Preparation method of single crystal glass ceramic and single crystal glass ceramic
The single-crystal β-CaSiO3 ceramic is formed through high-temperature pulse treatment, which solves the problem of contradiction between dielectric performance and mechanical properties of LTCC substrates, improves the dielectric constant and bending strength, and is suitable for high-frequency communication technology.
Patent Information
- Application Number
- CN202411133147.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-16
AI Technical Summary
The existing LTCC substrates with low dielectric constant are insufficient in high-frequency communication technology, and the sintering temperature limit is less than 900°C, making it difficult to meet the requirements of dielectric and mechanical properties at the same time.
The glass powder is processed by high-temperature pulse treatment. Through multi-stage heating, cooling and insulation, the temperature is maintained between 780 and 880℃, and a single-crystal β-CaSiO3 ceramic is formed to improve the dielectric constant, reduce dielectric loss and enhance resistance. Bending strength.
The balance of dielectric constant and dielectric loss of LTCC substrate is achieved, and the bending strength is significantly improved. It is suitable for the miniaturization and integrated environment of high-frequency communication technology.
Smart Images

Figure CN119019085A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of low-temperature co-fired ceramics, and in particular relates to a preparation method of single-crystal glass ceramics and a single-crystal glass ceramic. Background Art
[0002] Low Temperature Co-fired Ceramic (LTCC) technology is widely used in various electronic components due to its advantages of miniaturization, integration, and low cost. With the rapid development of high-frequency communication technology, the requirements for the comprehensive performance of LTCC materials are constantly increasing, and the contradictory relationship between the various properties of LTCC has become increasingly prominent.
[0003] The dielectric constant (K value) of existing low-dielectric-constant LTCC substrates is usually in the range of 5 to 8. Due to the low relative dielectric constant of air (approximately equal to 1), some existing LTCC substrates also use inorganic porous materials to reduce the dielectric properties of LTCC substrate materials. However, the large number of voids in the inorganic porous materials will inevitably lead to a decrease in the mechanical strength of the formed LTCC substrate and a rapid increase in dielectric loss. In the context of miniaturization and integration of high-frequency communication technology, LTCC substrates need to have certain bending and compression resistance to face high-load packaging environments. In addition, since the melting point of silver (Ag) is 961°C, the densification temperature of LTCC substrates is usually less than 900°C.
[0004] In the microcrystalline glass system, a combination of multiple glasses can usually be used to coordinate the comprehensive performance of LTCC materials, but how to adjust the sintering process parameters to meet the appropriate sintering temperature, low dielectric constant, low dielectric loss and high bending strength required for the LTCC substrate is still a problem that needs to be solved urgently in this field.
[0005] In order to overcome the above-mentioned defects of the prior art, the art is in urgent need of a method for preparing a single crystal glass ceramic and a single crystal glass ceramic that can balance and improve the dielectric constant, dielectric loss and bending strength of the LTCC substrate material. Summary of the invention
[0006] A brief summary of one or more aspects is given below to provide a basic understanding of these aspects. This summary is not an exhaustive overview of all conceived aspects, and is neither intended to identify the key or critical elements of all aspects nor to define the scope of any or all aspects. Its only purpose is to give some concepts of one or more aspects in a simplified form as a prelude to a more detailed description that will be given later.
[0007] In order to overcome the above-mentioned defects in the prior art, the present invention provides a method for preparing a single crystal glass ceramic and a single crystal glass ceramic, which can balance and improve the dielectric constant, dielectric loss and bending strength of the LTCC substrate material.
[0008] Specifically, the preparation method of the above-mentioned single crystal glass ceramics provided in accordance with the first aspect of the present invention comprises the steps of: preparing raw materials and processing the raw materials to obtain glass powder; and processing the glass powder by a high temperature pulse method to obtain single crystal glass ceramics after cooling, wherein the high temperature pulse method is achieved through multiple stages of heating, cooling and / or heat preservation, and the temperature of the high temperature pulse method is maintained between 780 and 880°C.
[0009] Preferably, in one embodiment of the present invention, the multiple stages of the high temperature pulse method include a first stage, a second stage, a third stage and / or a fourth stage, and the second stage and the third stage are repeated cycles of heating, cooling and / or keeping warm.
[0010] Preferably, in one embodiment of the present invention, the first stage includes a staged cooling process, and the first stage includes the steps of: heating to 780-820°C at a heating rate of 3-5°C / min, and keeping warm for 30-120 minutes; heating to 850-880°C at a heating rate of 1-2°C / min, and then cooling to 820-840°C at a cooling rate of 1-2°C / min; and changing the cooling rate, cooling to 780-800°C at a cooling rate of 0.5-2°C / min, and keeping warm for 60 minutes.
[0011] Preferably, in one embodiment of the present invention, after the first stage is completed, the high temperature pulse method performs the second stage of repeated cycles, the number of repeated cycles of the second stage is 2 to 8 times, and the second stage includes a staged cooling process, and the second stage includes the steps of: heating to 850 to 880°C at a heating rate of 1 to 2°C / min, and keeping warm for 30 to 120 minutes; cooling to 820 to 840°C at a cooling rate of 1 to 2°C / min; and changing the cooling rate, cooling to 780 to 800°C at a cooling rate of 0.5 to 2°C / min, and keeping warm for 30 to 120 minutes.
[0012] Preferably, in one embodiment of the present invention, after the second stage is completed, the high temperature pulse method performs the third stage of repeated cycles, and the number of repeated cycles of the third stage is 2 to 8 times, including the steps of: heating to 850 to 870°C at a heating rate of 1 to 3°C / min, and keeping warm for 30 to 120 minutes; and cooling to 780 to 800°C at a cooling rate of 0.5 to 2°C / min, and keeping warm for 30 to 120 minutes.
[0013] Preferably, in one embodiment of the present invention, after the third stage is completed, the high temperature pulse method performs the fourth stage, and the fourth stage includes the steps of heating to 850-880°C at a heating rate of 1-2°C / min and keeping warm for 60-380 minutes.
[0014] Preferably, in one embodiment of the present invention, the step of preparing raw materials and processing the raw materials to obtain glass powder includes: weighing the raw materials and mixing them thoroughly, melting the mixed raw materials at 1300-1500°C for 1-3 hours to obtain molten glass; rapidly cooling the molten glass by a cooling rolling mill to obtain glass sheets; placing the glass sheets in a grinder for preliminary crushing to obtain glass particles; and passing the glass particles through an air flow mill in combination with an air flow classifier to form the glass powder.
[0015] Preferably, in an embodiment of the present invention, the glass particles have a particle size ranging from 0.5 to 2.0 mm.
[0016] Preferably, in an embodiment of the present invention, the preset particle size range of the glass powder is 3.0-4.0 μm.
[0017] Preferably, in one embodiment of the present invention, the glass powder includes 40.4-47.2 mol% of CaO, 10-17 mol% of B2O3, 36-42 mol% of SiO2 and 0-5.34 mol% of Al2O3.
[0018] In addition, the single crystal glass ceramic provided according to the second aspect of the present invention is manufactured by the method for manufacturing the single crystal glass ceramic provided according to the first aspect of the present invention.
[0019] Preferably, in one embodiment of the present invention, the main crystal phase of the single crystal glass ceramic is single crystal β-CaSiO3. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The above features and advantages of the present invention can be better understood after reading the detailed description of the embodiments of the present disclosure in conjunction with the following drawings. In the drawings, the components are not necessarily drawn to scale, and components with similar related properties or features may have the same or similar reference numerals.
[0021] Figure 1 A flow chart showing a method for preparing single crystal glass ceramics according to some embodiments of the present invention is shown;
[0022] Figure 2 Shows a microscopic morphology of single crystal glass ceramics provided according to some embodiments of the present invention;
[0023] Figure 3The performance test results of various glass ceramics provided according to multiple embodiments of the present invention and multiple comparative examples are shown;
[0024] Figure 4 The bending strength results of various glass ceramics provided according to various embodiments of the present invention and various comparative examples are shown; and
[0025] Figure 5 A comparison chart of the XRD spectra of the glass ceramics provided in Example 1 of the present invention and Comparative Example 1 is shown.
[0026] Reference numerals:
[0027] 100: Preparation method of single crystal glass ceramics;
[0028] S110-S120: steps; and
[0029] 501, 502: lines. DETAILED DESCRIPTION
[0030] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. Note that the aspects described below in conjunction with the accompanying drawings and specific embodiments are only exemplary and should not be construed as limiting the scope of protection of the present invention in any way.
[0031] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0032] In addition, the terms "upper", "lower", "left", "right", "top", "bottom", "horizontal" and "vertical" used in the following description should be understood as the directions shown in the paragraph and the related drawings. Such relative terms are only used for the convenience of description and do not mean that the device described therein must be manufactured or operated in a specific direction, and therefore should not be understood as limiting the present invention.
[0033] It is understood that although the terms "first", "second", "third", etc. may be used herein to describe various components, regions, layers and / or parts, these components, regions, layers and / or parts should not be limited by these terms, and these terms are only used to distinguish different components, regions, layers and / or parts. Therefore, the first component, region, layer and / or part discussed below may be referred to as a second component, region, layer and / or part without departing from some embodiments of the present invention.
[0034] As mentioned above, in the context of miniaturization and integration of high-frequency communication technology, the requirements for the comprehensive performance of LTCC materials are constantly increasing, and the contradictory relationship between the various properties of LTCC has become increasingly prominent. At present, the existing LTCC substrate materials are mainly microcrystalline glass systems and glass / ceramic composite systems. Under the microcrystalline glass system, a variety of glasses can usually be used to coordinate the comprehensive performance of LTCC materials, but how to adjust the sintering process parameters to meet the appropriate sintering temperature, low dielectric constant, low dielectric loss and high bending strength required by the LTCC substrate is still a problem to be solved in this field.
[0035] In order to overcome the above-mentioned defects in the prior art, the present invention provides a method for preparing a single crystal glass ceramic and a single crystal glass ceramic, which can balance and improve the dielectric constant, dielectric loss and bending strength of the LTCC substrate material.
[0036] The above-mentioned single crystal glass ceramics will be described below in conjunction with some examples of methods for preparing single crystal glass ceramics. Those skilled in the art will understand that these examples of methods for preparing single crystal glass ceramics are only some non-limiting implementation methods provided by the present invention, and are intended to clearly demonstrate the main concept of the present invention and provide some specific solutions that are convenient for the public to implement, and do not limit the execution subject and execution order of each step in the method for preparing single crystal glass ceramics.
[0037] Please refer to Figure 1 , Figure 1 A flow chart of a method for preparing single crystal glass ceramics provided according to some embodiments of the present invention is shown.
[0038] like Figure 1 As shown, the method 100 for preparing single crystal glass ceramics may include step S110: preparing raw materials and processing the raw materials to obtain glass powder.
[0039] The preparation method 100 of single crystal glass ceramics can be applied to all microcrystalline glass formulas. Here, the preparation method 100 of single crystal glass ceramics is described in detail by taking a glass powder with a formula of 40.4-47.2 mol% CaO, 10-17 mol% B2O3, 36-42 mol% SiO2 and 0-5.34 mol% Al2O3 as an example.
[0040] In a preferred embodiment, the raw materials include SiO2, H3BO3, CaCO3, and Al(OH)3 weighed in a stoichiometric ratio. SiO2 can use AR (Analytical Reagent) grade silicon oxide as a raw material, B2O3 can use electronic grade boric acid as a raw material, CaO can use calcium carbonate as a raw material, and Al2O3 can use aluminum hydroxide as a raw material.
[0041] After weighing the raw materials according to the stoichiometric ratio, the raw materials can be fully mixed using a mixer. In order to make the raw materials mixed more evenly, zirconium beads (i.e., grinding bodies) can be loaded into the mixing tank at a 1:1 ball-to-material ratio (ratio of material to grinding body mass) for mixing, and the mixing time is 2 hours.
[0042] Afterwards, the mixed raw materials are melted, and the melted glass liquid is poured into a cooling mill for rapid cooling to obtain a glass sheet. The mixed raw materials can be melted at 1300-1500°C for 1-3 hours. Specifically, in order to prevent contamination by other elements, a platinum crucible can be used during the melting process. In addition, in order to prevent excessive volatilization of the boron element, a pressed cake batch feeding process can also be used for melting. The melted glass liquid is poured into a cooling mill for rapid cooling, thereby rapidly cooling the glass liquid into a glass sheet. Here, the cooling mill can be a double-roll cooling mill.
[0043] Then, the glass flakes are put into a grinder for preliminary crushing to obtain glass particles. In one embodiment, the glass flakes can be initially crushed into glass particles with a particle size range of about 0.5 to 2.0 mm by a three-cylinder grinder. Here, the glass particles are calcium borosilicate (CBS) glass particles. The glass particles are passed through an air flow mill in conjunction with an air flow classifier to obtain a glass powder within a preset particle size distribution range. The preset particle size distribution range of the glass powder can be 3.0 to 4.0 μm.
[0044] Thus, a glass powder including 40.4 to 47.2 mol% of CaO, 10 to 17 mol% of B2O3, 36 to 42 mol% of SiO2 and 0 to 5.34 mol% of Al2O3 can be obtained.
[0045] Please continue to refer to Figure 1 The preparation method 100 of single crystal glass ceramics may further include step S120: treating the glass powder by a high temperature pulse method, and obtaining single crystal glass ceramics after cooling, wherein the high temperature pulse method is achieved by multi-stage heating, cooling and / or heat preservation, and the temperature of the high temperature pulse method is maintained between 780 and 880°C.
[0046] Preferably, the multi-stage high temperature pulse method may include a first stage, a second stage, a third stage and / or a fourth stage, wherein the second stage and the third stage are repeated cycles of heating, cooling and / or heat preservation processes.
[0047] Before the formation of a stable phase, microcrystalline glass will preferentially generate a metastable phase with an intermediate state to ensure the transition of energy. Here, the high-temperature pulse method provided by the method 100 for preparing single crystal glass ceramics can transform the metastable phase into a stable phase single crystal by adjusting the sintering process and utilizing the abnormal grain growth (AGG, Abnormal Grain Growth) mechanism, thereby realizing the single crystalization of glass ceramics. Specifically, through high and low temperature pulse cycles, the method 100 for preparing single crystal glass ceramics can accelerate the speed at which large grains of β-CaSiO3 devour small grains of α-CaSiO3, and convert them into single crystals of β-CaSiO3 at a lower temperature, thereby forming glass ceramics with only a single target crystal phase of β-CaSiO3, thereby improving the mechanical strength of single crystal glass ceramics.
[0048] In a preferred embodiment, the high temperature pulse method may include a first stage, which includes staged cooling. In the first stage, the high temperature pulse method treats the glass powder at a heating rate of 3 to 5°C / min, heats to 780 to 820°C and then keeps the temperature for 30 to 120 minutes. Then heat to 850 to 880°C at a heating rate of 1 to 2°C / min. After that, cool to 820 to 840°C at a cooling rate of 1 to 2°C / min, then change the cooling rate, cool to 780 to 800°C at a cooling rate of 0.5 to 2°C / min, and keep the temperature for 60 minutes.
[0049] The high temperature pulse method also includes a second stage after the first stage. The second stage includes cooling in stages. The second stage can be repeated in a cycle, and preferably, the number of repeated cycles of the second stage can be 2 to 8 times. Specifically, the second stage includes the steps of heating to 850 to 880°C at a heating rate of 1 to 2°C / min and keeping warm for 30 to 120 minutes. Thereafter, cooling to 820 to 840°C at a cooling rate of 1 to 2°C / min, and then changing the cooling rate to cool to 780 to 800°C at a cooling rate of 0.5 to 2°C / min, and keeping warm for 30 to 120 minutes.
[0050] After the second stage, the high temperature pulse method can perform a third stage of repeated cycles. Preferably, the number of repeated cycles of the third stage can be 2 to 8 times. The third stage includes: heating to 850 to 870°C at a heating rate of 1 to 3°C / min and keeping warm for 30 to 120 minutes. Then, cooling to 780 to 800°C at a cooling rate of 0.5 to 2°C / min and keeping warm for 30 to 120 minutes.
[0051] Please refer to Figure 2 , Figure 2 Shown are microscopic morphologies of single crystal glass ceramics provided according to some embodiments of the present invention.
[0052] Finally, the high temperature pulse method may further include a fourth stage, heating the temperature to 850-880°C at a heating rate of 1-2°C / min and keeping the temperature for 60-380 minutes. After the fourth stage, the treated glass powder is cooled to form the single crystal glass ceramic provided by the second aspect of the present invention, such as Figure 2 As shown, the single crystal glass ceramics are dense and non-porous. In addition, the main crystal phase of the formed single crystal glass ceramics is single crystal β-CaSiO3.
[0053] The following are several preferred embodiments, based on which the preparation method of the single crystal glass ceramics and the single crystal glass ceramics proposed in the present invention are described in detail.
[0054] In the preparation process of the single crystal glass ceramics provided in Example 1, the raw materials can be prepared according to the stoichiometric ratio requirements. The SiO2 included in the glass powder can use silicon oxide of the national medicine AR level as a raw material, the raw material of B2O3 can be electronic grade boric acid, CaO can use calcium carbonate as a raw material, and Al2O3 can use aluminum hydroxide as a raw material. Afterwards, a mixer is used to fully mix the raw materials, and zirconium beads can be loaded into the mixing tank at a ball-to-material ratio of 1:1, and the mixing time is 2 hours. A platinum crucible is then used to melt the raw materials, and a press cake batch feeding process is used to prevent excessive volatilization of the boron element. The melting temperature is 1300-1500°C, and the melting time is 1 to 3 hours. Afterwards, the melted glass liquid is poured into a double-roll cooling mill for rapid cooling, thereby rapidly cooling the glass liquid into a glass sheet. The glass sheet is then initially broken into glass particles of about 0.5 to 2.0 mm by a three-cylinder grinder, and the glass particles are then passed through an airflow mill in conjunction with an airflow classifier to obtain a glass powder of 3 to 4 μm. The composition of the glass powder is 41.68 mol% of CaO, 15.01 mol% of B2O3, 40.97 mol% of SiO2 and 2.34 mol% of Al2O3.
[0055] After that, the glass powder was treated by a high temperature pulse method. In the first stage, the temperature was first increased to 800°C at a heating rate of 5°C / min and kept at that temperature for 30 minutes. After that, the temperature was increased to 880°C at a heating rate of 1°C / min, and then cooled to 820°C at a cooling rate of 1°C / min. Subsequently, the cooling rate was changed to 800°C at a cooling rate of 0.5°C / min and kept at that temperature for 60 minutes.
[0056] Then, the second stage was performed, and the second stage was repeated 4 times. In the second stage, the temperature was first increased to 880°C at a heating rate of 1°C / min and kept at that temperature for 60 minutes. After that, the temperature was decreased to 820°C at a cooling rate of 1°C / min, and then the cooling rate was changed to 800°C at a cooling rate of 0.5°C / min and kept at that temperature for 60 minutes.
[0057] After the second stage was repeated 4 times, the third stage was performed. Here, the third stage was repeated 4 times. In the third stage, the temperature was first increased to 870°C at a heating rate of 1°C / min and kept at that temperature for 60 minutes, and then the temperature was decreased to 800°C at a cooling rate of 0.5°C / min and kept at that temperature for 60 minutes.
[0058] Finally, after the third stage, the fourth stage is performed. The temperature is raised to 880°C at a heating rate of 1°C / min and kept at this temperature for 360 minutes. After cooling, a large area of single crystal β-CaSiO3 glass ceramics can be obtained.
[0059] Please refer to Figure 3 and Figure 4 , Figure 3 The performance test results of various glass ceramics provided according to multiple embodiments and multiple comparative examples are shown. Figure 4 The flexural strength results of various glass ceramics provided according to various embodiments of the present invention and various comparative examples are shown.
[0060] like Figure 3 As shown, at 10 MHz, the dielectric constant of the single crystal glass ceramic obtained in Example 1 is 4.08, and the dielectric loss is 0.00327; at 15 GHz, the dielectric constant of the single crystal glass ceramic is 4.10, and the dielectric loss is 0.00325; Figure 4 As shown, the bending strength of the single crystal glass ceramic obtained in Example 1 is 278 MPa. It can be seen that the single crystal glass ceramic provided by the present invention has a small dielectric constant (4.10@15GHz) and dielectric loss (0.00325) and a high mechanical strength (278 MPa).
[0061] In the preparation process of the single crystal glass ceramics provided in Example 2, the raw materials can be prepared according to the stoichiometric ratio requirements. The SiO2 included in the glass powder can use silicon oxide of the national medicine AR level as a raw material, the raw material of B2O3 can be electronic grade boric acid, CaO can use calcium carbonate as a raw material, and Al2O3 can use aluminum hydroxide as a raw material. Afterwards, a mixer is used to fully mix the raw materials, and zirconium beads can be loaded into the mixing tank at a ball-to-material ratio of 1:1, and the mixing time is 2 hours. A platinum crucible is then used to melt the raw materials, and a press cake batch feeding process is used to prevent excessive volatilization of the boron element. The melting temperature is 1300-1500°C, and the melting time is 1 to 3 hours. Afterwards, the melted glass liquid is poured into a double-roll cooling mill for rapid cooling, thereby rapidly cooling the glass liquid into a glass sheet. The glass sheet is then initially broken into glass particles of about 0.5 to 2.0 mm by a three-cylinder grinder, and the glass particles are then passed through an airflow mill in conjunction with an airflow classifier to obtain a glass powder of 3 to 4 μm. The composition of the glass powder is 41.68 mol% of CaO, 15.01 mol% of B2O3, 40.97 mol% of SiO2 and 2.34 mol% of Al2O3.
[0062] After that, the glass powder was treated by a high temperature pulse method. In the first stage, the temperature was first increased to 800°C at a heating rate of 5°C / min and kept at that temperature for 30 minutes. After that, the temperature was increased to 880°C at a heating rate of 1°C / min, and then cooled to 820°C at a cooling rate of 1°C / min. Subsequently, the cooling rate was changed to 800°C at a cooling rate of 0.5°C / min and kept at that temperature for 60 minutes.
[0063] Then, the second stage was performed, and the second stage was repeated twice. In the second stage, the temperature was first increased to 880°C at a heating rate of 1°C / min and kept at that temperature for 60 minutes. After that, the temperature was decreased to 820°C at a cooling rate of 1°C / min, and then the cooling rate was changed to 800°C at a cooling rate of 0.5°C / min and kept at that temperature for 60 minutes.
[0064] After the second stage was repeated twice, the third stage was performed. Here, the third stage was repeated 6 times. In the third stage, the temperature was first increased to 870°C at a heating rate of 1°C / min and kept at that temperature for 60 minutes, and then the temperature was decreased to 800°C at a cooling rate of 0.5°C / min and kept at that temperature for 60 minutes.
[0065] Finally, after the third stage, the fourth stage is performed. The temperature is raised to 880°C at a heating rate of 1°C / min and kept at this temperature for 360 minutes. After cooling, a large area of single crystal β-CaSiO3 glass ceramics can be obtained.
[0066] like Figure 3As shown, at 10 MHz, the dielectric constant of the single crystal glass ceramic obtained in Example 2 is 4.15, and the dielectric loss is 0.00330; at 15 GHz, the dielectric constant of the single crystal glass ceramic is 4.20, and the dielectric loss is 0.00328; Figure 4 As shown, the flexural strength of the single crystal glass ceramics obtained in Example 2 is 270 MPa.
[0067] In the preparation process of the single crystal glass ceramics provided in Example 3, the raw materials can be prepared according to the stoichiometric ratio requirements. The SiO2 included in the glass powder can use silicon oxide of the national medicine AR level as a raw material, the raw material of B2O3 can be electronic grade boric acid, CaO can use calcium carbonate as a raw material, and Al2O3 can use aluminum hydroxide as a raw material. Afterwards, a mixer is used to fully mix the raw materials, and zirconium beads can be loaded into the mixing tank at a ball-to-material ratio of 1:1, and the mixing time is 2 hours. A platinum crucible is then used to melt the raw materials, and a press cake batch feeding process is used to prevent excessive volatilization of the boron element. The melting temperature is 1300-1500°C, and the melting time is 1 to 3 hours. Afterwards, the melted glass liquid is poured into a double-roll cooling mill for rapid cooling, thereby rapidly cooling the glass liquid into a glass sheet. The glass sheet is then initially broken into glass particles of about 0.5 to 2.0 mm by a three-cylinder grinder, and the glass particles are then passed through an air flow mill in conjunction with an air flow classifier to obtain a glass powder of 3 to 4 μm. The composition of the glass powder is 41.68 mol% of CaO, 15.01 mol% of B2O3, 40.97 mol% of SiO2 and 2.34 mol% of Al2O3.
[0068] After that, the glass powder was treated by a high temperature pulse method. In the first stage, the temperature was first increased to 780°C at a heating rate of 3°C / min and kept at that temperature for 60 minutes. After that, the temperature was increased to 850°C at a heating rate of 2°C / min, and then cooled to 830°C at a cooling rate of 2°C / min. Subsequently, the cooling rate was changed to 780°C at a cooling rate of 1°C / min and kept at that temperature for 60 minutes.
[0069] Then, the second stage was performed, and the second stage was repeated 8 times. In the second stage, the temperature was first increased to 880°C at a heating rate of 2°C / min and kept at this temperature for 80 minutes. After that, the temperature was decreased to 820°C at a cooling rate of 2°C / min, and then the cooling rate was changed to 780°C at a cooling rate of 1°C / min and kept at this temperature for 80 minutes.
[0070] After the second stage was repeated 8 times, the third stage was performed. Here, the third stage was repeated 5 times. In the third stage, the temperature was first increased to 870°C at a heating rate of 2°C / min and kept at that temperature for 80 minutes, and then the temperature was decreased to 780°C at a cooling rate of 1°C / min and kept at that temperature for 80 minutes.
[0071] Finally, after the third stage, the fourth stage is performed. The temperature is raised to 880°C at a heating rate of 1°C / min and kept at this temperature for 380 minutes. After cooling, a large area of single crystal β-CaSiO3 glass ceramics can be obtained.
[0072] like Figure 3 As shown, at 10 MHz, the dielectric constant of the single crystal glass ceramic obtained in Example 3 is 4.21, and the dielectric loss is 0.00329; at 15 GHz, the dielectric constant of the single crystal glass ceramic is 4.26, and the dielectric loss is 0.00327; Figure 4 As shown, the flexural strength of the single crystal glass ceramics obtained in Example 3 is 267 MPa.
[0073] The following are a number of comparative examples compared with the above-mentioned Example 1, based on which the preparation method of the single crystal glass ceramics proposed in the present invention and the performance effect of the prepared single crystal glass ceramics are further explained.
[0074] In Comparative Example 1, the glass powder obtained in Example 1 was treated by a heat treatment method. Specifically, the temperature was raised to 880° C. at a heating rate of 5° C. / min and kept at that temperature for 20 minutes. After cooling, glass ceramics were obtained.
[0075] like Figure 3 As shown, at 10 MHz, the dielectric constant of the glass ceramic obtained in Comparative Example 1 is 5.17, and the dielectric loss is 0.00376; at 15 GHz, the dielectric constant of the glass ceramic is 4.25, and the dielectric loss is 0.00386; Figure 4 As shown, the bending strength of the glass ceramic obtained in Comparative Example 1 is 196 MPa. It can be seen that the dielectric properties and mechanical strength of the glass ceramic obtained by a simple heat treatment method are far lower than those of the single crystal glass ceramic provided by the present invention.
[0076] For further information, please refer to Figure 5 , Figure 5 A comparison chart of the XRD spectra of the glass ceramics provided in Example 1 of the present invention and Comparative Example 1 is shown.
[0077] like Figure 5 As shown, the crystal type of the glass ceramics provided in Example 1 and Comparative Example 1 can be determined according to the intensity of the diffraction peak through the XRD (X-Ray Diffraction) spectrum. Line 501 is the result of the XRD spectrum of the single crystal glass ceramic provided in Example 1, and line 502 is the result of the XRD spectrum of the glass ceramic provided in Comparative Example 1. Figure 5It can be seen that the diffraction peak intensity of line 501 is much greater than that of line 502, which means that compared with a simple heat treatment method, the preparation method of the single crystal glass ceramic provided by the present invention is more conducive to forming glass ceramics with only a single target crystal phase β-CaSiO3.
[0078] The difference between Comparative Examples 2 and 3 and Example 1 is that Comparative Examples 2 and 3 only use one heat treatment cycle (i.e., the second stage and / or the third stage in the high-temperature pulse method) to process the glass powder obtained in Example 1.
[0079] Comparative Example 2 omits the third stage in the high temperature pulse method. Specifically, in the first stage, the temperature is first increased to 800°C at a heating rate of 5°C / min and kept at this temperature for 30 minutes. Thereafter, the temperature is increased to 880°C at a heating rate of 1°C / min and then cooled to 820°C at a cooling rate of 1°C / min. Subsequently, the cooling rate is changed to 800°C at a cooling rate of 0.5°C / min and kept at this temperature for 60 minutes.
[0080] Then, the second stage was performed, and the second stage was repeated 4 times. In the second stage, the temperature was first increased to 880°C at a heating rate of 1°C / min and kept at that temperature for 60 minutes. After that, the temperature was decreased to 820°C at a cooling rate of 1°C / min, and then the cooling rate was changed to 800°C at a cooling rate of 0.5°C / min and kept at that temperature for 60 minutes.
[0081] Finally, skip the third stage and proceed to the fourth stage. The temperature is raised to 880°C at a heating rate of 1°C / min and kept at this temperature for 360 minutes. After cooling, glass ceramics can be obtained.
[0082] like Figure 3 As shown, at 10 MHz, the dielectric constant of the glass ceramic obtained in Comparative Example 2 is 5.10, and the dielectric loss is 0.00312; at 15 GHz, the dielectric constant of the glass ceramic is 5.15, and the dielectric loss is 0.00302; Figure 4 As shown, the bending strength of the glass ceramic obtained in Comparative Example 2 is 185 MPa. It can be seen that the high temperature pulse method using only one heat treatment cycle will make the dielectric properties and mechanical strength of the formed glass ceramic far lower than the single crystal glass ceramic provided by the present invention.
[0083] Comparative Example 3 omits the second stage in the high temperature pulse method. Specifically, in the first stage, the temperature is first increased to 800°C at a heating rate of 5°C / min and kept at this temperature for 30 minutes. Thereafter, the temperature is increased to 880°C at a heating rate of 1°C / min and then cooled to 820°C at a cooling rate of 1°C / min. Subsequently, the cooling rate is changed to 800°C at a cooling rate of 0.5°C / min and kept at this temperature for 60 minutes.
[0084] Then, the second stage was skipped and the third stage was executed. The third stage was repeated 4 times. In the third stage, the temperature was first increased to 870°C at a heating rate of 1°C / min and kept at that temperature for 60 minutes, and then cooled to 800°C at a cooling rate of 0.5°C / min and kept at that temperature for 60 minutes. Compared with comparative example 2, comparative example 3 skipped the staged cooling in the second stage and directly cooled to 800°C at a cooling rate of 0.5°C / min.
[0085] Finally, the fourth stage is performed. The temperature is raised to 880°C at a heating rate of 1°C / min and kept at this temperature for 360 minutes. After cooling, glass ceramics can be obtained.
[0086] like Figure 3 As shown, at 10 MHz, the dielectric constant of the glass ceramic obtained in Comparative Example 3 is 5.23, and the dielectric loss is 0.00267; at 15 GHz, the dielectric constant of the glass ceramic is 5.00, and the dielectric loss is 0.00254; Figure 4 As shown, the bending strength of the glass ceramic obtained in Comparative Example 3 is 211 MPa. It can be seen that the high temperature pulse method using only one heat treatment cycle will make the dielectric properties and mechanical strength of the formed glass ceramic far lower than the single crystal glass ceramic provided by the present invention.
[0087] In summary, the single crystal glass ceramics provided by the present invention have a smaller dielectric constant and dielectric loss and high mechanical strength, can balance and improve the dielectric constant, dielectric loss and bending strength of the LTCC substrate, and have good application prospects, and are thus widely used in modern 5G / 6G electronic communications fields such as mobile communications, high-frequency electronics, wireless local area networks, satellite communications, and aerospace electronics.
[0088] Although the above methods are illustrated and described as a series of actions for simplicity of explanation, it should be understood and appreciated that these methods are not limited by the order of the actions, because according to one or more embodiments, some actions may occur in a different order and / or concurrently with other actions from those illustrated and described herein or not illustrated and described herein but understandable to those skilled in the art.
[0089] The previous description of the disclosure is provided to enable any person skilled in the art to make or use the disclosure. Various modifications to the disclosure will be apparent to those skilled in the art, and the general principles defined herein may be applied to other variations without departing from the spirit or scope of the disclosure. Thus, the disclosure is not intended to be limited to the examples and designs described herein, but should be granted the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for preparing single crystal glass ceramics, characterized in that: Includes steps: preparing raw materials and processing the raw materials to obtain glass powder; as well as The glass powder is processed by a high temperature pulse method, and single crystal glass ceramics are obtained after cooling, wherein the high temperature pulse method is achieved through multiple stages of heating, cooling and / or heat preservation, and the temperature of the high temperature pulse method is maintained between 780 and 880°C.
2. The method for preparing a single crystal glass ceramic according to claim 1, wherein: The multi-stage high temperature pulse method includes a first stage, a second stage, a third stage and / or a fourth stage, wherein the second stage and the third stage are repeated cycles of heating, cooling and / or keeping warm.
3. The method for preparing a single crystal glass ceramic according to claim 2, characterized in that: The first stage includes a staged cooling process, and the first stage includes the steps of: Raise the temperature to 780-820°C at a heating rate of 3-5°C / min and keep the temperature for 30-120 minutes; Heating the temperature to 850-880°C at a heating rate of 1-2°C / min, and then cooling the temperature to 820-840°C at a cooling rate of 1-2°C / min; and Change the cooling rate, cool down to 780-800°C at a cooling rate of 0.5-2°C / min, and keep it warm for 60 minutes.
4. The method for preparing a single crystal glass ceramic according to claim 2, wherein: After the first stage, the high temperature pulse method performs the second stage of repeated cycles, the number of repeated cycles of the second stage is 2 to 8 times, the second stage includes a staged cooling process, and the second stage includes the steps of: Raise the temperature to 850-880°C at a heating rate of 1-2°C / min and keep the temperature for 30-120 minutes; Cooling to 820-840°C at a cooling rate of 1-2°C / min; and Change the cooling rate, cool down to 780-800°C at a cooling rate of 0.5-2°C / min, and keep it at that temperature for 30-120 minutes.
5. The method for preparing a single crystal glass ceramic according to claim 2, characterized in that: After the second stage is completed, the high temperature pulse method performs the third stage of repeated cycles, the number of repeated cycles of the third stage is 2 to 8 times, including the steps of: Heating the temperature to 850-870°C at a heating rate of 1-3°C / min and keeping the temperature for 30-120 minutes; and The temperature is lowered to 780-800°C at a cooling rate of 0.5-2°C / min and kept at this temperature for 30-120 minutes.
6. The method for preparing a single crystal glass ceramic according to claim 2, wherein: After the third stage is completed, the high temperature pulse method performs the fourth stage, which includes the following steps: The temperature is raised to 850-880°C at a heating rate of 1-2°C / min and maintained at this temperature for 60-380 minutes.
7. The method for preparing a single crystal glass ceramic according to claim 1, characterized in that: The steps of preparing raw materials and processing the raw materials to obtain glass powder include: Weighing the raw materials and mixing them thoroughly, melting the mixed raw materials at 1300-1500° C. for 1-3 hours to obtain glass liquid; Rapidly cooling the glass liquid by a cooling rolling mill to obtain a glass sheet; placing the glass flakes into a grinder for preliminary crushing to obtain glass particles; and The glass particles are subjected to a jet mill and an air flow classifier to form the glass powder.
8. The method for preparing a single crystal glass ceramic according to claim 7, characterized in that: The particle size of the glass particles ranges from 0.5 to 2.0 mm.
9. The method for preparing a single crystal glass ceramic according to claim 7, characterized in that: The preset particle size range of the glass powder is 3.0-4.0 μm.
10. The method for preparing a single crystal glass ceramic according to claim 1, characterized in that: The glass powder includes 40.4-47.2 mol% of CaO, 10-17 mol% of B2O3, 36-42 mol% of SiO2 and 0-5.34 mol% of Al2O3.
11. A single crystal glass ceramic, characterized in that: The single crystal glass ceramic is prepared by the preparation method of the single crystal glass ceramic according to any one of claims 1 to 10.
12. The single crystal glass ceramic according to claim 11, characterized in that: The main crystal phase of the single crystal glass ceramic is single crystal β-CaSiO3.
Citation Information
Patent Citations
K2O-Na2O-Nb2O5-SiO2-B2O3 system glass ceramic material used for energy storage, and preparation method thereof
CN105254180A
Glass ceramics pottery granite and production method
CN1159431A
Method of producing a glass-ceramic
US4201559A