Gas ion implanted lithium-manganese-rich positive electrode material as well as preparation method and application thereof

By injecting oxygen negative ions and nitrogen negative ions into the lithium-rich manganese positive electrode material, the surface coated coating is formed, which solves the problems of uneven doping and easy coating falling off, and significantly improves the cycle stability and electrochemical performance of lithium batteries. .

CN119038624APending Publication Date: 2024-11-29XIAN TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410988458.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-29

Smart Images

  • Figure CN119038624A_ABST
    Figure CN119038624A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of lithium ion batteries, and particularly relates to a gas ion implanted lithium-manganese-rich positive electrode material as well as a preparation method and application thereof. The preparation method comprises the following steps: firstly, obtaining a uniformly mixed precursor solution according to an element ratio; performing high-temperature spray drying on the precursor solution to obtain precursor powder of the material; sintering the precursor powder at high temperature to obtain a lithium-manganese-rich positive electrode powder material; doping and replacing gas anions through gas ion injection, and adjusting process parameters and injection time; and finally, deflating and sampling the cavity to obtain the lithium-rich manganese-based positive electrode material injected with the gas ions. Gas elements such as oxygen negative ions and nitrogen negative ions are injected into the lithium-rich manganese-based positive electrode material through an ion implanter, the first-circle capacity of the battery under the voltage of 4.8 V reaches 263.85 mAh / g or above, the first-circle efficiency can reach 80.10%, the 100-circle circulation capacity retention rate reaches 90.01%, and the circulation stability is remarkably superior to that of a common lithium-rich manganese positive electrode material battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of lithium-ion batteries, and in particular relates to a gas ion-implanted lithium-manganese-rich positive electrode material, a preparation method and an application thereof. Background Art

[0002] Since the 1970s, the development and utilization of new energy has been highly valued by countries around the world. Many countries have made the development and utilization of new energy an important part of their energy strategy, put forward clear development goals, and formulated laws and policies to encourage the development of new energy. New energy has developed rapidly. The development of alternative energy, clean energy and eco-friendly energy with near zero emissions has become a top priority.

[0003] Rechargeable lithium-ion secondary batteries (LI Bs) have become one of the most popular energy storage systems today due to their good stability, high conversion efficiency, small size, and environmental protection. Lithium-ion batteries are mainly composed of positive electrodes, separators, electrolytes, and negative electrodes. As an important component of lithium batteries, the positive electrode material has a higher output voltage and specific capacity, which will lead to a higher energy density. The output voltage of the battery depends largely on the working potential of the positive electrode material, and the specific capacity of the electrode material is related to the number of transferred electrons per unit molecular mass. As the largest component in terms of weight and cost in LI Bs, the positive electrode material is still one of the main bottlenecks in achieving high performance of LI Bs.

[0004] With the continuous improvement of battery power density, the requirements for lithium battery capacity and cycle performance are becoming higher and higher. Ordinary lithium-rich manganese cathode materials can no longer meet commercial needs. A series of modification treatments are required to achieve improvements in the working voltage window, specific capacity, and cycle performance. Reducing the size of the cathode material can greatly improve its conductivity and obtain good electrochemical properties. The Li+ diffusion rate is greatly improved, but the size reduction will lead to lower material packing density and reaction between the electrode material and the electrolyte; ion doping and coating have gradually become the mainstream due to their low cost, simple process, and stable chemical properties. However, there are problems such as uneven doping and easy detachment of the coating layer. Although conventional ball milling and other process methods are simple, they cannot achieve the effect of uniform coating of the cathode material, resulting in limited improvement in battery performance.

[0005] Therefore, it is extremely important to adopt new preparation processes to achieve comprehensive modification of positive electrode materials. Summary of the invention

[0006] The present invention provides a gas ion implanted lithium-rich manganese-based positive electrode material, a preparation method and an application thereof, which solve the problems of uneven doping of the lithium-rich manganese-based positive electrode material, easy shedding of the coating layer and poor battery cycle stability.

[0007] To achieve the above object, the present invention provides the following technical solution: a method for preparing a gas ion-implanted lithium-rich manganese-based positive electrode material, comprising the following steps:

[0008] Step 1: Weigh a lithium source, a nickel source, a cobalt source, a manganese source, and a complexing agent according to the molar percentage of the elements Li:Ni:Co:Mn=1.53:0.165:0.165:0.665 and dissolve them in water to obtain a uniformly mixed precursor solution;

[0009] Step 2: obtaining a precursor powder of the material by high temperature spray drying the precursor solution;

[0010] Step 3: sintering the above-mentioned precursor powder at high temperature to obtain lithium-rich manganese positive electrode powder material;

[0011] Step 4: Place the weighed lithium-manganese-rich cathode powder material into the cavity of the gas ion implanter, connect the target gas, and turn on the mechanical pump and molecular pump to evacuate the cavity;

[0012] Step 5: Turn on the gas high-pressure chamber power supply to preheat, turn on the valve control, cleaning, air intake, purify the chamber, set the air intake volume to 1-5sccm, turn on the excitation power supply, set the current to 1-6mA, and set the voltage to 200-700V;

[0013] Step 6: Turn on the high voltage power supply, set the current to 1-6mA, set the voltage to 10-50kV, and start gas ion injection;

[0014] Step 7: After 0.5-8 hours, turn off the air intake, turn off the trigger power supply and power on, turn off the molecular pump and mechanical pump, and perform cavity venting sampling to obtain a lithium-rich manganese-based positive electrode material injected with gas ions.

[0015] Furthermore, in the above step 1, the lithium source, nickel source, cobalt source, and manganese source are selected from one or a combination of sulfate, nitrate, acetate, and oxalate; the complexing agent is any one of citric acid, ammonia water, carbonate, and bicarbonate, and the concentration of the precursor solution is 0.1 to 10 mol / L; the solubility of the complexing agent in the precursor solution is 0.05 to 5 mol / L.

[0016] Furthermore, in the above step 2, the inlet temperature of the spray drying is 150-280°C, the outlet temperature is 70-120°C, the peristaltic pump speed is 200-1000ml / h, the needle passing frequency is 5-30Hz, and the spray pressure is 0.1-0.5MPa; the atmosphere of the spray drying is one or more atmospheres of air and oxygen.

[0017] Furthermore, the specific operation of high temperature sintering in the above step three is: feeding the precursor powder into a muffle furnace, heating the temperature from room temperature to 600°C to 1200°C at a heating rate of 1°C / min to 10°C / min, keeping the temperature for 0.2 to 24 hours, and then cooling naturally.

[0018] Furthermore, the target gas connected in the above step four is one or a combination of nitrogen, oxygen, ammonia, hydrogen, carbon monoxide, carbon dioxide, sulfur dioxide, toluene, hydrogen sulfide, ethane, propane, ethylene, propylene, acetylene, propyne, chlorine, nitrogen oxides, hydrogen fluoride, sulfur dioxide, and sulfur trioxide.

[0019] Furthermore, in the above step 4, the target gas introduced is nitrogen or oxygen.

[0020] Furthermore, in step 4, the chamber is vacuumed to 1.5x10 -4 Pa.

[0021] Furthermore, the above preparation method produces a gas ion-implanted lithium-rich manganese-based positive electrode material.

[0022] Furthermore, in the application of the above-mentioned gas ion implantation lithium-rich manganese-based positive electrode material, the lithium-rich manganese-based positive electrode material is prepared as a lithium-rich manganese-based positive electrode sheet, the lithium-rich manganese-based positive electrode material, the conductive agent (SuperP) and the binder (sodium carboxymethyl cellulose CMC) are mixed into a slurry in a mass ratio of 85:10:5, and the slurry is coated on an aluminum foil current collector to obtain a positive electrode sheet to prepare a button battery.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. In the dynamic cycle process of lithium-rich manganese cathode materials, redox reactions occur continuously, and the precipitation of lattice oxygen, immersion in electrolyte, and transmission of ions cause the layered structure of the material to collapse, and the material cycle performance is greatly reduced. The present invention uses an ion implanter to inject gas elements such as oxygen anions and nitrogen anions into the lithium-rich manganese-based cathode material, and fills the oxygen vacancies through strong bonds with gas anions, thereby improving the stability of the lithium-rich manganese layered structure and forming a surface coating, thereby improving the cycle stability of the lithium-rich manganese-based cathode material.

[0025] 2. The present invention uses a high-pressure ion implanter to inject oxygen and nitrogen and other gas elements into the lithium-rich manganese-based positive electrode material. The introduction of nitrogen anions and oxygen anions can fill the unstable oxygen vacancy gaps in the material structure, while improving the stability of its internal structure and forming a surface coating, thereby achieving uniform doping of N and O elements, greatly improving the long-cycle performance, voltage and capacity attenuation problems of lithium batteries, and greatly improving the battery cycle stability performance.

[0026] 3. The lithium-rich manganese-based positive electrode material prepared by the present invention has a battery first-cycle capacity of more than 263.85 mAh / g at a voltage of 4.8 V, a first-cycle efficiency of 80.10%, and a 100-cycle cycle capacity retention rate of 90.01%. The cycle stability performance is significantly better than that of ordinary lithium-rich manganese positive electrode material batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 These are the X-ray diffraction data of the lithium-rich manganese material obtained in Example 1 after oxygen gas injection for 1.5 h.

[0028] Figure 2 This is a scanning electron microscope image of the lithium-rich manganese material obtained in Example 1 after oxygen gas injection for 1.5 hours.

[0029] Figure 3 The electrochemical performance data of the lithium-rich manganese material obtained in Example 1 after oxygen gas injection for 1.5 hours.

[0030] Figure 4 These are the X-ray diffraction data of the lithium-rich manganese material obtained in Example 2 after nitrogen gas injection for 1.5 h.

[0031] Figure 5 This is a scanning electron microscope image of the lithium-rich manganese material prepared in Example 2 after nitrogen gas injection for 1.5 hours.

[0032] Figure 6 The electrochemical performance data of the lithium-rich manganese material obtained in Example 2 after nitrogen gas injection for 1.5 hours.

[0033] Figure 7 These are the X-ray diffraction data of the lithium-rich manganese material obtained in Example 3 after oxygen gas injection for 2 hours.

[0034] Figure 8 This is a scanning electron microscope image of the lithium-rich manganese material obtained in Example 3 after oxygen gas injection for 2 hours.

[0035] Fig. 9 The electrochemical performance data of the lithium-rich manganese material obtained in Example 3 after oxygen gas injection for 2 hours.

[0036] Fig.10 These are the X-ray diffraction data of the lithium-rich manganese material obtained in Example 4 after nitrogen gas injection for 2 hours.

[0037] Fig.11 This is a scanning electron microscope image of the lithium-rich manganese material obtained in Example 4 after nitrogen gas injection for 2 hours.

[0038] Fig.12 The electrochemical performance data of the lithium-rich manganese material prepared in Example 4 after nitrogen gas injection for 2 hours.

[0039] Fig.13These are the X-ray diffraction data of the lithium-rich manganese material obtained in Example 5 after oxygen gas injection for 3 hours.

[0040] Fig.14 This is a scanning electron microscope image of the lithium-rich manganese material obtained in Example 5 after oxygen gas injection for 3 hours.

[0041] Fig.15 The electrochemical performance data of the lithium-rich manganese material obtained in Example 5 after oxygen gas injection for 3 hours.

[0042] Fig.16 These are the X-ray diffraction data of the lithium-rich manganese material obtained in Example 6 after nitrogen gas injection for 3 hours.

[0043] Fig.17 This is a scanning electron microscope image of the lithium-rich manganese material obtained in Example 6 after nitrogen gas injection for 3 hours.

[0044] Fig.18 The electrochemical performance data of the lithium-rich manganese material obtained in Example 6 after nitrogen gas injection for 3 hours.

[0045] Fig.19 This is the X-ray diffraction data of the standard lithium-rich manganese material prepared in Comparative Example 1.

[0046] Fig. 20 This is a scanning electron microscope image of the standard lithium-rich manganese material prepared in Comparative Example 1.

[0047] Fig.21 The electrochemical performance data of the standard lithium-rich manganese material prepared in Comparative Example 1. DETAILED DESCRIPTION

[0048] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0049] The present invention adopts lithium-manganese-rich positive electrode material with specific element composition, realizes doping substitution of gas anions through gas ion implantation technology, adjusts process parameters and implantation time, and realizes structural modification of the lithium-manganese-rich positive electrode material.

[0050] Embodiment 1, a method for preparing a gas ion implanted lithium-rich manganese positive electrode material, comprising the following steps:

[0051] Step 1: Synthesize 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33)O2 uses lithium acetate, nickel acetate, cobalt acetate, and manganese acetate, which are dissolved in deionized water in a stoichiometric ratio of 1.2:0.13:0.13:0.54 to prepare a 2 mol / L mixed salt solution, and 3 mol / L of chelating agent citric acid is added to the solution, and the solution is stirred on a magnetic stirrer for 1 hour to mix the solution evenly.

[0052] Step 2: Pump the mixed spray solution into the spray dryer, select an inlet air temperature of 230°C, an outlet air temperature of 115°C, a peristaltic pump speed of 600-800 ml / h, a needle passing frequency of 15 Hz, and a spray pressure of 0.2 MPa.

[0053] Step 3: Collect the precursor after spraying, place it in a corundum boat, send it into a crucible and calcine it in a muffle furnace at a heating rate of 3°C / min. After heating to 1000°C, keep the temperature for 20 minutes, and continuously introduce fresh air into the muffle furnace. After cooling in the furnace, lithium-rich manganese-based layered oxide (LNCM) is obtained.

[0054] Step 4: Weigh out 285 mg of lithium-rich manganese-based layered oxide (LNCM) and place it in the chamber of the high-pressure ion implanter. Connect oxygen and turn on the mechanical pump and molecular pump to evacuate the chamber to 1.5x10 -4 Pa.

[0055] Step 5. Turn on the gas high-pressure chamber power supply to preheat, turn on valve control, cleaning, air intake, purify the cavity, set the air intake volume to 1-5sccm, turn on the excitation power supply, set the current to 1-6mA, and set the voltage to 200-700V.

[0056] Step 6: Turn on the high-voltage power supply, set the current to 1-6mA, set the voltage to 10-50kV, set to the target voltage, and start ion implantation.

[0057] Step 7: After 1.5 hours, turn off the air intake, turn off the trigger power supply and power on, turn off the mechanical pump and molecular pump, and finally vent the cavity for sampling to obtain the O2 ion-implanted lithium manganese-rich positive electrode material, recorded as (1.5O2-LNCM).

[0058] Example 2

[0059] The preparation process of gas ion implantation is similar to that of Example 1, except that the synthetic material is 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33)O2 material was weighed and prepared into a spray solution according to the corresponding stoichiometric ratio, and the precursor was obtained after spray drying. The precursor was placed in an oxygen atmosphere, and the temperature was raised from room temperature to 1000 degrees Celsius at a rate of 3°C / min. After keeping the temperature for 20 minutes, it was cooled to room temperature with the furnace. 285 mg of lithium-rich manganese-based layered oxide (LNCM) was weighed and placed in a high-pressure ion implantation chamber, nitrogen was connected, and the mechanical pump and molecular pump were turned on to evacuate the chamber to 1.5x10 -4 Pa. Turn on the gas high-pressure chamber power supply to preheat, turn on valve control, cleaning, air intake, purify the cavity, set the air intake volume to 1-5sccm, turn on the excitation power supply, set the current to 1-6mA, and set the voltage to 200-700V. Turn on the high-voltage power supply, set the current to 1-6mA, set the voltage to 10-50kV, set to the target voltage, and start the ion implantation experiment. The gas injection time is 1.5 hours. Turn off the air intake, turn off the trigger power supply and power on, turn off the mechanical pump and molecular pump, and finally vent the cavity for sampling to obtain the N2 ion-implanted lithium-rich manganese-based positive electrode material, recorded as (1.5N2-LNCM).

[0060] Example 3

[0061] The preparation process of gas ion implantation is similar to that of Example 1, except that the synthetic material is 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 material was weighed and prepared into a spray solution according to the corresponding stoichiometric ratio, and the precursor was obtained after spray drying. The precursor was placed in an oxygen atmosphere, and the temperature was raised from room temperature to 1000 degrees Celsius at a rate of 3°C / min. After keeping the temperature for 20 minutes, it was cooled to room temperature with the furnace. 285 mg of lithium-rich manganese-based layered oxide (LNCM) was weighed and placed in a high-pressure ion implantation chamber, nitrogen was connected, and the mechanical pump and molecular pump were turned on to evacuate the chamber to 1.5x10 -4 Pa. Turn on the gas high-pressure chamber power supply to preheat, turn on valve control, cleaning, air intake, purify the cavity, set the air intake volume to 1-5sccm, turn on the excitation power supply, set the current to 1-6mA, and set the voltage to 200-700V. Power on the high-voltage power supply, set the current to 1-6mA, set the voltage to 10-50kV, set to the target voltage, and start the ion implantation experiment. The gas injection time is 2 hours. Turn off the air intake, turn off the trigger power supply and power on, turn off the mechanical pump and molecular pump, and finally vent the cavity for sampling to obtain the O2 ion-implanted lithium-rich manganese-based positive electrode material, recorded as (2O2-LNCM).

[0062] Example 4

[0063] The preparation process of gas ion implantation is similar to that of Example 1, except that the synthetic material is 0.5Li2MnO3·0.5Li(Ni 0.33Co 0.33 Mn 0.33 )O2 material was weighed and prepared into a spray solution according to the corresponding stoichiometric ratio, and the precursor was obtained after spray drying. The precursor was placed in an oxygen atmosphere, and the temperature was raised from room temperature to 1000 degrees Celsius at a rate of 3°C / min. After keeping the temperature for 20 minutes, it was cooled to room temperature with the furnace. 285 mg of lithium-rich manganese-based layered oxide (LNCM) was weighed and placed in a high-pressure ion implantation chamber, nitrogen was connected, and the mechanical pump and molecular pump were turned on to evacuate the chamber to 1.5x10 -4 Pa. Turn on the gas high-pressure chamber power supply to preheat, turn on valve control, cleaning, air intake, purify the cavity, set the air intake volume to 1-5sccm, turn on the excitation power supply, set the current to 1-6mA, and set the voltage to 200-700V. Turn on the high-voltage power supply, set the current to 1-6mA, set the voltage to 10-50kV, set to the target voltage, and start the ion implantation experiment. The gas injection time is 2 hours. Turn off the air intake, turn off the trigger power supply and power on, turn off the mechanical pump and molecular pump, and finally vent the cavity for sampling to obtain the N2 ion-implanted lithium-rich manganese-based positive electrode material, recorded as (2N2-LNCM).

[0064] Example 5

[0065] The preparation process of gas ion implantation is similar to that of Example 1, except that the synthetic material is 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 material was weighed and prepared into a spray solution according to the corresponding stoichiometric ratio, and the precursor was obtained after spray drying. The precursor was placed in an oxygen atmosphere, and the temperature was raised from room temperature to 1000 degrees Celsius at a rate of 3°C / min. After keeping the temperature for 20 minutes, it was cooled to room temperature with the furnace. 285 mg of lithium-rich manganese-based layered oxide (LNCM) was weighed and placed in a high-pressure ion implantation chamber, nitrogen was connected, and the mechanical pump and molecular pump were turned on to evacuate the chamber to 1.5x10 -4 Pa. Turn on the gas high-pressure chamber power supply to preheat, turn on valve control, cleaning, air intake, purify the cavity, set the air intake volume to 1-5sccm, turn on the excitation power supply, set the current to 1-6mA, and set the voltage to 200-700V. Turn on the high-voltage power supply, set the current to 1-6mA, set the voltage to 10-50kV, set to the target voltage, and start the ion implantation experiment. The gas injection time is 3 hours. Turn off the air intake, turn off the trigger power supply and power on, turn off the mechanical pump and molecular pump, and finally vent the cavity for sampling to obtain the O2 ion-implanted lithium-rich manganese-based positive electrode material, recorded as (3O2-LNCM).

[0066] Example 6

[0067] The preparation process of gas ion implantation is similar to that of Example 1, except that the synthetic material is 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 material was weighed and prepared into a spray solution according to the corresponding stoichiometric ratio, and the precursor was obtained after spray drying. The precursor was placed in an oxygen atmosphere, and the temperature was raised from room temperature to 1000 degrees Celsius at a rate of 3°C / min. After keeping the temperature for 20 minutes, it was cooled to room temperature with the furnace. 285 mg of lithium-rich manganese-based layered oxide (LNCM) was weighed and placed in a high-pressure ion implantation chamber, nitrogen was connected, and the mechanical pump and molecular pump were turned on to evacuate the chamber to 1.5x10 -4 Pa. Turn on the gas high-pressure chamber power supply to preheat, turn on valve control, cleaning, air intake, purify the cavity, set the air intake volume to 1-5sccm, turn on the excitation power supply, set the current to 1-6mA, and set the voltage to 200-700V. Turn on the high-voltage power supply, set the current to 1-6mA, set the voltage to 10-50kV, set to the target voltage, and start the ion implantation experiment. The gas injection time is 3 hours. Turn off the air intake, turn off the trigger power supply and power on, turn off the mechanical pump and molecular pump, and finally vent the cavity for sampling to obtain the N2 ion-implanted lithium-rich manganese-based positive electrode material, recorded as (3N2-LNCM).

[0068] Comparative Example

[0069] Select the basic 0.5Li2MnO3·0.5Li(Ni 0.33 Co 0.33 Mn 0.33 )O2 layered lithium-rich manganese-based positive electrode material was experimented, similar to Example 1, the temperature was increased from room temperature to 500°C at a rate of 5°C / min, and then the temperature was increased to 800°C at a rate of 5°C / min after maintaining the temperature for 3 hours. After maintaining the temperature for 10 hours, it was naturally cooled to room temperature. The ratio of lithium acetate: nickel acetate: cobalt acetate: manganese acetate was 1.2:0.13:0.13:0.54, and a 2 mol / L mixed metal salt solution was prepared. Granulation was performed by spray drying to prepare a precursor of the layered lithium-rich manganese-based positive electrode material.

[0070] The precursor was placed in a muffle furnace with air for sintering, and the temperature was increased from room temperature to 1000°C at a heating rate of 5°C / min and kept constant for 20 minutes, and then naturally cooled to room temperature.

[0071] Test analysis:

[0072] The lithium-rich manganese positive electrode material, conductive agent (SuperP), and binder (sodium carboxymethyl cellulose CMC) obtained in Examples 1-6 and the comparative example are mixed into a slurry in a mass ratio of 85:10:5. The stirring rate is 500 rad / min. After stirring evenly, a scraper is used to coat the slurry on an aluminum foil current collector to obtain a positive electrode sheet. The scraper thickness is 0.2 mm. The vacuum oven temperature is 110°C and the time is 20 h to obtain a lithium-rich manganese-based positive electrode sheet.

[0073] The lithium-rich manganese-based positive electrode sheets were cut into round pieces of uniform size, dried, and assembled into 2025 button batteries in a glove box filled with argon gas with oxygen and water content less than 0.01ppm. The button batteries were placed in an oven for long-term activation treatment at a temperature of 45°C and a treatment time of 40h. After being taken out, the battery cycle performance test was carried out at different current densities.

[0074] Electrochemical performance The charge and discharge test of 2025 button cell was carried out on the Xinwei test system, with metal Li sheet as reference electrode and counter electrode, Celgard-2400 as diaphragm, Xinzhoubang 3045I as electrolyte, and the test voltage window was 2.0~4.8V. The test temperature was 27±1℃, and the activation rate was 0.1C (1C=200mAh / g) for the first three cycles, and the 1C rate cycle was used from the 4th cycle. The performance test results are shown in Table 1.

[0075] Table 1

[0076] First discharge capacity (mAh / g) 100 cycles capacity retention rate (%) Example 1 259.94 89.41 Example 2 250.94 86.15 Example 3 263.85 90.01 Example 4 256.97 87.12 Example 5 254.81 89.66 Example 6 242.30 89.36 Comparative Example 1 214.07 72.68

[0077] As can be seen from Table 1, the battery prepared by the lithium-rich manganese-based positive electrode material of the present invention with oxygen ion implantation for 2h has the best electrochemical performance, the first discharge capacity can reach 263.85mAh / g, and the capacity retention rate after 100 cycles reaches more than 90.01%.

[0078] See also Figure 3 , 6 , 9, 12, 15, 18 and 21:

[0079] (1) By comparing Examples 1 and 2, Examples 3 and 4, and Examples 5 and 6, it can be seen that in the process of preparing the lithium-rich manganese-based positive electrode material by gas ion injection of the present invention, under the same injection time conditions, the first cycle charge and discharge capacity and 100 cycle capacity retention rate of the battery prepared by the lithium-rich manganese-based positive electrode material injected with O2 gas are higher than those of the battery prepared by the lithium-rich manganese-based positive electrode material injected with N2 gas.

[0080] (2) By comparing Examples 1, 3 and 5, and 2, 4 and 6, it can be seen that in the process of preparing the lithium-rich manganese-based positive electrode material by gas ion injection of the invention, under the same gas conditions, as the gas ion injection time increases, the battery capacity and capacity retention rate of the lithium-rich manganese-based positive electrode material prepared therefrom first increase and then decrease. The battery performance of the material with a gas injection time of 2h is better than that of the lithium-rich manganese-based positive electrode material battery with a gas injection time of 1.5h, and the battery performance of the lithium-rich manganese-based positive electrode material battery with a gas injection time of 3h is lower than that of the material battery with a gas injection time of 2h.

[0081] See also Figure 1 , 7 , 13 and 19: From the comparison between Examples 1, 3, 5 and Comparative Example 1, it can be seen that the injection of O2 gas ions into the lithium-rich manganese-based positive electrode material described in the present invention improves the structural stability and electrochemical properties of the lithium-rich layered oxide thereof.

[0082] See also Figure 4 , 9 , 13 and 19: From the comparison of Examples 2, 4, 6 and Comparative Example 1, it can be seen that the injection of N2 gas ions into the lithium-rich manganese-based positive electrode material described in the present invention improves the structural stability of its lithium-rich layered oxide and enhances the first-cycle capacity and capacity retention rate of the battery.

[0083] See also Figure 2 , 5 , 8, 11, 14, 17 and 20: By comparison of Examples 1, 2, 3, 4, 5, 6 and Comparative Example 1, it can be seen that the gas ion-injected lithium-manganese-rich positive electrode material particles are evenly distributed, there is no irregular morphology on the surface, and the gas ions are evenly injected into the material structure.

[0084] In summary, embodiment 3 is the best embodiment.

[0085] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a gas ion-implanted lithium-rich manganese-based positive electrode material, characterized in that: The following steps are involved: Step 1: Weigh a lithium source, a nickel source, a cobalt source, a manganese source, and a complexing agent according to the molar percentage of the elements Li:Ni:Co:Mn=1.53:0.165:0.165:0.665 and dissolve them in water to obtain a uniformly mixed precursor solution; Step 2: obtaining a precursor powder of the material by high temperature spray drying the precursor solution; Step 3: sintering the above-mentioned precursor powder at high temperature to obtain lithium-rich manganese positive electrode powder material; Step 4: Place the weighed lithium-manganese-rich cathode powder material into the cavity of the gas ion implanter, connect the target gas, and turn on the mechanical pump and molecular pump to evacuate the cavity; Step 5: Turn on the gas high-pressure chamber power supply to preheat, turn on the valve control, cleaning, air intake, purify the chamber, set the air intake volume to 1-5sccm, turn on the excitation power supply, set the current to 1-6mA, and set the voltage to 200-700V; Step 6: Turn on the high voltage power supply, set the current to 1-6mA, set the voltage to 10-50kV, and start gas ion injection; Step 7: After 0.5-8 hours, turn off the air intake, turn off the trigger power supply and power on, turn off the molecular pump and mechanical pump, and perform cavity venting sampling to obtain a lithium-rich manganese-based positive electrode material injected with gas ions.

2. The method for preparing a gas ion implanted lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In the step 1, the lithium source, nickel source, cobalt source and manganese source are selected from one or a combination of sulfate, nitrate, acetate and oxalate; the complexing agent is any one of citric acid, ammonia water, carbonate and bicarbonate; the concentration of the precursor solution is 0.1-10 mol / L; and the solubility of the complexing agent in the precursor solution is 0.05-5 mol / L.

3. The method for preparing a gas ion implanted lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In the step 2, the inlet temperature of the spray drying is 150-280°C, the outlet temperature is 70-120°C, the peristaltic pump speed is 200-1000ml / h, the needle passing frequency is 5-30Hz, and the spray pressure is 0.1-0.5MPa; the atmosphere of the spray drying is one or more atmospheres of air and oxygen.

4. The method for preparing a gas ion implanted lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The specific operation of high temperature sintering in step three is: feeding the precursor powder into a muffle furnace, heating the temperature from room temperature to 600°C~1200°C at a heating rate of 1°C / min~10°C / min, keeping the temperature for 0.2~24 hours, and then cooling naturally.

5. The method for preparing a gas ion implanted lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The target gas connected in step 4 is one or a combination of nitrogen, oxygen, ammonia, hydrogen, carbon monoxide, carbon dioxide, sulfur dioxide, toluene, hydrogen sulfide, ethane, propane, ethylene, propylene, acetylene, propyne, chlorine, nitrogen oxides, hydrogen fluoride, sulfur dioxide, and sulfur trioxide.

6. The method for preparing a gas ion implanted lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In the step 4, the target gas connected is nitrogen or oxygen.

7. The method for preparing a gas ion implanted lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: In step 4, the chamber is vacuumed to 1.5x10 -4 Pa.

8. A gas ion implanted lithium-rich manganese-based positive electrode material prepared by the preparation method according to claim 1.

9. The use of a gas ion implanted lithium-rich manganese-based positive electrode material according to claim 1, characterized in that: The lithium-rich manganese-based positive electrode material is prepared as a lithium-rich manganese-based positive electrode sheet. The lithium-rich manganese-based positive electrode material, a conductive agent (SuperP) and a binder (sodium carboxymethyl cellulose CMC) are mixed into a slurry at a mass ratio of 85:10:5, and the slurry is coated on an aluminum foil current collector to obtain a positive electrode sheet, thereby preparing a button battery.