MOFs catalyst with NDI-X as ligand, preparation method and application in zinc-nitrate battery
By using NDI-X as the ligand MOFs catalyst, the electronic structure of the metal node is optimized, and the problem of low nitrate reduction efficiency in zinc-nitrate batteries is solved, achieving high-efficiency ammonia synthesis and improved battery performance.
Patent Information
- Application Number
- CN202411067138.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-26
AI Technical Summary
There is a large kinetic energy barrier for nitrate reduction in existing zinc-nitrate batteries, and the activity and selectivity of existing high-load Cu-MOFs catalysts are poor, making it difficult to effectively regulate metal copper nodes, affecting the catalytic reaction. efficiency.
Using NDI-X, a derivative of di(3,5-dimethylpyrazole)naphthalene diimide as ligand, MOFs catalyst with high metal load was prepared by synthesis optimization and applied to zinc-nitrate batteries. , optimize the electronic structure of metal nodes to improve catalytic activity and selectivity.
A large output voltage and high power density were achieved, the Faraday efficiency was as high as 98.2%, and the ammonia yield was significantly improved, showing high activity and high selectivity in ammonia synthesis.
Smart Images

Figure CN119019699A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, preparation methods and aqueous energy storage batteries, and in particular to a MOFs catalyst with NDI-X as a ligand, a preparation method and application in a zinc-nitrate battery. Background Art
[0002] The existing zinc-nitrate battery includes a positive electrode, a positive electrode electrolyte, a negative electrode and a negative electrode electrolyte. The positive electrode electrolyte and the negative electrode electrolyte are separated by a diaphragm. The positive electrode is a carbon cloth loaded with MOFs catalyst, the positive electrode electrolyte is a mixed solution of KNO3 and KOH, the negative electrode is an active metal zinc sheet, and the negative electrode electrolyte is a KOH solution. During discharge, nitrate reduction occurs at the positive electrode to generate ammonia, and zinc oxidation occurs at the negative electrode. Therefore, the zinc-nitrate battery can purify nitrate-containing wastewater and produce chemical ammonia while generating electricity. However, since nitrate reduction involves multi-electron transfer and there is a large kinetic energy barrier, the development of an electrocatalyst with excellent nitrate reduction and ammonia synthesis performance is of great significance for the development of zinc-nitrate battery research.
[0003] Metal-organic frameworks (MOFs) are a type of porous material formed by metals and organic ligands connected by coordination bonds. They have the characteristics of clear sites, high specific surface area, adjustable pores, and designable composition and structure. They have the advantages of both homogeneous and heterogeneous catalysts and are widely used in catalysis and other fields. The electronic structure and catalytic activity of the metal nodes of MOFs materials are significantly affected by the surrounding ligands. Therefore, optimizing the structure of the ligands is an effective strategy to improve the catalytic activity and selectivity of MOFs. In addition, the synthesis strategy of MOFs mainly relies on harsh reaction conditions, the metal loading is relatively low, and the stability is also poor. The high-load Cu-MOFs disclosed in the prior art use di(3,5-dimethylpyrazole)naphthalene diimide (NDI) as a ligand, which has a relatively single function and is difficult to effectively regulate the metal copper nodes, resulting in poor activity and selectivity in catalytic reactions.
[0004] So far, there is no report on the preparation of bis(3,5-dimethylpyrazole)naphthalene diimide derivative NDI-X and its use as ligand to prepare metal-organic frameworks (MOFs). Summary of the invention
[0005] The present invention aims to solve the above-mentioned technical problems existing in the prior art and provides a MOFs catalyst with NDI-X as a ligand, a preparation method and an application in a zinc-nitrate battery.
[0006] The technical solution of the present invention is: a MOFs catalyst with NDI-X as a ligand, in which a metal element is combined with the ligand through a coordination bond, and the ligand is a derivative of di(3,5-dimethylpyrazole)naphthalene diimide NDI-X, wherein X is -NMe2 or -Br, and the substitution position is one of the four positions of the naphthalene ring.
[0007] Preferred metal elements are Cu, Bi, Zn, Fe or Co.
[0008] A method for preparing the MOFs catalyst with NDI-X as a ligand as described above is carried out according to the following steps: Step 1. Prepare ligand NDI-X; Step 1.1: Mix NDI ligand and sulfuric acid, dissolve them evenly and place them in a flask, wherein the molar ratio of the NDI ligand to the sulfuric acid is 1:20-40; add 1,3-dibromo-5,5-dimethylhydantoin to the solution and stir thoroughly, wherein the molar ratio of the NDI ligand to the 1,3-dibromo-5,5-dimethylhydantoin is 5-10:2-6; place the flask in ice water to obtain a precipitate, wash the precipitate with water and methanol respectively, and then vacuum dry to obtain a 2-bromo-1,4,5,8-naphthalenetetracarboxylic dianhydride ligand 2-Br-NDI; Step 1.2: dissolving 2-Br-NDI and 3,5-dimethylpyrazole in anhydrous dimethylformamide, wherein the molar ratio of 2-Br-NDI to 3,5-dimethylpyrazole is 1-5:2-4, and the amount ratio of 2-Br-NDI to anhydrous dimethylformamide is 2-6 mmol:20-50 mL; the mixture is fully reacted under an inert atmosphere, and then ether solvent is added to obtain a precipitate, and the obtained precipitate is recrystallized with a mixed solution of anhydrous dimethylformamide / ether / water, and the ligand NDI-Br is obtained after vacuum drying, wherein the volume ratio of anhydrous dimethylformamide / ether / water is 2:3:1; Step 1.3: dissolving the ligand NDI-Br in a mixed solution of dimethyl sulfoxide and dimethylamine / tetrahydrofuran, wherein the amount ratio of the ligand NDI-Br, dimethyl sulfoxide, and dimethylamine / tetrahydrofuran is 1-6 mmol:5-20 mL:2-12 mL, and the ratio of dimethylamine to tetrahydrofuran is 6-18 mmol / L; sealing the mixed solution for reaction, rapidly stirring and heating at 70-120°C for 12-24 h, pouring the reactant into stirred water to generate a precipitate, filtering and separating the generated precipitate, washing the precipitate with water and ethanol, respectively, and finally recrystallizing with dichloromethane / methanol to obtain a purified product, namely, the ligand NDI-NMe2, wherein the volume ratio of dichloromethane / methanol is 1:3; Step 2. Mix the metal salt and the ligand NDI-X in a molar ratio of 4-1:1-4 and dissolve them in a mixed solvent of dimethylformamide and methanol to obtain solution A, wherein the amount ratio of the metal salt to the mixed solvent is 0.1-0.6 mmol:3-10 mL, and the volume ratio of dimethylformamide to methanol is 4-6:1; Step 3. Add a nitric acid solution with a concentration of 0.1 - 2 mol / L into solution A at a ratio of 1-3:5-20 for thermal reaction, and obtain a MOFs catalyst with NDI-X as a ligand after washing and vacuum drying.
[0009] The preferred molar ratio of metal salt to ligand NDI-X is 3:2, 2:3, 1:1, 1:2 or 1:3.
[0010] Preferred metal salts are Cu(NO3)2, Bi(NO3)2, Zn(NO3)2, Fe(NO3)2 or Co(NO3)2.
[0011] The preferred thermal reaction temperature is 50-150° C. and the reaction time is 4-96 h.
[0012] An application of the above-mentioned MOFs catalyst with NDI-X as a ligand in zinc-nitrate batteries.
[0013] The present invention uses di(3,5-dimethylpyrazole)naphthalene diimide derivatives NDI-NMe2 or NDI-Br with the same structure but different substituent groups as ligands to prepare a MOFs-based single-atom catalyst with a metal loading of up to 30%. J. Mater. Chem. C 2014, 2 , 2869-2876. DOI: 10.1039 / C3TC32377C), with adjustable substituent groups, which can optimize the electronic structure of the metal node and be applied to the assembled zinc-nitrate battery device, showing a large output voltage (1.59 V) and a high power density (36.5 mWcm -2 ), with a Faradaic efficiency of 98.2% and an ammonia yield of 16.8 mg h -1 mg cat -1 , which can realize the synthesis of ammonia with high activity and high selectivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is the SEM image of Cu-NDI-NMe2 prepared in Example 2 of the present invention.
[0015] Figure 2This is the open circuit voltage diagram of zinc-nitrate batteries assembled with Cu-NDI, Cu-NDI-Br, and Cu-NDI-NMe2 as positive electrode materials. DETAILED DESCRIPTION
[0016] The sources of all raw materials in the present invention are not particularly limited and can be purchased from the market or prepared according to conventional methods known to those skilled in the art. Among them, NDI ligand is prepared according to the literature ( J. Mater. Chem. C 2014, 2 , 2869-2876. DOI: 10.1039 / C3TC32377C). The purity of all raw materials in the present invention is not particularly limited, and analytically pure materials are preferably used.
[0017] Example 1: Preparation of Cu-NDI-Br The preparation method of the MOFs catalyst using NDI-X as a ligand of the present invention is carried out according to the following steps: Step 1. Preparation of ligand NDI-Br; Step 1.1: Mix 15 mmol of NDI ligand and 20 mL of 18.4 mol / L sulfuric acid, dissolve them evenly and place them in a round-bottom flask; add 8 mmol of 1,3-dibromo-5,5-dimethylhydantoin to the solution in the round-bottom flask and stir them thoroughly for 12 hours, place the round-bottom flask in ice water to obtain a precipitate, wash the precipitate with water and methanol three times respectively, and then vacuum dry it to obtain 2-bromo-1,4,5,8-naphthalenetetracarboxylic dianhydride ligand 2-Br-NDI; Step 1.2: 6 mmol 2-Br-NDI and 8 mmol 3,5-dimethylpyrazole were dissolved in 30 mL anhydrous dimethylformamide (DMF); the mixture was heated at 160°C under an inert atmosphere, and rapidly stirred for 12 h. After cooling to room temperature, 150 mL of ether solvent was added to react fully to obtain a precipitate, and the obtained precipitate was recrystallized with 30 mL of a mixed solution of DMF / ether / water. After vacuum drying at 70°C, the ligand NDI-Br was obtained. The volume ratio of DMF / ether / water was 2:3:1. Step 2. Dissolve 0.1 mmol of Cu(NO3)2·3H2O and 0.05 mmol of ligand NDI-Br in 7 mL of a mixed solvent of dimethylformamide and methanol to obtain solution A, wherein the volume ratio of dimethylformamide to methanol is 6:1. Place solution A in a threaded glass bottle; Step 3: Add 0.5 mL of 1 mol / L nitric acid solution to 7 mL of solution A, transfer the glass bottle to an oven, heat to 80 °C and react for 24 h. After the reaction is cooled to room temperature, separate the solid, wash it with DMF and anhydrous methanol for 3-5 times, and dry it in a vacuum oven at 60-100 °C for 12-24 h to obtain Cu-NDI-Br.
[0018] Example 2: Preparation of Cu-NDI-NMe2 Step 1. Preparation of ligand NDI-NMe2 2 mmol of the ligand NDI-Br prepared in Example 1 was dissolved in 10 mL of dimethyl sulfoxide (DMSO) and 6 mL of a 12 mmol / L dimethylamine / tetrahydrofuran mixed solution, the mixed solution was sealed in a Schlenk tube, and heated at 70°C with rapid stirring for 24 h. After the reaction was completed and cooled to room temperature, the reactant was poured into a certain amount of stirred water to generate a precipitate; the generated precipitate was filtered and separated, and washed with water and ethanol respectively; finally, it was recrystallized with 60 mL of dichloromethane / methanol (volume ratio of 1:3) to obtain the ligand NDI-NMe2; Step 2. Dissolve 0.1 mmol of Cu(NO3)2·3H2O and 0.05 mmol of ligand NDI-NMe2 in 7 mL of a mixed solvent of dimethylformamide and methanol to obtain solution A, wherein the volume ratio of dimethylformamide to methanol is 6:1. Place solution A in a threaded glass bottle; Step 3: Add 0.5 mL of 1 mol / L nitric acid solution to 7 mL of solution A, transfer the glass bottle to an oven, heat to 80°C and react for 24 h. After the reaction is cooled to room temperature, separate the solid, wash it with DMF and anhydrous methanol 3-5 times in sequence, and dry it in a vacuum oven at 60-100°C for 12-24 h to obtain Cu-NDI-NMe2.
[0019] The SEM image of Cu-NDI-NMe2 is as follows Figure 2 As shown. Figure 2 It can be seen that Cu-NDI-NMe2 presents a nanorod morphology with uniform size. The nodes of Cu-NDI-NMe2 material are Cu 12 (OH) 12 N 24 , copper adopts CuN2(OH)2 coordination mode.
[0020] Comparative Example: Preparation of MOFs-based Single Atom Copper Catalyst Cu-NDI Step 1. Dissolve 0.1 mmol of Cu(NO3)2·3H2O and 0.05 mmol of NDI ligand in 7 mL of a mixed solvent of dimethylformamide and methanol to obtain solution A, wherein the volume ratio of dimethylformamide to methanol is 6:1, and put the mixed solution into a threaded glass bottle; Step 2. Add 0.5 ml of 1 mol / L nitric acid solution to 7 mL of the mixed solution, transfer the threaded glass bottle to an oven, heat to 80 °C for 24 h, cool the reaction to room temperature, separate the solid, wash with DMF and anhydrous methanol 3-5 times in sequence, and dry in a vacuum oven at 60-100 °C for 12-24 h to obtain Cu-NDI.
[0021] Experiment: Zinc-nitrate battery performance test A zinc-nitrate battery using a two-electrode system and a double-chamber electrolytic cell separated by a bipolar membrane was used to test the battery discharge and nitrate reduction to produce ammonia performance.
[0022] The negative electrode of the zinc-nitrate battery is a metal zinc sheet, and the electrolyte is a 1 mol / L KOH solution; the positive electrode is a carbon cloth loaded with the catalyst prepared in Example 1, 2 or Comparative Example 1, and the electrolyte is a 1 mol / L KOH+0.1 mol / L KNO3 solution.
[0023] The open circuit voltage test results are as follows: Figure 2 shown. Figure 2 The open circuit voltage test results of zinc-nitrate batteries assembled with Cu-NDI-NMe2, Cu-NDI-Br and Cu-NDI materials are shown in the figure from top to bottom in Example 2, Example 1 and Comparative Example. The results show that the performance of zinc-nitrate batteries assembled with Cu-NDI-NMe2 materials prepared in Example 1 and Example 2 is better than that of the comparative example. In particular, the zinc-nitrate battery assembled with Cu-NDI-NMe2 materials prepared in Example 2 exhibits excellent nitrate reduction ammonia synthesis activity, selectivity and stability during discharge, and the maximum power density can reach 36.5 mW cm -2 , the Faradaic efficiency was 98.2% and the ammonia yield was 16.8 mg h -1 mg cat -1 In addition, the battery exhibited excellent output voltage stability in a series of different constant current discharge processes, indicating that the MOFs catalyst with NDI-X as a ligand prepared in the present invention has excellent performance when applied to zinc-nitrate batteries.
Claims
1. A MOFs catalyst with NDI-X as a ligand, wherein the metal element is combined with the ligand through a coordination bond, characterized in that: The ligand is a derivative of di(3,5-dimethylpyrazole)naphthalene diimide, NDI-X, wherein X is -NMe2 or -Br, and the substitution position is one of the four positions of the naphthalene ring.
2. The MOFs catalyst with NDI-X as a ligand according to claim 1, characterized in that: The metal element is Cu, Bi, Zn, Fe or Co.
3. A method for preparing a MOFs catalyst with NDI-X as a ligand as claimed in claim 1, characterized in that Follow these steps: Step 1. Prepare ligand NDI-X; Step 1.1: Mix NDI ligand and sulfuric acid, dissolve them evenly and place them in a flask, wherein the molar ratio of the NDI ligand to the sulfuric acid is 1:20-40; add 1,3-dibromo-5,5-dimethylhydantoin to the solution and stir thoroughly, wherein the molar ratio of the NDI ligand to the 1,3-dibromo-5,5-dimethylhydantoin is 5-10:2-6; place the flask in ice water to obtain a precipitate, wash the precipitate with water and methanol respectively, and then vacuum dry to obtain a 2-bromo-1,4,5,8-naphthalenetetracarboxylic dianhydride ligand 2-Br-NDI; Step 1.2: dissolving 2-Br-NDI and 3,5-dimethylpyrazole in anhydrous dimethylformamide, wherein the molar ratio of 2-Br-NDI to 3,5-dimethylpyrazole is 1-5:2-4, and the amount ratio of 2-Br-NDI to anhydrous dimethylformamide is 2-6mmol:20-50mL; the mixture is fully reacted under an inert atmosphere, and then ether solvent is added to obtain a precipitate, and the obtained precipitate is recrystallized with a mixed solution of anhydrous dimethylformamide / ether / water, and the ligand NDI-Br is obtained after vacuum drying, and the volume ratio of anhydrous dimethylformamide / ether / water is 2:3:1; Step 1.3: dissolving the ligand NDI-Br in a mixed solution of dimethyl sulfoxide and dimethylamine / tetrahydrofuran, wherein the amount ratio of the ligand NDI-Br, dimethyl sulfoxide, and dimethylamine / tetrahydrofuran is 1-6 mmol: 5-20 mL: 2-12 mL, and the ratio of dimethylamine to tetrahydrofuran is 6-18 mmol / L; sealing the mixed solution for reaction, rapidly stirring and heating at 70-120° C. for 12-24 h, pouring the reactant into stirred water to generate a precipitate, filtering and separating the generated precipitate, washing the precipitate with water and ethanol, respectively, and finally recrystallizing with dichloromethane / methanol to obtain a purified product, namely, the ligand NDI-NMe2, wherein the volume ratio of dichloromethane / methanol is 1:3; Step 2. Mix the metal salt and the ligand NDI-X in a molar ratio of 4-1:1-4 and dissolve them in a mixed solvent of dimethylformamide and methanol to obtain solution A, wherein the amount ratio of the metal salt to the mixed solvent is 0.1-0.6 mmol:3-10 mL, and the volume ratio of dimethylformamide to methanol is 4-6:1; Step 3. A nitric acid solution with a concentration of 0.1-2 mol / L is added to solution A in a ratio of 1-3:5-20 for thermal reaction, and a MOFs catalyst with NDI-X as a ligand is obtained after washing and vacuum drying.
4. The method for preparing a MOFs catalyst with NDI-X as a ligand according to claim 3, characterized in that The molar ratio of the metal salt to the ligand NDI-X in step 2 is 3:2, 2:3, 1:1, 1:2 or 1:
3.
5. The method for preparing a MOFs catalyst with NDI-X as a ligand according to claim 4, characterized in that The metal salt in step 2 is Cu(NO3)2, Bi(NO3)2, Zn(NO3)2, Fe(NO3)2 or Co(NO3)2.
6. The method for preparing a MOFs catalyst with NDI-X as a ligand according to claim 3, 4 or 5, characterized in that The temperature of the thermal reaction in step 3 is 50-150° C., and the reaction time is 4 - 96 h.
7. Use of the MOFs catalyst with NDI-X as a ligand as claimed in claim 1 or 2 in a zinc-nitrate battery.