Ostwarld ripening process proceeds, hollow spherical magnetic beads are eventually formed. When the urea content in the system is increased, the ions precipitated in the system and the generated microbubbles also increase. In this case, violent collisions occur in the container, and the hollow core is destroyed. A large number of negatively charged anions (OH) produced by the hydrolysis of urea - and CO3 2- ) are wrapped around the grains, and driven by surface tension, the grains aggregate. As the Ostwald ripening process proceeds, the positively charged NH 4+ It is very likely to be adsorbed on the surface of the grains, thereby hindering the growth of the particles, thus forming pine cone-shaped magnetic beads. Different guides have different mechanisms for generating magnetic beads.

[0019] Compared with the prior art, this application has the following beneficial effects:

[0020] The present invention uses Fe 3+ As an iron source, it is dissolved in a solvent, and a specific structure-directing agent is added to partially reduce Fe by solvothermal method. 3+ The Fe3O4 microspheres with adjustable grain size and magnetic response (i.e. magnetic separation time) are synthesized in one step. The method of the invention has simple operation and high yield, and the morphology and particle size of the prepared Fe3O4 microspheres can be adjusted. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 This is a morphological structure diagram of the Fe3O4 magnetic particles obtained in Example 1.

[0022] Figure 2 This is a morphological structure diagram of the Fe3O4 magnetic particles obtained in Example 2.

[0023] Figure 3 This is a morphological structure diagram of the Fe3O4 magnetic particles obtained in Example 3.

[0024] Figure 4 This is a morphological structure diagram of the Fe3O4 magnetic particles obtained in Example 4.

[0025] Figure 5 This is a morphological structure diagram of the Fe3O4 magnetic particles obtained in Example 5.

[0026] Figure 6 This is a morphological structure diagram of the Fe3O4 magnetic particles obtained in Example 6.

[0027] Figure 7 This is a morphological structure diagram of the Fe3O4 magnetic particles obtained in Example 7.

[0028] Figure 8 This is a morphological structure diagram of the Fe3O4 magnetic particles obtained in Example 8.

[0029] Fig. 9 This is a morphological structure diagram of the Fe3O4 magnetic particles obtained in Example 9.

[0030] Fig.10 This is a morphological structure diagram of the Fe3O4 magnetic particles obtained in Example 10.

[0031] Fig.11 This is a morphological structure diagram of the magnetic beads obtained in Comparative Example 1.

[0032] Fig.12 This is a morphological structure diagram of the magnetic beads obtained in Comparative Example 2. DETAILED DESCRIPTION

[0033] Embodiments of the present invention are described in detail below, and the examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals represent the same or similar elements or elements with the same or similar functions from beginning to end. The embodiments described below by reference to the accompanying drawings are exemplary, are intended to be used to explain the present invention, and are not to be construed as limitations of the present invention. Those who do not indicate specific techniques or conditions in the embodiments are carried out according to the techniques or conditions described in the documents in this area or according to the product specification. Those who do not indicate the manufacturer of reagents or instruments used are all conventional products that can be obtained commercially.

[0034] The magnetic separation time of magnetic beads in the following experiment is as follows: accurately weigh 0.1g of sample powder, add 10mL of water into a 10mL glass bottle, and after sufficient ultrasonic dispersion, place a magnet vertically on one side of the glass bottle, and calculate the time it takes for the solution to change from turbid to clear.

[0035] A method for preparing ferroferric oxide nanoparticles with controllable morphology and particle size, characterized in that it comprises the following steps:

[0036] S1. Dissolve the iron salt in the polyol, and stir under ultrasonication until the iron salt is no longer soluble.

[0037] S2, adding a structure directing agent, continuing to stir, transferring the resulting liquid to a reaction kettle, sealing, and reacting at high temperature;

[0038] S3. After the reaction is completed, the product is naturally cooled to room temperature, and the obtained black product is washed several times with deionized water and ethanol to obtain ferrosoferric oxide nanoparticles.

[0039] Furthermore, in S1, the iron salt is at least one of ferric acetylacetonate, potassium ferrocyanide, ferrocene, ferric sulfate, ferric nitrate, and ferric chloride.

[0040] Furthermore, in S1, the polyol as the solvent is at least one of ethylene glycol, 1,2-propylene glycol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol and glycerol.

[0041] Furthermore, in S1, the concentration of the iron salt after the iron salt is dissolved in the polyol is 50 w / v% to 100 w / v%.

[0042] Further, in S2, the structure directing agent is at least one of sodium citrate, anhydrous sodium acetate, urea, polyethyleneimine, potassium nitrate, polyethylene glycol, potassium permanganate, sodium hydroxide, ethylenediamine, and polyvinyl pyrrolidone;

[0043] Optionally, the structure directing agent is added in an amount of 6 w / v% to 180 w / v%.

[0044] Furthermore, in S3, the high temperature reaction is carried out at 180-220° C. for 8-24 hours.

[0045] Furthermore, the morphology of the ferroferric oxide nanoparticles obtained in S3 is spherical, rod-shaped, polyhedral, hollow sphere, pine cone-shaped, honeycomb-shaped, and the ferroferric oxide particles have a size of 30 to 400 nm.

[0046] Example 1: Efficient preparation method of ferroferric oxide nanoparticles with controllable morphology and particle size

[0047] The following steps are involved:

[0048] S1. Weigh 50 g of ferric chloride and dissolve it in 100 mL of 1,2-propylene glycol. Ultrasonicate and stir until the iron salt is completely dissolved to prepare a 50% ferric chloride solution.

[0049] S2. Add 50 g of urea (the amount of urea added is 50 w / v%) as a structure directing agent, continue ultrasonication and stirring until dissolved, transfer the resulting liquid to a 500 mL polytetrafluoroethylene reactor, seal it, and react at 200° C. for 24 h.

[0050] S3. After the reaction, the reactor was cooled to room temperature and the solution was clearly stratified. The supernatant was removed and washed alternately with anhydrous ethanol and deionized water until the supernatant was clear. The black precipitate in the reactor was collected and dried in a vacuum oven at 60°C for 12 hours to obtain 10.7 g of hollow spherical Fe3O4 magnetic particles with a yield of 75%. The magnetic separation time of the magnetic beads was 4 seconds. The results are shown in Figure 1 , it can be seen that the microsphere particles are hollow spheres.

[0051] Example 2: Efficient preparation method of ferroferric oxide nanoparticles with controllable morphology and particle size

[0052] The following steps are involved:

[0053] S1. Weigh 50 g of ferric acetylacetonate and dissolve it in 100 mL of 1,2-propylene glycol. Ultrasonicate and stir until the iron salt is completely dissolved to prepare a 50% ferric acetylacetonate solution.

[0054] S2. Add 50 g of urea (the amount of urea added is 50 w / v%) as a structure directing agent, continue ultrasonication and stirring until dissolved, transfer the resulting liquid to a reactor, seal it, and react at 200° C. for 24 hours.

[0055] S3. After the reaction, the reactor was cooled to room temperature. When the solution was clearly stratified, the supernatant was removed and washed alternately with anhydrous ethanol and deionized water until the supernatant was clear. The black precipitate in the reactor was collected and dried in a vacuum oven at 60°C for 12 hours to obtain 8.7 g of pine cone-shaped Fe3O4 magnetic particles with a yield of 80%. The magnetic separation time of the magnetic beads was 8 seconds. The results are shown in Figure 2 , it can be seen that the microsphere particles are pine cone-shaped.

[0056] Example 3: Efficient preparation method of ferroferric oxide nanoparticles with controllable morphology and particle size

[0057] The following steps are involved:

[0058] S1. Weigh 50 g of ferric sulfate and dissolve it in 100 mL of 1,4-butanediol. Ultrasonicate and stir until the iron salt is completely dissolved to prepare a 50% ferric sulfate solution.

[0059] S2. Add 11 g potassium nitrate, 45 g sodium hydroxide and 22 g polyethyleneimine as structure directing agents, continue ultrasonication and stirring until dissolved, transfer the resulting liquid to a reactor, seal it, and react at 100°C for 8 h.

[0060] S3. After the reaction, the reactor was cooled to room temperature and the solution was clearly stratified. The supernatant was removed and washed alternately with anhydrous ethanol and deionized water until the supernatant was clear. The black precipitate in the reactor was collected and dried in a vacuum oven at 60°C for 12 hours to obtain 16.44 g of polyhedral Fe3O4 magnetic particles with a yield of 85%. The magnetic separation time of the magnetic beads was 5 seconds. The results are shown in Figure 3 , it can be seen that the microsphere particles are polyhedral irregular shapes.

[0061] Example 4: Efficient preparation method of ferroferric oxide nanoparticles with controllable morphology and particle size

[0062] The following steps are involved:

[0063] S1. Weigh 50 g of potassium ferrocyanide and dissolve it in 100 mL of 1,6-hexanediol. Ultrasonicate and stir until the iron salt is completely dissolved to prepare a 50% potassium ferrocyanide solution.

[0064] S2. Add 110 g potassium nitrate as a structure-directing agent, continue ultrasonication and stirring until dissolved, transfer the resulting liquid to a reactor, seal it, and react at 100° C. for 8 h.

[0065] S3. After the reaction, the reactor was cooled to room temperature. When the solution was clearly stratified, the supernatant was removed and washed alternately with anhydrous ethanol and deionized water until the supernatant was clear. The black precipitate in the reactor was collected and dried in a vacuum oven at 60°C for 12 hours to obtain 7.42g of nanorod-shaped Fe3O4 magnetic particles with a yield of 81%. The magnetic separation time of the magnetic beads was 7s. The results are shown in Figure 4 , it can be seen that the microsphere particles are nanorod-shaped.

[0066] Example 5: Efficient preparation method of ferroferric oxide nanoparticles with controllable morphology and particle size

[0067] The following steps are involved:

[0068] S1. Weigh 50 g of ferrocene and dissolve it in 100 mL of diethylene glycol. Ultrasonicate and stir until the iron salt is completely dissolved to prepare a 50% ferrocene solution.

[0069] S2. Add 30 g PEG 2000 and 150 g anhydrous sodium acetate as structure directing agents, continue ultrasonication and stirring until dissolved, transfer the resulting liquid to a reactor, seal it, and react at 200° C. for 8 h.

[0070] S3. After the reaction, the reactor was cooled to room temperature. When the solution was clearly stratified, the supernatant was removed and washed alternately with anhydrous ethanol and deionized water until the supernatant was clear. The black precipitate in the reactor was collected and dried in a vacuum oven at 60°C for 12 hours to obtain 16.6 g of spherical Fe3O4 magnetic particles with a yield of 80%. The magnetic separation time of the magnetic beads was 12 seconds. Figure 5 , it can be seen that the microsphere particles are spherical.

[0071] Example 6: Efficient preparation method of ferroferric oxide nanoparticles with controllable morphology and particle size

[0072] The following steps are involved:

[0073] S1. Weigh 50 g of ferric nitrate and dissolve it in 100 mL of propylene glycol. Ultrasonicate and stir until the iron salt is completely dissolved to prepare a 50% ferric nitrate solution.

[0074] S2. Add 20 g KMnO4 g and 80 g sodium citrate as structure directing agents, continue ultrasonication and stirring until dissolved, transfer the resulting liquid to a reactor, seal it, and react at 100°C for 8 h.

[0075] S3. After the reaction, the reactor was cooled to room temperature. When the solution was clearly stratified, the supernatant was removed and washed alternately with anhydrous ethanol and deionized water until the supernatant was clear. The black precipitate in the reactor was collected and dried in a vacuum oven at 60°C for 12 hours to obtain 13.1g of honeycomb Fe3O4 magnetic particles with a yield of 82%. The magnetic separation time of the magnetic beads was 19s. The results are shown in Figure 6 , it can be seen that the microsphere particles are honeycomb-shaped.

[0076] Example 7: Efficient preparation method of ferroferric oxide nanoparticles with controllable morphology and particle size

[0077] The following steps are involved:

[0078] S1. Weigh 100 g of ferric chloride and dissolve it in 100 mL of ethylene glycol. Ultrasonicate and stir until the iron salt is completely dissolved to prepare a 100% ferric chloride solution.

[0079] S2. Add 72 g of anhydrous sodium acetate, 50 mL of ethylenediamine, and 10 g of polyvinyl pyrrolidone as structure-directing agents, continue ultrasonication and stirring until dissolved, transfer the resulting liquid to a reactor, seal it, and react at 200°C for 12 h.

[0080] S3. After the reaction is completed, the reactor is cooled to room temperature. After the solution is clearly stratified, the supernatant is removed and washed alternately with anhydrous ethanol and deionized water until the supernatant is clear. The black precipitate in the reactor is collected and dried in a vacuum oven at 60°C for 12 hours to obtain 22.8 g of 30-50 nm spherical Fe3O4 magnetic particles with a yield of 79.6%. The magnetic separation time of the magnetic beads is 11 seconds. The results are shown in Figure 7 , it can be seen that the microsphere particles are spherical.

[0081] Example 8: Efficient preparation method of ferroferric oxide nanoparticles with controllable morphology and particle size

[0082] The following steps are involved:

[0083] S1. Weigh 100 g of ferric sulfate and dissolve it in 100 mL of ethylene glycol. Ultrasonicate and stir until the iron salt is completely dissolved to prepare a 100% ferric sulfate solution.

[0084] S2. Add 70 g of anhydrous sodium acetate and 30 g of sodium citrate as structure directing agents, continue ultrasonication and stirring until dissolved, transfer the resulting liquid to a reactor, seal it, and react at 200°C for 10 hours.

[0085] S3. After the reaction is completed, the reactor is cooled to room temperature. After the solution is clearly stratified, the supernatant is removed and washed alternately with anhydrous ethanol and deionized water until the supernatant is clear. The black precipitate in the reactor is collected and dried in a vacuum oven at 60°C for 12 hours to obtain 31.7 g of 120-170 nm spherical Fe3O4 magnetic particles with a yield of 82%. The magnetic separation time of the magnetic beads is 12 seconds. The results are shown in Figure 8 , it can be seen that the microsphere particles are spherical.

[0086] Example 9: Efficient preparation method of ferroferric oxide nanoparticles with controllable morphology and particle size

[0087] The following steps are involved:

[0088] S1. Weigh 100 g of ferric nitrate and dissolve it in 100 mL of ethylene glycol. Ultrasonicate and stir until the iron salt is completely dissolved to prepare a 100% ferric nitrate solution.

[0089] S2. Add 100 g of anhydrous sodium acetate and 20 g of sodium citrate as structure directing agents, continue ultrasonication and stirring until dissolved, transfer the resulting liquid to a reactor, seal it, and react at 200°C for 8 h.

[0090] S3. After the reaction is completed, the reactor is cooled to room temperature. After the solution is clearly stratified, the supernatant is removed and washed alternately with anhydrous ethanol and deionized water until the supernatant is clear. The black precipitate in the reactor is collected and dried in a vacuum oven at 60°C for 12 hours to obtain 25.6 g of 220-270 nm spherical Fe3O4 magnetic particles with a yield of 80%. The magnetic separation time of the magnetic beads is 13 seconds. The results are shown in Fig. 9 , it can be seen that the microsphere particles are spherical.

[0091] Example 10: Efficient preparation method of ferroferric oxide nanoparticles with controllable morphology and particle size

[0092] The following steps are involved:

[0093] S1. Weigh 100 g of potassium ferrocyanide and dissolve it in 100 mL of ethylene glycol. Ultrasonicate and stir until the iron salt is completely dissolved to prepare a 100% potassium ferrocyanide solution.

[0094] S2. Add 180 g of anhydrous sodium acetate, 30 g of sodium citrate, and 6 g of PEG 2000 as structure-directing agents, continue ultrasonication and stirring until dissolved, transfer the resulting liquid to a reactor, seal it, and react at 200° C. for 10 h.

[0095] S3. After the reaction is completed, the reactor is cooled to room temperature. After the solution is clearly stratified, the supernatant is removed and washed alternately with anhydrous ethanol and deionized water until the supernatant is clear. The black precipitate in the reactor is collected and dried in a vacuum oven at 60°C for 12 hours to obtain 15.6 g of 350-400 nm spherical Fe3O4 magnetic particles with a yield of 85%. The magnetic separation time of the magnetic beads is 14 seconds. The results are shown in Fig.10 , it can be seen that the microsphere particles are spherical.

[0096] Comparative Example 1: Preparation of FeO3 Nanoparticles

[0097] Add 1.30 g FeCl3·6H2O and 0.40 g sodium citrate dihydrate to 20 mL ethylene glycol until completely dissolved;

[0098] Then, 2.40 g of NaAc was added under stirring. The mixture was stirred vigorously for 30 min to make it uniform;

[0099] Then transfer to a polytetrafluoroethylene liner with a volume of 100mL and seal it in a stainless steel reactor. Heat the autoclave to 200℃ and keep the constant temperature for 10h, then stop the reaction and let it cool to room temperature. Wash the black product with ethanol and deionized water three times respectively, collect the black precipitate in the autoclave, dry it in a vacuum oven at 60℃ for 12h, and obtain 0.148g of magnetic beads with a yield of 40%. The magnetic separation time of the magnetic beads is 20s. The results are shown in Fig.11 .

[0100] Comparative Example 2: Preparation of FeO3 Nanoparticles

[0101] Weigh 1.35 g FeCl3·6H2O, add it to 40 mL ethylene glycol, and stir to dissolve it;

[0102] Then, 3.6 g NaAc and 1.0 g polyethylene glycol 2000 were added and stirring was continued for 0.5 h;

[0103] The obtained solution was transferred into a hydrothermal reactor with a volume of 100 mL, and the hydrothermal reactor was placed in a forced air drying oven at a temperature of 200°C to start the hydrothermal reaction. After 8 hours of reaction, the hydrothermal reactor was taken out and cooled to room temperature. The black precipitate in the reactor was collected and dried in a vacuum drying oven at 60°C for 12 hours to obtain 0.135 g of magnetic beads with a yield of 35%. The magnetic separation time of the magnetic beads was 22 seconds. The results are shown in Fig.12 .

[0104] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and intent of the present invention.

Claims

1. A method for preparing ferroferric oxide nanoparticles with controllable morphology and particle size, It is characterized in that The following steps are involved: S1. Dissolve the iron salt in the polyol, and stir under ultrasonication until the iron salt is no longer soluble. S2, adding a structure directing agent, continuing to stir, transferring the resulting liquid to a reaction kettle, sealing, and reacting at high temperature; S3. After the reaction is completed, the product is naturally cooled to room temperature, and the obtained black product is washed several times with deionized water and ethanol to obtain ferrosoferric oxide nanoparticles.

2. The method for preparing ferroferric oxide nanoparticles with controllable morphology and particle size according to claim 1, It is characterized in that In S1, the iron salt is at least one of ferric acetylacetonate, potassium ferrocyanide, ferrocene, ferric sulfate, ferric nitrate, and ferric chloride.

3. The method for efficiently preparing ferroferric oxide nanoparticles with controllable morphology and particle size according to claim 1, It is characterized in that In S1, the polyol is at least one of ethylene glycol, 1,2-propylene glycol, 1,4-butanediol, 1,6-hexanediol, diethylene glycol, dipropylene glycol and glycerol.

4. The method for preparing ferroferric oxide nanoparticles with controllable morphology and particle size according to claim 1, It is characterized in that In S1, the concentration of the iron salt after it is dissolved in the polyol is 50 w / v% to 100 w / v%.

5. The method for preparing ferroferric oxide nanoparticles with controllable morphology and particle size according to claim 1, It is characterized in that In S2, the structure directing agent is at least one of sodium citrate, anhydrous sodium acetate, urea, polyethyleneimine, potassium nitrate, polyethylene glycol, potassium permanganate, sodium hydroxide, ethylenediamine, and polyvinyl pyrrolidone; Optionally, the structure directing agent is added in an amount of 6 w / v% to 180 w / v%.

6. The method for preparing ferroferric oxide nanoparticles with controllable morphology and particle size according to claim 1, It is characterized in that In S3, the high temperature reaction is carried out at 180-220° C. for 8-24 hours.

7. The method for preparing ferroferric oxide nanoparticles with controllable morphology and particle size according to claim 1, It is characterized in that The morphology of the ferroferric oxide nanoparticles obtained in S3 is spherical, rod-shaped, polyhedral, hollow sphere, pine cone-shaped, honeycomb-shaped, and the ferroferric oxide particles have a size of 30 to 400 nm.

Citation Information

Patent Citations

  • Method for preparing ferroferric oxide magnetic nanospheres

    CN101767836A

  • Preparation method of ferroferric oxide magnetic carrier

    CN103318974A

  • Superparamagnetic response ferroferric oxide nano-particles and preparation and modification methods thereof

    CN113636601A

  • Metal oxide particles coated with polyethylene glycol and their synthesis

    US20120201760A1

  • KR20200045716A

Cited By

  • Magnetic nanoprobe with small size and high magnetic particle imaging performance as well as preparation method and application of magnetic nanoprobe

    CN120267859A

  • Magnetic nanoprobe with small size and high magnetic particle imaging performance, preparation method and application thereof

    CN120267859B