Lithium ion battery negative electrode binder and preparation method thereof

Through the active radical polymerization method, a specific functional group is introduced into the negative electrode binder of lithium-ion battery to form a block structure of styrene butadiene latex water-based binder, which solves the problems of weak bonding force and poor thermal stability in the prior art. It significantly improves the cycle life and mechanical properties of lithium-ion batteries.

CN119019593AInactive Publication Date: 2024-11-26XINXIANG RIXIN CHEM IND CO LTD +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411512041.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-28
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The negative electrode adhesives of existing lithium-ion batteries have problems such as weak bonding force, high volume change rate and unsatisfactory thermal stability, which affect the cycle life of the battery.

Method used

Using the reactive radical polymerization method, functional groups such as hydroxyl groups, carboxyl groups, and sulfonic acid groups are introduced, and by modifying styrene butadiene latex, the elasticity and adhesion of the binder are improved, and the water group with block structure is prepared. Lithium battery electrode adhesive.

Benefits of technology

It significantly improves the cycle life of the battery, reduces the cost of binder, enhances mechanical strength and flexibility, inhibits electrode expansion, improves the cycle performance and capacity of the battery, and achieves the 500 cycle capacity retention rate of 3C fast charging. More than 85%.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of lithium batteries, in particular to a lithium ion battery negative electrode binder and a preparation method thereof. The adhesive is prepared by adding an initiator, an emulsifier and water into the following raw materials in parts by weight: 20 to 40 parts of styrene, 20 to 35 parts of butadiene, 0.1 to 0.5 part of sodium methallyl sulfonate, 1 to 4 parts of acrylic acid, 1 to 4 parts of hydroxyethyl acrylate, 0.1 to 0.5 part of N-hydroxymethyl acrylamide, 0.5 to 1 part of hydroxypropyl methacrylate, 0.4 to 1 part of methacrylic acid, 0.5 to 2 parts of acrylonitrile and 0.5 to 1.5 parts of acrylamide. According to the negative electrode binder, the elasticity and cohesiveness of the binder are improved by adopting an active free radical polymerization method, and a strong acting force is formed between the binder and an electrode material by introducing a special group, so that the electrode structure of a battery electrode is kept stable in a reciprocating charge-discharge cycle, and the cycle life of the battery is greatly prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer organic materials, and in particular to a lithium ion battery negative electrode binder and a preparation method thereof. Background Art

[0002] The consumption of resources in modern society is increasing. People are paying more and more attention to how to improve the efficiency of energy utilization, and the demand for renewable clean energy is becoming more and more urgent. In recent years, the new energy industry has flourished, and lithium-ion battery technology has gradually matured and has become increasingly widespread in practical applications. The negative electrode binder is an important component of lithium-ion batteries. It plays the role of a collector and diaphragm, an electronic conductive bridge between the electrode and the external circuit of the battery, and a link to maintain the stability of the structure of the active substance. It has an important impact on improving the cycle of lithium-ion batteries. CN201810400738.5, an invention patent discloses a binder for lithium-ion batteries and a preparation method. The binder for lithium-ion batteries is compounded by an emulsion blending method with a carboxylated graphene aqueous dispersion and carboxylated styrene butadiene latex to successfully prepare a carboxylated graphene / carboxylated styrene butadiene latex composite binder with a peeling structure. CN202311239734.0, this invention patent discloses a binder for improving the electrical properties of silicon-based negative electrodes, the binder comprising methyl cellulose, citric acid, sodium alginate, polystyrene butadiene copolymer, a film-forming agent and deionized water. In order to solve environmental problems, water-based negative electrode binders have gradually become the key research direction of the industry. At present, the main negative electrode binder for lithium-ion batteries is styrene-butadiene rubber latex, but there are problems such as weak bonding force, high volume change rate, and unsatisfactory thermal stability. When used as a binder, its solubility and solid content, adhesion, mechanical strength, stability, etc. are key performance indicators. In the production process of lithium-ion batteries, the negative electrode binder needs to use an aqueous solution with a certain solid content and viscosity to uniformly coat the active material and the conductive agent, and then dry and roll to form a pole piece. The choice of solvent, increasing the solid content of the binder aqueous solution, and increasing the viscosity are of great significance for enhancing the processing performance of the negative electrode sheet. The negative electrode binder plays a bridging role in the process of pole sheet conduction and lithium ion transfer, and enhancing the polarity or flexibility of the binder segment plays an important role in improving the conductivity and mechanical processing performance of the pole piece. Therefore, there is an urgent need to develop a new type of negative electrode binder that can improve the bonding strength, stability and mechanical properties, thereby increasing the cycle life of lithium-ion batteries. Summary of the invention

[0003] The purpose of the present invention is to provide a negative electrode binder for lithium ion batteries and a preparation method thereof. The negative electrode binder improves the elasticity and adhesion of the binder by adopting an active free radical polymerization method, and forms a strong force between the binder and the electrode material by introducing special groups, so that the battery electrode maintains a stable electrode structure during reciprocating charge and discharge cycles, thereby greatly improving the cycle life of the battery.

[0004] Based on the above purpose, the present invention adopts the following technical solutions: A negative electrode binder for a lithium ion battery, characterized in that the binder is prepared by adding an initiator, an emulsifier and water to the following raw materials in parts by weight: 20-40 parts of styrene, 20-35 parts of butadiene, 0.1-0.5 parts of sodium methacrylate sulfonate, 1-4 parts of acrylic acid, 1-4 parts of hydroxyethyl acrylate, 0.1-0.5 parts of N-hydroxymethyl acrylamide, 0.5-1 parts of hydroxypropyl methacrylate, 0.4-1 parts of methacrylic acid, 0.5-2 parts of acrylonitrile and 0.5-1.5 parts of acrylamide.

[0005] Preferably, the amounts of the initiator and the emulsifier are 0.5-3% and 0.8-6% of the weight of styrene, respectively.

[0006] Preferably, the binder is a water emulsion adhesive with a solid content of 48-55%.

[0007] Preferably, the emulsifier is at least two of sodium carboxymethyl cellulose, polyoxyethylene stearate and glucitol ester.

[0008] Preferably, the emulsifier is sodium carboxymethyl cellulose, polyoxyethylene stearate and glucitol ester, and the weight ratio of the three is 1:0.3-0.5:0.4-0.6.

[0009] Preferably, the initiator is ammonium sulfate and benzoyl peroxide.

[0010] Preferably, in the initiator, the weight ratio of ammonium sulfate to benzoyl peroxide is 1:0.8-2.2.

[0011] The present invention also aims to provide a method for preparing a negative electrode binder for a lithium ion battery, comprising the following steps: S1, first mix water and emulsifier evenly, then add acrylic acid, sodium methacrylic acid sulfonate, hydroxyethyl acrylate, hydroxypropyl methacrylate, and methacrylic acid at a temperature of 25-40°C, and mix to obtain a mixed solution A; S2, mixing styrene, butadiene, N-hydroxymethyl acrylamide, acrylonitrile and acrylamide to obtain a mixed solution B; S3, mixing the mixed solution A and the mixed solution B, adding an initiator, and then heating the system to 80-110° C. and reacting for 2-4 hours; S4, the reaction solution is degassed, neutralized with alkali and then filtered to obtain the negative electrode binder.

[0012] Preferably, in step S1, the weight ratio of the emulsifier to water is 1:55-80.

[0013] Preferably, in step S4, tert-butyl hydroperoxide is added during degassing, and the added alkali is adjusted to be liquid alkali.

[0014] Sodium methyl methacrylate sulfonate introduces a sulfonic acid group, which reacts with cations (such as Na + ) has a strong affinity, which enhances the insensitivity of latex to external cationic attack, thereby improving the salt resistance and high temperature resistance of the binder.

[0015] The addition of acrylic acid and methacrylic acid introduces carboxyl groups (-COOH), which can form hydrogen bonds or chemical reactions with a variety of substances, thereby improving the bonding properties of styrene-butadiene latex. At the same time, after the participation of acrylic acid in copolymerization, the surface charge of latex particles can be increased, so that the repulsive force between particles is enhanced, and the aggregation and flocculation between particles are reduced, thereby improving the mechanical stability of the latex. The presence of carboxyl groups improves the water resistance and chemical resistance of the latex, so that it can still maintain good bonding properties in a humid or chemical environment. Furthermore, the acrylic acid-modified styrene-butadiene latex may participate in chemical reactions during the curing process to form a cross-linked structure and enhance the bonding properties of the latex. This cross-linked structure gives the latex good mechanical properties and durability.

[0016] Hydroxypropyl methacrylate contains vinyl and hydroxyl functional groups. It acts as a crosslinking monomer in styrene-butadiene latex. It undergoes a crosslinking reaction with the polymer chain through heating or the action of a catalyst to form a three-dimensional network structure, thereby improving the cohesion and mechanical strength of the latex binder. Due to its crosslinking effect, it can form a stronger adhesion between the latex binder and the bonded material, thereby improving the bonding strength. The presence of hydroxyl groups improves the water resistance and chemical resistance of the latex, allowing it to maintain good bonding properties in a humid or chemical environment.

[0017] Hydroxyethyl acrylate has a hydroxyl (-OH) functional group and can copolymerize with other monomers to increase the bonding properties of the adhesive. The hydroxyl group can also form hydrogen bonds with polar groups on the surface of the bonded material, thereby increasing the bonding strength. The addition of hydroxyethyl acrylate can improve the flexibility and impact resistance of the adhesive, making it more durable during use. Hydroxyethyl acrylate has low viscosity and high solubility, and can be used to adjust the rheological properties of the adhesive, making it easier to construct and process. The introduction of hydroxyethyl acrylate can improve the adhesion of the adhesive to various substrates, including metal, plastic, glass, etc.

[0018] N-hydroxymethyl acrylamide contains vinyl and hydroxymethyl groups in its molecular structure, which can act as a cross-linking monomer in the polymerization reaction. It can undergo a cross-linking reaction with the polymer chain through heating or the action of a catalyst to form a three-dimensional network structure, thereby increasing the cohesion and mechanical strength of the latex binder. Due to its cross-linking effect, it can form a stronger adhesion between the latex binder and the bonded material, thereby increasing the bonding strength. At the same time, it can also improve the water resistance and chemical resistance of the latex binder, allowing it to maintain good bonding properties in a humid or chemical environment.

[0019] The cyano functional group introduced by acrylonitrile has good compatibility with oil substances, thereby improving the oil resistance of the adhesive. The polymer chain formed by the copolymerization of acrylonitrile has high strength and hardness, thereby enhancing the mechanical strength of the adhesive. The cyano functional group can form a strong interaction with the surface of the bonded material to improve the bonding strength. The presence of cyano improves the chemical resistance and heat resistance of the adhesive, prevents sedimentation or stratification during storage and use, and improves the stability of the adhesive.

[0020] The amide group (-CONH2) introduced by acrylamide (AM) in the styrene-butadiene latex binder forms a strong interaction with the surface of the bonded material through hydrogen bonds, thereby improving the bonding strength. The amide group introduced by acrylamide can increase the flexibility of the binder, improve its impact resistance, and make the binder less likely to break when subjected to external forces. The introduction of the amide group can improve the rheological properties of the binder, making the binder easier to operate and apply during construction. The amide group has good chemical stability and can improve the binder's tolerance to various chemical substances.

[0021] The present invention has the following beneficial effects: The present invention prepares a styrene butadiene latex water-based lithium battery electrode binder with a block structure by adopting an active free radical polymerization method. The binder is prepared by modifying and copolymerizing styrene butadiene latex to introduce hydroxyl, carboxyl, sulfonic acid, vinyl, methylol, cyano functional groups and amide groups, thereby effectively improving its bonding performance, flexibility and mechanical strength, so that the binder forms a strong force between electrode materials, which is beneficial to maintaining the stability of the electrode structure of the battery electrode in a reciprocating charge and discharge cycle, greatly improving the cycle life of the battery, and the amount of the binder is 1.5% of the negative electrode material, and the binder cost is reduced by 30%. By controlling the affinity between the binder and the electrolyte, the increase in internal resistance is prevented to a certain extent, and the battery resistance is reduced by 15%; by controlling the monomer composition on the surface of the binder particles and performing surface modification, the bonding force between the binder and the metal electrode, the chemical stability against the electrolyte, and the stability of the colloid in the binder slurry are improved. At the same time, by improving the flexibility and mechanical strength of the binder, the expansion of the battery electrode is suppressed, and the battery capacity is increased from the original 58-61mAh to 65-68mAh; by improving the salt and chemical resistance of the binder, the cycle performance of the lithium-ion battery is improved, 3C fast charging is achieved, and the capacity retention rate after 500 cycles can reach more than 85%.

[0022] Further, the present invention uses sodium carboxymethyl cellulose, polyoxyethylene stearate and glucose alcohol fat as emulsifiers, wherein sodium carboxymethyl cellulose as an ionic emulsifier can increase the viscosity of latex, thereby improving its stability during mixing and coating, helping to disperse solid particles in latex, preventing them from aggregating and settling, thereby improving the uniformity and stability of latex. In the preparation of negative electrode slurry, CMC-Na can avoid the formation of gel, especially sesame paste gel, ensuring that the slurry has good fluidity. But at the same time, CMC-Na can increase the viscosity of styrene-butadiene latex, the curing time is long during coating, it is easy to decompose at high temperature, unstable, and not resistant to high temperature. Adding non-ionic emulsifiers, the three are used together, polyoxyethylene stearate has excellent emulsification performance and stability, can reduce the surface tension of grease, increase the friction coefficient, and in styrene-butadiene latex, polyoxyethylene stearate can form fine particles while maintaining the stability of latex without significantly affecting the viscosity. Glucose alcohol fat is a natural non-ionic emulsifier, the main components of which are glucose alcohol and alkyl glucoside. It has low surface tension, good temperature resistance and stability. In styrene-butadiene latex, glucose alcohol ester can form smaller particles without significantly increasing the viscosity of the latex, and is suitable for applications that require good stability and temperature resistance. The three emulsifiers are used in conjunction with each other to better control the viscosity of styrene-butadiene latex and ensure that the slurry has good fluidity. At the same time, polyoxyethylene stearate and glucose alcohol ester have good stability, and glucose alcohol ester also has good temperature resistance. The addition of the two improves the stability of styrene-butadiene latex and improves the defect of easy decomposition at high temperatures caused by sodium carboxymethyl cellulose. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention is described in detail below, but the following embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other implementation methods obtained by those skilled in the art without making creative work belong to the scope of protection of the present invention.

[0024] Example 1 A negative electrode binder for lithium-ion batteries is prepared by emulsion polymerization of styrene-butadiene latex, an initiator, and an emulsifier. The styrene-butadiene latex is prepared from the following monomers by weight: 30 parts of styrene, 28 parts of butadiene, 0.3 parts of sodium methacrylic acid, 3 parts of acrylic acid, 3 parts of hydroxyethyl acrylate, 0.3 parts of N-hydroxymethyl acrylamide, 0.8 parts of hydroxypropyl methacrylate, 0.7 parts of methacrylic acid, 1.2 parts of acrylonitrile, and 1.0 parts of acrylamide. The mass ratio of styrene to emulsifier and initiator is 100:3:2. The emulsifier is sodium carboxymethyl cellulose, polyoxyethylene stearate, and glucose alcohol, and the weight ratio of the three is 1:0.4:0.5. The weight ratio of ammonium sulfate and benzoyl peroxide in the initiator is 1:1.5.

[0025] The preparation method of the above-mentioned lithium ion battery negative electrode binder comprises the following steps: S1, firstly mix water and emulsifier evenly, then add acrylic acid, sodium methacrylic acid sulfonate, hydroxyethyl acrylate, hydroxypropyl methacrylate, and methacrylic acid at a temperature of 32°C, and mix to obtain a mixed solution A, wherein the weight ratio of the emulsifier to water is 1:68; S2, mixing styrene, butadiene, N-hydroxymethyl acrylamide, acrylonitrile and acrylamide to obtain a mixed solution B; S3, mixing the mixed solution A and the mixed solution B, adding an initiator, and then heating the system to 95°C and reacting for 3 hours; S4, the reaction liquid is placed in a degassing kettle for degassing, and tert-butyl hydroperoxide, a reducing agent and liquid alkali are added during the degassing process; S5, placing the degassed material into a preparation kettle, continuing to add tert-butyl hydroperoxide, liquid alkali, and a defoaming agent to remove water vapor, unreacted monomers, and bubbles, and then filtering to obtain a negative electrode binder for a lithium-ion battery.

[0026] The binder obtained in Example 1 is an aqueous emulsion with a solid content of 51%.

[0027] Example 2 A negative electrode binder for lithium-ion batteries is prepared by emulsion polymerization of styrene-butadiene latex, an initiator, and an emulsifier. The styrene-butadiene latex is prepared by the following monomers by weight: 20 parts of styrene, 28 parts of butadiene, 0.5 parts of sodium methacrylic acid, 4 parts of acrylic acid, 1 part of hydroxyethyl acrylate, 0.1 parts of N-hydroxymethyl acrylamide, 0.5 parts of hydroxypropyl methacrylate, 0.4 parts of methacrylic acid, 2 parts of acrylonitrile, and 0.5 parts of acrylamide. The mass ratio of styrene to emulsifier and initiator is 100:0.8:3. The emulsifier is sodium carboxymethyl cellulose, polyoxyethylene stearate, and glucose alcohol, and the weight ratio of the three is 1:0.3:0.6. The weight ratio of ammonium sulfate and benzoyl peroxide in the initiator is 1:2.2.

[0028] The preparation method of the above-mentioned lithium ion battery negative electrode binder comprises the following steps: S1, firstly mix water and emulsifier evenly, then add acrylic acid, sodium methacrylic acid sulfonate, hydroxyethyl acrylate, hydroxypropyl methacrylate, and methacrylic acid at a temperature of 40°C, and mix to obtain a mixed solution A, wherein the weight ratio of the emulsifier to water is 1:80; S2, mixing styrene, butadiene, N-hydroxymethyl acrylamide, acrylonitrile and acrylamide to obtain a mixed solution B; S3, mixing the mixed solution A and the mixed solution B, adding an initiator, and then heating the system to 80° C. and reacting for 4 hours; S4, the reaction liquid is placed in a degassing kettle for degassing, and tert-butyl hydroperoxide, a reducing agent and liquid alkali are added during the degassing process; S5, placing the degassed material into a preparation kettle, continuing to add tert-butyl hydroperoxide, liquid alkali, and a defoaming agent to remove water vapor, unreacted monomers, and bubbles, and then filtering to obtain a negative electrode binder for a lithium-ion battery.

[0029] The binder obtained in Example 2 is an aqueous emulsion with a solid content of 48%.

[0030] Example 3 A negative electrode binder for lithium-ion batteries is prepared by emulsion polymerization of styrene-butadiene latex, an initiator, and an emulsifier. The styrene-butadiene latex is prepared from the following monomers by weight: 40 parts of styrene, 35 parts of butadiene, 0.1 parts of sodium methacrylic acid, 1 part of acrylic acid, 4 parts of hydroxyethyl acrylate, 0.5 parts of N-hydroxymethyl acrylamide, 1 part of hydroxypropyl methacrylate, 1 part of methacrylic acid, 0.5 parts of acrylonitrile, and 1.5 parts of acrylamide. The mass ratio of styrene to emulsifier and initiator is 100:6:0.5. The emulsifier is sodium carboxymethyl cellulose, polyoxyethylene stearate, and glucose alcohol, and the weight ratio of the three is 1:0.5:0.4. The weight ratio of ammonium sulfate and benzoyl peroxide in the initiator is 1:0.8.

[0031] The preparation method of the above-mentioned lithium ion battery negative electrode binder comprises the following steps: S1, firstly mix water and emulsifier evenly, then add acrylic acid, sodium methacrylic acid sulfonate, hydroxyethyl acrylate, hydroxypropyl methacrylate, and methacrylic acid at a temperature of 25°C, and mix to obtain a mixed solution A, wherein the weight ratio of the emulsifier to water is 1:55; S2, mixing styrene, butadiene, N-hydroxymethyl acrylamide, acrylonitrile and acrylamide to obtain a mixed solution B; S3, mixing the mixed solution A and the mixed solution B, adding an initiator, and then heating the system to 110° C. and reacting for 2 hours; S4, the reaction liquid is placed in a degassing kettle for degassing, and tert-butyl hydroperoxide, a reducing agent and liquid alkali are added during the degassing process; S5, placing the degassed material into a preparation kettle, continuing to add tert-butyl hydroperoxide, liquid alkali, and a defoaming agent to remove water vapor, unreacted monomers, and bubbles, and then filtering to obtain a negative electrode binder for a lithium-ion battery.

[0032] The binder obtained in Example 3 is an aqueous emulsion with a solid content of 55%.

[0033] Comparative Example 1 In a preparation method of a negative electrode binder for a lithium ion battery, the mixing in step S1 is a one-step mixing, specifically, emulsifier, acrylic acid, sodium methacrylic acid, hydroxyethyl acrylate, hydroxypropyl methacrylate, and methacrylic acid are mixed with water to obtain a mixed solution A, wherein the weight ratio of the emulsifier to water is 1:68; the rest is the same as in Example 1.

[0034] The following is a comparison of the states after mixing in step S1 in Examples 1-3 and Comparative Example 1, as shown in Table 1.

[0035] Table 1. Mixed state of mixed solution A in Examples 1-3 and Comparative Example 1 sample Color Status Example 1 Uniform color Example 2 Uniform color Example 3 Uniform color Comparative Example 1 Uneven color, darker in some areas It can be seen from Table 1 that in step S1, by adopting the method of the present invention of premixing first and then adding other components for mixing, the mixed solution A is mixed more evenly and stably, which is more conducive to the subsequent reaction.

[0036] Comparative Example 2 A negative electrode binder for a lithium ion battery, wherein the emulsifier is sodium carboxymethyl cellulose, polyoxyethylene stearate, and glucose alcohol, the weight ratio of the three is 1:0.2:0.7, and the rest is the same as in Example 1.

[0037] Comparative Example 3 A negative electrode binder for a lithium ion battery, wherein the emulsifier is sodium carboxymethyl cellulose, polyoxyethylene stearate, and glucose alcohol, the weight ratio of the three is 1:0.6:0.3, and the rest is the same as in Example 1.

[0038] Comparative Example 4 A negative electrode binder for a lithium ion battery, wherein the emulsifier is sodium carboxymethyl cellulose, polyoxyethylene stearate, and glucose alcohol, the weight ratio of the three is 1:0.55:0.35, and the rest is the same as in Example 1.

[0039] Comparative Example 5 A negative electrode binder for a lithium ion battery, wherein the emulsifier is a mixture of sodium carboxymethyl cellulose and polyoxyethylene stearate, the weight ratio of the mixture is 1:0.9, and the rest is the same as in Example 1.

[0040] Comparative Example 6 A negative electrode binder for a lithium ion battery, wherein the emulsifier is a mixture of polyoxyethylene stearate and glucitol ester, the weight ratio of the mixture is 0.4:1.5, and the rest is the same as in Example 1.

[0041] Comparative Example 7 A negative electrode binder for lithium ion batteries, wherein the emulsifier is a mixture of sodium carboxymethyl cellulose and glucose alcohol ester, the weight ratio of the two is 1:0.9, and the rest is the same as in Example 1.

[0042] Comparative Example 8 A negative electrode binder for a lithium ion battery, wherein the emulsifier is replaced by a single emulsifier, sodium carboxymethyl cellulose, and the rest is the same as in Example 1.

[0043] Comparative Example 9 A negative electrode binder for a lithium ion battery, wherein the emulsifier is replaced by a single emulsifier, polyoxyethylene stearate, and the rest is the same as in Example 1.

[0044] Comparative Example 10 A negative electrode binder for a lithium ion battery, wherein the emulsifier is replaced by a single emulsifier, glucose alcohol ester, and the rest is the same as in Example 1.

[0045] Performance testing 1. Viscosity test Test method: After the rheometer is preheated for 30 minutes, put the adhesive into the measuring cup of the large rotor, fill it to the inner line of the measuring cup, put in the rotor, take out the base and put it into the instrument, put your hand on the rotor head position and tighten the bottom clockwise, align the line of the rotor head with the scale line on the top of the rheometer, then pull down the lid to make it stable, set the parameters, start the rheometer, and measure and record.

[0046] 2. Peel strength Styrene-butadiene latex is used as a binder for electrode materials in lithium-ion batteries, and its peel strength test standard follows GB / T 2790-1995 "Adhesive 180° Peel Strength Test Method Flexible Material to Rigid Material".

[0047] The test process includes preparing the adhesive sample, then peeling the adhesive sample from the adhesive opening at a certain rate, and the two adherends gradually separate along the length of the adhered surface. The peeling force applied by the flexible adherend is basically parallel to the adhesive surface. The test results are expressed in N / m.

[0048] 3. Mechanical stability test Mechanical stability refers to the state in which latex can maintain self-stabilization under high shear stress. Put about 80g of latex in a corresponding container. To avoid splashing of latex at a high stirring rate, its height should not be higher than 4 / 5 of the container. After fixing the container in the base of the mechanical stability tester, stir the latex at a speed of 10000r / min. The test time is 10min, observe the experimental phenomenon and record the data. In addition, if a large amount of foam is generated during the stirring process of the latex, a small amount of defoaming agent can be added to prevent a large amount of foam from overflowing and the experiment cannot be carried out normally.

[0049] After stirring stops, take out the container containing latex. Use deionized water to carefully flush out the coagulation inside the stirring rod and the container, put it into a small-aperture screen, rinse the container with deionized water many times, place it in a small-particle screen after filtering, and then rinse the coagulation in the filter screen repeatedly with deionized water to ensure that all enter the screen, and finally rinse the coagulation in the screen with deionized water until the milky white color presented by the latex is absent. Then use filter paper to wipe the water around the screen and put it into a constant temperature drying oven, and dry it at a temperature of 120°C. After 2h, take out the screen and place it in a desiccator to cool to room temperature and weigh it. Dry it at 120°C for 30min, cool it in a desiccator, and weigh it. If the difference between two adjacent weighings is not more than 0.5mg, calculate and record it according to the formula.

[0050] Solidification % = (M1 / M2) × 100 Among them, M1 is the mass of the sample and M2 is the mass of the solidified material.

[0051] Table 2. Adhesive viscosity and peel strength test results sample Viscosity mPa·s Peel strength (N / m) Mechanical stability % Example 1 40.5 20.6 0.013 Example 2 46.4 19.4 0.015 Example 3 48.7 21.1 0.014 Comparative Example 1 31.2 15.4 0.028 Comparative Example 2 67.4 17.8 0.025 Comparative Example 3 72.5 14.4 0.027 Comparative Example 4 78.7 18.3 0.029 Comparative Example 5 68.6 15.6 0.021 Comparative Example 6 32.5 14.4 0.029 Comparative Example 7 72.5 18.1 0.026 Comparative Example 8 80.5 18.5 0.028 Comparative Example 9 32.4 15.6 0.025 Comparative Example 10 28.2 16.4 0.027 2. Battery cycle life The binders obtained in Examples 1-3 and Comparative Examples 1-10 were used in lithium ion batteries, and then the obtained lithium ion batteries were subjected to cycle life tests. The specific test method is as follows: 25℃ cycle test: After OCV measurement, take the battery that is charged to 100% SOC at 0.2C, place the battery in a (25±3)℃ environment, let it stand for 3h, and when the battery cell reaches (25±3)℃, charge it to 4.45V at 1C constant current, cut off current 0.05C, and then discharge it to 3V at 0.5C. Repeat the charge and discharge cycle 500 times, record the discharge capacity after the cycle and divide it by the discharge capacity of the first cycle to get the cycle capacity retention rate.

[0052] Test samples: The lithium ion battery prepared by using the binder of Example 1-3 as the negative electrode binder is Example Sample 1-3, and the lithium ion battery prepared by using the binder of Comparative Example 1-10 as the negative electrode binder is Comparative Example Sample 1-10.

[0053] Test results: as shown in Table 3.

[0054] Table 3. Battery cycle life test results of the binders of Examples 1-3 and Comparative Examples 1-10 for lithium-ion batteries sample Capacity retention after 500 cycles% Example 1 88.3 Example 2 86.6 Example 3 85.9 Comparative Example 1 68.4 Comparative Example 2 65.3 Comparative Example 3 76.2 Comparative Example 4 78.4 Comparative Example 5 83.2 Comparative Example 6 81.3 Comparative Example 7 74.8 Comparative Example 8 79.4 Comparative Example 9 82.3 Comparative Example 10 81.7 It can be seen from the above table that the lithium ion batteries prepared by using the binders of Examples 1 to 3 of the present invention in the preparation of negative electrodes for lithium ion batteries have better battery cycle life.

[0055] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A lithium ion battery negative electrode binder, characterized in that: The adhesive is prepared by adding an initiator, an emulsifier and water to the following raw materials in parts by weight: 20-40 parts of styrene, 20-35 parts of butadiene, 0.1-0.5 parts of sodium methacrylic acid, 1-4 parts of acrylic acid, 1-4 parts of hydroxyethyl acrylate, 0.1-0.5 parts of N-hydroxymethyl acrylamide, 0.5-1 parts of hydroxypropyl methacrylate, 0.4-1 parts of methacrylic acid, 0.5-2 parts of acrylonitrile and 0.5-1.5 parts of acrylamide.

2. The negative electrode binder for lithium ion batteries according to claim 1, characterized in that: The dosage of the initiator and the emulsifier is 0.5-3% and 0.8-6% of the weight of styrene respectively.

3. The negative electrode binder for lithium ion batteries according to claim 1, characterized in that: The binder is a water emulsion adhesive with a solid content of 48-55%.

4. The negative electrode binder for lithium ion batteries according to claim 1, characterized in that: The emulsifier is at least two of sodium carboxymethyl cellulose, polyoxyethylene stearate and glucitol ester.

5. The negative electrode binder for lithium ion batteries according to claim 4, characterized in that: The emulsifiers are sodium carboxymethyl cellulose, polyoxyethylene stearate and glucose alcohol, and the weight ratio of the three is 1:0.3-0.5:0.4-0.

6.

6. The negative electrode binder for lithium ion batteries according to claim 1, characterized in that: The initiators are ammonium sulfate and benzoyl peroxide.

7. The negative electrode binder for lithium ion batteries according to claim 6, characterized in that: In the initiator, the weight ratio of ammonium sulfate to benzoyl peroxide is 1:0.8-2.

2.

8. The method for preparing a negative electrode binder for a lithium ion battery according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, first mix water and emulsifier evenly, then add acrylic acid, sodium methacrylic acid sulfonate, hydroxyethyl acrylate, hydroxypropyl methacrylate, and methacrylic acid at a temperature of 25-40°C, and mix to obtain a mixed solution A; S2, mixing styrene, butadiene, N-hydroxymethyl acrylamide, acrylonitrile and acrylamide to obtain a mixed solution B; S3, mixing the mixed solution A and the mixed solution B, adding an initiator, and then heating the system to 80-110° C. and reacting for 2-4 hours; S4, the reaction solution is degassed, neutralized with alkali and then filtered to obtain the negative electrode binder.

9. The method for preparing a negative electrode binder for a lithium ion battery according to claim 8, characterized in that: In the step S1, the weight ratio of the emulsifier to water is 1:55-80.

10. The method for preparing a negative electrode binder for a lithium ion battery according to claim 8, characterized in that: In the step S4, tert-butyl hydroperoxide is added during degassing to adjust the added alkali to liquid alkali.

Citation Information

Patent Citations

  • Butadiene-styrene latex and preparation method thereof

    CN107936166A

  • Slurry composition, preparation method thereof, negative electrode of battery and lithium-ion battery

    CN110416547A

  • Copolymer latex for negative electrode of lithium ion secondary battery, preparation method and application

    CN111825804A

  • Negative electrode binder for lithium-ion battery, preparation method of negative electrode binder and lithium-ion battery containing negative electrode binder

    CN112151802A

  • Preparation method of carboxylic butadiene-styrene latex for lithium battery

    CN118027290A