Copper-based MOFs (Metal-Organic Frameworks) taking NDI-F as ligand, preparation method of copper-based MOFs and application of copper-based MOFs in preparation of ammonia by electro-catalytic reduction of nitrate
By using NDI-F as a ligand copper-based MOFs catalyst, the kinetics and selectivity problems in electrocatalytic nitrate reduction synthesis of ammonia were solved, and efficient ammonia synthesis was achieved. The synthesis method was simple and easy to use and had wide application prospects.
Patent Information
- Application Number
- CN202411067346.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, electrocatalytic nitrate reduction synthetic ammonia has problems with large kinetic energy barriers, poor activity and selectivity, and traditional synthetic ammonia technology consumes high energy and is unfriendly in the environment. Nothing is found on the two (3,5-2). Methylpyrazole) Naphthalene diimide derivative NDI-F as a copper-based MOFs ligand.
Using NDI-F as a ligand, bonding with copper elements through coordination bonds, a copper-based MOFs catalyst with high copper load was prepared, and nitrate reduction reaction was carried out under electrocatalytic conditions, using a simple gentle solvent thermal synthesis method , the copper site exists in the form of monodisperse nodes, significantly improving catalytic activity and selectivity.
It achieves high Faraday efficiency and ammonia yield, solves the problems of slow kinetics and poor activity selectivity, and the synthesis method is simple and easy to implement, and has wide application prospects.
Smart Images

Figure CN119019700A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, preparation methods and electrocatalytic nitrate reduction to ammonia production, and in particular to copper-based MOFs with NDI-F as a ligand, a preparation method and application in electrocatalytic nitrate reduction to ammonia production. Background Art
[0002] As the world's second largest chemical raw material, ammonia is not only an important chemical raw material for modern fertilizers, but also an important hydrogen energy carrier with its zero carbon and high hydrogen content, which has attracted widespread attention. The traditional ammonia synthesis process mainly relies on the Haber-Bosch process, which requires extremely harsh reaction conditions such as high temperature and high pressure, with high energy consumption and high carbon dioxide emissions. Electrocatalytic nitrogen reduction to synthesize ammonia at room temperature and atmospheric pressure is an environmentally friendly and sustainable reaction route, but due to the high bond energy and low solubility of nitrogen molecules, there are problems of low yield and efficiency. Nitrate is widely present in wastewater, especially in groundwater, which is one of the main nitrogen pollutants. The accumulation of nitrate in the environment leads to an increase in the concentration of toxic nitrite converted from nitrate, which brings health problems to organisms. In addition, compared with nitrogen molecules, nitrate has the advantages of low bond energy and high solubility in water. The reduction of nitrate to synthesize ammonia through electrocatalytic technology can not only promote the purification of wastewater resources, but also obtain high value-added chemical ammonia. The electrocatalytic nitrate reduction reaction is carried out in an H-type double-chamber reaction cell, with the cathode chamber and the anode chamber separated by a proton exchange membrane. The cathode chamber uses a hydrophobic carbon cloth loaded with a catalyst as the working electrode, and a KCl solution-saturated Ag / AgCl electrode as the reference electrode; the anode chamber uses a platinum sheet as the counter electrode, and the nitrate in the cathode solution is electrochemically reduced to synthesize ammonia through constant potential polarization. However, since nitrate reduction involves multiple electron transfers and there is a large kinetic energy barrier, the development of an electrocatalyst with excellent nitrate reduction and ammonia synthesis performance is of great significance for the efficient conversion of nitrate and high activity and high selectivity in ammonia production.
[0003] Metal-organic frameworks (MOFs) are a type of porous material formed by metals and organic ligands connected by coordination bonds. They have the characteristics of clear sites, high specific surface area, adjustable pores, and designable composition and structure. They have the advantages of both homogeneous and heterogeneous catalysts and are widely used in catalysis and other fields. The electronic structure and catalytic activity of the metal nodes of MOFs materials are significantly affected by the surrounding ligands. Therefore, optimizing the structure of the ligands is an effective strategy to improve the catalytic activity and selectivity of MOFs. In addition, the synthesis strategy of MOFs mainly relies on harsh reaction conditions, the metal loading is relatively low, and the stability is also poor. The high-load Cu-MOFs disclosed in the prior art use di(3,5-dimethylpyrazole)naphthalene diimide (NDI) as a ligand, which has a relatively single function and is difficult to effectively regulate the metal copper nodes, resulting in poor activity and selectivity in catalytic reactions.
[0004] So far, there is no report on the preparation of bis(3,5-dimethylpyrazole)naphthalene diimide derivative NDI-F and using it as a ligand to prepare copper-based organic frameworks (MOFs). Summary of the invention
[0005] The present invention aims to solve the above-mentioned technical problems existing in the prior art and provides a copper-based MOFs with NDI-F as a ligand, a preparation method and an application in electrocatalytic nitrate reduction to produce ammonia.
[0006] The technical solution of the present invention is: a copper-based MOFs with NDI-F as a ligand, in which the metal element Cu is combined with the ligand through a coordination bond, and the ligand is a derivative of di(3,5-dimethylpyrazole)naphthalene diimide NDI-F, and the substitution position is one of the four positions of the naphthalene ring.
[0007] A method for preparing the above-mentioned copper-based MOFs with NDI-F as a ligand is characterized by following the steps: Step 1. preparing ligand NDI-F; Step 1.1: Mix NDI ligand and sulfuric acid, dissolve them evenly and place them in a flask, wherein the molar ratio of the NDI ligand to the sulfuric acid is 1:20-40, add 1,3-dibromo-5,5-dimethylhydantoin to the solution and stir thoroughly, wherein the molar ratio of the NDI ligand to the 1,3-dibromo-5,5-dimethylhydantoin is 5-10:2-6; place the flask in ice water to obtain a precipitate, wash the precipitate with water and methanol respectively, and then vacuum dry to obtain a 2-bromo-1,4,5,8-naphthalenetetracarboxylic dianhydride ligand 2-Br-NDI; Step 1.2: dissolving 2-Br-NDI and 3,5-dimethylpyrazole in anhydrous dimethylformamide, wherein the molar ratio of 2-Br-NDI to 3,5-dimethylpyrazole is 1-5:2-4, and the amount ratio of 2-Br-NDI to anhydrous dimethylformamide is 2-6 mmol:20-50 mL; the mixture is fully reacted under an inert atmosphere, and then ether solvent is added to obtain a precipitate, and the obtained precipitate is recrystallized with a mixed solution of anhydrous dimethylformamide / ether / water, and the ligand NDI-Br is obtained after vacuum drying, wherein the volume ratio of anhydrous dimethylformamide / ether / water is 2:3:1; Step 1.3 Step 1.3 Dissolve NDI-Br ligand, 18-crown ether-6 and anhydrous potassium fluoride in a dimethyl sulfoxide solution, wherein the amount ratio of the NDI-Br ligand, 18-crown ether-6, anhydrous potassium fluoride and dimethyl sulfoxide is 1-3 mmol:1-2mmol:6-10 mmol:10-50mL, seal the mixed solution, and heat it at 100-180°C with rapid stirring for 1-6 h, add water to the reactant and stir to form a precipitate, filter and separate the generated precipitate, wash the precipitate with water and ethanol, and finally recrystallize it with dichloromethane / methanol to obtain a purified product, i.e., ligand NDI-F, wherein the volume ratio of dichloromethane / methanol is 1:3; Step 2. The copper salt and the ligand NDI-F are mixed in a molar ratio of 4-1:1-4 and dissolved in a mixed solvent of dimethylformamide and methanol to obtain a solution A, wherein the amount ratio of the copper salt to the mixed solvent is 0.1-0.6 mmol:3-10 mL, and the volume ratio of the dimethylformamide to methanol is 4-6:1; Step 3. A nitric acid solution with a concentration of 0.1-2 mol / L is added to solution A in a ratio of 1-3:5-20 for thermal reaction, and a MOFs catalyst with NDI-F ligand is obtained after washing and vacuum drying.
[0008] Preferably, the molar ratio of the copper salt to the ligand NDI-F is 3:2, 2:3, 1:1, 1:2 or 1:3.
[0009] Preferably, the copper salt is at least one of Cu(NO3)2, CuCl2, CuSO4, Cu(OAc)2, and Cu(acac)2.
[0010] Preferably, the temperature of the thermal reaction is 50-150° C. and the reaction time is 4-96 h.
[0011] An application of the above copper-based MOFs with NDI-F as a ligand in the electrocatalytic reduction of nitrate to produce ammonia.
[0012] The present invention first prepares a di(3,5-dimethylpyrazole)naphthalene diimide derivative NDI-F and uses it as a ligand, and then uses it with copper salts through a simple and mild solvothermal synthesis method to prepare a MOFs-based single-atom catalyst with a copper loading of up to 30%. The copper sites exist in the MOFs in the form of monodispersed nodes. The catalyst exhibits excellent ammonia production rate and Faraday efficiency in electrocatalytic ammonia synthesis, significantly changing the electrocatalytic activity and selectivity of the catalyst. Experiments show that the Faraday efficiency is as high as 98.6%, and the ammonia yield is 21.8 mg h -1 mg cat -1 . It solves the problems of slow kinetics, poor activity and selectivity faced by nitrate reduction to synthesize ammonia, and the synthesis method is simple and easy, with great application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 is a SEM image of Cu-NDI-F prepared in an embodiment of the present invention.
[0014] Figure 2 These are the XRD patterns of Cu-NDI-F, Cu-NDI, and Cu-NDI-Br.
[0015] Figure 3 This is the performance diagram of electrocatalytic nitrate reduction to ammonia synthesis using Cu-NDI, Cu-NDI-Br, and Cu-NDI-F as working electrode materials. DETAILED DESCRIPTION
[0016] The sources of all raw materials in the present invention are not particularly limited and can be purchased from the market or prepared according to conventional methods known to those skilled in the art. NDI is prepared according to the literature ( J. Mater. Chem. C 2014, 2 , 2869-2876. DOI: 10.1039 / C3TC32377C). The purity of all raw materials in the present invention is not particularly limited, and analytically pure materials are preferably used.
[0017] Embodiment 1: The present invention provides a method for preparing an NDI-F ligand: Step 1. Preparation of ligand NDI-F Step 1.1: Mix 15 mmol of NDI ligand and 20 mL of 18.4 mol / L sulfuric acid, dissolve them evenly and place them in a round-bottom flask; add 6 mmol of 1,3-dibromo-5,5-dimethylhydantoin to the solution in the round-bottom flask and stir them for 12 hours; place the round-bottom flask in ice water to obtain a precipitate; wash the precipitate with water and methanol three times respectively and then dry it in vacuum to obtain 2-bromo-1,4,5,8-naphthalenetetracarboxylic dianhydride ligand 2-Br-NDI; Step 1.2: Dissolve 4 mmol 2-Br-NDI and 7 mmol 3,5-dimethylpyrazole in 40 mL anhydrous dimethylformamide (DMF); heat the mixture at 150 °C under a nitrogen atmosphere, stir rapidly for 12 h, cool to room temperature, add 150 mL ether solvent to react fully to obtain a precipitate, and recrystallize the obtained precipitate with 30 mL of a mixed solution of DMF / ether / water, and dry it in vacuo at 70 °C to obtain the ligand NDI-Br, wherein the volume ratio of DMF / ether / water is 2:3:1; Step 1.3: Dissolve 0.2 mmol NDI-Br ligand, 0.1 mmol 18-crown ether-6 and 1.5 mmol anhydrous potassium fluoride in 2 mL dimethyl sulfoxide (DMSO). After reacting at 180°C for 1 h, add a certain amount of water to the reactant and stir to precipitate a brown solid. Use 20 mL of dichloromethane / methanol as raw material, with a volume ratio of dichloromethane to methanol of 1:3, and recrystallize and purify the precipitate to obtain purified NDI-F ligand.
[0018] Step 2. Dissolve 0.1 mmol of Cu(NO3)2·3H2O and 0.05 mmol of ligand NDI-F in 7 mL of a mixed solvent of dimethylformamide and methanol to obtain solution A, wherein the volume ratio of dimethylformamide to methanol is 6:1. Place solution A in a threaded glass bottle; Step 3. Add 0.5 mL of 1 mol / L nitric acid solution to 7 mL of solution A, transfer the threaded glass bottle to an oven, heat to 80 °C for 24 h, cool the reaction to room temperature, separate the solid, wash with DMF and anhydrous methanol 3-5 times in sequence, and dry in a vacuum oven at 60-100 °C for 12-24 h to obtain Cu-NDI-F.
[0019] The SEM image of Cu-NDI-F is shown in Figure 1 As shown. Figure 1 It can be seen that Cu-NDI-F presents a nanorod morphology structure with uniform size.
[0020] Comparative Example 1: Cu-NDI Step 1. Dissolve 0.1 mmol of Cu(NO3)2·3H2O and 0.05 mmol of NDI ligand in 7 mL of a mixed solvent of dimethylformamide and methanol to obtain solution A, wherein the volume ratio of dimethylformamide to methanol is 6:1, and put the mixed solution into a threaded glass bottle; Step 2. Add 0.5 ml of 1 mol / L nitric acid solution to 7 mL of the mixed solution, transfer the threaded glass bottle to an oven, heat to 80 °C for 24 h, cool the reaction to room temperature, separate the solid, wash with DMF and anhydrous methanol 3-5 times in sequence, and dry in a vacuum oven at 60-100 °C for 12-24 h to obtain Cu-NDI.
[0021] Comparative Example 2: Cu-NDI-Br Step 1. Dissolve 0.1 mmol of Cu(NO3)2·3H2O and 0.05 mmol of NDI-Br ligand (obtained in step 1.2 of Example 1) in 7 mL of a mixed solvent of dimethylformamide and methanol to obtain solution A, wherein the volume ratio of dimethylformamide to methanol is 6:1, and put the mixed solution into a threaded glass bottle; Step 2. Add 0.5 ml of 1 mol / L nitric acid solution to 7 mL of the mixed solution, transfer the threaded glass bottle to an oven, heat to 80 °C for 24 h, cool the reaction to room temperature, separate the solid, wash with DMF and anhydrous methanol 3-5 times, and dry in a vacuum oven at 60-100 °C for 12-24 h to obtain Cu-NDI-Br.
[0022] The XRD patterns of Cu-NDI-F, Cu-NDI and Cu-NDI-Br are as follows Figure 2 As shown, from Figure 2 It can be seen that the three MOFs catalysts have the same crystal structure, indicating that adjusting the substituent groups in the ligand will not have a significant effect on the structure of MOFs.
[0023] Experiment: Electrocatalytic nitrate reduction performance test The catalyst Cu-NDI-F prepared in Example 1, the catalyst Cu-NDI prepared in Comparative Example 1, and the catalyst Cu-NDI-Br prepared in Comparative Example 2 were used for electrochemical testing. The specific operation method is as follows: a three-electrode system was used for testing, Ag / AgCl was used as a reference electrode, a platinum sheet was used as a counter electrode, and a carbon cloth loaded with Cu-MOFs of Example 1, Comparative Examples 1 and 2 was used as a working electrode, and the electrochemical performance was evaluated in 0.1 M KHCO3 and 0.1 M KHCO3+0.1 M KNO3, respectively. Cyclic voltammetry, linear sweep voltammetry and constant potential polarization curve tests were carried out in the system. The ammonia production efficiency and ammonia Faraday efficiency of the three catalysts are shown in Figure 2. Figure 3 shown. Figure 3It shows that the ammonia production efficiency and ammonia Faraday efficiency of Cu-NDI-F in Example 1 of the present invention are better than those of Cu-NDI and Cu-NDI-Br catalysts obtained in Comparative Examples 1 and 2, and has higher nitrate reduction activity.
Claims
1. A copper-based MOFs with NDI-F as ligand, in which the metal element Cu is combined with the ligand through a coordination bond. Features: The ligand is a derivative of di(3,5-dimethylpyrazole)naphthalene diimide, NDI-F, and the substitution position is one of the four positions of the naphthalene ring.
2. A method for preparing copper-based MOFs with NDI-F as a ligand as claimed in claim 1, Features Follow these steps: Step 1. Prepare ligand NDI-F; Step 1.1: Mix NDI ligand and sulfuric acid, dissolve them evenly and place them in a flask, wherein the molar ratio of the NDI ligand to the sulfuric acid is 1:20-40; add 1,3-dibromo-5,5-dimethylhydantoin to the solution and stir thoroughly, wherein the molar ratio of the NDI ligand to the 1,3-dibromo-5,5-dimethylhydantoin is 5-10:2-6; place the flask in ice water to obtain a precipitate, wash the precipitate with water and methanol respectively, and then vacuum dry to obtain a 2-bromo-1,4,5,8-naphthalenetetracarboxylic dianhydride ligand 2-Br-NDI; Step 1.2: dissolving 2-Br-NDI and 3,5-dimethylpyrazole in anhydrous dimethylformamide, wherein the molar ratio of 2-Br-NDI to 3,5-dimethylpyrazole is 1-5:2-4, and the amount ratio of 2-Br-NDI to anhydrous dimethylformamide is 2-6mmol:20-50mL; the mixture is fully reacted under an inert atmosphere, and then ether solvent is added to obtain a precipitate, and the obtained precipitate is recrystallized with a mixed solution of anhydrous dimethylformamide / ether / water, and the ligand NDI-Br is obtained after vacuum drying, and the volume ratio of anhydrous dimethylformamide / ether / water is 2:3:1; Step 1.3: dissolving NDI-Br ligand, 18-crown ether-6 and anhydrous potassium fluoride in a dimethyl sulfoxide solution, wherein the amount ratio of the NDI-Br ligand, 18-crown ether-6, anhydrous potassium fluoride and dimethyl sulfoxide is 1-3 mmol:1-2 mmol:6-10 mmol:10-50 mL, and rapidly stirring and heating the mixed solution at 100-180° C. for 1-6 h, adding water to the reactant and stirring to form a precipitate, filtering and separating the generated precipitate, washing the precipitate with water and ethanol, respectively, and finally recrystallizing with dichloromethane / methanol to obtain a purified product, i.e., ligand NDI-F, wherein the volume ratio of dichloromethane / methanol is 1:3; Step 2. The copper salt and the ligand NDI-F are mixed in a molar ratio of 4-1:1-4 and dissolved in a mixed solvent of dimethylformamide and methanol to obtain a solution A, wherein the amount ratio of the copper salt to the mixed solvent is 0.1-0.6 mmol:3-10 mL, and the volume ratio of the dimethylformamide to methanol is 4-6:1; Step 3. A nitric acid solution with a concentration of 0.1-2 mol / L is added to solution A in a ratio of 1-3:5-20 for thermal reaction, and a MOFs catalyst with NDI-F ligand is obtained after washing and vacuum drying.
3. The method for preparing copper-based MOFs with NDI-F as a ligand according to claim 2, Features The molar ratio of the copper salt to the ligand NDI-F in step 2 is 3:2, 2:3, 1:1, 1:2 or 1:
3.
4. The method for preparing copper-based MOFs with NDI-F as a ligand according to claim 3, Features The copper salt in step 2 is Cu(NO 3 ) 2 , CuCl 2 ,CuSO 4 、Cu(OAc) 2 、Cu(acac) 2 At least one of .
5. The method for preparing copper-based MOFs with NDI-F as a ligand according to claim 2, 3 or 4, Features The temperature of the thermal reaction in step 3 is 50-150° C., and the reaction time is 4-96 h.
6. An application of the copper-based MOFs with NDI-F as a ligand as claimed in claim 1 in electrocatalytic nitrate reduction to produce ammonia.