Large-area Prussian blue film and preparation method thereof

By reacting Ti3C2Tx MXene nanosheets with solutions of ferrocyanide, trivalent ferric salt and potassium salt on conductive substrates, the uniformity and efficiency of large-area film preparation are solved, and efficient electrochromicity is achieved And charge and discharge performance, suitable for multi-function smart windows and zinc ion batteries.

CN119019185AActive Publication Date: 2024-11-26NORTHWESTERN POLYTECHNICAL UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411139466.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The existing Prussian blue film preparation methods are difficult to achieve uniform and rapid preparation on large-size substrates, especially in the fields of electrochromic devices and ion batteries.

Method used

Ti3C2Tx MXene nanosheets react with solutions of ferrocyanide, trivalent ferrous salt and potassium salt to form a Prussian blue film on the conductive substrate. The film thickness and uniformity are controlled by regulating the MXene concentration, number of coatings and soaking time.

Benefits of technology

It realizes the rapid and simple preparation of large-area Prussian blue films at room temperature, with high efficiency electrochromic and charging and discharging performance, is suitable for multi-function smart windows and zinc ion batteries, and maintains 96% optical modulation after 200 cycles. Range and 70% discharge capacity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019185A_ABST
    Figure CN119019185A_ABST
Patent Text Reader

Abstract

The invention discloses a large-area Prussian blue film and a preparation method thereof, belongs to the technical field of electrochromism and ion batteries, and solves the problem that the large-scale production of the current large-area Prussian blue film is difficult to realize. According to the preparation method, trivalent iron ions are reduced by using MXene low-valence titanium elements to generate divalent iron ions, in-situ growth of the Prussian blue film is realized on the basis of coordination of the divalent iron ions and ferricyanide in a solution, and the Prussian blue film with a proper thickness is obtained by adjusting the concentration of MXene, the coating frequency and the reaction time. The preparation process of the large-area Prussian blue film provided by the invention does not need high-temperature treatment, strict preparation conditions and complex preparation equipment, the process is simple and rapid, the size of the conductive substrate is not limited, and large-scale preparation of the Prussian blue film is easy to realize; and an efficient way is provided for practical application of the Prussian blue film in electrochromic devices and ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrochromic and ion batteries, and in particular relates to a large-area Prussian blue film and a preparation method thereof. Background Art

[0002] The development and use of new energy materials and devices is an effective way to alleviate energy shortages. Among them, electrochromic devices are considered to be a new type of energy-saving product with development and application potential. Electrochromic devices can regulate the optical properties of materials such as transmittance, absorption or reflection under the action of an applied voltage. Electrochromic devices are applied to different occasions, and smart products such as electrochromic smart windows, anti-glare rearview mirrors, and electrochromic glasses are derived. Since the working principle of ion embedding and migration of electrochromic materials is similar to that of ion batteries, electrochromic materials can also be used in ion battery positive electrode materials. The devices constructed in this way have the characteristics of electrochromic and charging and discharging multifunctional integration. This multifunctional device can be used as an electrochromic smart window to reduce the energy consumption of lighting and refrigeration by regulating the transmission of light and heat entering buildings and vehicles. At the same time, it can store electrical energy in the color change reaction process as an ion battery, which makes the electrochromic device more efficient and practical. The multifunctional smart windows used in buildings and transportation vehicles require the preparation of electrochromic films with controllable and uniform thickness on large-size substrates. Therefore, it is of great significance to develop large-area film preparation technology for electrochromic and battery fields.

[0003] Prussian blue is an electrochromic material with rich color changes. Its open framework structure is conducive to the embedding and extraction of ions. This structural characteristic allows it to accommodate monovalent and polyvalent metal ions as a host material. Therefore, it is also used in the research of positive electrode materials for lithium, sodium, potassium, zinc and other ion batteries. Therefore, Prussian blue has broad application scenarios and important research significance in the fields of electrochromism and ion batteries. The currently reported methods for preparing Prussian blue thin films mainly include hydrothermal method (Solar Energy Materials and Solar Cells, 2018, 177: 9-14), electrodeposition method (ThinSolidFilm, 2013, 542: 45-5 (1) and spray pyrolysis method (Optik, 2017, 129: 130-139). The hydrothermal method is limited by the size of the high-pressure reaction vessel and it is difficult to prepare large-area thin films. When preparing by electrodeposition, due to the poor conductivity of the transparent electrode, uneven thin films will occur when deposited over a large area. The spray pyrolysis method requires spraying the solution at high temperature, which poses safety risks and energy consumption problems.

[0004] In summary, the above methods are difficult to achieve the preparation of large-area Prussian blue films. With the rapid development of urban modernization, glass curtain walls are gradually replacing building walls, and new energy vehicles are constantly innovating in energy conservation and emission reduction. Therefore, the development of a simple method suitable for large-scale preparation of large-area Prussian blue films is of great significance for the research and practical application of multifunctional electrochromic smart windows. Summary of the invention

[0005] The purpose of the present invention is to provide a large-area Prussian blue film and a preparation method thereof, so as to solve the problem that the existing preparation method of the Prussian blue film is difficult to achieve uniform and rapid preparation on a large-size substrate.

[0006] To achieve the above object, the present invention provides a method for preparing a large-area Prussian blue film, comprising the following steps:

[0007] (1) Ti3C2T x MXene nanosheets are dispersed in the dispersion solvent and evenly coated on the surface of the conductive substrate;

[0008] (2) dissolving ferrocyanide, ferric salt and potassium salt in water to obtain a uniform solution;

[0009] (3) Immersing the conductive substrate obtained in step (1) in the solution of step (2) to react, and forming a Prussian blue film on the surface of the conductive substrate after the reaction is completed.

[0010] Preferably, in step (1), the dispersion solvent is deionized water or anhydrous ethanol, Ti3C2T x The concentration of MXene nanosheets in the dispersion solvent is 1 to 5 mg / mL, and the coating method is either blade coating or spray coating.

[0011] Preferably, in step (1), the conductive substrate is any one of electrode materials such as a transparent tin-doped indium oxide substrate, a fluorine-doped tin oxide substrate, an aluminum-doped zinc oxide substrate, a silver nanowire transparent conductive substrate or an opaque carbon nanotube substrate, a graphene substrate or a metal foil, and the size of the conductive substrate is not limited.

[0012] Preferably, in step (2), the ferrocyanide is one or more of potassium ferrocyanide and sodium ferrocyanide, and the molar concentration is 2 to 50 mmol / L;

[0013] The iron salt is one or more of ferric chloride, ferric nitrate and ferric sulfate, and the molar concentration is 2 to 50 mmol / L;

[0014] The potassium salt is one or more of potassium chloride, potassium sulfate and potassium nitrate, and the molar concentration is 2-100 mmol / L.

[0015] Preferably, the total immersion time in step (3) is 30 to 200 seconds, and the immersion is divided into one immersion or multiple immersions. Before each immersion, Ti3C2T x MXene nanosheet dispersion.

[0016] Preferably, in step (1), the Ti3C2T x MXene nanosheets are prepared by in situ etching of Ti3AlC2MAX phase with a mixed solution of lithium fluoride and concentrated hydrochloric acid.

[0017] The invention also provides a large-area Prussian blue film prepared by the preparation method.

[0018] Mechanism of the invention:

[0019] like Figure 1 The present invention pre-coats Ti3C2Tx MXene nanosheets onto the surface of a conductive substrate. The low-valent titanium in MXene is reducible. The precursor solution contains trivalent iron salts and ferrocyanide. The trivalent iron is reduced by low-valent titanium to generate divalent iron ions. The generated divalent iron ions coordinate with the ferrocyanide in the solution to form a Prussian blue / MXene composite material in situ on the MXene surface. The uniformity and size of the Prussian blue film are determined by the process of nanosheet deposition. The size of the conductive substrate can be any size and can be customized according to demand. The film thickness of Prussian blue can be increased by repeatedly depositing MXene-immersion reaction and adjusting experimental parameters.

[0020] Therefore, the present invention adopts the above-mentioned large-area Prussian blue film and preparation method thereof, and its beneficial effects are:

[0021] 1. Based on the redox reaction of low-valent titanium element in MXene and trivalent iron ions, divalent iron ions are generated. The divalent iron ions coordinate with ferrocyanide in the solution to form a Prussian blue film in situ on the surface of MXene. By adjusting the MXene concentration, coating times and immersion time, a Prussian blue film of appropriate thickness can be obtained.

[0022] 2. Compared with the existing technology, the preparation process of this method is simple and fast, and does not require strict preparation conditions and complex preparation equipment. It can achieve the preparation of Prussian blue films larger than 30×30 cm, providing an economical and efficient way for the practical application of electrochromic devices.

[0023] 3. The prepared Prussian blue / MXene composite material utilizes the excellent conductivity and porous properties of MXene, which is beneficial to the transmission of ions and electrons during electrochromism and charging and discharging, and improves the color change and charging and discharging rate and stability of the device.

[0024] 4. The device constructed by using the Prussian blue film prepared by the present invention and the metal zinc electrode has an optical modulation range of 60% as an electrochromic device, and after 200 cycles, the optical modulation range remains at 96% of the initial value.

[0025] 5. The device using the Prussian blue film prepared by the present invention and the metal zinc electrode structure as a zinc ion battery has a discharge capacity of 56.3 mAh m -2 , and after 100 cycles the capacity still remains at 70% of the initial value.

[0026] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Schematic diagram of the preparation mechanism of the present invention.

[0028] Figure 2 This is a photograph of a Prussian blue film with an area of ​​30×30 cm prepared in Example 1 of the present invention.

[0029] Figure 3 This is a planar image of a Prussian blue film obtained in Example 1 of the present invention, taken under a scanning electron microscope.

[0030] Figure 4 This is a cross-sectional image of a Prussian blue film obtained in Example 1 of the present invention, taken under a scanning electron microscope.

[0031] Figure 5 This is a schematic diagram of the structure of a device assembled from a Prussian blue film and a zinc electrode prepared in Example 1 of the present invention.

[0032] Figure 6 This is the time-transmission spectrum of the Prussian blue electrochromic film prepared in Example 1 of the present invention.

[0033] Figure 7 This is a test chart of the cyclic stability of the Prussian blue electrochromic film prepared in Example 1 of the present invention.

[0034] Figure 8 This is a test chart of the charge and discharge cycle stability of a zinc ion battery using the Prussian blue film prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0035] Based on the attached Figure 1 The present invention provides a method for preparing a large-area Prussian blue film, comprising the following steps:

[0036] (1) Ti3C2T xMXene nanosheets are dispersed in a dispersion solvent and uniformly coated on the surface of a conductive substrate; the dispersion solvent is deionized water or anhydrous ethanol, Ti3C2T x The concentration of MXene nanosheets in the dispersion solvent is 1 to 5 mg / mL, and the coating method is either blade coating or spray coating.

[0037] The conductive substrate is any one of electrode materials such as a transparent tin-doped indium oxide substrate, a fluorine-doped tin oxide substrate, an aluminum-doped zinc oxide substrate, a silver nanowire transparent conductive substrate, or an opaque carbon nanotube substrate, a graphene substrate, or a metal foil, and the size of the conductive substrate is not limited.

[0038] (2) Dissolving ferrocyanide, trivalent iron salt and potassium salt in water to obtain a uniform solution; the ferrocyanide is one or more of potassium ferrocyanide and sodium ferrocyanide, with a molar concentration of 2 to 50 mmol / L; the iron salt is one or more of ferric chloride, ferric nitrate and ferric sulfate, with a molar concentration of 2 to 50 mmol / L; the potassium salt is one or more of potassium chloride, potassium sulfate and potassium nitrate, with a molar concentration of 2 to 100 mmol / L.

[0039] (3) soaking the conductive substrate obtained in step (1) in the solution of step (2) to react, and forming a Prussian blue film on the surface of the conductive substrate after the reaction is completed. The total soaking time in step (3) is 30 to 200 seconds, and the soaking is divided into one soaking or multiple soakings. Before each soaking, Ti3C2T x MXene nanosheet dispersion.

[0040] In step (1), Ti3C2T x MXene nanosheets are prepared by in situ etching of Ti3AlC2MAX phase with a mixed solution of lithium fluoride and concentrated hydrochloric acid.

[0041] The present invention is further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Any other changes, modifications, substitutions, combinations, simplifications made without violating the spirit and principle of the present invention should all be equivalent replacement methods and are included in the protection scope of the present invention. In addition, it should be understood that after reading the content of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application, and all belong to the scope of protection of the present invention.

[0042] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.

[0043] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.

[0044] Unless otherwise specified in the present invention, the reagents, instruments, and equipment used are those commonly used by technicians in this field.

[0045] Embodiment 1:

[0046] Ti3C2T was prepared by in-situ etching of Ti3AlC2 MAX phase using a mixed solution of lithium fluoride and concentrated hydrochloric acid. x MXene nanosheets, wherein the etching solution contains 2 g of lithium fluoride, 10 mL of deionized water, 30 mL of concentrated hydrochloric acid, and 1.6 g of Ti3AlC2. x MXene nanosheets were dissolved in anhydrous ethanol at a concentration of 5 mg / mL. x The MXene dispersion was sprayed onto 2×3 cm and 30×30 cm tin-doped indium oxide substrates. Potassium ferrocyanide, ferric chloride trihydrate and potassium chloride were dissolved in deionized water. The concentration of potassium ferrocyanide was 10 mmol / L, the concentration of ferric chloride trihydrate was 10 mmol / L, and the concentration of potassium chloride was 50 mmol / L. The conductive substrate on which MXene was deposited was immersed in the above solution for 30 seconds, and the conductive substrate was sprayed with Ti3C2T for five times. x MXene dispersion-immersion reaction, Ti3C2T x The spraying amount of MXene dispersion is 0.01mL / cm 2 , taken out, washed and dried, a layer of Prussian blue electrochromic film can be obtained on the tin-doped indium oxide substrates of two sizes.

[0047] Figure 2 This is a photo of a large area (30×30 cm) of Prussian blue film. Figure 3 This is a scanning electron microscope image of the Prussian blue electrochromic film (plane). It can be seen that nano-particles of Prussian blue are evenly distributed on the surface of the conductive substrate. Figure 4This is a scanning electron microscope image of a Prussian blue electrochromic film (cross section), showing that the average thickness of the Prussian blue film is about 300 nm.

[0048] In order to test the performance of the prepared Prussian blue film, a device was constructed by combining a 2×3 cm Prussian blue electrode and a zinc electrode. The device structure is shown in the figure below. Figure 5 shown.

[0049] The electrochromic and energy storage characteristics test results are as follows Figure 6 , Figure 7 and Figure 8 As shown:

[0050] Figure 6 This is a time-transmittance spectrum of the electrochromic reaction of the Prussian blue film of an embodiment of the present invention. It can be seen from the figure that the optical modulation of the Prussian blue electrochromic film at a wavelength of 700nm is 60%;

[0051] Figure 7 This is a cyclic stability test of the electrochromic Prussian blue film of an embodiment of the present invention. From the results in the figure, it can be seen that after 200 cycles of testing at a wavelength of 700nm, the optical modulation range of the material remains at 96% of the initial value, which has good stability.

[0052] Figure 8 The Prussian blue film of the present invention is used for the charge and discharge cycle stability test of the zinc ion battery. The results in the figure show that the initial capacity of the battery is 56.3 mAh m -2 , after 100 cycles, the capacity remained at 70% of the initial value, with good stability.

[0053] Embodiment 2:

[0054] Ti3C2T was prepared by in-situ etching of Ti3AlC2 MAX phase using a mixed solution of lithium fluoride and concentrated hydrochloric acid. x MXene nanosheets, Ti3C2T x MXene nanosheets were dissolved in deionized water at a concentration of 5 mg / mL. x The MXene aqueous dispersion was sprayed onto the tin-doped indium oxide substrate. Potassium ferrocyanide, ferric chloride trihydrate and potassium chloride were dissolved in deionized water. The concentration of potassium ferrocyanide was 10 mmol / L, the concentration of ferric chloride trihydrate was 10 mmol / L, and the concentration of potassium chloride was 50 mmol / L. x The MXene substrate was immersed in the above solution and reacted for 30 seconds, and the color of the generated blue Prussian blue film no longer deepened. After washing and drying, a layer of Prussian blue electrochromic film was obtained.

[0055] Embodiment 3:

[0056] Ti3C2T x MXene nanosheets were dissolved in anhydrous ethanol at a concentration of 3 mg / mL. The aqueous MXene dispersion was sprayed onto a tin-doped indium oxide substrate. Potassium ferrocyanide, ferric chloride trihydrate, and potassium chloride were dissolved in deionized water. The concentration of potassium ferrocyanide was 10 mmol / L, the concentration of ferric chloride trihydrate was 10 mmol / L, and the concentration of potassium chloride was 50 mmol / L. Ti3C2T x The MXene substrate was immersed in the above solution and reacted for 30 seconds, and the color of the generated blue Prussian blue film no longer deepened. After washing and drying, a layer of Prussian blue electrochromic film was obtained.

[0057] Embodiment 4:

[0058] Ti3C2T x MXene nanosheets were dissolved in deionized water at a concentration of 3 mg / mL. x The MXene dispersion was sprayed onto the tin-doped indium oxide substrate. Sodium ferrocyanide, ferric chloride trihydrate and potassium chloride were dissolved in deionized water, wherein the concentration of potassium ferrocyanide was 10 mmol / L, the concentration of ferric chloride trihydrate was 10 mmol / L, and the concentration of potassium chloride was 50 mmol / L. x The MXene substrate was immersed in the above solution and reacted for 30 seconds, and the color of the generated blue Prussian blue film no longer deepened. After washing and drying, a layer of Prussian blue electrochromic film was obtained.

[0059] Embodiment 5:

[0060] Ti3C2T x MXene nanosheets were dissolved in anhydrous ethanol at a concentration of 5 mg / mL. x The MXene dispersion was sprayed onto a tin-doped indium oxide substrate. Sodium ferrocyanide, ferric nitrate and potassium sulfate were dissolved in deionized water, wherein the concentration of sodium ferrocyanide was 2 mmol / L, the concentration of ferric nitrate was 2 mmol / L, and the concentration of potassium sulfate was 2 mmol / L. The substrate on which the MXene was deposited was immersed in the above solution for 30 seconds, then washed and dried to obtain a layer of Prussian blue electrochromic film formed in situ on the surface of the conductive substrate.

[0061] In summary, the large-area Prussian blue film and the preparation method thereof proposed in the present invention is a method that can be carried out at room temperature, has a simple and fast process, is not limited in the size of the conductive substrate, and is easy to prepare on a large scale.

[0062] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing a large-area Prussian blue film. It is characterized in that The following steps are involved: (1) Ti 3 C 2 T x MXene nanosheets are dispersed in the dispersion solvent and evenly coated on the surface of the conductive substrate; (2) dissolving ferrocyanide, ferric salt and potassium salt in water to obtain a uniform solution; (3) Immersing the conductive substrate obtained in step (1) in the solution of step (2) to react, and forming a Prussian blue film on the surface of the conductive substrate after the reaction is completed.

2. A method for preparing a large-area Prussian blue film according to claim 1, It is characterized in that In step (1), the dispersion solvent is deionized water or anhydrous ethanol, Ti 3 C 2 T x The concentration of MXene nanosheets in the dispersion solvent is 1 to 5 mg / mL, and the coating method is either blade coating or spray coating.

3. The method for preparing a large-area Prussian blue film according to claim 1, It is characterized in that In step (1), the conductive substrate is any one of electrode materials such as a transparent tin-doped indium oxide substrate, a fluorine-doped tin oxide substrate, an aluminum-doped zinc oxide substrate, a silver nanowire transparent conductive substrate, or an opaque carbon nanotube substrate, a graphene substrate, or a metal foil, and the size of the conductive substrate is not limited.

4. The method for preparing a large-area Prussian blue film according to claim 1, It is characterized in that In step (2), the ferrocyanide is one or more of potassium ferrocyanide and sodium ferrocyanide, and the molar concentration is 2 to 50 mmol / L; The iron salt is one or more of ferric chloride, ferric nitrate and ferric sulfate, and the molar concentration is 2 to 50 mmol / L; The potassium salt is one or more of potassium chloride, potassium sulfate and potassium nitrate, and the molar concentration is 2-100 mmol / L.

5. The method for preparing a large-area Prussian blue film according to claim 1, It is characterized in that The total immersion time in step (3) is 30 to 200 seconds, and the immersion is divided into one immersion or multiple immersions. Before each immersion, Ti is coated on the conductive substrate. 3 C 2 T x MXene nanosheet dispersion.

6. The method for preparing a large-area Prussian blue film according to claim 1, It is characterized in that In step (1), the Ti 3 C 2 T x MXene nanosheets are in situ etched from Ti by a mixed solution of lithium fluoride and concentrated hydrochloric acid. 3 AlC 2 MAX phase was prepared.

7. A large area Prussian blue film, It is characterized in that The large-area Prussian blue film is prepared by the preparation method of a large-area Prussian blue film according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Prussian blue analog / MXene composite electrode material and in-situ preparation method and application thereof

    CN110783536A

  • In-situ preparation method of two-dimensional Prussian blue analogue @ MXene composite electrocatalyst

    CN112058286A

  • In-situ preparation method of two-dimensional metal selenide@MXene composite electrocatalyst

    CN112058287A

  • Preparation method of Prussian blue electrochromic film

    CN113867065A

  • In-situ self-assembled large-area multicolor electrochromic device and preparation method and application thereof