Zinc-containing sodium ion battery positive electrode material precursor and preparation method thereof

By using co-deposition method to add zinc salt to excessive alkaline solution to form metazinate in the positive electrode material of sodium ion battery, the problems of uneven distribution and low density of zinc are solved, and the cycle reversibility and discharge capacity of sodium ion battery are improved. , achieving efficient electrochemical performance.

CN119018945AActive Publication Date: 2024-11-26HENAN KELONG NEW ENERGY CO LTD

Patent Information

Application Number
CN202411482941.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-11-26
Estimated Expiration
2044-10-23

AI Technical Summary

Technical Problem

The tap density of existing sodium ion battery cathode materials is low, which affects its electrochemical performance. The zinc element is unevenly distributed in the traditional co-precipitation method, resulting in unstable crystal structure and affecting cyclic reversibility and discharge capacity.

Method used

Co-deposition method is adopted to add zinc salt to excessive alkaline solution to form metazinate salts to participate in co-deposition reactions, forming uniformly distributed zinc elements, improving crystallinity and tap density, and controlling reaction conditions through precision metering pumps to ensure uniform particles and high crystallinity.

Benefits of technology

The cycling reversibility and discharge capacity of sodium ion batteries are improved, ensuring the stability and efficient electrochemical performance of the cathode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018945A_ABST
    Figure CN119018945A_ABST
Patent Text Reader

Abstract

The invention discloses a precursor of a zinc-containing sodium ion positive electrode material and a preparation method thereof, zinc salt solution with certain concentration prepared in the prior art is replaced by adding zinc salt into excessive alkali liquor to form metazincate to participate in a co-deposition reaction, and the precursor prepared by the method is uniform in primary particle and relatively high in tap density; and the addition of the zinc element in the positive electrode material is beneficial for improving the crystallization degree of the positive electrode material, and zinc is a pricing element, can stabilize the crystal structure of an active substance during charging and discharging, and prevents the crystal structure from collapsing due to instability in the charging and discharging processes, so that the cyclic reversibility and the specific discharge capacity of the sodium-ion battery are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sodium ion battery positive electrode materials, and specifically relates to a zinc-containing sodium ion positive electrode material precursor and a preparation method thereof. Background Art

[0002] At present, the new energy battery industry is divided into lead-acid batteries, lithium iron phosphate batteries, lithium-ion batteries and sodium-ion batteries. Among them, lead-acid batteries are relatively environmentally unfriendly, lithium iron phosphate batteries are environmentally friendly but have poor low-temperature performance, lithium-ion batteries have environmental advantages over lithium iron phosphate batteries but have poor high and low temperature performance, and sodium-ion batteries also have relative advantages in environmental protection and high and low temperature performance. For current sodium-ion batteries, due to the large radius of Na ions and the slow transmission process, their capacity is relatively low. If the nickel content is increased to increase the capacity, the cost will increase.

[0003] The patent application with application publication number CN 117401726A discloses a zinc-doped sodium ion battery positive electrode material precursor and a preparation method thereof. The material is modified by adding zinc element, and the zinc-doped sodium ion battery positive electrode material precursor is prepared by coprecipitation method. The specific preparation steps are: step 1, preparing metal salt solution of Zn, Fe, Mn and Ni according to the stoichiometric ratio; step 2, preparing a mother liquor solution with a pH value of 10.5-10.8 and an ammonia concentration of 10±1g / L in a container; step 3, adding the metal salt solution, sodium hydroxide solution and ammonia solution to the container at different flow rates at the same time, and performing a coprecipitation reaction to obtain a coprecipitation product; step 4, filtering, washing and drying the coprecipitation product to obtain a zinc-doped sodium ion battery positive electrode material precursor, which can increase the contact area with the electrolyte, improve the sodium ion transmission efficiency, and thus improve the electrochemical performance. However, in this method, metal salt solutions of Zn, Fe, Mn, and Ni are used for coprecipitation reaction with sodium hydroxide solution and ammonia solution, and the tap density of the obtained precursor is 0.85~0.98g / cm 3 , its tap density still needs to be further improved to better meet the requirements of high electrochemical performance of sodium-ion batteries. Summary of the invention

[0004] The technical problem solved by the present invention is to provide a zinc-sodium ion positive electrode material precursor and a preparation method thereof. During the preparation process of the precursor, zinc element is doped by co-deposition, so that the zinc element can be evenly distributed. The difference between the present invention and the previous co-deposition is that during the co-deposition reaction process, the zinc salt solution of a certain concentration is replaced by adding zinc salt into excess alkali solution to form zincate to participate in the co-deposition reaction. The precursor prepared by this method has uniform primary particles and a high tap density. The addition of zinc element to the positive electrode material is beneficial to improving its crystallization degree, because zinc is a pricing element, which can stabilize the crystal structure of the active material during charging and discharging, and prevent the crystal structure from being unstable and collapsing during charging and discharging, thereby greatly improving the cycle reversibility and discharge specific capacity of the sodium ion battery.

[0005] The present invention adopts the following technical solution to solve the above technical problems, a method for preparing a positive electrode material precursor containing zinc and sodium ions, characterized in that the specific steps are: Step S1, preparing a nickel-manganese-iron mixed salt solution, wherein the nickel salt in the nickel-manganese-iron mixed salt solution is one or more of nickel sulfate, nickel nitrate or nickel chloride, the manganese salt is one or more of manganese sulfate, manganese nitrate or manganese chloride, and the ferrous salt is one or more of ferrous sulfate, ferrous nitrate or ferrous chloride; dissolving a zinc salt in an excess of alkali solution to prepare a zincate and alkali mixed solution, i.e., a zinc salt solution, wherein the zinc salt is one or more of zinc sulfate, zinc chloride or zinc nitrate, and the alkali solution is a sodium hydroxide solution or a potassium hydroxide solution; preparing a precipitant solution, wherein the precipitant in the precipitant solution is one or more of sodium hydroxide, potassium hydroxide or lithium hydroxide; preparing a complexing agent solution, wherein the complexing agent in the complexing agent solution is one or more of ammonia water or ammonium bicarbonate; Step S2, adding a mixed solution of a precipitant solution, a complexing agent solution and pure water to the reactor and continuously introducing a protective gas, and then respectively pumping a nickel-manganese-iron mixed salt solution, a zinc salt solution, a precipitant solution and a complexing agent solution into the reactor through a precision metering pump for co-precipitation reaction, and stopping the reaction when the particle size of the precipitated particles grows to 3-15 μm. During the entire reaction process, the reactor temperature is 30-80° C., the pH value is 9-13, the complexing agent content is 1-20 g / L, and the stirring speed is 200-1000 rpm. The reaction slurry obtained by the reaction is subjected to solid-liquid separation to obtain a dehydrated precursor material, and then the precursor material is dried at 80-150° C. to obtain Ni X Fe Y Mn 1-X-Y-Z Zn Z (OH)2 precursor.

[0006] It is further defined that the concentration of the nickel-manganese-iron mixed salt solution in step S1 is 1.0-2.5 mol / L; the concentration of zincate in the zinc salt solution is 0.1-0.5 mol / L; the concentration of the precipitant solution is 1-8 mol / L; and the concentration of the complexing agent solution is 1-10 mol / L.

[0007] The zinc-sodium ion positive electrode material precursor of the present invention has a molecular formula of Ni X Fe Y Mn 1-X-Y-Z Zn Z (OH)2, wherein 0<X<0.5, 0<Y<0.5, 0.01≤Z<0.2.

[0008] Compared with the prior art, the present invention has the following obvious beneficial effects: (1) The present invention adopts a co-precipitation method to add zinc element, so that the zinc element doping is more uniform. Zinc salt is added to an excess of sodium hydroxide solution and mixed to form sodium metazincate to participate in the co-precipitation reaction. The precursor prepared by this method has uniform primary particle distribution and high tap density.

[0009] (2) Ni prepared by the present invention X Fe Y Mn 1-X-Y-Z Zn Z The (OH)2 precursor has high crystallinity and stable crystal structure. The sodium ion positive electrode material prepared by sintering is not easy to collapse during the battery charging and discharging process. The prepared sodium ion battery has high capacity and good cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 This is a SEM image of the precursor prepared in Example 1; Figure 2 This is a SEM image of the precursor prepared in Example 2; Figure 3 This is a SEM image of the precursor prepared in Example 3; Figure 4 The discharge capacity comparison curves of sodium ion batteries assembled by sintering the precursors prepared in Example 1 and Comparative Examples 1-2 to prepare positive electrode materials. DETAILED DESCRIPTION

[0011] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention. Example 1

[0012] Step S1: preparing a nickel-manganese-iron mixed salt solution with a total metal concentration of 2.0 mol / L using nickel sulfate, manganese sulfate and ferrous sulfate, wherein the molar ratio of nickel, manganese and iron is 38.9:38.9:22.2; adding zinc sulfate to the prepared 6 mol / L sodium hydroxide solution to form a mixed solution of sodium metazincate and sodium hydroxide, wherein the specific preparation process is to add 120 g of zinc sulfate to 1 L, 6 mol / L sodium hydroxide solution; preparing a 4 mol / L ammonia solution as a complexing agent solution, and preparing a 6 mol / L sodium hydroxide solution as a precipitant solution; Step S2: Add 79L of pure water, 0.635L of complexing agent solution and 0.365L of precipitant solution to the reactor to prepare a base liquid with a total volume of 80L, adjust its pH value to 12.5-12.6, the ammonia content to 1-1.5g / L, and the temperature to 50°C. Turn on the stirring device, the stirring speed is 950r / min, and then continue to introduce nitrogen gas to the liquid surface of the reactor at a rate of 10L / min. The prepared nickel-manganese-iron mixed salt solution, sodium metazincate and sodium hydroxide mixed solution, complexing agent solution and precipitant solution are added to the reactor through 4 precision metering pumps for co-precipitation reaction. During the above reaction, the reaction temperature is 50°C, the pH value is controlled at 11.5-11.6, the flow rate of the nickel-manganese-iron mixed salt solution is 80 mL / min, the ammonia content is 5-6 g / L, and the particle size of the precipitated particles is grown to 4.5 μm before the reaction is stopped. The slurry obtained by the reaction is centrifuged for solid-liquid separation, and after separation, it is washed and dried to obtain Ni 0.35 Fe 0.20 Mn 0.35 Zn 0.10 (OH)2 precursor.

[0013] Test: The Ni 0.35 Fe 0.20 Mn 0.35 Zn 0.10 The (OH)2 precursor was tested by scanning electron microscopy. Figure 1 This is a scanning electron microscope image of the precursor prepared in this example. It can be seen from the figure that the prepared Ni 35 Fe 20 Mn 35 Zn 10 The (OH)2 precursor has good sphericity and uniform primary particles; the precursor D prepared in this embodiment was measured by Malvern particle size tester. 50 The surface area is 4.486 μm, and its specific surface area is 12.20 m 2 / g, and its tap density was measured to be 1.88g / cm 3 .

[0014] Comparative Example 1 Step S1: preparing a nickel-manganese-iron mixed salt solution with a total metal concentration of 2.0 mol / L using nickel sulfate, manganese sulfate and ferrous sulfate, wherein the molar ratio of nickel, manganese and iron is 38.9:38.9:22.2; preparing a 0.35 mol / L zinc sulfate solution, and then mixing the zinc sulfate solution with 9 mol / L ammonia water at a volume ratio of 1:0.27 to form a zinc ammonia complex solution, preparing a 4 mol / L ammonia solution as a complexing agent solution; and preparing a 6 mol / L sodium hydroxide solution as a precipitant solution.

[0015] Step S2: Add 79L of pure water, 0.635L of complexing agent solution and 0.365L of precipitant solution to the reactor to prepare a base solution with a total volume of 80L, adjust its pH value to 12.5-12.6, the ammonia content to 1-1.5g / L, and the temperature to 50°C. Turn on the stirring device, the stirring speed is 950r / min, and then continue to introduce nitrogen gas to the liquid surface of the reactor at a rate of 10L / min. The prepared nickel-manganese-iron mixed salt solution, zinc-ammonia complex solution, precipitant solution and complexing agent solution are added to the reactor through 4 precision metering pumps for co-precipitation reaction. During the above reaction, the reaction temperature was 50 °C, the pH value was controlled at 11.5-11.6, the flow rate of the nickel-manganese-iron mixed salt solution was 80 mL / min, the ammonia content was 5-6 g / L, and the reaction was stopped when the particle size of the precipitated particles grew to 4.5 μm. The slurry obtained by the reaction was centrifuged for solid-liquid separation, and the separated solid was washed and dried to obtain Ni 0.35 Fe 0.20 Mn 0.35 Zn 0.10 (OH)2 precursor.

[0016] Test: The Ni 0.35 Fe 0.20 Mn 0.35 Zn 0.10 The (OH)2 precursor was tested by scanning electron microscopy. Figure 2 The scanning electron microscope image of the precursor prepared in this comparative example; the particle size of the precursor D prepared in this example was measured by Malvern particle size tester. 50 The surface area is 4.636 μm, and its specific surface area is 17.22 m 2 / g, and its tap density was measured to be 1.58g / cm 3 .

[0017] Comparative Example 2 Step S1: preparing a nickel-manganese-iron-zinc mixed salt solution with a total metal concentration of 2.0 mol / L using nickel sulfate, manganese sulfate, ferrous sulfate and zinc sulfate, wherein the molar ratio of nickel, manganese, iron and zinc is 35 / 35 / 20 / 10; preparing a 4 mol / L ammonia solution as a complexing agent solution; preparing a 6 mol / L sodium hydroxide solution as a precipitant solution.

[0018] Step S2: Add 79L pure water, 0.635L complexing agent solution and 0.365L precipitant solution to the reactor to prepare a bottom liquid with a total volume of 80L, adjust its pH value to 12.5-12.6, ammonia content to 1-1.5g / L, and temperature to 50°C. Turn on the stirring device, the stirring speed is 950r / min, and then continue to introduce nitrogen at a rate of 10L / min below the liquid surface of the reactor. The prepared nickel-manganese-iron-zinc mixed salt solution, precipitant solution and complexing agent solution are added to the reactor through three precision metering pumps for coprecipitation reaction. During the above-mentioned entire reaction process, the reaction temperature is 50°C, the pH value is controlled at 11.5-11.6, the mixed liquid flow rate is 80mL / min, the ammonia content is 5-6g / L, the particle size of the precipitated particles is long to 4.5μm to stop the reaction, and the slurry obtained by the reaction is centrifuged for solid-liquid separation, and after separation, it is washed and dried to obtain Ni0. 35 Fe 0.20 Mn 0.35 Zn 0.10 (OH)2 precursor.

[0019] Test: The Ni 0.35 Fe 0.20 Mn 0.35 Zn 0.10 The (OH)2 precursor was tested by scanning electron microscopy. Figure 3 The scanning electron microscope image of the precursor prepared in this comparative example; the particle size of the precursor D prepared in this example was measured by Malvern particle size tester. 50 The surface area is 4.536 μm, and its specific surface area is 20.42 m 2 / g, and its tap density was measured to be 1.38g / cm 3 .

[0020] Figure 4 It is a discharge capacity comparison curve of the sodium ion battery assembled with the positive electrode material prepared by sintering the precursors obtained in Example 1 and Comparative Examples 1-2. It can be seen from the figure that the zinc doping process of Example 1 is compared with the zinc doping process of Comparative Examples 1-2. The cycle reversibility and discharge specific capacity of the sodium ion battery assembled with the positive electrode material prepared by sintering the precursor finally prepared by the present invention are greatly improved.

[0021] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.

Claims

1. A method for preparing a zinc-sodium ion positive electrode material precursor, characterized in that The specific steps are: Step S1, preparing a nickel-manganese-iron mixed salt solution, wherein the nickel salt in the nickel-manganese-iron mixed salt solution is one or more of nickel sulfate, nickel nitrate or nickel chloride, the manganese salt is one or more of manganese sulfate, manganese nitrate or manganese chloride, and the ferrous salt is one or more of ferrous sulfate, ferrous nitrate or ferrous chloride; dissolving a zinc salt in an excess of alkali solution to prepare a zincate and alkali mixed solution, i.e., a zinc salt solution, wherein the zinc salt is one or more of zinc sulfate, zinc chloride or zinc nitrate, and the alkali solution is a sodium hydroxide solution or a potassium hydroxide solution; preparing a precipitant solution, wherein the precipitant in the precipitant solution is one or more of sodium hydroxide, potassium hydroxide or lithium hydroxide; preparing a complexing agent solution, wherein the complexing agent in the complexing agent solution is one or more of ammonia water or ammonium bicarbonate; Step S2, adding a mixed solution of a precipitant solution, a complexing agent solution and pure water to the reactor and continuously introducing a protective gas, and then respectively pumping a nickel-manganese-iron mixed salt solution, a zinc salt solution, a precipitant solution and a complexing agent solution into the reactor through a precision metering pump for co-precipitation reaction, and stopping the reaction when the particle size of the precipitated particles grows to 3-15 μm. During the entire reaction process, the reactor temperature is 30-80° C., the pH value is 9-13, the complexing agent content is 1-20 g / L, and the stirring speed is 200-1000 rpm. The reaction slurry obtained by the reaction is subjected to solid-liquid separation to obtain a dehydrated precursor material, and then the precursor material is dried at 80-150° C. to obtain Ni X Fe Y Mn 1-X-Y-Z Zn Z (OH)2 precursor.

2. The method for preparing a zinc-sodium ion positive electrode material precursor according to claim 1, characterized in that: The concentration of the nickel-manganese-iron mixed salt solution in step S1 is 1.0-2.5 mol / L; the concentration of zincate in the zinc salt solution is 0.1-0.5 mol / L; the concentration of the precipitant solution is 1-8 mol / L; and the concentration of the complexing agent solution is 1-10 mol / L.

3. The zinc-sodium ion positive electrode material precursor prepared by the method according to claim 1 or 2, characterized in that: The molecular formula of the precursor is Ni X Fe Y Mn 1-X-Y-Z Zn Z (OH)2, wherein 0<X<0.5, 0<Y<0.5, 0.01≤Z<0.2.

Citation Information

Patent Citations

  • Modified sodium ion battery positive electrode precursor as well as preparation method and application thereof

    CN116102086A

  • Sodium ion positive electrode material precursor, preparation method and positive electrode material

    CN116621234A

  • Zinc-doped sodium ion battery positive electrode material precursor and preparation method thereof

    CN117401726A

  • Precursor with hollow structure, preparation method of precursor, positive electrode material, positive electrode and battery

    CN117602682A

  • Single-crystal positive electrode material of sodium ion battery and preparation method of single-crystal positive electrode material

    CN118272922A

Cited By

  • Preparation method of nickel-manganese-titanium-zinc sodium ion battery positive electrode material precursor

    CN119191389A