Chemically tempered plate-like glass or glass ceramic article and method of manufacture and use

By adopting chemical tempering and multi-stage ion exchange processes in glass or glass ceramic covers of electronic display equipment, the composition and thickness are optimized, and the problem of insufficient mechanical strength of existing covers is solved, which significantly improves its under high load and impact Durability.

CN119019091APending Publication Date: 2024-11-26SCHOTT AG +1
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202410646341.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-23
Filing Date
2024-05-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing glass or glass ceramic covers for electronic display devices are insufficient in mechanical strength and are difficult to withstand high loads and shocks, especially in case of operational errors, which may lead to crack propagation and mechanical failure.

Method used

Use glass or glass ceramic products with a thickness of 300μm to 1000μm, and their mechanical strength is enhanced through chemical tempering processes, and specific components are combined such as SiO2, Al2O3, Li2O and Na2O, and the compressive stress characteristic curve is optimized through multi-stage ion exchange steps to improve the cover plate resistance.

Benefits of technology

A cover plate that causes mechanical failure only under high loads under load conditions is achieved, significantly improving the strength and durability of glass or glass ceramic products, especially with higher resistance under the action of blunt or smooth surfaces sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019091A_ABST
    Figure CN119019091A_ABST
Patent Text Reader

Abstract

The invention relates to a chemically tempered plate-like glass or glass ceramic article for use as a cover plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention generally relates to a glass or glass-ceramic article for use as a cover plate, in particular a cover plate for an electronic display device. In addition, the present invention also relates to a method for manufacturing such an article and the use of the article. Background Art

[0002] Cover plates for electronic display devices have long been known, which are also called protective covers (front covers or back covers), glass covers or cover glasses, for example. These cover plates are used to cover the electronic components located thereunder and are further used as observation windows, especially as front covers. These cover plates are now usually configured so that they include chemically tempered glass plates or glass ceramic plates. This glass plate or glass ceramic plate usually has a very small thickness of about 1 mm or less, because this can minimize the weight of a display device (such as a smartphone or other portable electronic device) equipped with such a cover plate.

[0003] Due to the extremely small thickness, the mechanical strength of the glass is reduced, so, as mentioned above, the glass needs to be mechanically strengthened by corresponding treatments. In the case of thin glass mentioned in the prior art, this strengthening is achieved by a chemical toughening process, in which the glass sheet is immersed in an immersion bath containing molten salts. Within the scope of the present disclosure, this immersion bath is also synonymously called an exchange bath, because ion exchange with the molten salt occurs during the immersion in the bath.

[0004] In this way, smaller cations in the glass of the glass sheet are exchanged for larger cations of the exchange bath. For example, it is known to exchange sodium ions for potassium ions. Due to their size, these potassium ions generate compressive stresses in the exchange region near the surface of the glass sheet, which are balanced by tensile stresses within the glass sheet. This increases the overall resistance of the glass sheet to mechanical loads.

[0005] It is also known that glass ceramics can also be chemically toughened. In this case, the above-described exchange mechanism also applies in principle to glass ceramics. In the context of the present disclosure, glass ceramics generally refer to materials that are crystallized in a controlled or at least controllable manner on the basis of green glass, resulting in a structure of relatively small crystals (or grains) with a fairly uniform particle size distribution, wherein the average particle size of these crystals (or grains) preferably does not exceed 2 μm.

[0006] By simple ion exchange, smaller cations (such as Na + ) with larger cations (such as K +) in a typical tempered profile in which the stresses drop sharply from the surface to the interior of the glass or glass ceramic article. This is particularly important when subjected to blunt or smooth surfaces, so-called "blunt impact loads", because bending loads occur here, which can cause transverse cracks to propagate and lead to mechanical failure of the cover under load. Exposure to rough surfaces and sharp objects can also cause problems. In addition, users are making increasingly higher demands on the load-bearing capacity of mobile devices and their covers. In the event of an operating error, such devices should be able to withstand a fall from a certain height as non-destructively as possible, for example not only onto a table but also onto the ground.

[0007] The prior art also discloses glass and glass ceramic plates with tempered profiles produced in a cost-intensive manner, such as the publications EP 2 819 966 B1, US 2020 / 0002225 A1 and US 2010 / 0009154 A1, US 2021 / 0292225 A1, CN 111116040 A, WO 20261710 A1 and WO 20261711 A1, WO 16070048 A1, WO 19236975 A2, WO 17177109 A1, WO 16073539 A1 and US 20180305251 A1. However, these glass and glass ceramic plates have in common that they do not have sufficient strength for use. Summary of the invention

[0008] The object of the invention is to provide a cover panel with increased strength, ie a cover panel in which only very high loads will lead to mechanical failure of the cover panel when loaded.

[0009] Further aspects of the invention relate to a method for producing such a cover plate and to the use of such a cover plate.

[0010] The objects of the invention are solved by the subject matter of the independent claims.For preferred embodiments, reference is made to the dependent claims, the description and the drawings of the present disclosure.

[0011] The present invention therefore relates to a plate-shaped glass or glass-ceramic article for use as a cover plate, preferably a front plate, preferably for a mobile device.

[0012] Within the scope of the present disclosure, plate-shaped glass or glass-ceramic products and glass plates or glass-ceramic plates are used synonymously.

[0013] The thickness d of the plate-shaped glass or glass ceramic product is 300 μm to 1000 μm.

[0014] Preferably, its thickness does not exceed 650 μm.

[0015] The glass or glass ceramic product comprises glass or glass ceramic, the composition of which comprises the components SiO2, Al2O3, Li2O and Na2O. The glass or glass ceramic product preferably comprises LAS glass or LAS glass ceramic.

[0016] The product is chemically toughened.

[0017] The chemically toughened plate-shaped glass or glass-ceramic product has a compressive stress at a distance of 30 μm from the surface of the main side. The compressive stress at a distance of 30 μm from the surface of the main side is referred to as CS 30 . It is at least 60MPa.

[0018] Chemically toughened plate glass or glass ceramic products have compressive stress at a distance of 50 μm from the surface of the main side. The compressive stress at a distance of 50 μm from the surface of the main side is called CS. 50 .

[0019] The main side surface is the surface of the glass plate or glass ceramic plate with the largest area relative to the other surfaces. In addition to the two main side surfaces, the glass plate preferably also has four surfaces connected to the two main side surfaces, which are called edge surfaces. In the case of non-rectangular glass plates, this glass plate can also have fewer edge surfaces, for example only one edge surface. The transition from the main side surface to the edge surface is called an edge. The plate-shaped product according to the invention can basically have a rectangular shape. This glass plate or glass ceramic plate can especially have eight corners.

[0020] A glass plate or glass ceramic plate has a length, a width and a thickness. The length usually corresponds to the maximum side length of a main side, the width usually corresponds to the minimum side length of a main side, and the thickness corresponds to the shortest distance between two main sides of the glass plate. The main sides of the glass plate are arranged in particular parallel to one another.

[0021] Compressive stress CS on the same main side 30 and CS 50 The ratios V relative to each other are as follows:

[0022]

[0023] Where d = thickness of the glass article (in μm).

[0024] Therefore, the glass and glass ceramic articles according to the invention have a CS 30 With CS 50 The ratio of CS is particularly low. 30 describes the compressive stress near the surface, while CS 50The compressive stresses are described in the vicinity of the depth of the compressive stress zone (DoCL), and therefore these values ​​are elucidating for the development of the stress curve. Depending on the thickness of the article, the DoCL is preferably in the range of 85 μm to 220 μm, or even up to 250 μm. The DoCL value of this article is preferably at least 19.0% of its thickness, preferably 21.0% of its thickness.

[0025] Lower ratio This helps achieve particularly high strength. The gentle stress drop from the surface to the inside indicated by this value prevents crack formation and crack propagation that could occur when load occurs.

[0026] Particularly preferred is the ratio

[0027] ratio is thickness-dependent. Its value decreases with increasing thickness. In the case of the glasses and glass-ceramic articles according to the invention, this thickness dependence is not significant, since these glasses and glass-ceramic articles have a relatively high CS even at low thicknesses. 50 value, thus having a relatively small ratio, so that even with thinner embodiments, in particular with a maximum of 650 μm, a high strength is achieved.

[0028] The above-mentioned characteristic parameters of chemical toughening, namely CS, can be determined with the aid of suitable measuring equipment, such as the measuring equipment SLP-1000 of the manufacturer Orihara Industrial Co., Ltd. 30 , CS 50 and DoCL.

[0029] The upper limit of the thickness of the plate-shaped glass or glass ceramic product is preferably 700 μm, particularly preferably only 650 μm.

[0030] In the case of such thinner glass panes, the strength is significantly increased compared to glass panes with a different stress profile.

[0031] The chemically toughened plate glass or glass-ceramic article has a CS of preferably at least 80 MPa. 30 .

[0032] The chemically toughened plate glass or glass ceramic article has a CS of preferably at least 40 MPa. 50 .

[0033] The glass or glass ceramic product according to the invention containing SiO2, Al2O3, Li2O and Na2O is preferably realized by means of a glass or glass ceramic comprising the following components (in mol %):

[0034]

[0035] Here, a lower maximum content of 6 mol % or only 3 mol % or even only 1.5 mol % of Na2O has proven to be important for the positive properties of the preparations according to the invention, in particular for higher CS 50 Value and CS 30 With CS 50 A lower ratio is advantageous.

[0036] In the case of an embodiment of the article comprising glass, the SiO 2 content is particularly preferably 55 mol % to 70 mol %.

[0037] If B2O3 is present, especially in the case of an embodiment with a glass article and preferably with a minimum content of 2 mol%, this has a positive effect on the meltability. Contents above 10 mol% may result in lower chemical resistance and CS 30 and CS 50 Therefore, the content of B2O3 is preferably limited to 10 mol%, particularly preferably limited to 8 mol%.

[0038] In the case of an embodiment of the product comprising a glass ceramic, it is particularly preferred that the glass ceramic is free of B 2 O 3 .

[0039] If K2O is present, it has a positive effect on the meltability. In addition, K2O in the glass improves K-diffusion and allows deeper tempering (K-DoL) in the final tempering step. The K2O content is preferably limited to 1 mol%, since too high a K2O content has a negative effect on K-induced tempering (KCS).

[0040] If MgO is present, preferably in a minimum content of 0.1 mol%, it has a positive effect on meltability. Contents above 6 mol% promote crystallization and are therefore preferably avoided.

[0041] If P2O5 is present, in particular in the case of an embodiment with a glass article and preferably with a minimum content of 0.1 mol %, the diffusion of alkalis in the glass is positively influenced. This is advantageous because the duration of the ion exchange can be shortened. The P2O5 content should preferably be at most 2 mol %, particularly preferably at most 1.5 mol %, since excessively high contents can lead to corrosion of refractory materials in glass production. In the case of an embodiment with a glass ceramic article, it is particularly preferred that the glass ceramic does not contain P2O5.

[0042] If ZrO2 is present, preferably in a minimum content of 0.1 mol%, the chemical resistance of the glass is positively influenced. In addition, in glass ceramics, ZrO2 is used as a nucleating agent, thereby enabling controlled ceramicization / crystallization of green glass. However, high contents of ZrO2 can lead to devitrification. Therefore, its content is preferably limited to less than 2 mol%, particularly preferably to less than 1.5 mol%, and in particular in the case of embodiments of articles with glass, preferably to less than 1.0 mol%.

[0043] According to one embodiment, the glass or glass ceramic product or the glass or glass ceramic contained in the glass or glass ceramic product contains Y2O3, La2O3 and / or Nb2O5 only in the form of unavoidable traces of not more than 0.1 mol % each.

[0044] In embodiments, the glass or glass ceramic may contain up to 2 wt % of common fining agents such as As 2 O 3 , Sb 2 O 3 , SnO 2 , CeO 2 , halides (eg chlorides) or sulfur-containing compounds.

[0045] For reasons of environmental protection and work safety, particularly preferred are embodiments in which the glass or glass ceramic of the glass plate or glass ceramic plate contains no or essentially no As2O3 and / or Sb2O3. This also applies to other toxic or environmentally harmful components, such as PbO, TeO2, CdO, etc. In the context of the present disclosure, "essentially free of" is to be understood as containing only impurities that cannot be avoided in the case of conventional economic processing methods (for example, due to the raw materials). In the context of the present disclosure, "free of" means that these components are present only in trace amounts, i.e., in a content of up to 500 ppm, preferably up to 100 ppm, relative to weight.

[0046] Furthermore, as long as the article is not used as a back cover, the glass or glass ceramic preferably contains no or essentially no coloring components, in particular no V2O5, CoO, NiO, Cr2O3 and / or CuO.

[0047] The thermal expansion coefficient CTE (20°C-300°C) of the tempered glass plate or glass ceramic plate is preferably up to 7.0*10 -6 / K.

[0048] The coefficient of thermal expansion CTE (20°C-300°C) of the tempered glass plate is preferably at least 3.5*10 -6 / K.

[0049] The thermal expansion coefficient CTE (20°C-300°C) of the tempered glass ceramic plate is preferably at least 0.05*10 -6 / K or at least 0.5*10 -6 / K.

[0050] The glass comprised by the glass article may be green glass, ie a glass that is crystallizable in a controlled manner under specific conditions or a glass that does not crystallize in a controlled manner under conventional ceramizing conditions.

[0051] The glass comprised by the glass article preferably has a ratio of (Al2O3+B2O3) / (Li2O+Na2O+K2O)>1. In this case, the oxide content is expressed in mol%. At values ​​of this ratio>1, a highly crosslinked glass network with fewer oxygen separation points results, which has a positive effect on the mechanical stability. Preferably, (Al2O3+B2O3) / (Li2O+Na2O+K2O)<3.

[0052] The glass comprised by the glass article preferably has a ratio of (Li2O) / (Na2O+K2O)>3. In this case, the oxide content is expressed in mol%. Such a large value of this ratio leads to a CS after chemical tempering. 30 and CS 50 The absolute value of the value is higher.

[0053] The glass included in the glass article particularly preferably has

[0054] Na2O < 1.5 mol% and / or

[0055] 3>(Al2O3+B2O3) / (Li2O+Na2O+K2O)>1.4 and / or

[0056] 15>(B2O3+CaO)>7 and / or (CaO+MgO) / (Na2O)>2.5.

[0057] It is particularly preferred that the thermal expansion coefficient of the glass product CTE (20°C-300°C) is less than 5.5*10 -6 / K.

[0058] According to one embodiment, it is advantageous if the glass ceramic comprised by the glass ceramic product is designed as a lithium aluminum silicate glass ceramic and preferably comprises high quartz mixed crystals and / or keatite mixed crystals and / or lithium metasilicate and / or lithium disilicate.

[0059] Preferably, the lithium aluminum silicate glass ceramic has keatite mixed crystals as a crystalline phase, preferably as the main crystalline phase. Lithium aluminum silicate glass ceramics are well-known materials with significant advantages in the manufacture of glass ceramics. Therefore, it is also advantageous to form a glass ceramic comprising keatite mixed crystals as a crystalline phase (or crystalline phases), because it is easy to temper. Keatite or keatite mixed crystal crystalline phases obviously have a crystal structure that is easy to ion exchange, especially when lithium is exchanged with sodium and / or sodium and / or lithium is exchanged with potassium.

[0060] Therefore, a low thickness of the glass pane of 300 μm to 1000 μm is also advantageous and even more important in the case of a glass ceramic embodiment than in a glass embodiment, since in this way a high light transmittance can be achieved in addition to a low weight of the pane.

[0061] According to a preferred embodiment, the glass ceramic contains keatite or keatite mixed crystals as the main crystalline phase, which is understood to mean that more than 50 vol% of the crystalline phase contained in the glass ceramic has a keatite crystal structure. Preferably, up to 98.5 vol% or even 100 vol% of the crystalline phase contained in the glass ceramic may have a keatite crystal structure, i.e. keatite or keatite mixed crystals. However, the glass ceramic may also contain secondary phases, such as nucleating agents present in crystalline form.

[0062] In general, without being limited to a specific embodiment, according to one embodiment, the glass ceramic of the glass ceramic plate may contain the following oxide-based components (in mol %): SiO2 50-78, preferably 60-75

[0063] Al2O3 5-20, preferably 9-15

[0064] Li2O 5-15, preferably 7-13.

[0065] These are silicate glass ceramics that melt very well like glass and do not crystallize immediately and uncontrolled. In this general composition range, in particular the known lithium aluminum silicate glass ceramics can be produced, which are well known, for example, in terms of melting and ceramicizing conditions. The lithium content in the glass ceramic is also advantageous, since this allows an exchange of lithium with sodium and / or potassium.

[0066] According to one embodiment, a special component of the glass ceramic is SnO2. SnO2 can be used, for example, as a fining agent in the melt, and can also be used as a nucleating agent in the glass ceramic itself. Therefore, according to one embodiment, the glass ceramic of the glass ceramic plate preferably contains SnO2, preferably up to 2 mol%.

[0067] According to an embodiment, the components ZrO2 and TiO2 can also be used as nucleating agents in the glass ceramic. It has been shown that nucleation and in particular the content of nucleating agents in the glass ceramic and their ratio relative to one another play a decisive role in the formation of only slightly colored silicate glass ceramics with good light transmittance and low haze. Therefore, according to one embodiment, the glass ceramic includes TiO2, preferably up to 3 mol % TiO2.

[0068] Furthermore, according to one embodiment, a very effective nucleating agent in the glass ceramic is ZrO 2. Therefore, according to one embodiment, the glass ceramic comprises ZrO 2, preferably up to 3 mol %.

[0069] According to one embodiment, the glass ceramic of the glass ceramic plate comprises a crystalline phase having a grain size of less than 120 nm. The glass ceramic preferably comprises grains of at most less than 90 nm.

[0070] Preferably, the glass or glass ceramic product according to the invention is produced by subjecting the glass or glass ceramic to at least two-stage ion exchange, wherein in the last exchange step, an exchange bath having a potassium salt content higher than that of the exchange bath used in the preceding exchange step or steps is used.

[0071] As a result, higher K-induced compressive stresses are generated near the surface in the last exchange step, which make the product, in particular a glass product, more resistant to the effects of blunt or smooth surfaces (so-called “blunt impact loads”).

[0072] In the case of glass-ceramic products, a one-stage ion exchange of the glass-ceramic is sufficient.

[0073] Preferably, the glass product according to the present invention can be manufactured by a method comprising:

[0074] Melting process;

[0075] and subsequent thermoforming;

[0076] Ion exchange, which has:

[0077] a first ion exchange step, the duration of which is 1 hour to 10 hours, at a temperature between 380° C. and 460° C., the composition of the exchange bath being at least 0 wt % to a maximum of 50 wt % of a potassium salt, in particular KNO3, and at a maximum of 100 wt % to at least 50 wt % of a sodium salt, in particular NaNO3, and

[0078] a final ion exchange step, with a duration of 0.5 to 5 hours, at a temperature between 380° C. and 460° C., the composition of the exchange bath being at least 50 wt % to a maximum of 100 wt % of a potassium salt, in particular KNO3, and at most 50 wt % to at least 0 wt % of a sodium salt, in particular NaNO3,

[0079] · optional one or more further ion exchange steps between the first and the last ion exchange step,

[0080] Preferably, the one or more further ion exchange steps are carried out in an exchange bath having a different composition than the first and last ion exchange steps.

[0081] Conventional hot forming processes such as stretching processes can be used, for example, using a float process or a down-draw process. Ingot casting and sawing can also be used to produce glass sheets.

[0082] Preferably, the glass-ceramic product according to the present invention can be manufactured in a method, which comprises: a melting process;

[0083] and subsequent thermoforming;

[0084] Thermal treatment of a silicate green glass, wherein at least one nucleation step and at least one ceramization step are performed;

[0085] Ion exchange, which has:

[0086] a first ion exchange step of duration between 1 hour and 10 hours at a temperature between 380° C. and 500° C., the composition of the exchange bath being at least 0 wt % up to 50 wt % of a potassium salt, in particular KNO3, and up to 100 wt % up to at least 50 wt % of a sodium salt, in particular NaNO3; and

[0087] an optional final ion exchange step of duration between 0.2 and 5 hours at a temperature between 380° C. and 500° C., the composition of the exchange bath being at least 50 wt % up to 100 wt % of potassium salts, in particular KNO3, and up to 50 wt % to at least 0 wt % of sodium salts, in particular NaNO3;

[0088] · optional one or more further ion exchange steps between the first and last ion exchange steps;

[0089] Preferably, the one or more further ion exchange steps are carried out in an exchange bath having a different composition than the first and last ion exchange steps.

[0090] Conventional hot forming processes such as stretching processes can be used, for example, using a float process or a down-draw process. Ingot casting and sawing can also be used to produce glass sheets.

[0091] The at least one nucleation step mentioned in the heat treatment is preferably carried out in a temperature range of 650° C. to 850° C., preferably for a duration of 5 min to 60 h.

[0092] The at least one ceramizing step mentioned in the heat treatment is preferably carried out in a temperature range of 700° C. to 1100° C., preferably for a duration of 3 min to 120 h.

[0093] Thus, the present disclosure also generally relates to a glass or glass-ceramic article produced or producible by a method according to one embodiment.

[0094] In addition, the present disclosure relates to the use of a glass or glass ceramic product according to one embodiment and / or produced by a method according to one embodiment as a cover plate, preferably a front plate, in particular in electronic devices, in particular electronic display devices, in particular mobile electronic display devices, for example, in mobile touch panels and / or mobile digital display devices such as smartphones or smart watches as a cover plate, preferably a front plate.

[0095] An exchange bath refers to a molten salt, wherein the molten salt is used in an ion exchange process for glass or glass ceramics or glass or glass ceramic products. Within the scope of the present disclosure, the terms exchange bath and ion exchange bath are used synonymously.

[0096] Typically, technically pure salts are used for the exchange bath. This means that, although, for example, only sodium nitrate is used as raw material for the exchange bath, the exchange bath may still contain certain impurities. In this case, the exchange bath is a melt of a salt, for example sodium nitrate, or a mixture of salts, for example a mixture of sodium and potassium salts. In this case, the composition of the exchange bath is given in relation to the nominal composition of the exchange bath, without taking into account any impurities that may be present. Therefore, within the scope of the present disclosure, if a 100% sodium nitrate melt is mentioned, this means that only sodium nitrate is used as raw material. However, the actual content of sodium nitrate in the exchange bath may deviate from this and usually does, since technical raw materials, in particular, have a certain amount of impurities. However, this impurity amount is usually less than 5% by weight, in particular less than 1% by weight, relative to the total weight of the exchange bath.

[0097] However, in certain cases it may also be advantageous to use particularly pure salts, ie not technically pure, but for example particularly pure in analytical quality. This may be particularly advantageous if glass or glass ceramic plates which can be ion-exchanged very selectively are to be tempered.

[0098] Thus, according to an exemplary embodiment, salts with a purity of 3n (99.9% by weight) can be used, in particular when only exchange with specific ions is present. However, it is preferred to use technically purer salts, since these are much less expensive than high-purity salts. Here, the purity is usually 2n, i.e., for example, 99.5% by weight.

[0099] In the case of an exchange bath with a mixture of different salts, the nominal contents of these salts are given accordingly, without taking into account any technically relevant impurities in the raw materials. Thus, an exchange bath with 90 wt. % KNO3 and 10 wt. % NaNO3 can still have small amounts of impurities, but these are caused by the raw materials and their content should generally be below 5 wt. %, in particular below 1 wt. %, relative to the total weight of the exchange bath.

[0100] The above statements regarding the composition of the exchange bath apply correspondingly here.

[0101] Furthermore, during the ion exchange process, the composition of the exchange bath may also change, since lithium ions in particular migrate from the glass or glass ceramic or the glass or glass ceramic product into the exchange bath as a result of the continued ion exchange. However, unless expressly stated otherwise, such changes in the composition of the exchange bath due to aging are not taken into account here. Rather, within the scope of the present disclosure, when the composition of the exchange bath is given, this is based on the nominal original composition.

[0102] The preferred ion exchange process is an at least two-stage exchange. More than two exchange steps can also be used, which may be advantageous for the targeted adjustment of a specific stress characteristic curve.

[0103] The potassium salt content of the exchange bath of the last exchange step is preferably higher than that of the exchange bath of the first exchange step, and when more than two exchange stages are used, it is particularly preferably higher than that of the exchange baths of all preceding steps.

[0104] Thus, in particular in the case of the mentioned low-sodium glass ceramics, in particular glasses, it is possible to obtain a product having a compressive stress CS in particular depending on the thickness of the product between 85 and 250 μm or between 85 and 220 μm. 30 and CS 50 The stress characteristic curve realizes the corresponding compressive stress depth DoCL, which satisfies the ratio

[0105]

[0106] And thus leads to high strength.

[0107] It is particularly preferred to use the ratio

[0108] A particularly preferred ion exchange process comprises a first ion exchange step, the duration of which is 1 hour to 10 hours, the temperature being between 380° C. and 460° C., the composition of the exchange bath being at least 0 wt % to a maximum of 50 wt % of potassium salt, in particular KNO3, and a maximum of 100 wt % to at least 50 wt % of sodium salt, in particular NaNO3. The expression 0 wt % of potassium salt indicates that the ion exchange can also be carried out in a pure sodium salt bath instead of a mixed salt bath. However, a mixed salt bath having a potassium salt content of >0 wt % and a sodium salt content of <100 wt % is preferably used.

[0109] A particularly preferred ion exchange process comprises a final ion exchange step, the duration of which is 0.5 hours to 5 hours, the temperature being between 380° C. and 460° C., the composition of the exchange bath being at least 50 wt % to a maximum of 100 wt % of potassium salt, in particular KNO3, and at a maximum of 50 wt % to at least 0 wt % of sodium salt, in particular NaNO3. The expression 0 wt % of sodium salt indicates that the ion exchange can also be carried out in a pure potassium salt bath instead of a mixed salt bath. However, a mixed salt bath having a sodium salt content of >0 wt % and a potassium salt content of <100 wt % is preferably used.

[0110] Particularly preferred ion exchange processes include one or more additional ion exchange steps optionally performed between the first and last ion exchange steps. The one or more additional ion exchange steps are preferably performed in an exchange bath having a different composition than the first and last ion exchange steps.

[0111] Example

[0112] The present invention is described in detail below with reference to examples.

[0113] Table 1 lists the composition of the glass of the glass article as an example of the glass according to the present invention (Example) and the comparative glass (Comparative Example).

[0114] The materials listed in Table 1 were melted and refined at a certain temperature using raw materials commonly used in the glass industry. Castings with dimensions of approximately 140 mm x 100 mm x 30 mm were cast, stress relieved in an annealing furnace and cooled to room temperature. Test specimens for measuring properties were produced from these castings. Test specimens with a thickness of between 500 μm and 700 μm were produced by sawing and subsequent polishing.

[0115] Example A is a comparative example. Examples B, C and D are examples.

[0116] Table 1

[0117] Composition [mol%] B C D A <![CDATA[SiO2]]> 69 69.4 69.7 65.1 <![CDATA[Al2O3]]> 10.4 11.1 14.1 11.6 <![CDATA[Li2O]]> 8.4 9 9.4 10.3 <![CDATA[Na2O]]> 2.3 1.3 0.7 9.9 <![CDATA[B2O3]]> 3.7 3.3 <![CDATA[ZrO2]]> 0.1 0.5 1 1.9 CaO 2.8 4.2 0.1 <![CDATA[K2O]]> 0.2 0.2 0.1 0.2 MgO 2 0.1 1.6 0.5 <![CDATA[CeO2]]> 0.1 0.3 0.02 <![CDATA[Nd2O3]]> 0.1 ZnO 0.1 0.1 0.4 0.1 <![CDATA[P2O5]]> 0.3 0.1 0.1 0.3 <![CDATA[Fe2O3]]> <![CDATA[TiO2]]> 1.3 SrO 0.2 0.3 <![CDATA[SnO2]]> 0.1 0.1 0.2 <![CDATA[SO3]]> 0.02 Cl 0.3 1.3

[0118] Under the different tempering conditions listed in Table 2, the samples with different thicknesses in the examples shown in Table 1 were chemically tempered.

[0119] Here, IOX1 represents a first ion exchange step in a first exchange bath, and IOX2 represents a second ion exchange step in a second exchange bath.

[0120] The corresponding tempering duration t is expressed in hours [h], the corresponding tempering temperature T is expressed in degrees C. The corresponding KNO3 and NaNO3 contents in the exchange bath are expressed in wt%.

[0121] Table 2

[0122]

[0123] The results of chemical toughening according to Table 2 are listed in Table 3. It shows:

[0124] Compressive stress at 30 μm from the main side surface: CS 30 , unit is MPa,

[0125] Compressive stress at 50 μm from the surface of the same main side: CS 50 , unit is MPa,

[0126] Dimensionless ratio CS 30 / CS 50

[0127] and the depth of the compressive stress zone on the same main side: DoCL, in μm.

[0128] CS in the table 30 and CS 50 The values ​​given are rounded and therefore may differ from the given CS in some cases. 30 / CS 50 The value has an assumed deviation.

[0129] Table 3

[0130] The samples in Table 2 Thickness [μm] <![CDATA[CS 30 [MPa]]]> <![CDATA[CS 50 [MPa]]]> <![CDATA[CS 30 / CS 50 ]]> DoCL[μm] A1 500 111 60 1.85 90 A2 550 135 74 1.82 103 A3 600 136 80 1.71 108 A4 700 160 96 1.67 121 B1 530 91 68 1.32 120 B2 550 106 81 1.31 123 B3 580 100 77 1.29 127 B4 630 113 90 1.25 142 B5 680 116 95 1.22 152 B6 700 117 95 1.23 147 C1 502 137 99 1.39 107 C2 700 173 135 1.28 136 D1 504 100 71 1.42 108 D2 610 158 127 1.24 149 D3 694 84 71 1.19 158 BRIEF DESCRIPTION OF THE DRAWINGS

[0131] Figure 1 The data in Table 3 are shown in graphical form.

[0132] Figure 2 Test results of a kit drop test as a measure of strength are shown.

[0133] Figure 3 Shown is an overall view of the drop test setup with individual components labeled.

[0134] Figure 4 Schematic diagram showing the sample holder and trigger mechanism for the kit drop test.

[0135] Figure 5 Schematic diagram showing an aluminum housing and a plastic plate as a sample holder and a sample model.

[0136] Figure 6 A schematic diagram showing the alignment of the sample model in the sample holder with the aid of a 2D level is shown. DETAILED DESCRIPTION

[0137] Figure 1 The data in Table 3 are shown in graphical form.

[0138] The corresponding thickness of the glass sample (in μm) is plotted on the x-axis.

[0139] Corresponding ratio Plotted on the y-axis.

[0140] In addition to the individual measuring points, the line

[0141] It will have

[0142] According to an embodiment of the present invention,

[0143] This type of implementation is distinguished.

[0144] This ratio is crucial for increasing the strength of the glass and glass-ceramic panels according to the invention, e.g. Figure 2 shown.

[0145] Figure 2 The test results of the kit drop test as a measure of strength are described. This test was performed with a grit of 60, which is a fairly coarse grit and is particularly demanding on the test material.

[0146] The tempered samples with B component (ie, samples B2 and B6) having two different thicknesses (ie, 550 μm and 700 μm) were compared with the tempered samples with A component (ie, samples A2 and A4) having the same two thicknesses.

[0147] Figures 3 to 6 This involves the performance of a so-called set drop test, which determines the set drop strength.

[0148] The set drop test (Set-Drop-Test) is preferably carried out as follows:

[0149] The plate is fixed to the sample holder and dropped from a cumulative drop height onto a defined background. An overview of the overall structure is shown in Figure 3 shown. Figure 5 The cover used in the kit drop test is 99mm long and 59mm wide. Figure 4 As shown, the sample model is magnetically fixed to the sample holder.

[0150] First, a plastic sheet is bonded into a metal housing with the aid of double-sided tape, the shape and weight of which are similar to the holder of a mobile device such as a smartphone. For example, a plastic sheet with a thickness between 4.35 mm and 4.6 mm is suitable here (see Figure 5The bonding is then carried out by means of a double-sided adhesive tape, preferably a double-sided adhesive tape with a thickness of about 100 μm. The plate-shaped glass article to be tested is adhered to the plastic plate using a double-sided tape of 05338, product number, so that a distance of between 350 μm and 450 μm is obtained between the upper edge of the housing or the support and the upper edge of the glass article. The cover plate is higher than the housing frame and there is no direct contact between the cover plate and the aluminum housing. The "device" thus produced, which simulates the installation of a cover plate in a mobile device and is a kind of "dummy" of a real mobile device (here in particular a smartphone), is then placed on a surface of size DIN A4, the so-called impact surface, with the glass side falling with an initial velocity of 0 in the vertical direction, i.e. in the direction of fall. The impact surface is produced as follows: Sandpaper with a suitable grit, for example 60 grit (#60), is adhered to the base plate using a double-sided tape, for example with a thickness of 100 μm. Tesa (10m / 15mm), transparent, double-sided, product number 05338, is used as adhesive tape. In the context of the present invention, the particle size is defined in accordance with the standards of the European Federation of Abrasive Manufacturers (FEPA), see for example also DIN ISO 6344, in particular DIN ISO 6344-2:2000-04, Coated abrasives - Grain size analysis - Part 2: Determination of the particle size distribution of large grains P 12 to P 220 (ISO 6344-2:1998). The weight of the base plate is about 3 kg, the values ​​disclosed here are for an aluminum base plate.

[0151] The base plate must be solid and preferably made of aluminum or steel. The sandpaper must be completely covered and taped with adhesive tape and must be free of bubbles. The impact surface can only be used for five drop tests and must be replaced after the fifth drop test. Place the sample (i.e. the obtained set) into the test device and align it using a 2D level (circular bubble) so that the set is stored horizontally with the cover sheet pointing to the ground, i.e. the impact surface (see Figure 6 ). The first drop height is 20 cm, if no breakage occurs, the drop height is increased in 10 cm increments until the glass breaks. Record the break height, break origin and break appearance. Test 10 to 15 samples and take the average value.

[0152] This kit drop test is a general measure of the strength of an article, especially the so-called "sharp impact" strength. It simulates the dropping of an article, especially a glass sheet, onto a rough surface, wherein many smaller sharp objects (such as asphalt, concrete or sand grains from sandpaper) may enter the glass sheet being tested.

[0153] Figure 2 It is shown that, compared with Comparative Example A, Example B exhibits a higher rupture height, ie, a higher set drop strength, at both sample thicknesses.

[0154] The above improvements are particularly beneficial for the reliability of the cover plate in mobile terminal devices, especially mobile electronic display devices (eg, mobile touch panels and / or mobile digital display devices, such as smart phones or smart watches).

[0155] Therefore, this ratio It is a measure of the strength of a tempered glass or glass ceramic article. Therefore, determining and understanding these variables allows the selection of appropriate materials without the need for complex strength measurements and statistical analysis of results, such as kit drop tests. This greatly simplifies experimental work, especially when tempering conditions vary and a large number of samples are generated. The present disclosure also includes a method for determining whether a tempered glass or glass ceramic panel is suitable for use as a cover panel.

[0156] The present invention utilizes The tempered plate-shaped glass and glass ceramic products are used to provide glass and glass ceramic plates, which have high reliability in use due to their improved strength and are therefore particularly suitable as cover plates in mobile terminal devices.

Claims

1. A chemically toughened plate-shaped glass or glass ceramic product, preferably used as a cover plate, preferably a front plate, preferably for a mobile device The glass or glass ceramic product comprises glass or glass ceramic, wherein the glass or glass ceramic comprises components SiO2, Al2O3, Li2O and Na2O, having a thickness d of 300 μm to 1000 μm, and having a compressive stress CS of at least 60 MPa at a distance of 30 μm from the main side surface 30 , And has a compressive stress CS at 50 μm from the main side surface 50 , The compressive stress CS on the same main side 30 and CS 50 The ratio V relative to each other is expressed as follows: Wherein d = the thickness of the glass article, in μm.

2. The glass or glass ceramic product according to claim 1, characterized in that: CS of at least 80MPa 30 and / or CS of at least 40 MPa 50 .

3. The glass or glass ceramic product according to claim 1 or 2, characterized in that: Its thickness is at most 700 μm, preferably at most 650 μm.

4. The glass or glass ceramic product according to any one of claims 1 to 3, It includes the following components, in mol %:

5. The glass or glass ceramic product according to any one of claims 1 to 4, characterized in that Maximum 7.0*10 -6 / K thermal expansion coefficient CTE (20℃-300℃).

6. The glass product according to any one of claims 1 to 5, characterized in that At least 3.5*10 -6 / K thermal expansion coefficient CTE (20℃-300℃).

7. The glass or glass ceramic article according to any one of claims 1 to 6, which is made by subjecting the glass or glass ceramic to at least two stages of ion exchange, wherein in the final exchange step, the exchange bath used has a potassium salt content that is higher than the potassium salt content of the exchange bath used in the previous one or more previous exchange steps.

8. The glass or glass ceramic product according to claim 7, characterized in that: The ion exchange comprises the following steps: a first ion exchange step, the duration of which is from 1 hour to 10 hours, at a temperature between 380° C. and 460° C. in the case of glass products and between 380° C. and 500° C. in the case of glass-ceramic products, the composition of the exchange bath being at least 0 wt % to a maximum of 50 wt % of potassium salts, in particular KNO3 and at a maximum of 100 wt % to at least 50 wt % of sodium salts, in particular NaNO3, and a final ion exchange step, in the case of glass products, of duration from 0.5 to 5 hours and in the case of glass ceramic products, of duration from 0.2 to 5 hours, in the case of glass products, at a temperature between 380° C. and 460° C. and in the case of glass ceramic products, at a temperature between 380° C. and 500° C., the composition of the exchange bath being at least 50% by weight to at most 100% by weight of potassium salts, in particular KNO3, and at most 50% by weight to at least 0% by weight of sodium salts, in particular NaNO3, · optional one or more further ion exchange steps between the first ion exchange step and the last ion exchange step, Preferably, the one or more further ion exchange steps are carried out in an exchange bath having a different composition than the first ion exchange step and the last ion exchange step.

9. Use of the glass or glass ceramic product according to any one of claims 1 to 8 as a cover plate, preferably a front plate, in particular in electronic devices, in particular electronic display devices, in particular mobile electronic display devices, for example, in mobile touch panels and / or mobile digital display devices such as smartphones or smart watches as a cover plate, preferably a front plate.

10. A method of making a glass or glass ceramic article according to any one of claims 1 to 6, the method comprising ion exchange, comprising a first ion exchange step, the duration of which is from 1 hour to 10 hours, at a temperature between 380° C. and 460° C. in the case of glass products and between 380° C. and 500° C. in the case of glass-ceramic products, the composition of the exchange bath being at least 0 wt % to a maximum of 50 wt % of potassium salts, in particular KNO3 and at a maximum of 100 wt % to at least 50 wt % of sodium salts, in particular NaNO3, and a final ion exchange step, in the case of glass products, of duration from 0.5 to 5 hours and in the case of glass ceramic products, of duration from 0.2 to 5 hours, in the case of glass products, at a temperature between 380° C. and 460° C. and in the case of glass ceramic products, at a temperature between 380° C. and 500° C., the composition of the exchange bath being at least 50% by weight and up to 100% by weight of potassium salts, in particular KNO3, and up to 50% by weight and up to 0% by weight of sodium salts, in particular NaNO3, · optional one or more further ion exchange steps between the first ion exchange step and the last ion exchange step, Preferably, the one or more further ion exchange steps are carried out in an exchange bath having a different composition than the first ion exchange step and the last ion exchange step.

Citation Information

Patent Citations

  • Toughened glass product with non-single surface compressive stress slope and preparation method thereof

    CN111116040A

  • Ion exchanged glasses via non-error function compressive stress profiles

    EP2819966B1

  • Glass with compressive surface for consumer applications

    US20100009154A1

  • Chemically strengthened glass

    US20180305251A1

  • Glass-based articles with improved stress profiles

    US20200002225A1