Tire sidewall composition and tire sidewall
By using rubber compositions such as polyisoprene, polybutadiene and other rubber compositions in the sidewall of the tire, combined with specific accelerators and fillers, the problem of frost on the tire surface caused by high wax content is solved, and the wax cream is reduced The emergence and enhance the durability and performance of the tire.
Patent Information
- Application Number
- CN202410645966.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-23
- Filing Date
- 2024-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
High content of wax causes visible frost on the tire surface in the sidewall of the tire, affecting aesthetics, while reducing or eliminating wax levels without damaging durability.
Using rubber compositions containing polyisoprene, polybutadiene, sulfur, diphenylguanidine, tetrabenzylthiuram disulfide and sulfonamide, combined with rosin acid and A filler such as carbon black forms a new tire sidewall composition.
It significantly reduces the appearance of wax cream, improves incision growth performance, and maintains the tire's ozone resistance and tear performance, improving the tire's appearance and performance.
Smart Images

Figure CN119019765A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a tire sidewall composition and a tire sidewall. Background Art
[0002] High levels of wax are commonly used in sidewall compounds to prevent static ozone weather cracking. 6PPD is commonly used in sidewalls for dynamic ozone resistance. In addition, tire sidewall compounds are dynamically flexed millions of times during their expected service life. The cut growth properties should remain excellent during these service lives. Blends of natural rubber and polybutadiene are also used in combination with wax and 6PPD to produce desirable cut growth properties.
[0003] The use of high levels of wax results in visible blooming of the tire surface, which can be objectionable to consumers. There is a need for a tire sidewall composition that reduces and / or eliminates wax levels without compromising the durability of the tire sidewall. Summary of the invention
[0004] In some embodiments, a tire having a visible sidewall is disclosed that includes, based on parts by weight per 100 parts by weight of rubber (phr): (A) a blend of polymers comprising at least polyisoprene and polybutadiene; (B) a reinforcing filler; and (C) a cure package comprising sulfur and at least three accelerators, including diphenylguanidine and tetrabenzylthiuram disulfide and sulfenamide.
[0005] The amount of tetrabenzylthiuram disulfide in the rubber composition may be about 0.25 to about 2.5 phr, preferably about 0.5 to about 1.5 phr.
[0006] In some embodiments, the polyisoprene comprises natural rubber or synthetic polyisoprene.
[0007] Particular embodiments include from about 30 phr to about 60 phr of natural rubber or synthetic polyisoprene and from about 40 phr to about 70 phr of cis 1,4-polybutadiene rubber.
[0008] In some embodiments, the reinforcing filler comprises carbon black, optionally in combination with silica.
[0009] The tire may further comprise rosin acid. In some embodiments, the amount of rosin acid is from about 0.25 to about 3.0 phr, preferably from about 0.5 to about 2.0 phr.
[0010] In some embodiments, the amount of diphenylguanidine may be from about 0.25 phr to about 3.0 phr.
[0011] In some embodiments, the amount of sulfenamide is from about 0.25 phr to about 3.0 phr, preferably from about 0.5 phr to about 2.0 phr.
[0012] In some embodiments, the amount of filler may be from about 30 phr to about 70 phr, preferably from about 35 phr to about 55 phr.
[0013] In some embodiments, the rubber composition comprises at least 25% less wax relative to a compound without rosin acid, diphenylguanidine, and tetrabenzylthiuram disulfide.
[0014] In some embodiments, the rubber composition may be partially or completely free of wax relative to a compound that does not contain rosin acid and does not contain the disclosed cure package.
[0015] In some embodiments, the rubber composition has a 6PPD that is reduced by at least 25% relative to a compound that does not contain rosin acid and does not contain the disclosed cure package. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The following is a brief description of the drawings, which are presented for the purpose of illustrating exemplary embodiments disclosed herein and not for the purpose of limiting the same.
[0017] Figure 1 is a partial side view of a non-limiting example of a tire according to some embodiments of the present disclosure.
[0018] Figure 2 is a flow chart illustrating a non-limiting example of a method of forming an article according to some embodiments of the present disclosure. DETAILED DESCRIPTION
[0019] The present disclosure may be understood more readily by reference to the following detailed description and accompanying drawings of desirable embodiments included therein.In the following specification and the claims that follow, reference will be made to a number of terms which shall be defined to have the following meanings.
[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those of ordinary skill in the art are generally understood. In the event of a conflict, this document (including definitions) shall prevail. Preferred methods and materials are described below, although similar or equivalent methods and materials may be used in the practice or testing of the present disclosure. All publications, patent applications, patents and other references mentioned herein are incorporated by reference in their entirety. The materials, methods and products disclosed herein are illustrative only and are not intended to be limiting.
[0021] The singular forms "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.
[0022] As used in the specification and claims, the term "comprising" may include the embodiments "consisting of" and "consisting essentially of. As used herein, the terms "comprising," "including," "having," "having," "may," "containing," and variations thereof are intended to be open-ended transitional phrases requiring the presence of specified ingredients / steps and allowing for the presence of other ingredients / steps. However, such descriptions should be construed as also describing compositions, mixtures, or methods as "consisting of" and "consisting essentially of" the listed ingredients / steps, allowing for the presence of only the specified ingredients / steps, as well as any impurities that may result therefrom, and excluding other ingredients / steps.
[0023] Unless otherwise indicated, the numerical values in the specification should be understood to include the same values when reduced to the same number of significant figures and values that differ from the stated value by less than experimental error. The type of conventional measurement techniques used to determine the particular value.
[0024] All ranges disclosed herein are inclusive of the recited endpoints and are independently combinable (e.g., a range "from 2 to 10" includes endpoints 2 and 10 and all intermediate values). The endpoints of the ranges and any values disclosed herein are not limited to the exact ranges or values; they are imprecise enough to include values approximating these ranges and / or values.
[0025] As used herein, approximate language can be applied to modify any quantitative representation that can be changed without causing a change in the basic function associated therewith. Therefore, in some cases, the value modified by one or more terms (such as "about" and "substantially") may not be limited to the specified exact value. The modifier "about" should also be considered to disclose a range defined by the absolute values of the two endpoints. For example, the expression "about 2 to about 4" also discloses a range of "2 to 4". The term "about" can refer to plus or minus 10% of a specified number. For example, "about 10%" can represent a range of 9% to 11%, and "about 1" can represent 0.9-1.1.
[0026] For the recitation of numerical ranges herein, each intervening number with the same degree of precision is expressly contemplated. For example, for the range of 6-9, in addition to 6 and 9, the numbers 7 and 8 are also contemplated, and for the range 6.0-7.0, the numbers 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, and 7.0 are expressly contemplated.
[0027] As used herein, and in accordance with conventional practice, the term "phr" means "parts of the respective material per 100 parts by weight of rubber". The terms "rubber" and "elastomer" may be used interchangeably unless otherwise indicated. The terms "rubber composition", "compounded rubber" and "rubber compound" may be used interchangeably to refer to "rubber that has been blended or mixed with various ingredients and materials", and the terms "cured" and "vulcanized" may also be used interchangeably unless otherwise indicated, and these terms are well known to those skilled in the art of rubber mixing or rubber compounding.
[0028] Figure 1 1 is a partial side view of a non-limiting example of a tire 100 according to some embodiments of the present disclosure. The tire 100 includes a tread portion 110, a bead portion 120, and a sidewall portion 130 located between the tread portion 110 and the bead portion 120. The tread portion 110, the bead portion 120, and the sidewall portion 130 of the tire according to the present disclosure are not limited to Figure 1 For example, there may be multiple sidewall sections, ribs, patterns, colors, etc. Figure 1 An example of a tire sidewall composition in which the present invention may be used is shown below.
[0029] Figure 2 is a flow chart illustrating a non-limiting example of a method 240 of forming an article (eg, a tire) according to some embodiments of the present disclosure. The method 240 includes providing a tire sidewall composition 250, non-productive mixing 260, productive mixing 270, and vulcanization 280.
[0030] The disclosed invention unexpectedly allows for a reduction in wax levels (e.g., at least 25% reduction from typical wax levels in the sidewall of up to 4 phr) and reduces or eliminates visible wax bloom in the vulcanizate. The inclusion of the disclosed cure package with rosin acid unexpectedly results in a significant improvement in cut growth performance.
[0031] In one embodiment, rosin acid may be mixed in the non-productive mix stage 260 and the cure package may be mixed in the productive stage 270. Sulfur and accelerators may be mixed with the non-productive mix from stage 260 in the productive mix stage 270 prior to vulcanization 280.
[0032] Abietic acid
[0033] Abietic acid may be included in the composition in an amount from about 0.25 phr to about 3.0 phr. In some embodiments, the abietic acid content is from about 0.5 phr to about 2.0 phr.
[0034] diphenylguanidine
[0035] Diphenylguanidine may be included in the composition in an amount of about 0.25 phr to about 3.0 phr. In some embodiments, the diphenylguanidine is present in an amount of about 0.5 phr to about 2.5 phr.
[0036] Tetrabenzylthiuram disulfide
[0037] Tetrabenzylthiuram disulfide can be included in the composition in an amount of about 0.25 phr to about 2.5 phr. In some embodiments, the tetrabenzylthiuram disulfide content is about 0.5 phr to about 1.5 phr.
[0038] The composition supplied to the non-productive mixing stage further contains at least one elastomer (for example at least one diene elastomer) and a reinforcing filler.
[0039] Elastomer
[0040] In some embodiments, the elastomer is selected from natural rubber, synthetic polyisoprene, and / or polybutadiene.
[0041] In a particular embodiment, the at least one diene elastomer comprises from about 30 phr to about 60 phr of natural rubber or synthetic polyisoprene and from about 40 phr to about 70 phr of cis-1,4-polybutadiene.
[0042] Polybutadiene
[0043] In some embodiments, the polybutadiene is cis-1,4-polybutadiene. However, in other embodiments, the polybutadiene is lithium-produced polybutadiene. The lithium-produced polybutadiene may have a trans content of about 45% to 55%, a cis content of about 35% to 45%, and a vinyl content of about 7.5% to 12.5%.
[0044] Cis 1,4-polybutadiene may be included in the composition in an amount of about 10 to about 60 phr. In some embodiments, the cis 1,4-polybutadiene content is about 20 to about 50 phr, including about 30 to about 40 phr or about 35 phr.
[0045] In some embodiments, the cis 1,4 content of the cis 1,4-polybutadiene may be at least 95%, at least 96%, at least 97%, or at least 98%.
[0046] Non-limiting examples of suitable cis-1,4-polybutadiene include 1207, 1208, 1208G, 1208W, 1280, 1222, 1223 and 1224, all of which are available from The Goodyear Tire and Rubber Company.
[0047] Lithium produced polybutadiene generally has a higher trans content than cis content. Lithium produced polybutadiene may have a glass transition temperature (T) of about -92°C to about -88°C. g ).
[0048] cis-1,4-polyisoprene
[0049] The cis 1,4-polyisoprene rubber can be a natural rubber or a synthetic rubber. In some preferred embodiments, the cis 1,4-polyisoprene is a natural rubber.
[0050] Cis 1,4-polyisoprene can be included in the composition in an amount of about 40 to about 70 phr.
[0051] Non-limiting examples of natural rubber grades include TSR10 and TSR20.
[0052] filler
[0053] The filler content may be from about 30 phr to about 70 phr, preferably from about 35 phr to about 55 phr.
[0054] Non-limiting representative examples of rubber reinforced carbon black and their ASTM names are shown in The Vanderbilt Rubber Handbook, 13th edition, 1990, pages 417 and 418. The document is incorporated herein by reference. As noted, such rubber reinforced carbon blacks may have, for example, iodine absorption values (particle size measurement) of 60 to 240 g / kg and DBP (dibutyl phthalate; structural measurement) values of 34 to 150 cc / 100 g. A non-limiting example of suitable carbon black is ASTM N326, which has a DBP value of about 72 and an iodine value of about 82.
[0055] Reinforcing fillers typically include carbon black and optional silica (e.g., synthetic precipitated silica). The total amount of filler may be from about 30 phr to about 70 phr, preferably from about 35 phr to about 55 phr. The present disclosure contemplates that when carbon black and silica are used in combination, carbon black will constitute the majority of the filler content.
[0056] The precipitated silica reinforcement material may be characterized, for example, by a BET surface area, measured using nitrogen, of, for example, about 40 to about 600, and more typically about 50 to about 300 square meters per gram. The BET method for measuring surface area may be described, for example, in the Journal of the American Chemical Society, Vol. 60, and in ASTM D3037.
[0057] Various commercially available precipitated silicas may be used, such as, but not intended to be limiting, silicas from PPG Industries under the Hi-Sil trademark, such as 210, 243, 315, etc.; silicas from Solvay, such as Zeosil 1165MP TM and Zeosil165GR TM ; silicas from Evonik, for example under the designations VN2 and VN3; and chemically treated (pre-hydrophobized) precipitated silicas, for example Agilon™ 400 from PPG.
[0058] A coupling agent may be included, however in some embodiments, the rubber composition does not include any coupling agent even when carbon black and silica are used as fillers.
[0059] The rubber composition may optionally further comprise up to about 15, or about 2 to about 15 phr of at least one additional diene-based elastomer selected from at least one rubber of styrene / butadiene copolymers, isoprene / butadiene copolymers and styrene / isoprene / butadiene terpolymers prepared by organic solvent solution polymerization or emulsion polymerization. The additional solvent-polymerized elastomer may also be a tin-coupled elastomer.
[0060] The rubber composition can be prepared by simple mixing. In some embodiments, mixing will be performed using a closed mixer or an open mixer (e.g., dual opposing rolls). Closed mixers are preferred, and it is generally preferred to mix the triglyceride oil and filler into the elastomeric composition during at least one non-productive compounding stage. Figure 2 , which can be referred to as a non-productive mixing phase 260 .
[0061] The rubber composition of the present disclosure optionally contains one or more additional compounding ingredients and / or additives. Typical amounts of processing aids and rubber compounding ingredients include about 1 to about 50 phr. Such processing aids may include, for example, aromatic, naphthenic, paraffinic processing oils, vegetable triglycerides, and plant-derived oils. Stearic acid may be present, although embodiments contemplate rosin acid as a substitute for stearic acid.
[0062] Vulcanization 280 is performed in the presence of the curing package of the present disclosure.
[0063] Accelerator is used to control the required time and / or temperature of vulcanization and improve the property of vulcanized rubber.The combination of accelerator of the present disclosure produces synergistic effect to final property and is better than the effect produced by using any accelerator alone.The example of sulfonamide accelerator comprises N-oxydiethylenebenzothiazole-2-sulfonamide, N-tert-butyl-2-benzothiazole sulfonamide and N-cyclohexyl-2-benzothiazole sulfonamide.
[0064] The compositions according to the present disclosure exhibit improved appearance while maintaining the key cure properties of ozone resistance, tear and cut growth.
[0065] The following examples are provided to illustrate the apparatus and methods of the present disclosure. These examples are illustrative only and are not intended to limit the present disclosure to the materials, conditions or method parameters set forth therein.
[0066] Example
[0067] Examples were produced using a combination of rosin acid and diphenylguanidine in a tire sidewall compound. Wax levels were significantly reduced, producing tires with no visible wax bloom, better surface appearance, and excellent static ozone protection.
[0068]
[0069] The invention in Experiment B showed improved equivalent performance in dynamic, ozone and cut growth.
[0070] This written description uses examples to describe the present disclosure, including the best mode, and also enables any technician in the field to implement and use the present disclosure. Other examples that come to mind to those skilled in the art are intended to fall within the scope of the present disclosure if they have structural elements that are not different from the same concept, or if they include equivalent structural elements with insubstantial differences. It should be understood that the above-disclosed variants and other features and functions or their alternatives can be combined into many other different systems or applications. Those skilled in the art can then make various currently unforeseen or unanticipated substitutions, modifications, changes or improvements therein, which are also intended to be covered by the appended claims.
Claims
1. A tire having a visible sidewall, wherein the rubber composition of the sidewall comprises, in parts by weight per 100 parts by weight of rubber (phr): (A) a polymer blend comprising at least polyisoprene and polybutadiene; (B) a reinforcing filler comprising silica, carbon black, or a combination of the two; and (C) a cure package comprising Sulfur; and At least three accelerators including diphenylguanidine and tetrabenzylthiuram disulfide and sulfenamide.
2. The tire according to claim 1, wherein the amount of tetrabenzylthiuram disulfide is from about 0.25 to about 2.5 phr.
3. The tire according to claim 1, wherein the amount of tetrabenzylthiuram disulfide is from about 0.5 to about 1.5 phr.
4. The tire of claim 1, wherein the polyisoprene is natural rubber, synthetic polyisoprene, or a combination thereof.
5. The tire according to claim 1, further comprising: about 30 phr to about 60 phr of natural rubber or synthetic polyisoprene; and about 40 phr to about 70 phr of cis-1,4-polybutadiene rubber.
6. The tire of claim 1 wherein the reinforcing filler comprises carbon black.
7. The tire of claim 1 wherein the reinforcing filler comprises a blend of carbon black and silica. The tire according to claim 1 , further comprising rosin acid.
9. The tire of claim 8, wherein the amount of rosin acid is from about 0.25 phr to about 3.0 phr.
10. The tire of claim 8, wherein the amount of rosin acid is from about 0.5 phr to about 2.0 phr.
11. The tire of claim 1, wherein the amount of diphenylguanidine is from about 0.25 phr to about 3.0 phr.
12. The tire of claim 1, wherein the amount of diphenylguanidine is from about 0.5 phr to about 2.5 phr.
13. The tire of claim 1, wherein the amount of sulfenamide is from about 0.25 phr to about 2.5 phr.
14. The tire of claim 1, wherein the amount of filler is from about 30 phr to about 70 phr.
15. The tire of claim 1 wherein the rubber composition comprises at least 25% less wax relative to a compound without rosin acid and the cure package.
16. The tire of claim 1, wherein the rubber composition comprises at least 25% less 6PPD relative to a compound without rosin acid and the cure package.
17. The tire of claim 1, wherein the rubber composition is partially or completely free of wax.