Boiling-resistant odor-removing antibacterial enamel glaze as well as preparation method and application thereof
By using water-resistant antibacterial enamel glaze prepared with feldspar and other materials, a trapped hole structure is formed to lock nano zinc oxide, which solves the problem of poor antibacterial performance of the oven inner liner in high-temperature water vapor environment, and achieves long-term antibacterial and odor removal Effective, reduce costs.
Patent Information
- Application Number
- CN202411160996.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-22
AI Technical Summary
The antibacterial enamel layer in the existing oven liner has poor antibacterial performance in high temperature and water vapor environments, which can easily lead to bacterial growth and odor residues, and is costly.
Boiled antibacterial enamel glaze prepared with feldspar, pyroxene, sodium titanate, cerium oxide, polyol, clay, carbonamide, barium molybdate and nano zinc oxide, and then forming a trap through sintering and grinding. The hole structure locks nano zinc oxide to achieve long-term antibacterial and odor removal functions.
The enamel glaze still maintains excellent antibacterial properties after soaking in distilled water in 50℃ for 7 days. It is effective against E. coli and Staphylococcus aureus, and its odor removal ability reaches 99.8%, solving the problems of bacterial growth and odor residue in the oven. Reduced costs.
Smart Images

Figure BDA0005006403690000101 
Figure BDA0005006403690000111 
Figure BDA0005006403690000151
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of novel polymer coatings and relates to an enamel material, in particular to an antibacterial enamel material capable of resisting boiling and removing odor, and a preparation method and application thereof. Background Art
[0002] At present, in order to meet the different needs of families, enamel inner pots are often larger. If the oven is not used for a long time or is not cleaned in time, due to the residue of food and water vapor, Escherichia coli, Staphylococcus aureus, etc. in the inner pot will breed, which will not only affect the quality of food, but also may endanger the health of users. In addition, the inner pot of the oven is not convenient to disassemble, which can easily cause a vicious cycle of pollution and affect the normal use of users. As people pay more and more attention to the quality of life and the hygiene of the family environment, they hope that daily necessities have sterilization and disinfection functions. The inner pots of ovens in the industry generally have poor antibacterial and antibacterial properties, which are difficult to meet the national standards.
[0003] At present, the antibacterial agent used in the antibacterial enamel layer in the industry generally adopts ionic silver salts such as silver nitrate and titanium silver, and the antibacterial purpose is achieved by adjusting the amount of silver ions added. Silver ions are easy to volatilize during the heating process, which is easy to cause waste in the production process and reduce the antibacterial properties of the enamel; only the free silver ions precipitated in the process can produce antibacterial properties. These precipitated anions may be absorbed by the human body through food and cause certain harm. There is an antibacterial enamel cookware, the antibacterial agent adopts the enamel layer of photocatalyst. The photocatalyst needs to be under the action of light to have an antibacterial effect, and the oven liner is in a closed environment. Therefore, the photocatalyst used in the oven liner does not have antibacterial ability. There is also an antibacterial electric oven enamel liner and a manufacturing method thereof. The antibacterial agent adopts nano-silver, nano-copper and nano-silver phosphate antibacterial enamel coating. Since nano-silver and nano-copper are not resistant to high temperature and boiling, they are easy to agglomerate and oxidize, resulting in uneven antibacterial properties and poor antibacterial durability in the antibacterial enamel layer. For an oven liner using this enamel layer, the antibacterial effect of the enamel layer gradually decreases or even disappears as the oven liner is used for a long time in high and low temperatures and water vapor.
[0004] There is also an antibacterial low-temperature resistant thermal insulation material, which improves its antibacterial properties by adding an antibacterial agent composed of silver-loaded zirconium phosphate, etc., and has good antibacterial properties and good antibacterial durability, but requires a larger amount of addition to achieve a better antibacterial effect. Since the antibacterial agent is expensive, a larger addition amount will increase the cost.
[0005] Electric steamers and steam ovens are kitchen appliances that use electric heating elements to generate heat and steam to cook food. The electric steamers and steam ovens currently on the market can only cook food and do not have the functions of disinfection and deodorization. Every time you use an electric steamer or steam oven to cook food, there will be odors left in the appliance. If you do not clean it thoroughly after each use and there is dirt left, it will not only produce odors but also breed bacteria after a long time of use.
[0006] In view of the defects of existing electric steamers and steam ovens such as residual odor and easy breeding of bacteria, it is necessary to provide an antibacterial enamel glaze that is resistant to boiling and removes odor. Summary of the invention
[0007] In view of the shortcomings of the prior art, the purpose of the present invention is to provide an antibacterial enamel glaze that is resistant to boiling and has a deodorizing effect, and a preparation method and application thereof. The enamel glaze of the present invention has the functions of being resistant to boiling and having a lasting antibacterial and deodorizing effect, and can still maintain excellent activity in a high temperature environment, so as to solve the problem of bacteria breeding and odor residue in equipment such as electric steamers and steam ovens.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In the first aspect, the present invention provides an antibacterial enamel glaze that is resistant to boiling water and removes odors. The raw materials for preparing the antibacterial enamel glaze that is resistant to boiling water and removes odors include, by weight: 40 to 50 parts of feldspar, 15 to 25 parts of pyroxene, 10 to 15 parts of sodium silicate titanate, 4 to 6 parts of cerium oxide, 1 to 2 parts of polyol, 1 to 3 parts of clay, 1 to 2 parts of carbonamide, 0.5 to 2 parts of soda ash, 0.3 to 0.6 parts of barium molybdate, and 3 to 5 parts of nano zinc oxide.
[0010] The enamel material provided by the present invention has the functions of being resistant to boiling and having a lasting antibacterial and deodorizing effect, and can still maintain excellent activity in a high temperature environment, thereby solving the problems of bacteria breeding and odor residue in equipment such as electric steamers and steam ovens.
[0011] Exemplarily, in the raw materials for preparing the boiling-resistant and odor-removing antibacterial enamel glaze, the weight proportion of the feldspar is 40 to 50 parts, for example, 40 parts, 42 parts, 44 parts, 46 parts, 48 parts or 50 parts, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0012] The weight percentage of the pyroxene is 15 to 25 parts, for example, 15 parts, 17 parts, 19 parts, 21 parts, 23 parts or 25 parts, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0013] The weight proportion of the sodium titanate is 10 to 15 parts, for example, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts or 15 parts, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0014] The weight proportion of the cerium oxide is 4 to 6 parts, for example, 4 parts, 4.4 parts, 4.8 parts, 5.2 parts, 5.6 parts or 6 parts, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0015] The weight proportion of the polyol is 1 to 2 parts, for example, 1 part, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts or 2 parts, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0016] The weight proportion of the clay is 1 to 3 parts, for example, 1 part, 1.4 parts, 1.8 parts, 2.2 parts, 2.6 parts or 3 parts, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0017] The weight proportion of the carbonamide is 1 to 2 parts, for example, 1 part, 1.2 parts, 1.4 parts, 1.6 parts, 1.8 parts or 2 parts, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0018] The weight proportion of the soda ash is 0.5 to 2 parts, for example, 0.5, 0.8, 1.1, 1.4, 1.7 or 2 parts, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0019] The weight portion of the barium molybdate is 0.3 to 0.6 parts, for example, 0.3 parts, 0.4 parts, 0.5 parts or 0.6 parts, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0020] The weight proportion of the nano zinc oxide is 3 to 5 parts, for example, 3 parts, 3.4 parts, 3.8 parts, 4.2 parts, 4.6 parts or 5 parts, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0021] As a preferred technical solution of the present invention, the feldspar includes any one of potassium feldspar, sodium feldspar or calcium feldspar, or a combination of at least two of them. Typical but non-limiting combinations include: a combination of potassium feldspar and sodium feldspar, a combination of potassium feldspar and calcium feldspar, a combination of sodium feldspar and calcium feldspar, or a combination of potassium feldspar, sodium feldspar and calcium feldspar.
[0022] Preferably, the average particle size of the feldspar is 300-350 mesh, for example, 300 mesh, 310 mesh, 320 mesh, 330 mesh, 340 mesh or 350 mesh, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0023] In the present invention, the feldspar is selected from the XH-32 model and / or the XH-4785 model of Shijiazhuang Xinhui Mineral Products Co., Ltd. The feldspar acts as a barren raw material before the glaze is fired, which can reduce the drying shrinkage and deformation of the green body, improve the drying performance, and shorten the drying time; during firing, it can be used as a flux to reduce the firing temperature, promote the melting of clay, and diffuse and penetrate each other in the liquid phase to accelerate the formation of mullite, and the formed feldspar glass body is filled between the mullite grains of the green body, making the green body dense and reducing the gaps, thereby improving its mechanical strength and dielectric properties. In addition, the formation of feldspar glass can also improve the light transmittance and transparency of the green body, giving the green body higher mechanical strength and chemical stability.
[0024] In addition, the weight proportion of the feldspar is 40 to 50 parts. If the content is too much, the antibacterial enamel glaze will break due to brittleness. If the content is too little, the porosity of the antibacterial enamel glaze will increase and the friction resistance will be reduced.
[0025] Preferably, the particle size of the pyroxene is 40 to 80 meshes, for example, 40 meshes, 50 meshes, 60 meshes, 70 meshes or 80 meshes, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0026] Preferably, the pyroxene is selected from Shandong Laizhou Baolailuo Stone Co., Ltd.
[0027] Preferably, the polyol comprises a non-isocyanate polyurethane diol and / or a polyethylene glycol.
[0028] In the present invention, during the preparation process of the enamel glaze, the carbon dioxide gas generated by the decomposition of the polyol at high temperature forms a large number of tiny circular pores, thereby obtaining a collapsed pore structure, which can absorb nano zinc oxide and lock it inside, thereby producing antibacterial and deodorizing functions, thereby realizing the long-term antibacterial and deodorizing functions of the enamel glaze.
[0029] Preferably, the average particle size of the nano zinc oxide is 25-35 nm, for example, 25 nm, 27 nm, 29 nm, 31 nm, 33 nm or 35 nm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0030] Preferably, the nano zinc oxide is selected from any one of CS2132PA, CS1952, SHL-CRE1021 or HSL-PA-2021 produced by Guangzhou Zhongxing Nano New Materials Co., Ltd., or a mixture of two thereof.
[0031] In the present invention, the cerium oxide can make the surface of the enamel coating smoother and more compact, and is conducive to the refinement of the precipitated phase, which can improve the toughness of the enamel coating and reduce the tendency of the coating to break during wear, thereby significantly improving the wear resistance of the enamel coating; its weight proportion is 4 to 6 parts. If its content is too much, the antibacterial enamel glaze will peel off due to excessive brittleness, and if its content is too little, the wear resistance of the antibacterial enamel glaze will be reduced.
[0032] As a preferred technical solution of the present invention, the particle size range of the boiling-resistant and odor-removing antibacterial enamel glaze is D50=3~8μm, for example, it can be 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm or 8μm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0033] In a second aspect, the present invention provides a method for preparing the antibacterial enamel glaze with water boiling resistance and deodorization as provided in the first aspect, the preparation method comprising the following steps:
[0034] The raw materials for preparing the antibacterial enamel material capable of resisting boiling water and removing odor are mixed according to the formula, stirred evenly, and then sintered, ground and aged in sequence to obtain the antibacterial enamel material capable of resisting boiling water and removing odor.
[0035] As a preferred technical solution of the present invention, the sintering temperature is 900-1000°C, for example, it can be 900°C, 920°C, 940°C, 960°C, 980°C or 1000°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0036] Preferably, the sintering time is 1 to 2 hours, for example, 1 hour, 1.2 hours, 1.4 hours, 1.6 hours, 1.8 hours or 2 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0037] In the present invention, the purpose of sintering is to improve the degree of alloying of the sintered body, enhance the metallurgical bonding surface between particles, and reduce porosity and spheroidization; if the sintering temperature is too high, the green body will begin to deform, soften, and expand due to overburning, and if the sintering temperature is too low, the porosity will increase.
[0038] In addition, the polyol in the raw material for preparing the enamel glaze of the present invention forms a depressed pore structure during the sintering process, which realizes the adsorption of nano zinc oxide, so that the nano zinc oxide is locked inside the coating during use and will not be freed, thereby realizing that the enamel glaze has long-lasting antibacterial and deodorizing functions.
[0039] As a preferred technical solution of the present invention, the grinding time is 80 to 140 minutes, for example, it can be 80 minutes, 100 minutes, 120 minutes or 140 minutes, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0040] Preferably, the static aging time is 4 to 5 hours, for example, it can be 4 hours, 4.2 hours, 4.4 hours, 4.6 hours, 4.8 hours or 5 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0041] In a third aspect, the present invention provides an application of the boiling-resistant, odor-removing antibacterial enamel glaze provided in the first aspect, wherein the boiling-resistant, odor-removing antibacterial enamel glaze is used to prepare enameled metal products.
[0042] As a preferred technical solution of the present invention, the method for preparing the enameled metal product comprises the following steps:
[0043] The metal substrate is sandblasted with corundum, and after cleaning, the metal substrate is powder-sprayed with enamel glaze, and a metal product with enamel coating is obtained after high-temperature treatment.
[0044] As a preferred technical solution of the present invention, the particle size of the corundum is 40 to 60 meshes, for example, it can be 40 mesh, 44 mesh, 48 mesh, 52 mesh, 56 mesh or 60 mesh, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0045] Preferably, the pressure of the sandblasting treatment is 0.4-0.6 MPa, for example, it can be 0.4 MPa, 0.44 MPa, 0.48 MPa, 0.52 MPa, 0.56 MPa or 0.6 MPa, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0046] Preferably, the cleanliness Sa of the metal substrate after sandblasting is ≥ 2.5, for example, it can be 2.5, 2.6, 2.7, 2.8, 2.9 or 3.0, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0047] Preferably, the roughness Rz of the metal substrate after sandblasting is ≥20 μm, for example, it can be 20 μm, 22 μm, 24 μm, 26 μm, 28 μm or 30 μm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0048] Preferably, the cleaning process comprises ultrasonic cleaning and drying processes performed sequentially.
[0049] The sandblasting treatment of the present invention can not only clean the surface of the metal substrate, but also increase the surface roughness of the metal substrate, which is beneficial to increase the bonding force between the enamel coating and the substrate.
[0050] Preferably, the powder spraying process comprises electrostatic powder spraying process.
[0051] Preferably, the adsorption amount of the enamel glaze in the electrostatic powder spraying treatment is 150-200g, for example, it can be 150g, 160g, 170g, 180g, 190g or 200g, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0052] Preferably, the temperature of the high temperature treatment is 830-870°C, for example, 830°C, 840°C, 850°C, 860°C or 870°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0053] Preferably, the high temperature treatment time is 8 to 12 minutes, for example, 8 minutes, 9 minutes, 10 minutes, 11 minutes or 12 minutes, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0054] In the present invention, the purpose of the high temperature treatment is to make the solid particles in the enamel glaze bond with each other, the grains grow, the voids (pores) and grain boundaries gradually decrease, the density increases, and finally a hard polycrystalline sintered body is formed. If the temperature of the high temperature treatment is too high, the body will begin to deform, soften, and expand due to over-burning, and if the temperature is too low, the porosity will increase.
[0055] Preferably, the thickness of the enamel coating is 150 to 500 μm, for example, it can be 150 μm, 200 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm or 500 μm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable; preferably, it is 200 to 350 μm.
[0056] As a preferred technical solution of the present invention, the method for preparing an enameled metal product using the antibacterial enamel glaze that is resistant to boiling and deodorizing provided by the present invention comprises the following steps:
[0057] (1) Use corundum with a particle size of 40 to 60 mesh to sandblast the metal substrate, clean it and set it aside;
[0058] The pressure of the sandblasting treatment is 0.4-0.6 MPa, and the cleanliness of the metal substrate after the sandblasting treatment is Sa≥2.5, and the roughness is Rz≥20 μm;
[0059] (2) Powder coating the metal substrate with enamel glaze, and then high temperature treatment at 830-870° C. for 8-12 min to obtain a metal product with an enamel coating having a thickness of 150-500 μm;
[0060] The preparation method of the enamel glaze comprises: mixing the raw materials for preparing the boiling-resistant and odor-removing antibacterial enamel glaze according to the formula, stirring evenly, sintering at 900-1000° C. for 1-2 hours, grinding for 80-140 minutes, and then aging for 4-5 hours;
[0061] The powder spraying treatment includes electrostatic powder spraying treatment; the adsorption amount of the enamel glaze in the electrostatic powder spraying treatment is 150-200g.
[0062] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0063] Compared with the prior art, the present invention has the following beneficial effects:
[0064] (1) The enamel coating provided by the present invention has the characteristic of being resistant to boiling water. After being immersed in 50°C distilled water for 7 days, it still has excellent antibacterial and deodorizing properties against Escherichia coli and Staphylococcus aureus;
[0065] (2) The enamel coating provided by the present invention has the functions of long-term antibacterial and deodorizing. The recessed hole structure can lock the nano zinc oxide inside and prevent it from being released, so that the antibacterial and deodorizing functions have the same service life as the enamel layer;
[0066] (3) The preparation method of the enamel coating provided by the present invention is simple, and the enamel coating and the metal substrate have a strong bonding force. DETAILED DESCRIPTION
[0067] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0068] Examples 1-6
[0069] A boiling-resistant and odor-removing antibacterial enamel glaze, which comprises the preparation raw materials as described in Table 1, specifically as follows, in parts by weight:
[0070] Table 1
[0071] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Feldspar 40 44 50 45 47 50 Pyroxene 25 22 24 23 24 15 Sodium Silicate Titanate 15 15 14 15 14 14.4 Cerium Oxide 6 6 4 6 5 6 Polyols 2 1.8 1.4 1.5 1 2 Clay 3 3 1 2.5 2 3 Carbamide 1.4 2 1 1 1.5 2 soda ash 2 1.5 0.6 2 2 2 Barium molybdate 0.6 0.5 0.3 0.5 0.5 0.6 Nano zinc oxide 5 4.2 3.7 3.5 3 5
[0072] The average particle size of the feldspar is 350 meshes, the particle size of the pyroxene is 60 meshes, the polyol includes non-isocyanate polyurethane diol and polyethylene glycol, and the average particle size of the nano zinc oxide is 30 nm.
[0073] Comparative Examples 1-6
[0074] A boiling-resistant and odor-removing antibacterial enamel glaze, which comprises the preparation raw materials as described in Table 2, specifically as follows, in parts by weight:
[0075] Table 2
[0076]
[0077]
[0078] The average particle size of the feldspar is 350 meshes, the particle size of the pyroxene is 60 meshes, the polyol includes non-isocyanate polyurethane diol and polyethylene glycol, and the average particle size of the nano zinc oxide is 30 nm.
[0079] Comparative Example 7
[0080] This comparative example provides an antibacterial enamel material that is resistant to boiling water and removes odors. The raw materials for preparing the enamel material differ from those in Example 1 only in that:
[0081] In this comparative example, the nano zinc oxide is adjusted to an equal weight of a silver salt antibacterial agent (silver activated carbon).
[0082] Comparative Example 8
[0083] This comparative example provides an antibacterial enamel material that is resistant to boiling water and removes odors. The raw materials for preparing the enamel material differ from those in Example 1 only in that:
[0084] In this comparative example, the nano zinc oxide is adjusted to an equal weight of copper salt antibacterial agent (copper oxychloride and copper hydroxide).
[0085] Application Example 1
[0086] This application example provides a method for preparing an enameled metal product using the raw materials provided in Example 1, the method comprising the following steps:
[0087] (1) The metal substrate is sandblasted with corundum having a particle size of 50 mesh and then cleaned for later use;
[0088] The pressure of the sandblasting treatment is 0.5 MPa, and the cleanliness Sa of the metal substrate after the sandblasting treatment is 2.5, and the roughness Rz is 25 μm;
[0089] (2) The metal substrate is powder-coated with enamel glaze, and a metal product with an enamel coating having a thickness of 250 μm is obtained after high-temperature treatment at 850° C. for 10 min;
[0090] The preparation method of the enamel glaze comprises: mixing the raw materials for preparing the antibacterial enamel glaze that is resistant to boiling and deodorizing according to the formula, stirring evenly, sintering at 950° C. for 1.5 hours, grinding for 110 minutes, and then aging for 4.5 hours;
[0091] The powder spraying treatment includes electrostatic powder spraying treatment; the adsorption amount of enamel glaze in the electrostatic powder spraying treatment is 175g.
[0092] Application Example 2
[0093] This application example provides a method for preparing an enameled metal product using the raw materials provided in Example 2, the method comprising the following steps:
[0094] (1) The metal substrate is sandblasted with corundum having a particle size of 40 mesh and then cleaned for later use;
[0095] The pressure of the sandblasting treatment is 0.4 MPa, and the cleanliness Sa of the metal substrate after the sandblasting treatment is 2.5, and the roughness Rz is 20 μm;
[0096] (2) The metal substrate is powder-coated with enamel glaze, and a metal product with an enamel coating having a thickness of 200 μm is obtained after high-temperature treatment at 830° C. for 12 min;
[0097] The preparation method of the enamel glaze comprises: mixing the raw materials for preparing the boiling-resistant and odor-removing antibacterial enamel glaze according to the formula, stirring evenly, sintering at 900° C. for 2 hours, grinding for 140 minutes, and then aging for 4 hours;
[0098] The powder spraying treatment includes electrostatic powder spraying treatment; the adsorption amount of the enamel glaze in the electrostatic powder spraying treatment is 150g.
[0099] Application Example 3
[0100] This application example provides a method for preparing an enameled metal product using the raw materials provided in Example 3, the method comprising the following steps:
[0101] (1) The metal substrate is sandblasted with corundum having a particle size of 60 mesh and then cleaned for later use;
[0102] The pressure of the sandblasting treatment is 0.6 MPa, and the cleanliness Sa of the metal substrate after the sandblasting treatment is 3.5, and the roughness Rz is 35 μm;
[0103] (2) The metal substrate is powder-coated with enamel glaze, and a metal product with an enamel coating having a thickness of 280 μm is obtained after high-temperature treatment at 870° C. for 12 min;
[0104] The preparation method of the enamel glaze comprises: mixing the raw materials for preparing the antibacterial enamel glaze that is resistant to boiling and deodorizing according to the formula, stirring evenly, sintering at a temperature of 1000° C. for 1 hour, grinding for 80 minutes, and then aging for 5 hours;
[0105] The powder spraying treatment includes electrostatic powder spraying treatment; the adsorption amount of enamel glaze in the electrostatic powder spraying treatment is 200g.
[0106] Application Examples 4-6
[0107] A method for preparing enameled metal products using the raw materials for preparing the antibacterial enamel glaze with boiling resistance and deodorization provided by Examples 4-6, the method is the same as that of Application Example 1.
[0108] Application Example 7
[0109] This application example provides a method for preparing an enameled metal product using the raw materials provided in Example 1. The method is different from Application Example 1 only in that:
[0110] In this application example, the temperature of the high temperature treatment in step (2) is adjusted to 800°C.
[0111] Application Example 8
[0112] This application example provides a method for preparing an enameled metal product using the raw materials provided in Example 1. The method is different from Application Example 1 only in that:
[0113] In this application example, the temperature of the high temperature treatment in step (2) is adjusted to 900°C.
[0114] Application Example 9
[0115] This application example provides a method for preparing an enameled metal product using the raw materials provided in Example 1. The method is different from Application Example 1 only in that:
[0116] In this application example, the sintering temperature in the preparation method of the enamel glaze in step (2) is adjusted to 850°C.
[0117] Application Example 10
[0118] This application example provides a method for preparing an enameled metal product using the raw materials provided in Example 1. The method is different from Application Example 1 only in that:
[0119] In this application example, the sintering temperature in the preparation method of the enamel glaze in step (2) is adjusted to 1050°C.
[0120] Comparative Application Examples 1-8
[0121] A method for preparing enameled metal products using the boiling-resistant, odor-removing antibacterial enamel glaze preparation raw materials provided in Comparative Examples 1-8, the method being the same as that in Application Example 1.
[0122] Performance testing:
[0123] The enamel coatings provided in the above application examples and comparative application examples were immersed in 50°C distilled water for 7 days and then subjected to performance tests:
[0124] (1) According to "GB / T 21551.2-2010 Annex A Antibacterial Performance Test Method (Film Pasting Method) and Effect Evaluation", the enamel coatings after boiling were tested for antibacterial properties of common infectious bacteria (such as Escherichia coli and Staphylococcus aureus). The results are shown in Table 3.
[0125] The calculation formula of antibacterial rate is: Antibacterial rate (%) = [(number of viable bacteria in control sample - number of viable bacteria in antibacterial enamel metal products) / number of viable bacteria in control sample] × 100%
[0126] (2) According to GB 21551.4-2010 Special requirements for refrigerators with antibacterial, sterilizing and purification functions for household and similar electrical appliances, the deodorizing function of the enamel coating after boiling was tested, and the results are shown in Table 3;
[0127] Table 3
[0128]
[0129] According to Table 3, we can know the following:
[0130] (1) Comprehensive analysis of application examples 1-6 shows that the enamel coating provided by the present invention has the functions of being resistant to boiling and having a long-lasting antibacterial and deodorizing effect. After boiling, it has excellent antibacterial properties against Escherichia coli and Staphylococcus aureus; it also has excellent removal performance against methyl mercaptan and trimethylamine; the antibacterial property of the enamel coating can still reach 99.9%, and the deodorizing ability can reach 99.8%;
[0131] (2) Comprehensive analysis of Application Examples 1 and 7-10 shows that the process parameters in the coating preparation process will affect the coating thickness, and thus affect the performance of the coating;
[0132] Among them, the high temperature treatment temperature in the coating preparation process will affect the solid particles of the enamel layer to bond with each other, the grains to grow, the gaps (pores) to increase, and the density to increase. Inappropriate high temperature treatment temperature will lead to the loss of nano zinc oxide; the sintering temperature in the preparation method of enamel glaze will increase the metallurgical bonding surface between the particles, affect the porosity and spheroidization, and inappropriate sintering temperature will cause the loss of nano zinc oxide;
[0133] (3) Comprehensive analysis of Application Example 1 and Comparative Application Examples 1-6 shows that the content of the ingredients in the enamel glaze formula will affect the coating performance;
[0134] Among them, the content of the feldspar will affect the deodorizing ability of the coating; the addition of excessive feldspar will cause white particles to appear on the surface of the coating. When the coating enamel is sintered, barium molybdate (adhesive) reacts with the metal matrix to produce gases such as CO, H2, and CO2. During cooling, some of the gases are not discharged, resulting in the formation of a uniformly distributed and sized multi-porous cross-sectional structure inside the coating. During the water boiling test, OH - It will enter the pores, destroy the coating structure, cause the loss of nano zinc oxide and make the deodorizing performance ineffective;
[0135] The content of cerium oxide will affect the deodorizing ability of the coating; the presence of cerium oxide will make the surface of the enamel coating smoother and more compact, and is conducive to the refinement of the precipitated phase; it can improve the toughness of the enamel coating and reduce the tendency of the coating to break during the test, thereby significantly improving the performance of the enamel coating, protecting the stability of the enamel coating, and locking the nano zinc oxide material;
[0136] The polyol is an important component for providing the nano zinc oxide with a collapsed pore structure. If the polyol is omitted, the nano zinc oxide cannot be evenly dispersed and embedded in the enamel coating.
[0137] The nano zinc oxide has antibacterial and deodorizing properties, but if its content is too high, it will cause agglomeration during the preparation of enamel powder, affecting the enamelling rate;
[0138] (4) Comprehensive analysis of Application Example 1 and Comparative Application Examples 7-8 shows that, compared with nano zinc oxide, after boiling in water, the silver salt and copper salt antibacterial agents are free in the coating and cannot achieve antibacterial and deodorizing effects.
[0139] In summary, the enamel glaze provided by the present invention has the functions of being resistant to boiling water and having long-lasting antibacterial and deodorizing effects, and can still maintain excellent activity in a high temperature environment, so as to solve the problems of bacterial growth and odor residue in equipment such as electric steamers and steam ovens.
[0140] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An antibacterial enamel material that is resistant to boiling water and removes odors. It is characterized in that The raw materials for preparing the boiling-resistant and odor-removing antibacterial enamel glaze include, by weight: 40 to 50 parts of feldspar, 15 to 25 parts of pyroxene, 10 to 15 parts of sodium silicate titanate, 4 to 6 parts of cerium oxide, 1 to 2 parts of polyol, 1 to 3 parts of clay, 1 to 2 parts of carbonamide, 0.5 to 2 parts of soda ash, 0.3 to 0.6 parts of barium molybdate, and 3 to 5 parts of nano zinc oxide.
2. The antibacterial enamel material having boiling resistance and deodorization according to claim 1, It is characterized in that The feldspar includes any one of potassium feldspar, sodium feldspar or calcium feldspar, or a combination of at least two of them; Preferably, the average particle size of the feldspar is 300-350 mesh; Preferably, the particle size of the pyroxene is 40 to 80 mesh; Preferably, the polyol comprises a non-isocyanate polyurethane diol and / or polyethylene glycol; Preferably, the average particle size of the nano zinc oxide is 25 to 35 nm.
3. The antibacterial enamel material having boiling resistance and deodorization according to claim 1 or 2, It is characterized in that The particle size range of the boiling-resistant and odor-removing antibacterial enamel material is D50=3-8 μm.
4. A method for preparing the antibacterial enamel glaze having boiling resistance and deodorization as claimed in any one of claims 1 to 3, It is characterized in that The preparation method comprises the following steps: The raw materials for preparing the antibacterial enamel material capable of resisting boiling water and removing odor are mixed according to the formula, stirred evenly, and then sintered, ground and aged in sequence to obtain the antibacterial enamel material capable of resisting boiling water and removing odor.
5. The preparation method according to claim 4, It is characterized in that The sintering temperature is 900-1000°C; Preferably, the sintering time is 1 to 2 hours.
6. The preparation method according to claim 4, It is characterized in that The grinding time is 80 to 140 minutes; Preferably, the static aging time is 4 to 5 hours.
7. An application of the antibacterial enamel material having boiling resistance and deodorization as claimed in any one of claims 1 to 3, It is characterized in that The antibacterial enamel material capable of resisting boiling and removing odor is used for preparing enamel metal products.
8. The use according to claim 7, It is characterized in that The preparation method of the enameled metal product comprises the following steps: The metal substrate is sandblasted, and after cleaning, the metal substrate is powder-sprayed with enamel glaze, and after high-temperature treatment, a metal product with an enamel coating is obtained.
9. The use according to claim 8, It is characterized in that The particle size of the corundum used in the sandblasting process is 40 to 60 meshes; Preferably, the pressure of the sandblasting treatment is 0.4-0.6 MPa; Preferably, the cleanliness Sa of the metal substrate after sandblasting is ≥2.5, and the roughness Rz is ≥20 μm; Preferably, the powder spraying process comprises electrostatic powder spraying process; Preferably, the adsorption amount of the enamel frit in the electrostatic powder spraying treatment is 150 to 200 g; Preferably, the temperature of the high temperature treatment is 830-870°C; Preferably, the high temperature treatment time is 8 to 12 minutes.
10. The use according to claim 8, It is characterized in that The thickness of the enamel coating is 150-500 μm, preferably 200-350 μm.
Citation Information
Patent Citations
Antibacterial enamel tank for water heater and production method thereof
CN102944063A
Antibacterial enamel material and preparation method and application thereof
CN105601113A
Enamel glaze material, enamel slurry, and preparation method and application thereof
CN105948500A
Ceramic tile with excellent thermal comfort and method for preparing ceramic tile
CN106220243A
Antibacterial ceramic and preparation method thereof
CN112299819A
Cited By
Enamel composite board as well as preparation method and application thereof
CN119567705A