Method for constructing intelligent hydrogel in double-layer hollow glass and intelligent hydrogel
By constructing intelligent hydrogel in double-layer hollow glass, combining methacrylic anhydride with hyaluronic acid and N-isopropyl acrylamide, the shortcomings of traditional windows in temperature regulation and energy efficiency are solved, and intelligent The hydrogel has high light transmittance and high solar energy regulation efficiency, and improves its stability and biodegradability.
Patent Information
- Application Number
- CN202411293178.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-14
AI Technical Summary
Traditional windows have shortcomings in temperature regulation and energy efficiency, and smart hydrogels have challenges in optical performance and thermochromic temperature regulation, especially the environmental stability and biological of poly(N-isopropylacrylamide) hydrogels. The degradability problem has not been effectively solved.
Constructing intelligent hydrogels in double-layer hollow glass. By combining methacrylic anhydride with materials such as hyaluronic acid and N-isopropyl acrylamide, ultrasonic treatment and constant temperature water bath method are used to prepare accurate and adjustable phase change temperature by using ultrasonic treatment and constant temperature water bath method. , PNIPAm/HAMA smart hydrogel with high light transmittance and high solar energy regulation efficiency.
It has achieved improved optical performance and stability of smart hydrogels, and can maintain high light transmittance and solar energy regulation capabilities in multiple cycles and environmental changes, reducing manufacturing costs, and improving the accurate regulation capabilities of thermochromic temperature.
Smart Images

Figure CN119019600A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer material preparation, and in particular to a method for constructing smart hydrogel in double-layer insulating glass and the smart hydrogel. Background Art
[0002] Buildings rely on temperature regulation systems, which in turn creates a demand for energy.
[0003] As the main medium for heat exchange between indoors and outdoors, windows play a very important role in energy conservation. However, traditional windows often lack the ability to adapt to changing environmental conditions, resulting in serious energy inefficiency. In contrast, smart windows can dynamically adapt to different stimuli, including humidity, electricity and heat changes, and actively adjust the transmission or reflection of sunlight. This adaptive ability not only helps stabilize indoor temperature, but also improves visual comfort, thereby improving the overall energy efficiency of the building.
[0004] Thermochromic hydrogels are temperature-sensitive materials whose physical properties change reversibly with temperature changes. They can be widely used in a variety of fields, including medical dressings, thermal sensors, and energy-saving devices. Poly(N-isopropylacrylamide) hydrogel (PNIPAm hydrogel) is a particularly noteworthy thermochromic material that is very sensitive to temperature changes. At its lower critical solution temperature (usually around 32°C), it changes sharply from transparent to opaque, and this transition is triggered by the phase separation of the polymer. Below the LCST, the polymer chains are dissolved by water molecules and remain in a transparent hydrated state with good light transmission. In order to improve the performance of poly(N-isopropylacrylamide) hydrogels, they have been integrated into composites with other polymers, nanoparticles, and metal-organic frameworks. However, this approach faces the challenges that physical doping may bring, mainly because doping inevitably reduces optical properties or increases critical temperature, thereby limiting its application in smart devices.
[0005] Smart gel is a gel that can respond sensitively to external stimuli and has the characteristics of absorption and sustained release. Modification of poly (N-isopropylacrylamide) hydrogel can further improve its performance. For example, CN114702693A discloses a synthesis method and application of trehalose-modified PNIPAm thermosensitive smart hydrogel. The trehalose-modified PNIPAm thermosensitive smart material has the advantages of high mechanical strength, fast thermal response rate, small volume change, and low energy consumption. However, its environmental stability and biodegradability still need to be explored. Summary of the invention
[0006] The purpose of the present invention is to provide a method for constructing smart hydrogel in double-layer insulating glass and smart hydrogel in order to solve the above problems. In view of the shortcomings of hydrogels with poor optical properties and too high thermochromic temperature, a method for constructing smart hydrogel with accurately adjustable phase change temperature, high light transmittance, high solar energy regulation efficiency and good stability in double-layer insulating glass is provided; and a smart hydrogel with accurately adjustable phase change temperature, high light transmittance, high solar energy regulation efficiency and good stability obtained by the method is provided.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] The first object of the present invention is to provide a method for constructing a smart hydrogel in a double-layer insulating glass, the method comprising the following steps:
[0009] (1) dissolving methacrylic anhydride and hyaluronic acid in deionized water, cooling to 0-4 degrees Celsius to obtain solution A, dropping sodium hydroxide solution into solution A to adjust the pH to 9-10; after the dropping is completed, stirring the obtained solution at 0-4 degrees Celsius, dialyzing the solution with deionized water at 4 degrees Celsius, and after the dialysis, freeze-drying the solution to obtain a solid of methacryloyl hyaluronic acid; using deionized water to dissolve the solid to obtain a methacryloyl hyaluronic acid solution;
[0010] (2) dissolving N-isopropylacrylamide and N,N'-methylenebisacrylamide in deionized water at 60 degrees Celsius to obtain a solution B, stirring the obtained solution B at 60 degrees Celsius and ultrasonically treating it, introducing nitrogen into the solution to obtain a transparent solution C, adding N,N,N',N'-tetramethylethylenediamine to the transparent solution C, and ultrasonically treating it to obtain a monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide;
[0011] (3) adding the methacrylated hyaluronic acid solution obtained in step (1) dropwise into the monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide obtained in step (2), and mixing them thoroughly to obtain a mixed solution; then adding ammonium persulfate to the mixed solution, and transferring it to a double-layer insulating glass mold, constructing a smart hydrogel in a constant temperature water bath at a synthesis temperature of 10 to 32 degrees Celsius, and obtaining a double-layer insulating glass containing the smart hydrogel.
[0012] Furthermore, when the synthesis temperature in step (3) is 17 degrees Celsius, the average pore size of the smart hydrogel is 8 microns to 36 microns.
[0013] Furthermore, when the synthesis temperature in step (3) is 21 degrees Celsius, the average pore size of the smart hydrogel is 10 microns to 40 microns.
[0014] Furthermore, when the synthesis temperature in step (3) is 25 degrees Celsius, the average pore size of the smart hydrogel is 12 microns to 46 microns.
[0015] Furthermore, in step (1), in solution A, the concentration of methacrylic anhydride is 1 to 8 g / L, and the concentration of hyaluronic acid is 5 to 31 g / L; the concentration of the sodium hydroxide solution is 1 mol / L; and the mass percentage concentration of the obtained methacryloyl hyaluronic acid solution is 2% to 35%.
[0016] Furthermore, the PNIPAm / HAMA smart hydrogel can withstand water retention performance tests. After 5 hours in an environment with a temperature and relative humidity of 30 degrees Celsius and 50%, the mass loss of the smart hydrogel containing 2% methacryloyl hyaluronic acid is 50%, the mass loss of the smart hydrogel containing 12% methacryloyl hyaluronic acid is 45%, the mass loss of the smart hydrogel containing 22% methacryloyl hyaluronic acid is 38%, and the mass loss of the hydrogel containing 12% methacryloyl hyaluronic acid after sealing is less than 1%.
[0017] Furthermore, in step (2), in solution B, the concentration of N-isopropylacrylamide is 140-370 g / L, and the concentration of N,N'-methylenebisacrylamide is 4.3-30 g / L; in solution C, the volume ratio of deionized water to N,N,N',N'-tetramethylethylenediamine is 1000:(16-79).
[0018] Furthermore, in step (3), the volume ratio of the methacrylated hyaluronic acid solution obtained in step (1) to the monomer solution of N,N'-methylenebisacrylamide obtained in step (2) is 2% to 22%.
[0019] Furthermore, in step (3), the constant temperature water bath is a super constant temperature water bath.
[0020] Furthermore, step (1) specifically includes the following steps:
[0021] 0.1 g to 0.8 g of methacrylic anhydride and 0.5 g to 3.1 g of hyaluronic acid are dissolved in 100 ml of deionized water, cooled to 0 to 4 degrees Celsius to obtain solution A, and a sodium hydroxide solution with a concentration of 1 mol per liter is added dropwise to solution A to adjust the pH to 9 to 10; after the addition is completed, the obtained solution is stirred at 0 to 4 degrees Celsius, and the solution is dialyzed with deionized water at 4 degrees Celsius. After the dialysis, the solution is freeze-dried to obtain a solid of methacryloyl hyaluronic acid; deionized water is used to dissolve the solid at a concentration of 1 mol per liter to obtain a methacryloyl hyaluronic acid solution, which is named HAMA.
[0022] Furthermore, step (2) specifically includes the following steps:
[0023] 1.4 g to 3.7 g of N-isopropylacrylamide and 43 mg to 300 mg of N,N'-methylenebisacrylamide are dissolved in 10 ml of deionized water at 60 degrees Celsius to obtain solution B, the obtained solution B is stirred and ultrasonically treated at 60 degrees Celsius, nitrogen is introduced into the solution to obtain a transparent solution C, 160 μl to 790 μl of N,N,N',N'-tetramethylethylenediamine is added to the transparent solution C, and ultrasonic treatment is performed to obtain a monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide.
[0024] Furthermore, step (3) specifically includes the following steps:
[0025] The methacrylated hyaluronic acid solution with a mass percentage concentration of 2% to 35% obtained in step (1) is added dropwise to the monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide obtained in step (2), and the mixture is fully mixed to obtain a mixed solution; then 1400 microliters of ammonium persulfate is added to the mixed solution, and the mixture is quickly transferred to a double-layer insulating glass mold, and a smart hydrogel is constructed in a super constant temperature water bath with a synthesis temperature of 10 to 32 degrees Celsius to obtain a double-layer insulating glass containing the smart hydrogel.
[0026] Furthermore, the PNIPAm / HAMA smart hydrogel has accurate phase transition temperature adjustability. When the concentration of methacryloyl hyaluronic acid remains unchanged, the phase transition temperature will be significantly reduced by reducing the synthesis temperature; when the synthesis temperature remains unchanged, the phase transition temperature will be significantly reduced by increasing the concentration of methacryloyl hyaluronic acid.
[0027] Furthermore, the PNIPAm / HAMA smart hydrogel has high light transmittance and high solar energy regulation efficiency. The double-layer insulating glass containing the smart hydrogel has a light transmittance of 91.1% to 98.5% in the visible light to near-infrared wavelength region of 380 nanometers to 2500 nanometers, a visible light modulation capacity of 74.5% to 80.9%, a solar light modulation capacity of 60.2% to 64.8%, and an infrared modulation capacity of 39.8% to 47.6%.
[0028] Furthermore, the PNIPAm / HAMA smart hydrogel can withstand the optical performance stability test. At a temperature of 35 degrees Celsius, the transmittance of the hydrogel remains stable and has no significant change after 50 measurement cycles.
[0029] The PNIPAm / HAMA smart hydrogel was able to withstand structural stability testing. After 500 cycles and after freezing at -5 degrees Celsius for 48 hours, the hydrogel area did not show significant shrinkage.
[0030] The second object of the present invention is to provide a smart hydrogel prepared by the method of constructing a smart hydrogel in a double-layer insulating glass.
[0031] Furthermore, the smart hydrogel is in a double-layer insulating glass.
[0032] Furthermore, the smart hydrogel is a smart hydrogel with accurately adjustable phase change temperature, high light transmittance, high solar energy regulation efficiency and good stability.
[0033] Furthermore, the smart hydrogel can be used to construct double-layer insulating glass containing the smart hydrogel for application as a smart window.
[0034] Compared with the prior art, the beneficial effects of the present invention are embodied in the following aspects:
[0035] The present invention first prepares a methacrylylated hyaluronic acid solution and a monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide, and then synthesizes a PNIPAm / HAMA smart hydrogel in a constant temperature water bath; the preparation method of the present invention has significant simplicity and realizes low manufacturing cost at the same time; the prepared PNIPAm / HAMA smart hydrogel has good optical properties and stability, has temperature-dependent characteristics, and can accurately control the thermochromic temperature.
[0036] The invention uses methacrylic anhydride, hyaluronic acid and sodium hydroxide as raw materials to prepare a methacrylated hyaluronic acid solution; then uses N-isopropylacrylamide, N,N'-methylenebisacrylamide and N,N,N',N'-tetramethylethylenediamine as raw materials to prepare a monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide; and prepares a PNIPAm / HAMA smart hydrogel with accurately adjustable phase change temperature, high light transmittance, high solar energy regulation efficiency and good stability in double-layer insulating glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The scanning electron microscope image of the PNIPAm / HAMA smart hydrogel prepared in Example 2 of the present invention at a synthesis temperature of 17 degrees Celsius and a mass percentage concentration of 2% of the methacryloyl hyaluronic acid solution.
[0038] Figure 2The scanning electron microscope image of the PNIPAm / HAMA smart hydrogel prepared in Example 2 of the present invention when the synthesis temperature is 21 degrees Celsius and the mass percentage concentration of the methacryloyl hyaluronic acid solution is 12%.
[0039] Figure 3 The scanning electron microscope image of the PNIPAm / HAMA smart hydrogel prepared in Example 2 of the present invention when the synthesis temperature is 25 degrees Celsius and the mass percentage concentration of the methacrylylated hyaluronic acid solution is 22%.
[0040] Figure 4 The differential scanning calorimetry graphs of the PNIPAm / HAMA smart hydrogels prepared in Example 3 of the present invention with a synthesis temperature of 17 degrees Celsius and a mass percentage concentration of methacryloyl hyaluronic acid solution of 2%, 12% and 22% respectively.
[0041] Figure 5 The differential scanning calorimetry graphs of the PNIPAm / HAMA smart hydrogels prepared in Example 3 of the present invention at a synthesis temperature of 21 degrees Celsius and with mass percentage concentrations of methacryloyl hyaluronic acid solutions of 2%, 12% and 22% respectively.
[0042] Figure 6 The differential scanning calorimetry graphs of the PNIPAm / HAMA smart hydrogels prepared in Example 3 of the present invention at a synthesis temperature of 25 degrees Celsius and with mass percentage concentrations of methacryloyl hyaluronic acid solutions of 2%, 12% and 22% respectively.
[0043] Figure 7 The transmission spectra of the PNIPAm / HAMA smart hydrogels with thicknesses of 100 μm and 2000 μm prepared in Example 4 of the present invention are in the visible light to near-infrared wavelength region of 380 nm to 2500 nm.
[0044] Figure 8 In Example 2 of the present invention, the water retention performance of the prepared PNIPAm / HAMA smart hydrogel was tested, and the mass change diagram of the PNIPAm / HAMA smart hydrogel before and after the water retention performance test is shown.
[0045] Fig. 9 In Example 2 of the present invention, the optical performance stability test was performed on the prepared PNIPAm / HAMA smart hydrogel, and a comparison chart of the transmittance of the PNIPAm / HAMA smart hydrogel before and after the optical performance stability test was shown (the mass percentage concentration of the methacryloyl hyaluronic acid solution was 12%).
[0046] Fig.10In Example 2 of the present invention, the prepared PNIPAm / HAMA smart hydrogel was subjected to a structural stability test, and a volume change diagram of the PNIPAm / HAMA smart hydrogel before and after the structural stability test is shown (the mass percentage concentration of the methacryloyl hyaluronic acid solution is 12%). DETAILED DESCRIPTION
[0047] The present invention is described in detail below in conjunction with specific embodiments, but is by no means intended to limit the present invention. Features such as preparation methods, materials, structures or composition ratios not explicitly described in this technical solution are considered to be common technical features disclosed in the prior art.
[0048] The following examples will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several modifications and improvements may be made without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.
[0049] The practice of the present invention may employ conventional techniques of chemistry within the skill of the art. In the following examples, efforts have been made to ensure accuracy with respect to the numbers used (including amounts, temperatures, reaction times, etc.), but some experimental errors and deviations should be taken into account.
[0050] The present invention provides a method and a smart hydrogel for constructing a smart hydrogel with accurate and adjustable phase change temperature, high light transmittance, high solar energy regulation efficiency and good stability in a double-layer insulating glass. The present invention first prepares a methacrylic acid solution and a monomer solution containing N-isopropyl acrylamide and N,N'-methylenebisacrylamide and adds N,N,N',N'-tetramethylethylenediamine, and then disperses them uniformly through ultrasonic treatment; then the monomer solution containing N-isopropyl acrylamide and N,N'-methylenebisacrylamide is fully mixed with the methacrylic acid solution, and ammonium persulfate is added to the mixed solution and quickly transferred to a double-layer insulating glass mold, and the smart hydrogel is prepared in a super constant temperature water bath. The preparation method of the present invention has significant simplicity and realizes low manufacturing cost. The double-layer insulating glass containing the smart hydrogel has a maximum light transmittance of 98.5%, a visible light modulation capacity of 80.9%, a solar light modulation capacity of 64.8% and an infrared modulation capacity of 47.6%. Its thermochromic temperature can be accurately controlled by adjusting the concentration of methacryloyl hyaluronic acid and the synthesis temperature. It also has good moisturizing properties and shows no obvious shrinkage after multiple cycles, showing excellent structural firmness.
[0051] Example 1
[0052] This embodiment provides a method for constructing a smart hydrogel in a double-layer insulating glass (a method for preparing a PNIPAm / HAMA smart hydrogel), comprising the following steps:
[0053] (1) Preparation of methacrylic acid hyaluronic acid solution: 0.75 g of methacrylic anhydride and 2 g of hyaluronic acid are dissolved in 100 ml of deionized water and cooled to 2 degrees Celsius; then, a sodium hydroxide solution (aqueous solution) with a concentration of 1 mol / L is added dropwise to the solution to adjust the pH to 9; after the addition is completed, the resulting solution is stirred at 0 to 4 degrees Celsius (generally, the stirring time is about 3 hours); the solution is dialyzed with deionized water (11000 Da) at 4 degrees Celsius, and the water is changed every 8 hours for 8 days; after the dialysis, the solution is freeze-dried at -60°C for 30 hours to obtain a white flocculent solid of methacrylic acid hyaluronic acid; deionized water is used to dissolve the solid to obtain a methacrylic acid hyaluronic acid solution, named HAMA, and the obtained methacrylic acid hyaluronic acid solution is a methacrylic acid hyaluronic acid solution with a mass percentage concentration of 2% to 35%;
[0054] (2) preparing a monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide: dissolving 2 g of N-isopropylacrylamide and 200 mg of N,N'-methylenebisacrylamide in 10 ml of deionized water at 60 degrees Celsius, and then subjecting the resulting solution to magnetic stirring at 60 degrees Celsius (generally, the stirring time is about 30 minutes and the stirring rate is 400 rpm) and ultrasonic treatment (generally, the ultrasonic dispersion time is about 20 minutes); after the ultrasonic treatment, nitrogen is introduced into the solution to remove oxygen to obtain a transparent solution (generally, the nitrogen introduction time is about 15 minutes); adding 560 μl of N,N,N',N'-tetramethylethylenediamine to the resulting solution, and subjecting the solution to ultrasonic treatment (generally, the ultrasonic dispersion time is about 20 minutes), to obtain a monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide;
[0055] (3) Preparation of smart hydrogel: 1400 μL of the methacrylated hyaluronic acid solution with a mass percentage concentration of 2% to 35% obtained in step (1) was added dropwise to 10 ml of the monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide obtained in step (2), and the mixture was thoroughly mixed; then 1400 μL of ammonium persulfate with a concentration of 1 gram per liter was added to the mixed solution, and the mixture was quickly transferred to a double-layer hollow glass mold, the thickness of the double-layer hollow glass mold was set to 2000 μm, and a smart hydrogel was constructed in a super constant temperature water bath at a temperature of 17 degrees Celsius, named PNIPAm / HAMA smart hydrogel, to obtain a double-layer hollow glass containing smart hydrogel.
[0056] When the mass percentage concentration of the methacryloyl hyaluronic acid solution added in step (3) is 2%, 12% and 22%, respectively, the average pore sizes of the prepared PNIPAm / HAMA smart hydrogels are 16 microns, 19 microns and 23 microns, respectively.
[0057] Example 2
[0058] This embodiment provides a method for constructing a smart hydrogel in a double-layer insulating glass (a method for preparing a PNIPAm / HAMA smart hydrogel), comprising the following steps:
[0059] (1) Preparation of methacrylic acid hyaluronic acid solution: 0.75 g of methacrylic anhydride and 2 g of hyaluronic acid are dissolved in 100 ml of deionized water and cooled to 2 degrees Celsius; then, a sodium hydroxide solution (aqueous solution) with a concentration of 1 mol / L is added dropwise to the solution to adjust the pH to 9; after the addition is completed, the resulting solution is stirred at 0 to 4 degrees Celsius (generally, the stirring time is about 3 hours); the solution is dialyzed with deionized water (11000 Da) at 4 degrees Celsius, and the water is changed every 8 hours for 8 days; after the dialysis, the solution is freeze-dried at -60°C for 30 hours to obtain a white flocculent solid of methacrylic acid hyaluronic acid; deionized water is used to dissolve the solid to obtain a methacrylic acid hyaluronic acid solution, named HAMA, and the obtained methacrylic acid hyaluronic acid solution is a methacrylic acid hyaluronic acid solution with a mass percentage concentration of 12%;
[0060] (2) preparing a monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide: dissolving 2 g of N-isopropylacrylamide and 200 mg of N,N'-methylenebisacrylamide in 10 ml of deionized water at 60 degrees Celsius, and then subjecting the resulting solution to magnetic stirring at 60 degrees Celsius (generally, the stirring time is about 30 minutes and the stirring rate is 400 rpm) and ultrasonic treatment (generally, the ultrasonic dispersion time is about 20 minutes); after the ultrasonic treatment, nitrogen is introduced into the solution to remove oxygen to obtain a transparent solution (generally, the nitrogen introduction time is about 15 minutes); adding 560 μl of N,N,N',N'-tetramethylethylenediamine to the resulting solution, and subjecting the solution to ultrasonic treatment (generally, the ultrasonic dispersion time is about 20 minutes), to obtain a monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide;
[0061] (3) Preparation of smart hydrogel: 1400 μL of the 12% mass percent methacrylated hyaluronic acid solution obtained in step (1) was added dropwise to 10 ml of the monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide obtained in step (2), and the mixture was thoroughly mixed; then 1400 μL of ammonium persulfate with a concentration of 1 g / L was added dropwise to the mixed solution, and the mixture was quickly transferred to a double-layer hollow glass mold, the thickness of the double-layer hollow glass mold was set to 200 μm, and a smart hydrogel was constructed in a super constant temperature water bath at temperatures of 17 degrees Celsius, 21 degrees Celsius and 25 degrees Celsius, named PNIPAm / HAMA smart hydrogel, to obtain a double-layer hollow glass containing the smart hydrogel.
[0062] When the hydrogel is prepared by a constant temperature water bath method at temperatures of 17 degrees Celsius, 21 degrees Celsius, and 25 degrees Celsius, the average pore sizes of the prepared PNIPAm / HAMA smart hydrogels are 2.1 nanometers, 1.7 nanometers, and 1.1 nanometers, respectively. Figure 1 , Figure 2 and Figure 3 The scanning electron microscope images of the hydrogels prepared when the constant temperature water bath temperature was 17 degrees Celsius, 21 degrees Celsius and 25 degrees Celsius respectively.
[0063] The water retention performance of the PNIPAm / HAMA smart hydrogel prepared in Example 2 was tested. The results are as follows: Figure 8 As shown, a double-layer insulating glass containing smart hydrogel was sealed using a waterproof and moisture-proof tape. After 5 hours in an environment with a temperature and a relative humidity of 30 degrees Celsius and 50%, respectively, the mass loss of the hydrogel containing different concentrations of methacryloyl hyaluronic acid solution was less than 50%, which was lower than the pure PNIPAm hydrogel in the comparative example. The mass loss of the hydrogel containing 12% methacryloyl hyaluronic acid after sealing was less than 1%, which was much lower than the pure PNIPAm hydrogel in the comparative example. That is, the water retention effect of the hydrogel containing different concentrations of methacryloyl hyaluronic acid solution was better than that of the pure PNIPAm hydrogel in the comparative example. The water retention effect of the hydrogel containing 12% methacryloyl hyaluronic acid after sealing was much better than that of the pure PNIPAm hydrogel in the comparative example, proving that the PNIPAm / HAMA smart hydrogel passed the water retention performance test and had good stability.
[0064] The optical performance stability test of the PNIPAm / HAMA smart hydrogel prepared in Example 2 was performed. Fig. 9As shown, at a temperature of 35 degrees Celsius, the transmittance of the hydrogel with a synthesis temperature of 25 degrees Celsius remained stable. Taking heating from low temperature (20 degrees Celsius) to high temperature (35 degrees Celsius) as a measurement cycle, the hydrogel did not change significantly after 50 measurement cycles, proving that the PNIPAm / HAMA smart hydrogel passed the optical performance stability test and had good stability.
[0065] The structural stability test of the PNIPAm / HAMA smart hydrogel prepared in Example 2 was performed. The results are as follows: Fig.10 As shown, with heating from low temperature (20 degrees Celsius) to high temperature (35 degrees Celsius) as a cycle, after 500 cycles and after freezing at -5 degrees Celsius for 144 hours, the area of the hydrogel in Example (2) with a synthesis temperature of 25 degrees Celsius did not show obvious shrinkage, proving that the PNIPAm / HAMA smart hydrogel passed the structural stability test and has good stability.
[0066] Example 3
[0067] The present embodiment provides a method for constructing a smart hydrogel in a double-layer insulating glass (a method for preparing a PNIPAm / HAMA smart hydrogel), which is basically the same as the preparation method in Example 2. The method for preparing a PNIPAm / HAMA smart hydrogel using a constant temperature water bath method is the same as that in Example 2, except that: in step (3), the concentration of the methacryloyl hyaluronic acid solution and the temperature of the constant temperature water bath are simultaneously controlled to obtain a PNIPAm / HAMA smart hydrogel having a mass percentage concentration of 2%, 12% and 22% of the methacryloyl hyaluronic acid solution at synthesis temperatures of 17 degrees Celsius, 21 degrees Celsius and 25 degrees Celsius, respectively.
[0068] Figure 4 , Figure 5 and Figure 6 The differential scanning calorimetry diagrams of PNIPAm / HAMA smart hydrogels with mass percentage concentrations of 2%, 12% and 22% of methacryloyl hyaluronic acid solutions at synthesis temperatures of 17 degrees Celsius, 21 degrees Celsius and 25 degrees Celsius respectively show that when the concentration of methacryloyl hyaluronic acid remains unchanged, the peak temperature of the exothermic peak decreases when the synthesis temperature decreases, proving that when the concentration of methacryloyl hyaluronic acid remains unchanged, the decrease in synthesis temperature will significantly reduce the phase transition temperature of the smart hydrogel; when the concentration of methacryloyl hyaluronic acid increases when the synthesis temperature remains unchanged, the peak temperature of the exothermic peak decreases, and when the synthesis temperature remains unchanged, the increase in the concentration of methacryloyl hyaluronic acid will also significantly reduce the phase transition temperature of the smart hydrogel.
[0069] Example 4
[0070] The present embodiment provides a method for constructing a smart hydrogel in a double-layer insulating glass (a method for preparing a PNIPAm / HAMA smart hydrogel), which is basically the same as the preparation method in Example 2. The method for preparing a PNIPAm / HAMA smart hydrogel by a constant temperature water bath method is the same as that in Example 2, except that: in step (3), the smart hydrogel is constructed in a super constant temperature water bath at a temperature of 17 degrees Celsius, and in step (3), the thickness of the double-layer insulating glass mold is set to 100 microns and 2000 microns, respectively, and PNIPAm / HAMA smart hydrogels with accurately adjustable phase change temperature, high light transmittance, high solar energy regulation efficiency and good stability are constructed in the double-layer insulating glass mold.
[0071] The transmission spectra of PNIPAm / HAMA smart hydrogels with thicknesses of 100 μm and 2000 μm in the visible to near-infrared wavelength region from 380 nm to 2500 nm are shown in Figure 2. Figure 7As shown, when the temperature is 20 degrees Celsius, the light transmittance reaches 98.5% when the wavelength is 300-780nm under the conditions of synthesis temperature of 17 degrees Celsius and thickness of 100 microns. When the wavelength is 200-2500nm, the sunlight modulation capacity reaches 53.6%. When the temperature is 17 degrees Celsius and thickness of 100 microns, the infrared modulation capacity reaches 100.6% when the wavelength is 1100-2500nm. 36.4%, under the conditions of synthesis temperature of 17 degrees Celsius and thickness of 2000 microns, the visible light modulation capacity reached 80.9% at a wavelength of 200-780nm, under the conditions of synthesis temperature of 17 degrees Celsius and thickness of 2000 microns, the sunlight modulation capacity reached 64.8% at a wavelength of 200-2500nm, under the conditions of synthesis temperature of 17 degrees Celsius and thickness of 2000 microns, the infrared modulation capacity reached 49.5 at a wavelength of 1100-2500nm. %; when the temperature is 40 degrees Celsius, the spectrum is measured. When the synthesis temperature is 17 degrees Celsius and the thickness is 100 microns, the transmittance reaches 94.3% when the wavelength is 300-780nm. When the synthesis temperature is 17 degrees Celsius and the thickness is 100 microns, the sunlight modulation capacity reaches 56.8% when the wavelength is 200-2500nm. When the synthesis temperature is 17 degrees Celsius and the thickness is 100 microns, the infrared modulation capacity reaches 32 .8%, under the conditions of synthesis temperature of 17 degrees Celsius and thickness of 2000 microns, the visible light modulation capacity reached 62.2% at a wavelength of 200-780nm, under the conditions of synthesis temperature of 17 degrees Celsius and thickness of 2000 microns, the sunlight modulation capacity reached 60.6% at a wavelength of 200-2500nm, and under the conditions of synthesis temperature of 17 degrees Celsius and thickness of 2000 microns, the infrared modulation capacity reached 32.7% at a wavelength of 1100-2500nm. By comparison, thickness has a significant impact on sunlight modulation capacity and infrared modulation capacity; spectral test temperature (and ambient temperature) has a significant impact on visible light transmittance and visible light modulation capacity.
[0072] Comparative Example
[0073] This comparative example provides a method for constructing a PNIPAm hydrogel in a double-layer insulating glass, comprising the following steps:
[0074] (1) preparing a monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide: dissolving 2 g of N-isopropylacrylamide and 200 mg of N,N'-methylenebisacrylamide in 10 ml of deionized water at 60 degrees Celsius, and then subjecting the resulting solution to magnetic stirring at 60 degrees Celsius (generally, the stirring time is about 30 minutes and the stirring rate is 400 rpm) and ultrasonic treatment (generally, the ultrasonic dispersion time is about 20 minutes); after the ultrasonic treatment, nitrogen gas is introduced into the solution to remove oxygen to obtain a transparent solution (generally, the nitrogen gas introduction time is about 15 minutes); adding 560 μl of N,N,N',N'-tetramethylethylenediamine to the resulting solution, and subjecting the solution to ultrasonic treatment (generally, the ultrasonic dispersion time is about 20 minutes), to obtain a monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide;
[0075] (2) Preparation of PNIPAm hydrogel: 10 ml of the monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide obtained in step (2) was taken, 1400 μL of ammonium persulfate with a concentration of 1 g / L was added thereto, and the solution was quickly transferred to a double-layer insulating glass mold, the thickness of the double-layer insulating glass mold was set to 200 μm, and a smart hydrogel named PNIPAm hydrogel was constructed in a super constant temperature water bath at temperatures of 17 degrees Celsius, 21 degrees Celsius and 25 degrees Celsius, thereby obtaining a double-layer insulating glass containing PNIPAm hydrogel.
[0076] The above is a description of the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above-mentioned description of the embodiments for the convenience of ordinary technicians in the technical field to understand and use the invention. It is obvious that those familiar with the technology in the field can easily make various modifications to these embodiments and apply the general principles described here to other embodiments without creative work. Therefore, the present invention is not limited to the above-mentioned embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A method for constructing smart hydrogel in double-layer insulating glass, characterized in that: The method comprises the following steps: (1) dissolving methacrylic anhydride and hyaluronic acid in deionized water, cooling to 0-4 degrees Celsius to obtain solution A, dropping sodium hydroxide solution into solution A to adjust the pH to 9-10; after the dropping is completed, stirring the obtained solution at 0-4 degrees Celsius, dialyzing the solution with deionized water at 4 degrees Celsius, and after the dialysis, freeze-drying the solution to obtain a solid of methacryloyl hyaluronic acid; using deionized water to dissolve the solid to obtain a methacryloyl hyaluronic acid solution; (2) dissolving N-isopropylacrylamide and N,N'-methylenebisacrylamide in deionized water at 60 degrees Celsius to obtain a solution B, stirring the obtained solution B at 60 degrees Celsius and ultrasonically treating it, introducing nitrogen into the solution to obtain a transparent solution C, adding N,N,N',N'-tetramethylethylenediamine to the transparent solution C, and ultrasonically treating it to obtain a monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide; (3) adding the methacrylated hyaluronic acid solution obtained in step (1) dropwise into the monomer solution containing N-isopropylacrylamide and N,N'-methylenebisacrylamide obtained in step (2), and mixing them thoroughly to obtain a mixed solution; then adding ammonium persulfate to the mixed solution, and transferring it to a double-layer insulating glass mold, constructing a smart hydrogel in a constant temperature water bath at a synthesis temperature of 10 to 32 degrees Celsius, and obtaining a double-layer insulating glass containing the smart hydrogel.
2. The method for constructing smart hydrogel in double-layer insulating glass according to claim 1, characterized in that: When the synthesis temperature in step (3) is 17 degrees Celsius, the average pore size of the smart hydrogel is 8 microns to 36 microns.
3. The method for constructing smart hydrogel in double-layer insulating glass according to claim 1, characterized in that: When the synthesis temperature in step (3) is 21 degrees Celsius, the average pore size of the smart hydrogel is 10 microns to 40 microns.
4. The method for constructing smart hydrogel in double-layer insulating glass according to claim 1, characterized in that: When the synthesis temperature in step (3) is 25 degrees Celsius, the average pore size of the smart hydrogel is 12 microns to 46 microns.
5. The method for constructing smart hydrogel in double-layer insulating glass according to claim 1, characterized in that: In step (1), in solution A, the concentration of methacrylic anhydride is 1 to 8 g / L, and the concentration of hyaluronic acid is 5 to 31 g / L; The concentration of the sodium hydroxide solution is 1 mol per liter; The mass percentage concentration of the obtained methacryloyl hyaluronic acid solution is 2% to 35%.
6. The method for constructing smart hydrogel in double-layer insulating glass according to claim 1, characterized in that: After 5 hours in an environment with a temperature and relative humidity of 30 degrees Celsius and 50%, respectively, the mass loss of the smart hydrogel containing 2% methacryloyl hyaluronic acid was 50%, the mass loss of the smart hydrogel containing 12% methacryloyl hyaluronic acid was 45%, the mass loss of the smart hydrogel containing 22% methacryloyl hyaluronic acid was 38%, and the mass loss of the hydrogel containing 12% methacryloyl hyaluronic acid after sealing was less than 1%.
7. The method for constructing smart hydrogel in double-layer insulating glass according to claim 1, characterized in that: In step (2), in solution B, the concentration of N-isopropylacrylamide is 140-370 g / L, and the concentration of N,N'-methylenebisacrylamide is 4.3-30 g / L; In the solution C, the volume ratio of deionized water to N,N,N',N'-tetramethylethylenediamine is 1000:(16-79).
8. The method for constructing smart hydrogel in double-layer insulating glass according to claim 1, characterized in that: In step (3), the volume ratio of the methacryloyl hyaluronic acid solution obtained in step (1) to the monomer solution of N,N'-methylenebisacrylamide obtained in step (2) is 2% to 22%.
9. The method for constructing smart hydrogel in double-layer insulating glass according to claim 1, characterized in that: The double-layer insulating glass containing smart hydrogel has a light transmittance of 91.1% to 98.5% in the visible light to near-infrared wavelength range of 380 nanometers to 2500 nanometers, a visible light modulation capacity of 74.5% to 80.9%, a solar light modulation capacity of 60.2% to 64.8%, and an infrared modulation capacity of 39.8% to 47.6%; The light transmittance of the smart hydrogel remains stable at a temperature of 35 degrees Celsius, and there is no obvious change after 50 measurement cycles; After 500 cycles and after being frozen at -5 degrees Celsius for 48 hours, the area of the smart hydrogel did not show obvious shrinkage.
10. A smart hydrogel prepared by the method for constructing a smart hydrogel in a double-layer insulating glass according to any one of claims 1 to 9.
Citation Information
Patent Citations
Hyaluronic acid / poly(N-epsilon-acryloyl-L-lysine) dual-network aquagel capable of biological reduction and preparation method thereof
CN104910569A
Preparing method for infrared response high-strength hydrogel for cartilago articularis repair
CN105107019A
High-strength photo-thermal response surface lubrication hydrogel and preparation method thereof
CN114933716A
Hydrogel composition and preparation thereof
CN115515543A
Composite hydrogel material with self-adaptive solar response as well as preparation method and application of composite hydrogel material
CN116041885A