Modified water-based self-extinction hydroxy acrylic dispersion as well as preparation method and application thereof

By optimizing the polyester intermediate formula and hybrid technology, the problems of traditional aqueous hydroxyacrylic dispersions are solved, and matte with high luster, good color expansion and impact resistance are achieved. Coating reduces the amount of matting powder and improves the water resistance of the coating.

CN119019618APending Publication Date: 2024-11-26HUBEI SHUANGJIAN FINE CHEM CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411285336.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional aqueous hydroxyacrylic dispersions have high gloss and poor pigment color expansion properties. They require a large amount of matting powder to prepare a matte coating. However, excessive matting powder will affect the mechanical properties and water resistance of the coating, and there is a risk of solvent swelling and damage. .

Method used

By optimizing the polyester intermediate formulation, introducing glycidyl tertiary carbonate, synthesize hydrophobic hydroxy polyester intermediates with alkane long side chains, and synthesize interpenetrating network polyester-acrylic acid microphase separation through hybrid technology, using The wetting and dispersion ability of polyester resin effectively wraps the matting powder and realizes the self-matting function.

Benefits of technology

Improves the fullness and water resistance of the coating, significantly reduces the amount of matting powder, improves the color expansion and mechanical properties of the coating, achieves a unique appearance of the matte coating that is both matte and bright, and improves impact resistance. performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005042967090000121
    Figure BDA0005042967090000121
  • Figure BDA0005042967090000131
    Figure BDA0005042967090000131
  • Figure BDA0005042967090000132
    Figure BDA0005042967090000132
Patent Text Reader

Abstract

The invention relates to the technical field of water-based hydroxyl acrylic acid dispersions, in particular to a modified water-based self-extinction hydroxyl acrylic acid dispersion and a preparation method and application thereof.The modified water-based self-extinction hydroxyl acrylic acid dispersion at least comprises, by weight, 150-250 parts of polyester intermediates, 0-15 parts of solvents, 50-150 parts of acrylic acid monomer mixtures A and 40-70 parts of acrylic acid monomer mixtures B, by optimizing a product formula system, the dispersion provided by the invention has outstanding matting property, excellent color contrast property, excellent fullness and comprehensive mechanical properties, and solves the technical problems that a matte colored paint is matte but not bright and is not high in fullness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water-based hydroxy acrylic acid dispersions, in particular to a modified water-based self-matting hydroxy acrylic acid dispersion and a preparation method and application thereof. Background Art

[0002] With the continuous improvement of environmental protection requirements in countries around the world and the introduction of various VOC emission restriction measures, "oil-to-water" has made great breakthroughs in the coatings industry. Waterborne hydroxy acrylic dispersion is the most widely used type of resin among many waterborne resins. Compared with solvent-based acrylic resins and water-soluble acrylic resins, its VOC content is greatly reduced, and the performance of waterborne amino baking varnish and two-component polyurethane topcoat prepared by it is completely comparable to solvent-based coatings. It is increasingly accepted in the field of industrial paint applications. After more than 20 years of technological updates and iterations, waterborne hydroxy acrylic dispersion technology is gradually expanding in the direction of functionalization.

[0003] The conventional aqueous hydroxy acrylic dispersion has high gloss and no matte property, and a large amount of matting powder needs to be added to prepare a matte coating. However, the pigment wettability of hydroxy acrylic resin is not outstanding among many resins. Excessive matting powder will cause insufficient coating of the resin, which will not only affect the pigment color development of the coating, but also affect the various mechanical properties, water resistance and chemical resistance of the resin due to the substantial increase in the pigment-to-base ratio. The current conventional solution mainly achieves the purpose of auxiliary matting by compounding aqueous hydroxy acrylic dispersion and hydroxy acrylic emulsion, thereby effectively reducing the amount of matting powder. For example, a highly water-resistant aqueous two-component matte clear topcoat and its preparation method disclosed in a Chinese patent (publication number CN111944402A) adopts this technical route, but it cannot solve the problem of poor color development, and there is also a risk of demulsification caused by the swelling damage of the particles of the hydroxy acrylic emulsion by the solvent in the aqueous hydroxy acrylic dispersion under long-term storage conditions. A Chinese patent (authorization publication number CN114478929B) discloses a polyurethane prepolymer modified matte hydroxyl acrylic dispersion technology, which modifies the hydroxyl acrylic aqueous dispersion by a self-made polyurethane prepolymer with a microgel structure, but still cannot solve the problem of poor color development of the resin. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a modified water-based self-matting hydroxyl acrylic dispersion. By optimizing the product formula system, the provided dispersion has outstanding matting, excellent color development, excellent fullness and comprehensive mechanical properties, solving the technical problems of matte paint being dull and not bright and having low fullness.

[0005] On one hand, the present invention provides a modified water-based self-matting hydroxyl acrylic dispersion, which comprises at least the following components by weight: 150-250 parts of a polyester intermediate, 0-15 parts of a solvent, 50-150 parts of an acrylic monomer mixture A, 40-70 parts of an acrylic monomer mixture B, 5-15 parts of an initiator solution, 5-15 parts of a neutralizer, and 150-400 parts of deionized water.

[0006] As a preferred technical solution, the polyester intermediate includes at least the following components by weight: 150-250 parts of polyol, 0-100 parts of versatile glycidyl carbonate, 180-250 parts of polyacid, 100-200 parts of monobasic acid, 0.01-0.5 parts of dibutyltin oxide, 15-30 parts of xylene, and 100-200 parts of propylene glycol butyl ether.

[0007] As a preferred technical solution, the mass ratio of tert-butyl glycidyl carbonate to polyol is (1-4):1, preferably (2-4):1.

[0008] As a preferred technical solution, the polyol is selected from at least one of trimethylolpropane, trimethylolethane, pentaerythritol, neopentyl glycol, 1,6-hexanediol, 1,5-pentanediol, 1,4-butanediol, 2-methyl-1,3-propanediol, 1,4-cyclohexanedimethanol, bisphenol A, diethylene glycol, ethylene glycol, and 1,3-propylene glycol.

[0009] Preferably, the polyol is at least one of trimethylolpropane, neopentyl glycol and 1,6-hexanediol.

[0010] As a preferred technical solution, the polyacid is at least one of isophthalic acid, terephthalic acid, phthalic anhydride, hexahydrophthalic anhydride, adipic acid, azelaic acid, and dimer acid.

[0011] Preferably, the polyacid is isophthalic acid and / or phthalic anhydride. Preferably, the mass ratio of isophthalic acid to phthalic anhydride is (7-9):(10-15).

[0012] As a preferred technical solution, the unit acid is at least one of benzoic acid, tert-butylbenzoic acid, stearic acid, coconut oil fatty acid, lauric acid and 2-ethylhexanoic acid.

[0013] Preferably, the monobasic acid is a combination of benzoic acid and coconut oil fatty acid, and the mass ratio of benzoic acid to coconut oil fatty acid is (3-5): (10-15).

[0014] As a preferred technical solution, the method for preparing the polyester intermediate comprises the following steps:

[0015] S1. Add polyol, tert-butyl carbonate, polyacid, monobasic acid, dibutyltin oxide, xylene and propylene glycol butyl ether into a reaction vessel, heat the materials to 90-110° C. and stir;

[0016] S2. Continue to heat up to 150-160°C, then heat up to 220-240°C at a uniform rate within 4-5 hours for reflux and heat preservation until the acid value drops below 5.0 mgKOH / g and then cool down;

[0017] S3, after the temperature drops to 150-160°C, the vacuum pump is turned on to extract all the residual xylene in the reaction container, and then propylene glycol butyl ether is added to dissolve and dilute and the temperature is continued to drop;

[0018] S4. Cool the temperature to below 80°C and filter the material to obtain the polyester intermediate.

[0019] As a preferred technical solution, the solvent is at least one of ethylene glycol butyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, diethylene glycol butyl ether, dipropylene glycol butyl ether, S-100# solvent oil, S-150# solvent oil, propylene glycol methyl ether acetate, and methyl isobutyl ketone.

[0020] Preferably, the solvent is at least one of propylene glycol butyl ether, ethylene glycol butyl ether and dipropylene glycol methyl ether.

[0021] As a preferred technical solution, the acrylic monomer mixture A at least includes acrylic monomer A and peroxide A; the acrylic monomer mixture B at least includes acrylic monomer B and peroxide B.

[0022] As a preferred technical solution, the acrylic monomer A includes: a hydroxyl-containing copolymerizable monomer, an aliphatic acrylate or an aliphatic methacrylate.

[0023] As a preferred technical solution, the acrylic monomer B includes: a carboxyl-containing copolymerizable monomer, a hydroxyl-containing copolymerizable monomer, an aliphatic acrylate or an aliphatic methacrylate.

[0024] Preferably, the carboxyl-containing copolymerizable monomer is at least one of acrylic acid and methacrylic acid;

[0025] Preferably, the hydroxyl-containing copolymerizable monomer is at least one of hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, and hydroxybutyl (meth)acrylate;

[0026] Preferably, the aliphatic (meth)acrylate includes at least one of methyl (meth)acrylate, ethyl (meth)acrylate, propyl methacrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, hexyl methacrylate, isooctyl (meth)acrylate, and lauric (meth)acrylate;

[0027] As a preferred technical solution, the acrylic monomer A and acrylic monomer B further include (meth)acrylic alicyclic ester or vinyl aromatic compound.

[0028] Preferably, the alicyclic (meth)acrylate is cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, tetrahydrofuran (meth)acrylate, and the vinyl aromatic compound is styrene, and at least one of the above monomers is selected;

[0029] As a preferred technical solution, the peroxides A and B are both selected from di-tert-amyl peroxide or di-tert-butyl peroxide.

[0030] As a preferred technical solution, the mass ratio of the initiator to the solvent in the initiator solution is (1-2): (8-12).

[0031] Preferably, the solvent is selected from at least one of propylene glycol butyl ether, ethylene glycol butyl ether and dipropylene glycol methyl ether.

[0032] Preferably, the initiator is at least one of benzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxybenzoate, di-tert-butyl peroxide and di-tert-amyl peroxide;

[0033] Preferably, the initiator is at least one of di-tert-butyl peroxide and di-tert-amyl peroxide;

[0034] Preferably, the neutralizing agent is at least one of N,N-dimethylethanolamine, triethylamine, diethanolamine, triethanolamine, AMP-95, potassium hydroxide and sodium hydroxide;

[0035] Preferably, the neutralizing agent is at least one of N,N-dimethylethanolamine and triethylamine.

[0036] Another aspect of the present invention provides a method for preparing a modified water-based self-matting hydroxylated acrylic dispersion, comprising at least the following steps:

[0037] (1) Put the polyester intermediate and solvent into a reaction vessel, start stirring and heat to 130-150° C.;

[0038] (2) adding the acrylic monomer mixture A dropwise into the reaction vessel at a uniform rate over a period of 1.0-3.5 hours, and then keeping the temperature for 0.5-1.5 hours;

[0039] (3) adding the acrylic monomer mixture B dropwise into the reaction vessel at a uniform rate over 1.0-3.0 hours;

[0040] (4) adding the initiator solution dropwise into the reaction vessel within 0.2-1 hour, and then keeping the temperature for 1.5-3.0 hours;

[0041] (5) Cooling to 80-100°C, adding a neutralizing agent for neutralization and then cooling;

[0042] (6) Cooling to 60-80° C., adding deionized water for high-speed dispersion, and obtaining a modified water-based self-matting hydroxyl acrylic dispersion.

[0043] The present invention optimizes the polyester intermediate formula system, especially introduces tert-butyl glycidyl carbonate into the polyester intermediate, synthesizes a hydrophobic hydroxy polyester intermediate with a long alkane side chain, so that the modified water-based self-matting hydroxy acrylic dispersion containing the polyester intermediate can effectively improve the fullness and water resistance of the coating when it is subsequently used. Further, by optimizing the acrylic monomer mixture A and the acrylic monomer mixture B, the carboxyl-containing copolymerizable monomer; the hydroxyl-containing copolymerizable monomer; (meth) acrylic acid aliphatic ester are simultaneously included, and then the interpenetrating network polyester-acrylic acid microphase separation hydrophobic component is synthesized by a hybrid technology and a solution polymerization process. Since the solubility parameters of the hydrophilic acrylic polymer component (acrylic monomer mixture B) and the polyester intermediate are very different, the phase separation microscopic morphology of the poor compatibility between the polyester resin and the acrylic resin is fully utilized by neutralization and emulsification with water to realize the self-matting function after film formation, and the excellent wetting and dispersing ability of the polyester resin can be fully utilized to realize the effective encapsulation of the matting powder, giving the coating excellent color development, and realizing the unique ideal appearance of the matte coating that is both matte and bright.

[0044] In addition, the present invention controls the acrylic monomers A and B to also include (meth)acrylic alicyclic esters or vinyl aromatic compounds, thereby maintaining the gloss of the coating at an appropriate level without affecting the fullness, color development and comprehensive mechanical properties of the coating.

[0045] The third aspect of the present invention provides an application of a modified water-based self-matting hydroxylated acrylic dispersion, which is applied to the preparation of matte baking varnish.

[0046] As a preferred technical solution, the raw materials for preparing the matte baking varnish include at least the following components by weight: 60-80 parts of modified water-based self-matting hydroxyl acrylic dispersion, 10-15 parts of amino resin, 0.1-0.5 parts of wetting agent, 1-5 parts of matting powder, 1-10 parts of color paste, 0.01-0.3 parts of defoaming agent, 5-10 parts of water, and 0.1-0.5 parts of thickener.

[0047] The matte baking varnish provided by the present invention introduces a modified water-based self-matting hydroxy acrylic dispersion, and the glossiness of the obtained matte baking varnish is significantly reduced compared with the conventional hydroxy acrylic dispersion, and the color difference L value is also greatly reduced, which not only brings a significant matting effect, but also has better pigment color development, showing a unique appearance of matte black and high fullness, and significantly improves the impact resistance of the product.

[0048] Beneficial Effects

[0049] 1. The present invention provides a modified water-based self-matting hydroxyl acrylic dispersion. By optimizing the product formula system, the provided dispersion has outstanding matting, excellent color development, excellent fullness and comprehensive mechanical properties, solving the technical problems of matte paint being dull and not bright and having low fullness.

[0050] 2. The present invention optimizes the polyester intermediate formula system, especially introduces tert-butyl glycidyl carbonate into the polyester intermediate to synthesize a hydrophobic hydroxy polyester intermediate with a long alkane side chain, so that the modified water-based self-matting hydroxy acrylic dispersion containing the polyester intermediate can effectively improve the fullness and water resistance of the coating in subsequent applications.

[0051] 3. By optimizing the acrylic monomer mixture A and the acrylic monomer mixture B, the carboxyl-containing copolymerizable monomer, the hydroxyl-containing copolymerizable monomer, and the (meth) acrylic aliphatic ester are simultaneously included, and then the interpenetrating network polyester-acrylic acid microphase separation hydrophobic component is synthesized by hybrid technology using a solution polymerization process. Since the solubility parameters of the hydrophilic acrylic polymer component (acrylic monomer mixture B) and the polyester intermediate are very different, the phase separation micromorphology with poor compatibility between the polyester resin and the acrylic resin is fully utilized through neutralization to form a salt and emulsification with water to achieve the self-matting function after film formation, and the excellent wetting and dispersing ability of the polyester resin can be fully utilized to achieve effective encapsulation of the matting powder, giving the coating excellent color development, and achieving a unique ideal appearance of the matte coating that is both matte and bright.

[0052] 4. The present invention controls the acrylic monomers A and B to also include (meth) acrylic alicyclic esters or vinyl aromatic compounds, thereby maintaining the gloss of the coating at an appropriate level without affecting the fullness, color development and comprehensive mechanical properties of the coating.

[0053] 5. The matte paint provided by the present invention introduces a modified water-based self-matting hydroxyl acrylic dispersion. Compared with the conventional hydroxyl acrylic dispersion, the gloss of the matte paint obtained is significantly reduced, and the color difference L value is also greatly reduced, which not only brings a significant matte effect, but also has better pigment color development, showing a unique appearance of matte black and high fullness, and significantly improves the impact resistance of the product. DETAILED DESCRIPTION

[0054] Example 1

[0055] Embodiment 1 of the present invention provides a modified water-based self-matting hydroxyl acrylic dispersion, which comprises the following components in parts by weight: 203.68 parts of a polyester intermediate, 5.50 parts of a solvent, 102.26 parts of an acrylic monomer mixture A, 66.2 parts of an acrylic monomer mixture B, 10.67 parts of an initiator solution, 9.31 parts of a neutralizer, and 337.22 parts of deionized water.

[0056] The polyester intermediate comprises the following components by weight: 184.59 parts of polyol, 67.19 parts of tert-butyl glycidyl carbonate, 214.65 parts of polyacid, 142.65 parts of monobasic acid, 0.23 parts of dibutyltin oxide, 22.35 parts of xylene, and 142.25 parts of propylene glycol butyl ether.

[0057] The polyol is trimethylolpropane.

[0058] The polyacid is phthalic anhydride

[0059] The unit acid is a combination of benzoic acid and coconut oil fatty acid, and the mass ratio of the benzoic acid to the coconut oil fatty acid is 40.5:102.15.

[0060] The preparation method of the polyester intermediate comprises the following steps:

[0061] S1. Add polyol, tert-butyl carbonate, polyacid, monobasic acid, dibutyltin oxide, xylene and propylene glycol butyl ether into a reaction container, heat the materials to 100° C. and stir;

[0062] S2, continue to heat up to 160 ° C, then uniformly heat up to 230 ° C within 4.5 hours for reflux and heat preservation until the acid value drops to 2.5 mgKOH / g, then start cooling;

[0063] S3, after the temperature drops to 160°C, start the vacuum pump to extract all the residual xylene in the reaction container, then add propylene glycol butyl ether to dissolve and dilute and continue to cool;

[0064] S4, cooling to below 80°C and filtering the material to obtain a polyester intermediate with a solid content of 80 wt%, which is subsequently diluted to 50 wt% for the preparation of a modified water-based self-matting hydroxyl acrylic dispersion.

[0065] The solvent is propylene glycol butyl ether.

[0066] In parts by weight, the acrylic monomer mixture A includes: 19.85 parts of styrene, 39.28 parts of methyl methacrylate, 20.25 parts of n-butyl acrylate, 20.25 parts of hydroxypropyl methacrylate and 2.63 parts of di-tert-butyl peroxide.

[0067] In parts by weight, the acrylic monomer mixture B includes: 12.48 parts of styrene, 5.67 parts of methyl methacrylate, 18.15 parts of n-butyl acrylate, 8.37 parts of hydroxypropyl methacrylate, 10.12 parts of hydroxypropyl acrylate, 8.37 parts of acrylic acid and 3.04 parts of di-tert-butyl peroxide.

[0068] In parts by weight, the initiator solution includes: 1.22 parts of initiator and 9.45 parts of propylene glycol butyl ether.

[0069] The initiator is di-tert-butyl peroxide.

[0070] The neutralizing agent is N,N-dimethylethanolamine.

[0071] Embodiment 1 of the present invention provides a method for preparing a modified water-based self-matting hydroxylated acrylic dispersion, comprising the following steps:

[0072] (1) Put the polyester intermediate and solvent into a reaction vessel, start stirring and raise the temperature to 140° C.;

[0073] (2) adding the acrylic monomer mixture A dropwise into the reaction vessel at a uniform rate over 2 hours, and then keeping the temperature for 1 hour;

[0074] (3) adding acrylic monomer mixture B dropwise into the reaction vessel at a uniform rate over 1.5 hours;

[0075] (4) adding the initiator solution dropwise into the reaction vessel within 0.5 hours, and then keeping the temperature for 2.5 hours; (5) cooling to 90° C., adding a neutralizing agent for neutralization, and then cooling;

[0076] (6) Cooling to 70° C., adding deionized water for high-speed dispersion, and obtaining a modified water-based self-matting hydroxyl acrylic dispersion.

[0077] Example 2

[0078] Embodiment 2 of the present invention provides a modified water-based self-matting hydroxyl acrylic dispersion, which comprises the following components in parts by weight: 163.68 parts of a polyester intermediate, 13.50 parts of a solvent, 135.17 parts of an acrylic monomer mixture A, 66.1 parts of an acrylic monomer mixture B, 10.6 parts of an initiator solution, 9.16 parts of a neutralizer, and 335.72 parts of deionized water.

[0079] The polyester intermediate is the same as in Example 1, except that it is subsequently diluted to 40 wt % for the preparation of modified water-based self-matting hydroxylated acrylic dispersion.

[0080] The solvent is dipropylene glycol methyl ether.

[0081] In parts by weight, the acrylic monomer mixture A includes: 21.20 parts of cyclohexyl methacrylate, 48.74 parts of methyl methacrylate, 34.42 parts of n-butyl acrylate, 27.27 parts of hydroxypropyl methacrylate and 3.54 parts of di-tert-butyl peroxide.

[0082] In parts by weight, the acrylic monomer mixture B includes: 11.14 parts of styrene, 2.16 parts of methyl methacrylate, 12.83 parts of n-butyl acrylate, 9.65 parts of isooctyl methacrylate, 9.72 parts of hydroxypropyl methacrylate, 9.45 parts of hydroxypropyl acrylate, 8.23 ​​parts of acrylic acid and 2.92 parts of di-tert-butyl peroxide.

[0083] In parts by weight, the initiator solution includes: 1.42 parts of initiator and 9.18 parts of propylene glycol butyl ether.

[0084] The initiator is di-tert-butyl peroxide.

[0085] The neutralizing agent is N,N-dimethylethanolamine.

[0086] Embodiment 2 of the present invention provides a method for preparing a modified water-based self-matting hydroxylated acrylic dispersion, comprising the following steps:

[0087] (1) Put the polyester intermediate and solvent into a reaction vessel, start stirring and raise the temperature to 145° C.;

[0088] (2) adding acrylic monomer mixture A dropwise into the reaction vessel at a uniform rate over 2.5 hours, and then keeping the temperature for 1 hour;

[0089] (3) adding acrylic monomer mixture B dropwise into the reaction vessel at a uniform rate over 1.5 hours;

[0090] (4) adding the initiator solution dropwise into the reaction vessel within 0.5 hours, and then keeping the temperature for 2 hours;

[0091] (5) cooling to 90° C., adding a neutralizing agent for neutralization, and then cooling;

[0092] (6) Cooling to 70° C., adding deionized water for high-speed dispersion, and obtaining a modified water-based self-matting hydroxyl acrylic dispersion.

[0093] Example 3

[0094] Embodiment 3 of the present invention provides a modified aqueous self-matting hydroxyl acrylic dispersion, which comprises the following components in parts by weight: 244.69 parts of a polyester intermediate, 0 parts of a solvent, 68.67 parts of an acrylic monomer mixture A, 66.26 parts of an acrylic monomer mixture B, 7.76 parts of an initiator solution, 9.46 parts of a neutralizer, and 345.32 parts of deionized water.

[0095] The polyester intermediate is the same as in Example 1, except that it is subsequently diluted to 60 wt % for the preparation of modified water-based self-matting hydroxylated acrylic dispersion.

[0096] In parts by weight, the acrylic monomer mixture A comprises: 21.20 parts of styrene, 28.08 parts of methyl methacrylate, 4.05 parts of isooctyl acrylate, 13.50 parts of hydroxypropyl methacrylate and 1.84 parts of di-tert-amyl peroxide.

[0097] In parts by weight, the acrylic monomer mixture B includes: 11.14 parts of isobornyl methacrylate, 5.80 parts of methyl methacrylate, 18.56 parts of n-butyl acrylate, 8.37 parts of hydroxypropyl methacrylate, 10.80 parts of hydroxypropyl acrylate, 8.50 parts of acrylic acid and 3.09 parts of di-tert-amyl peroxide.

[0098] In parts by weight, the initiator solution includes: 1.01 parts of initiator and 6.75 parts of propylene glycol butyl ether.

[0099] The initiator is di-tert-amyl oxide.

[0100] The neutralizing agent is N,N-dimethylethanolamine.

[0101] Embodiment 3 of the present invention provides a method for preparing a modified water-based self-matting hydroxylated acrylic dispersion, comprising the following steps:

[0102] (1) Put the polyester intermediate and solvent into a reaction vessel, start stirring and raise the temperature to 135° C.;

[0103] (2) adding the acrylic monomer mixture A dropwise into the reaction vessel at a uniform rate over 1.5 hours, and then keeping the temperature for 1 hour;

[0104] (3) adding acrylic monomer mixture B dropwise into the reaction vessel at a uniform rate over 1.5 hours;

[0105] (4) adding the initiator solution dropwise into the reaction vessel within 0.5 hours, and then keeping the temperature for 2 hours;

[0106] (5) cooling to 90° C., adding a neutralizing agent for neutralization, and then cooling;

[0107] (6) Cooling to 70° C., adding deionized water for high-speed dispersion, and obtaining a modified water-based self-matting hydroxyl acrylic dispersion.

[0108] Example 4

[0109] Embodiment 4 of the present invention provides a modified aqueous self-matting hydroxyl acrylic dispersion, which comprises the following components in parts by weight: 203.68 parts of a polyester intermediate, 5.50 parts of a solvent, 102.27 parts of an acrylic monomer mixture A, 66.21 parts of an acrylic monomer mixture B, 10.67 parts of an initiator solution, 10.5 parts of a neutralizer, and 337.16 parts of deionized water.

[0110] The polyester intermediate is the same as that in Example 1.

[0111] The solvent is propylene glycol butyl ether.

[0112] In parts by weight, the acrylic monomer mixture A includes: 61.43 parts of methyl methacrylate, 19.98 parts of n-butyl acrylate, 18.23 parts of hydroxyethyl methacrylate and 2.63 parts of di-tert-amyl peroxide.

[0113] In parts by weight, the acrylic monomer mixture B includes: 11.81 parts of styrene, 5.00 parts of methyl methacrylate, 17.48 parts of n-butyl acrylate, 9.04 parts of hydroxypropyl methacrylate, 11.47 parts of hydroxypropyl acrylate, 8.37 parts of acrylic acid and 3.04 parts of di-tert-amyl peroxide.

[0114] In parts by weight, the initiator solution includes: 1.22 parts of initiator and 9.45 parts of propylene glycol butyl ether.

[0115] The initiator is di-tert-amyl peroxide.

[0116] The neutralizing agent is triethylamine.

[0117] Embodiment 4 of the present invention provides a method for preparing a modified water-based self-matting hydroxylated acrylic dispersion, comprising the following steps:

[0118] (1) Put the polyester intermediate and solvent into a reaction vessel, start stirring and raise the temperature to 140° C.;

[0119] (2) adding the acrylic monomer mixture A dropwise into the reaction vessel at a uniform rate over 2 hours, and then keeping the temperature for 1 hour;

[0120] (3) adding acrylic monomer mixture B dropwise into the reaction vessel at a uniform rate over 1.5 hours;

[0121] (4) adding the initiator solution dropwise into the reaction vessel within 0.5 hours, and then keeping the temperature for 1.5 hours; (5) cooling to 90° C., adding a neutralizing agent for neutralization, and then cooling;

[0122] (6) Cooling to 70° C., adding deionized water for high-speed dispersion, and obtaining a modified water-based self-matting hydroxyl acrylic dispersion.

[0123] Comparative Example 1

[0124] Comparative Example 1 of the present invention provides a modified aqueous self-matting hydroxyl acrylic dispersion, which includes the following components in parts by weight: 46.17 parts of solvent, 266.61 parts of acrylic monomer mixture A, 66.32 parts of acrylic monomer mixture B, 11.13 parts of initiator solution, 9.51 parts of neutralizer, and 336.18 parts of deionized water.

[0125] The solvent is propylene glycol butyl ether.

[0126] In parts by weight, the acrylic monomer mixture A comprises: 26.59 parts of styrene, 49.95 parts of methyl methacrylate, 68.58 parts of n-butyl acrylate, 51.03 parts of isooctyl methacrylate, 63.45 parts of hydroxypropyl methacrylate and 7.01 parts of di-tert-butyl peroxide.

[0127] In parts by weight, the acrylic monomer mixture B includes: 12.48 parts of styrene, 2.29 parts of methyl methacrylate, 12.83 parts of n-butyl acrylate, 8.97 parts of isooctyl methacrylate, 8.37 parts of hydroxypropyl methacrylate, 10.12 parts of hydroxypropyl acrylate, 8.10 parts of acrylic acid and 3.16 parts of di-tert-butyl peroxide.

[0128] In parts by weight, the initiator solution includes: 1.68 parts of initiator and 9.45 parts of propylene glycol butyl ether.

[0129] The initiator is di-tert-butyl peroxide.

[0130] The neutralizing agent is N,N-dimethylethanolamine.

[0131] Comparative Example 1 of the present invention provides a method for preparing a modified water-based self-matting hydroxylated acrylic dispersion, comprising the following steps:

[0132] (1) Add the solvent into a reaction vessel, start stirring and raise the temperature to 145° C.

[0133] (2) adding the acrylic monomer mixture A dropwise into the reaction vessel at a uniform rate over 3 hours, and then keeping the temperature for 0.5 hours;

[0134] (3) adding acrylic monomer mixture B dropwise into the reaction vessel at a uniform rate over 1.5 hours;

[0135] (4) adding the initiator solution dropwise into the reaction vessel within 0.5 hours, and then keeping the temperature for 2 hours;

[0136] (5) cooling to 90° C., adding a neutralizing agent for neutralization, and then cooling;

[0137] (6) Cooling to 70° C., adding deionized water for high-speed dispersion, and obtaining a conventional water-based self-matting hydroxyl acrylic dispersion.

[0138] Comparative Example 2

[0139] Comparative Example 2 of the present invention provides a conventional aqueous self-matting hydroxyl acrylic dispersion, which comprises the following components in parts by weight: 203.68 parts of a polyester intermediate, 5.50 parts of a solvent, 102.26 parts of an acrylic monomer mixture A, 66.2 parts of an acrylic monomer mixture B, 10.67 parts of an initiator solution, 9.31 parts of a neutralizer, and 337.02 parts of deionized water.

[0140] The polyester intermediate comprises the following components by weight: 214.61 parts of polyol, 216.86 parts of polyacid, 177.62 parts of monoacid, 0.25 parts of dibutyltin oxide, 20 parts of xylene, and 139.5 parts of propylene glycol butyl ether.

[0141] The polyol is trimethylolpropane.

[0142] The polyacid is phthalic anhydride

[0143] The unit acid is a combination of benzoic acid and coconut oil fatty acid, and the mass ratio of the benzoic acid to the coconut oil fatty acid is 40.5:102.15.

[0144] The preparation method of the polyester intermediate comprises the following steps:

[0145] S1. Add polyol, tert-butyl carbonate, polyacid, monobasic acid, dibutyltin oxide, xylene and propylene glycol butyl ether into a reaction container, heat the materials to 100° C. and stir;

[0146] S2, continue to heat up to 160 ° C, then uniformly heat up to 230 ° C within 4.5 hours for reflux and heat preservation until the acid value drops to 2.8 mgKOH / g, then start cooling;

[0147] S3, after the temperature drops to 160°C, start the vacuum pump to extract all the residual xylene in the reaction container, then add propylene glycol butyl ether to dissolve and dilute and continue to cool;

[0148] S4, cooling to below 80°C and filtering the material to obtain a polyester intermediate with a solid content of 80 wt%, which is subsequently diluted to 50 wt% for the preparation of a modified water-based self-matting hydroxyl acrylic dispersion.

[0149] The solvent is propylene glycol butyl ether.

[0150] In parts by weight, the acrylic monomer mixture A includes: 19.85 parts of styrene, 39.28 parts of methyl methacrylate, 20.25 parts of n-butyl acrylate, 20.25 parts of hydroxypropyl methacrylate and 2.63 parts of di-tert-butyl peroxide.

[0151] The acrylic monomer mixture B comprises, by weight: 12.48 parts of styrene, 5.67 parts of methyl methacrylate, 18.15 parts of n-butyl acrylate, 8.37 parts of hydroxypropyl methacrylate, 10.12 parts of hydroxypropyl acrylate, 8.37 parts of acrylic acid and 3.04 parts of di-tert-butyl peroxide.

[0152] In parts by weight, the initiator solution includes: 1.22 parts of initiator and 9.45 parts of propylene glycol butyl ether.

[0153] The initiator is di-tert-butyl peroxide.

[0154] The neutralizing agent is N,N-dimethylethanolamine.

[0155] Comparative Example 2 of the present invention provides a method for preparing a conventional aqueous self-matting hydroxylated acrylic dispersion, comprising the following steps:

[0156] (1) Add the solvent into a reaction vessel, start stirring and raise the temperature to 145° C.

[0157] (2) adding the acrylic monomer mixture A dropwise into the reaction vessel at a uniform rate over 3 hours, and then keeping the temperature for 0.5 hours;

[0158] (3) adding acrylic monomer mixture B dropwise into the reaction vessel at a uniform rate over 1.5 hours;

[0159] (4) adding the initiator solution dropwise into the reaction vessel within 0.5 hours, and then keeping the temperature for 2 hours;

[0160] (5) cooling to 90° C., adding a neutralizing agent for neutralization, and then cooling;

[0161] (6) Cooling to 70° C., adding deionized water for high-speed dispersion, and obtaining a conventional water-based self-matting hydroxyl acrylic dispersion.

[0162] Application Examples 1-4, Application Comparative Examples 1-2

[0163] Application Examples 1-4 and Application Comparative Examples 1-2 of the present invention provide a matte black amino baking varnish, and the formula is shown in Table 1.

[0164] Table 1

[0165]

[0166]

[0167] The preparation method of the matte black amino baking varnish is as follows: the raw materials listed in Table 1 are mixed to obtain the product.

[0168] Performance Testing Methods

[0169] 1. The solid content, viscosity and pH of the hydroxylated acrylic acid dispersions prepared in the examples and comparative examples were tested. The test results are shown in Table 2.

[0170] Table 2

[0171]

[0172] 2. The coating appearance, glossiness, color difference L value, fullness, pencil hardness, adhesion, impact resistance and water resistance of the matte black amino baking varnish prepared in the application examples and the comparative examples were tested. The test results are shown in Table 3.

[0173] The test method is: the matte black amino paint prepared by the application example and the application comparison example is tested on the polished tinplate. The dry film thickness of the paint is 30μm. After flash drying at 80℃ for 10min, the temperature is raised to 140℃ and baked for 20min to carry out the corresponding test. The matte properties of the paint film are mainly judged by the glossiness at a 60-degree angle and the color difference L value. The lower the glossiness, the higher the matteness of the paint film, and the lower the L value, the better the color development of the paint film. The specific test standards are as follows:

[0174] (1) Coating appearance: Visual inspection is adopted. If the paint film is smooth and flat, it is qualified; otherwise, it is unqualified.

[0175] (2) Gloss: Refer to the test standard GB 1743-1979.

[0176] (3) Color difference L value: refer to the test standard GB11186.1.2-1989.

[0177] (4) Fullness: visual inspection.

[0178] (5) Pencil hardness: refer to the test standard GB / T6739-2006.

[0179] (6) Adhesion: Refer to the test standard GB / T1720-1988.

[0180] (7) Impact performance: refer to the test standard GB / T 1732-1993.

[0181] (8) Water resistance (40°C): Refer to the test standard GB / T1733-1993 and observe the immersion time for the test panels coated with the paint film to lose gloss, change color, wrinkle, fall off, rust, etc.

[0182] Table 3

[0183]

[0184] The matte black amino baking varnish obtained by application examples 1-4 of the present invention has excellent coating appearance, matte effect, color development, fullness, water resistance and comprehensive mechanical properties. Application example 4 does not contain (meth) acrylic acid alicyclic ester or styrene relative to application examples 1-3, and the glossiness of the prepared matte black baking varnish is further reduced, and the color difference L value does not change much, which can bring better coating matting effect. Application comparative example 1 has reduced water resistance and fullness relative to application examples 1-4. Application comparative example 2 cannot simultaneously ensure excellent matte effect and color development relative to application examples 1-4.

Claims

1. A modified water-based self-matting hydroxylated acrylic dispersion, characterized in that: The invention comprises at least the following components by weight: 150-250 parts of polyester intermediate, 0-15 parts of solvent, 50-150 parts of acrylic monomer mixture A, 40-70 parts of acrylic monomer mixture B, 5-15 parts of initiator solution, 5-15 parts of neutralizer and 150-400 parts of deionized water.

2. The modified water-based self-matting hydroxylated acrylic dispersion according to claim 1, characterized in that: The polyester intermediate comprises at least the following components by weight: 150-250 parts of polyol, 0-100 parts of tert-butyl glycidyl carbonate, 180-250 parts of polyacid, 100-200 parts of monobasic acid, 0.01-0.5 parts of dibutyltin oxide, 15-30 parts of xylene, and 100-200 parts of propylene glycol butyl ether.

3. The modified water-based self-matting hydroxylated acrylic dispersion according to claim 2, characterized in that: The mass ratio of the tert-butyl glycidyl carbonate to the polyol is (1-4):

1.

4. The modified water-based self-matting hydroxylated acrylic dispersion according to claim 3, characterized in that: The acrylic monomer mixture A at least includes acrylic monomer A and peroxide A; the acrylic monomer mixture B at least includes acrylic monomer B and peroxide B; the acrylic monomer A includes: a hydroxyl-containing copolymerizable monomer, an aliphatic acrylate or an aliphatic methacrylate; the acrylic monomer B includes: a carboxyl-containing copolymerizable monomer, a hydroxyl-containing copolymerizable monomer, an aliphatic acrylate or an aliphatic methacrylate.

5. The modified water-based self-matting hydroxylated acrylic dispersion according to claim 4, characterized in that: The aliphatic acrylate or aliphatic methacrylate includes at least one of methyl acrylate or methyl methacrylate, ethyl acrylate or ethyl methacrylate, propyl methacrylate, n-butyl acrylate or n-butyl methacrylate, isobutyl acrylate or isobutyl methacrylate, tert-butyl acrylate or tert-butyl methacrylate, hexyl methacrylate, isooctyl acrylate or isooctyl methacrylate, lauric acrylate or lauric methacrylate.

6. The modified water-based self-matting hydroxylated acrylic dispersion according to claim 5, characterized in that: The acrylic monomer A and the acrylic monomer B further include at least one of alicyclic acrylate, alicyclic methacrylate and vinyl aromatic compound.

7. The modified water-based self-matting hydroxylated acrylic dispersion according to claim 6, characterized in that: The solvent is at least one of ethylene glycol butyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, diethylene glycol butyl ether, dipropylene glycol butyl ether, S-100# solvent oil, S-150# solvent oil, propylene glycol methyl ether acetate, and methyl isobutyl ketone.

8. The modified water-based self-matting hydroxylated acrylic dispersion according to claim 7, characterized in that: The neutralizing agent is at least one of N,N-dimethylethanolamine, triethylamine, diethanolamine, triethanolamine, AMP-95, potassium hydroxide and sodium hydroxide.

9. A method for preparing the modified waterborne self-matting hydroxylated acrylic dispersion according to any one of claims 1 to 8, characterized in that: At least the following steps are included: (1) Put the polyester intermediate and solvent into a reaction vessel, start stirring and heat to 130-150° C.; (2) adding the acrylic monomer mixture A dropwise into the reaction vessel at a uniform rate over a period of 1.0-3.5 hours, and then keeping the temperature for 0.5-1.5 hours; (3) adding the acrylic monomer mixture B dropwise into the reaction vessel at a uniform rate over 1.0-3.0 hours; (4) adding the initiator solution dropwise into the reaction vessel within 0.2-1 hour, and then keeping the temperature for 1.5-3.0 hours; (5) Cooling to 80-100°C, adding a neutralizing agent for neutralization and then cooling; (6) Cooling to 60-80° C., adding deionized water for high-speed dispersion, and obtaining a modified water-based self-matting hydroxyl acrylic dispersion.

10. An application of the modified water-based self-matting hydroxylated acrylic dispersion according to any one of claims 1 to 8, characterized in that: The invention is used for preparing matte baking varnish. The raw materials for preparing the matte baking varnish include at least the following components by weight: 60-80 parts of modified water-based self-matting hydroxyl acrylic dispersion, 10-15 parts of amino resin, 0.1-0.5 parts of wetting agent, 1-5 parts of matting powder, 1-10 parts of color paste, 0.01-0.3 parts of defoaming agent, 5-10 parts of water and 0.1-0.5 parts of thickener.

Citation Information

Patent Citations

  • High-water-resistance water-based two-component matte varnish and preparation method thereof

    CN111944402A

  • A polyurethane prepolymer modified matte hydroxypropyl dispersion and its preparation method