Amber glass and preparation method thereof
By using the ratio of specific components and composite colorants in amber glass to form a tight glass network and long sulfur chains, the problems of unstable coloring and high light transmittance in existing amber glass are solved, and efficient resistance is achieved UV performance and uniform coloring effect, suitable for storage and packaging of high-end alcohol, medicine and cosmetics.
Patent Information
- Application Number
- CN202410976461.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-20
AI Technical Summary
The existing amber glass has unstable coloring, with a large average visible light transmittance, and there is a problem of light transmittance in the ultraviolet band and visible blue to purple band.
Amber glass made of SiO2, Al2O3, B2O3, Na2O, K2O, CaO, MgO and composite colorant, the composite colorant consists of Fe2O3, ferrous aluminosilicate, Na2SO4, NH4HSO4, high purity graphite powder and anhydrous ethanol. , prepared by ultrasonic mixing and melting processes, control the mole percentage and molar ratio of Na2O+K2O and CaO+MgO, reasonably adjust the Fe2+/Fe3+ ratio, form a tight glass network structure and long sulfur chains, improve coloring stability and ultraviolet resistance. .
The color uniformity and stability of amber glass is achieved, the visible light transmittance is reduced, and the UV resistance is significantly improved. It is suitable for cosmetics, medicines and alcohol storage packaging with high light protection requirements.
Smart Images

Figure FT_1 
Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of special glass and relates to amber glass and a preparation method thereof. Background Art
[0002] With the rapid development of my country's wine, beverage, food, medicine and other industries, the demand for various types of packaging glass bottles is increasing, and the quality requirements are getting higher and higher. Therefore, in order to continuously adapt to the use requirements of users, the glass bottle industry has increasingly stringent requirements on the quality of glass bottles. Sulfur-carbon-dyed amber glass is brown with red, bright and bright, and amber-like in color. Its ability to absorb ultraviolet rays is higher than other colored glasses commonly used in light industry on the market. It can better meet the light-proof storage needs of food and medicines and extend the shelf life. Therefore, high-end wines, cosmetics, and medicines are often stored in amber glass bottles.
[0003] There are currently three common coloring methods for amber glass, namely iron-manganese coloring, iron-titanium coloring, and sulfur-carbon coloring. Iron-manganese coloring has low corrosion resistance to stored materials, and the coloring is difficult to control. Iron-titanium coloring is currently a common coloring technology for brown medicinal glass. It has high chemical stability, but the addition of TiO2 to the glass is prone to crystallization and high cost. Traditional sulfur-carbon coloring usually uses high-alkali sodium-lime glass as the base glass for sulfur-carbon coloring. Common problems are bubbles and unstable coloring, but it can usually effectively cut off or shield the light sensitivity of ultraviolet rays or the blue to purple bands in visible light, which can avoid the decomposition of videos and drugs by light.
[0004] Patent publication number CN101428969A discloses a brown glass and its application, and obtains brown glass with relatively balanced chromaticity. However, from the perspective of patent technology effect, visible light still passes through the transmittance at 313nm, and the average visible transmittance is greater than 40%, and the light shielding effect is not good. Patent publication number CN114409254A discloses a high-transmittance infrared-resistant energy-saving color glass and its melting device, which provides a composite colorant idea, but the introduction of reducing agents such as oxalic acid will offset the sulfur-carbon coloring effect and does not promote the coloring effect. Summary of the invention
[0005] The purpose of the present invention is to solve the problems of unstable coloring of existing amber glass, large average visible light transmittance, and transmission of ultraviolet light and visible light blue-violet light, and to provide an amber glass and a preparation method thereof.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows: An amber glass, characterized in that it is made of the following raw materials in molar percentage: 69.4-71.8% SiO2, 0.48-1.8% Al2O3, 0.52-2.1% B2O3, 8.4-12.1% Na2O, 0.5-1.5% K2O, 8.2-11.7% CaO, 0.25-0.8% MgO and 2.2-7.9% composite colorant; wherein the total molar percentage of Na2O+K2O is 12.1-13.2%, and the molar ratio of Na2O to K2O is 17.1-17.6; the total molar percentage of CaO+MgO is 11.4-12.2%, and the molar ratio of CaO to MgO is 19.3-20.1.
[0007] Further, an amber glass is characterized in that it is made of the following raw materials in molar percentage: 69.6-71.5% SiO2, 0.51-1.72% Al2O3, 0.55-2.04% B2O3, 8.6-11.9% Na2O, 0.8-1.5% K2O, 8.5-11.5% CaO, 0.3-0.75% MgO and 2.3-7.8% composite colorant; wherein the total molar percentage of Na2O+K2O is 12.3-13.0%, and the molar ratio of Na2O to K2O is 17.3-17.4; the total molar percentage of CaO+MgO is 11.5-12.0%, and the molar ratio of CaO to MgO is 19.5-20.1.
[0008] Furthermore, the composite colorant is composed of the following raw materials in molar percentage: 0.06-0.07% Fe2O3, 0.01-0.05% ferrous aluminosilicate, 0.23-0.62% Na2SO4, 0.01-0.24% NH4HSO4, 0.25-2.6% high-purity graphite powder, and the balance is anhydrous ethanol.
[0009] Furthermore, the composite colorant is prepared by the following method: Fe2O3 and aluminum ferrosilicate are weighed according to the above ratio, 20 ml of anhydrous ethanol is added, and ultrasonic mixing is performed for 0.5 h to obtain a powder with uniform particles, and Na2SO4, NH4HSO4, and high-purity graphite powder are further weighed, 20 ml of anhydrous ethanol is added, and ultrasonic mixing is performed for 0.5-1 h to prepare a uniformly mixed composite colorant.
[0010] A method for preparing amber glass, characterized by comprising the following steps: (1) Prepare the composite colorant according to the above method, continue to add the remaining oxide composition according to the above ratio, add 50 ml of anhydrous ethanol, put it into the mixer for mixing, the speed is 50-200 r / min, and the time is 1-1.5 h; (2) After the batch material is placed in an oven for drying, it is placed in a platinum crucible for melting. The feeding temperature is 900-1000°C. After the feeding, nitrogen is introduced (to maintain the stability of the redox atmosphere in the furnace). The melting temperature is 1450-1520°C and the holding time is 0.5-1.5h. (3) The copper plate for glass casting is preheated in advance, the preheating temperature is 480℃~520℃, the melted and clarified glass liquid is taken out from the high-temperature furnace and cast on the preheated copper plate; (4) The cast glass is placed in an annealing furnace. The annealing temperature is: 480°C ~ 520°C for 1 hour, then cooled to 400°C at a rate of 5°C / min, and then cooled to 280°C at a rate of 3°C / min. Then, it is cooled to room temperature in the furnace to prepare amber glass.
[0011] Furthermore, the amber glass contains Fe 2+ / Fe 3+ It is 1.76-2.25.
[0012] Furthermore, the visible light transmittance (380-780nm) of the amber glass is ≤35%.
[0013] Furthermore, the transmittance (10-300nm) of the amber glass is 0.
[0014] Furthermore, the chromaticity L of the amber glass is 18-24, a is 5-8, and b is 4-8.
[0015] The present invention can improve the coloring stability of glass and reduce the transmittance by controlling the molar percentage of Na2O+K2O in the components to 12.1-13.2%, and the molar ratio of Na2O to K2O to 17.1-17.6; controlling the molar percentage of CaO+MgO to 11.4-12.2%, the total molar percentage of CaO+MgO to 11.4-12.2%, and the molar ratio of CaO to MgO to 19.3-20.1. This is mainly because: SiO2+Al2O3+ The content of B2O3 is 70.4-75.7%, which is the main body of the glass network, that is, the network former occupies more than 70% of the glass network structure, which fundamentally determines that the compactness of the glass network structure can reach a relatively ideal level); at the same time, the molar percentage of the alkali metal content Na2O+K2O is controlled at 12.1-13.2%. These two factors mainly determine the coloring stability and transmittance of the glass; the higher the alkali metal content, the more sulfur can be retained in the glass, and the longer the sulfur chain formed, the more conducive it is to produce brown and red amber. Limiting Na2O and K2O and increasing the sodium ion content can better promote the participation of alkali metals in the coloring process; the molar percentage of CaO+MgO is controlled at 11.4-12.2%, and the ratio of CaO to MgO is limited, mainly because the crystallization temperature affects the glass forming process, and CaO and MgO have different effects on the crystallization temperature of the glass. The present invention limits the ratio between the two, which can achieve the maximum reduction of the crystallization temperature, while reducing the glass viscosity, which is conducive to the molding of glassware and reduces the process difficulty.
[0016] The amber color of the glass in the present invention is due to alkali metal polysulfides and iron sulfides, a central atom Fe 3+ With three oxygen atoms (O 2- ) and a sulfur atom (S 2- ) forms a tetrahedral structure and acts as a coloring group for coloring. In the glass melt, a certain amount of chain sulfur will be formed under a certain condition, and they will polymerize to produce polysulfides during the cooling process. At high temperatures, the two ends of the sulfur chain are open, and generally they are saturated by absorbing alkali metal ions or alkali polysulfides. However, when polysulfides are formed, the glass will produce yellow to orange. The longer the sulfur chain, the darker and redder the color. However, when the reducing property in the glass is too strong, Fe 2+ When the process is excessive, Si is formed 4+ -O-Fe 2+ structure, and this hexacoordinated Fe 2+ The absorption in the near-infrared region will make the green-blue hue of ferrous ferrite bluer. Therefore, in order to prepare amber glass and improve its UV resistance, it is necessary to add an appropriate amount of reducing agent to the glass to strictly control the Fe content in the glass. 2+ / Fe 3+In the prior art, carbon powder, aluminum powder or silicon powder are added separately. The reducing agent alone has limited reducing performance. If too much is added, it will cause changes in glass properties, affect glass clarity, reduce glass transmittance, and the cost is too high. The present invention adopts a composite colorant to introduce Fe2O3 and aluminum ferrosilicate into the glass. 3+ 、Al 3+ , while Al 3+ It has strong oxidizing property; the introduction of NH4HSO4 has reducing property, and the introduction of S 2- It can also be used as a reducing agent, decomposing into CO and H2O after heating. In addition, it will also generate hydrogen when reacting with active metals to neutralize Al 3+ The oxidizing property of Na2SO4 can reduce the content of carbon powder and improve the coloring uniformity. Compared with carbon powder, high-purity graphite powder has extremely low impurity content, fine and uniform particles, and sufficient reaction, which can greatly improve the coloring stability. 2- As a glass clarifier, it ensures the glass clarification effect.
[0017] Beneficial effects of the present invention: (1) The viscosity of the preparation method of the present invention is low during the melting process, which is conducive to the molding of glass packaging containers and has low process difficulty; high-temperature feeding is adopted, which greatly reduces the C and S content in the glass melting process while ensuring that the coloring reaction is fully carried out. 2- The loss of Fe can be reduced, which improves the coloring efficiency and ensures the coloring uniformity. The composite colorant can strictly control the Fe 2+ / Fe 3+ 1.76-2.25, greatly improving the color uniformity and stability; (2) The amber glass prepared by the present invention has a visible light transmittance (380-780nm) of ≤35%, and a transmittance of 10-300nm of 0, which greatly improves the anti-ultraviolet performance and can be used for the storage and packaging of cosmetics, medicines, alcoholic beverages, etc. with high light protection requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is the high temperature viscosity curve of the amber glass of Example 1 of the present invention. DETAILED DESCRIPTION
[0019] In order to better understand the present invention, the present invention will be further described below in conjunction with embodiments: (1) Preparation of composite colorant: Fe2O3 and aluminum ferrosilicate were weighed according to Table 1, 20 ml of anhydrous ethanol was added, and ultrasonic mixing was performed for 0.5 h to obtain a powder with uniform particles. Na2SO4, NH4HSO4 and high-purity graphite powder were weighed, 20 ml of anhydrous ethanol was added, and ultrasonic mixing was performed for 0.5 h to prepare a composite colorant with uniform particles. (2) Continue to add the remaining oxide composition according to Table 1, add 50 ml of anhydrous ethanol, put it into the mixer for mixing, the speed is 120 r / min, and the time is 1 hour; (2) After the batch material is placed in an oven for drying, it is placed in a platinum crucible for melting. The feeding temperature is 950°C. After the feeding, nitrogen is introduced. The melting temperature is 1450°C and the holding time is 0.5 h. (3) The copper plate for glass casting is preheated in advance at a temperature of 500°C. The melted and clarified glass liquid is taken out from the high-temperature furnace and cast on the preheated copper plate. (4) The cast glass is placed in an annealing furnace. The annealing temperature is as follows: keep at 500°C for 1 hour, then cool to 400°C at a rate of 5°C / min, then cool to 280°C at a rate of 3°C / min, and then cool to room temperature in the furnace to produce amber glass.
[0020] The properties of the amber glass obtained in Examples 1 to 8 are shown in Table 1.
[0021] Table 1 Components and properties of Examples 1 to 8
[0022] It can be seen from Examples 1-8 that the glass is all amber in color, and the composite colorant has a better effect and can strictly control Fe 2+ / Fe 3+ The color is uniform, the visible light transmittance of the glass (380-780nm) is ≤35%, and the transmittance of 10-300nm is 0, which can greatly improve the coloring uniformity and stability. Figure 1 The high temperature viscosity diagram shows that the glass of the present invention has a low viscosity during the melting process, which is beneficial to the molding of glass packaging vessels and reduces the difficulty of the process.
Claims
1. A kind of amber glass, Features Made from the following molar percentages of raw materials: 69.4-71.8% SiO 2 , 0.48-1.8% Al 2 O 3 , 0.52-2.1% B 2 O 3 , 8.4-12.1% Na 2 O, 0.5-1.5% K 2 O, 8.2-11.7% CaO, 0.25-0.8% MgO and 2.2-7.9% composite colorant; among them, Na 2 O+K 2 The total molar percentage of O is 12.1-13.2%, and Na 2 O and K 2 The molar ratio of O is 17.1-17.6; the total molar percentage of CaO+MgO is 11.4-12.2%, and the molar ratio of CaO to MgO is 19.3-20.
1.
2. The amber glass according to claim 1, Features Made from the following molar percentages of raw materials: 69.6-71.5% SiO 2 , 0.51-1.72% Al 2 O 3 , 0.55-2.04% B 2 O 3 , 8.6-11.9% Na 2 O, 0.8-1.5% K 2 O, 8.5-11.5% CaO, 0.3-0.75% MgO and 2.3-7.8% composite colorant; among them, Na 2 O+K 2 The total molar percentage of O is 12.3-13.0%, and Na 2 O and K 2 The molar ratio of O is 17.3-17.4; the total molar percentage of CaO+MgO is 11.5-12.0%, and the molar ratio of CaO to MgO is 19.5-20.
1.
3. An amber glass according to claim 1 or 2, Features: The composite colorant is composed of the following raw materials in molar percentage: 0.06-0.07% Fe 2 O 3 , 0.01-0.05% of ferrous aluminosilicate, 0.23-0.62% of Na 2 SO 4 , 0.01-0.24% NH 4 HSO 4 , 0.25-2.6% high purity graphite powder, and the balance is anhydrous ethanol.
4. The amber glass according to claim 3, Features The composite colorant is prepared by the following method: Fe 2 O 3 , aluminum ferrosilicate, add 20 ml of anhydrous ethanol, and mix by ultrasonic for 0.5 h to obtain a powder with uniform particles. 2 SO 4 NH 4 HSO 4 , high-purity graphite powder, add 20 ml of anhydrous ethanol, and mix by ultrasonic for 0.5-1h to prepare a uniformly mixed composite colorant.
5. A method for preparing amber glass according to claim 1, Features The steps include: (1) Prepare a composite colorant, continue to add the remaining oxide composition according to the above ratio, add 50 ml of anhydrous ethanol, put it into a mixer for mixing, the speed is 50-200 r / min, and the time is 1-1.5 hours; (2) After the batch material is placed in an oven for drying, it is placed in a platinum crucible for melting. The feeding temperature is 900-1000°C. After the feeding, nitrogen is introduced. The melting temperature is 1450-1520°C and the holding time is 0.5-1.5h. (3) The copper plate for glass casting is preheated in advance, the preheating temperature is 480℃~520℃, the melted and clarified glass liquid is taken out from the high-temperature furnace and cast on the preheated copper plate; (4) The cast glass is placed in an annealing furnace. The annealing temperature is: 480°C ~ 520°C for 1 hour, then cooled to 400°C at a rate of 5°C / min, and then cooled to 280°C at a rate of 3°C / min. Then, it is cooled to room temperature in the furnace to prepare amber glass.
6. A method for preparing amber glass according to claim 5, Features: The amber glass contains Fe 2 + / Fe 3+ It is 1.76-2.
25.
7. A method for preparing amber glass according to claim 5, Features: The visible light transmittance of the amber glass is ≤35%.
8. A method for preparing amber glass according to claim 5, Features: The transmittance of the amber glass is 0 in the range of 10-300 nm.
9. A method for preparing amber glass according to claim 5, Features: The amber glass has a chromaticity L of 18-24, a of 5-8, and b of 4-8.
Citation Information
Patent Citations
Amber alumina silicate glass
CN103395985A
Sodium-calcium-silicon glass with high visible light transmittance
CN115052844A
Mixture for the production of an amber glass, amber glass, method for the production of tubes and blanks of tinted bulbs, and tinted bulbs obtained with said glass
CN1914127A
Deep-colored amber glass and glass bottle
JP2000233940A