Easily-processed and salt-fog-resistant electromagnetic shielding rubber material as well as preparation method and application thereof
By using internal lubricants such as oleic amide and titanate coupling agents in electromagnetic shielding rubber, the inter-chain effect of polymers and the formation of waxy films is weakened, and the material flowability and salt spray resistance are solved, and the electromagnetic protection ability is improved and optimization of production process.
Patent Information
- Application Number
- CN202411287099.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-13
AI Technical Summary
The existing electromagnetic shielding rubber materials have poor fluidity, difficulty in forming and insufficient salt spray corrosion resistance during processing, resulting in a degradation of electromagnetic shielding performance.
Use internal lubricants such as oleic acid amide and erucic acid amide to weaken the interaction force between polymer chains, improve the mobility of the molecular chain, and form a waxy film with the internal lubricant to isolate the external moisture, improving the material Fluidity and salt spray resistance.
It improves the easy processing performance and salt spray corrosion resistance of electromagnetic shielding rubber materials, reduces the Mooney's viscosity, reduces the extrusion and swelling effect, optimizes the molding process, and significantly improves the electromagnetic protection ability.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electromagnetic shielding materials, and in particular to an electromagnetic shielding rubber material which is easy to process and resistant to salt spray, and a preparation method and application thereof. Background Art
[0002] As the power of electronic equipment and devices continues to increase, a large amount of electromagnetic pollution is generated, which harms human health and interferes with the normal operation of equipment. As a new type of electromagnetic shielding material, electromagnetic shielding rubber is widely used in sealing scenarios in the field of electromagnetic protection due to its excellent conductivity and flexibility.
[0003] Rubber itself is an insulator. At present, the preparation of electromagnetic shielding rubber in industry often requires filling the rubber with a large amount of conductive metal powder. On the one hand, the mutual entanglement between the rubber macromolecule chains and the anchoring effect of the filler on the rubber restrict the movement of the rubber macromolecule chains, resulting in reduced fluidity of the composite material, difficulty in filling the mold during molding, and greater energy input during the processing process; and the rubber compound is prone to generate large internal stress during extrusion, resulting in extrusion expansion effect, and the size is difficult to control.
[0004] On the other hand, a large amount of fillers leads to a decrease in the cross-linking density of rubber, a decrease in cohesion, and external water molecules easily penetrate into the rubber, causing corrosion of the conductive metal powder, resulting in a sharp decrease in electromagnetic shielding performance. Therefore, studying how to weaken the inter-chain interaction of rubber macromolecules and improve the processing performance and salt spray corrosion resistance of electromagnetic shielding rubber materials have become two major issues that the industry needs to solve. Summary of the invention
[0005] In view of the deficiencies in the above-mentioned background technology, the present invention provides an electromagnetic shielding rubber material that is easy to process and resistant to salt spray, and a preparation method and application thereof. The present invention can weaken the interaction force between the internal chain segments of the polymer through internal lubricants such as oleamide, erucic acid amide, and stearic acid amide, making it easy for the molecular chains to slide, improving the mobility of the molecular chains, and thus improving the fluidity; and due to its own small molecular characteristics, it is easy to precipitate a waxy film on the surface to isolate external moisture. Therefore, the use of internal lubricants such as oleamide to modify electromagnetic shielding rubber makes it easy to process and resistant to salt spray, which is of great significance to improving its electromagnetic protection capability and optimizing the production process.
[0006] To achieve the above objectives, the first objective of the present invention is to provide an electromagnetic shielding rubber material that is easy to process and resistant to salt spray, comprising the following components by weight: 100 parts of silicone rubber kneaded glue or fluorosilicone rubber kneaded glue, 1-5 parts of structural control agent, 200-500 parts of conductive metal powder, 5-20 parts of conductive reinforcing agent, 4-10 parts of internal lubricant, 3-8 parts of composite coupling agent, 1-4 parts of vulcanizing agent, 1-2 parts of auxiliary cross-linking agent; Wherein, the internal lubricant is one or more of oleamide, erucamide, stearamide, ethylene bisstearamide, and glycerol fatty acid ester.
[0007] Preferably, the structuring control agent is one or more of methoxy silicone oil, dimethyldiethoxy silicone oil, hydroxy silicone oil, and fluorohydroxy silicone oil.
[0008] Preferably, the conductive metal powder is one or more of silver-coated aluminum powder, silver-coated nickel powder, and silver-coated glass microbeads, with a particle size of 10 to 60 μm and a spherical particle shape.
[0009] Preferably, the conductive reinforcing agent is silver powder with a particle size of 1-20 μm.
[0010] Preferably, the composite coupling agent is a mixture of a silane coupling agent and a titanate coupling agent; The mass ratio of the silane coupling agent to the titanate coupling agent is 1:1-2; Wherein, the silane coupling agent is one or more of KH-550, KH-560, and KH-792; The titanate coupling agent is one or more of NDZ-105, NDZ-102, and NDZ-201.
[0011] Preferably, the curing agent is one of bis(2,4-dimethylformamide), bis(2,5-dimethylformamide), DCP, and platinum vulcanizing agent; The auxiliary cross-linking agent is one of triallyl isocyanurate, triallyl cyanurate, and N,N′-p-phenylbismaleimide.
[0012] The second object of the present invention is to provide a method for preparing an electromagnetic shielding rubber material that is easy to process and resistant to salt spray, comprising the following steps: Set the mixer speed to 40~60rpm / min; Add rubber, structural control agent, conductive metal powder, conductive reinforcing agent, composite coupling agent and internal lubricant to the internal mixer in sequence, mix for 10-20 minutes, and control the temperature of the mixing chamber to be ≤100°C; take out the rubber material and place it aside to cool to room temperature, then put it into the internal mixer, add vulcanizing agent and auxiliary cross-linking agent, continue mixing for 5-10 minutes, control the temperature of the mixing chamber to be ≤60°C, and let it stand at room temperature for 2-4 hours after mixing to obtain the rubber material; The rubber compound is subjected to a first stage of compression vulcanization molding to obtain a vulcanized rubber compound; the vulcanized rubber compound is then subjected to a second stage of hot air vulcanization to obtain an electromagnetic shielding rubber material.
[0013] Preferably, in the one-stage compression vulcanization molding process, the vulcanization temperature is 160-180° C., the vulcanization time is 10-40 min, and the vulcanization pressure is 10-20 MPa.
[0014] Preferably, in the two-stage hot air vulcanization process, the vulcanization temperature is 180-200° C. and the vulcanization time is 1-4 hours.
[0015] The third object of the present invention is to provide a rubber material for use in electromagnetic shielding.
[0016] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides an electromagnetic shielding rubber material that is easy to process and resistant to salt spray, as well as a preparation method and application thereof. The present invention is based on the fact that internal lubricants such as oleamide, erucamide, and stearamide can penetrate into the rubber macromolecular chains, weaken the interaction force between the internal chain segments of the polymer, make the molecular chains easy to slide, and improve the mobility of the molecular chains, thereby improving fluidity; the titanate coupling agent has similar groups to the internal lubricant, and constructs a channel for the above-mentioned internal lubricant to precipitate to the rubber surface, and due to its own small molecule characteristics, the above-mentioned internal lubricant is easy to precipitate on the rubber surface to form a waxy film to isolate external moisture. Therefore, the use of internal lubricants such as oleamide to modify electromagnetic shielding rubber makes it both easy to process and resistant to salt spray, which is of great significance to improving its electromagnetic protection capability and optimizing the production process.
[0017] The rubber material provided by the present invention reduces the Mooney viscosity of the rubber material, improves the fluidity of the rubber material, weakens the intermolecular internal stress of the rubber macromolecule, can weaken the extrusion expansion effect when the rubber material is extruded, and optimizes the molding process. The present invention can achieve super-hydrophobicity of the rubber through the wax film precipitated on the surface, resist water from invading the rubber matrix, and improve the salt spray corrosion resistance of the electromagnetic shielding rubber. DETAILED DESCRIPTION
[0018] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments, but the embodiments are not intended to limit the present invention.
[0019] The first aspect of the present invention provides an electromagnetic shielding rubber material that is easy to process and resistant to salt spray, comprising the following components by weight: 100 parts of silicone rubber kneaded glue or fluorosilicone rubber kneaded glue, 1-5 parts of structural control agent, 200-500 parts of conductive metal powder, 5-20 parts of conductive reinforcing agent, 4-10 parts of internal lubricant, 3-8 parts of composite coupling agent, 1-4 parts of vulcanizing agent, 1-2 parts of auxiliary cross-linking agent; Wherein, the internal lubricant is one or more of oleamide, erucamide, stearamide, ethylene bisstearamide, and glycerol fatty acid ester.
[0020] The structuring control agent is one or more of methoxy silicone oil, dimethyldiethoxy silicone oil, hydroxy silicone oil, and fluorohydroxy silicone oil.
[0021] The conductive metal powder is one or more of silver-coated aluminum powder, silver-coated nickel powder, and silver-coated glass microbeads, with a particle size of 10 to 60 μm and a spherical particle shape.
[0022] The conductive reinforcing agent is silver powder with a particle size of 1-20 μm.
[0023] The composite coupling agent is a mixture of a silane coupling agent and a titanate coupling agent; The mass ratio of the silane coupling agent to the titanate coupling agent is 1:1-2; Wherein, the silane coupling agent is one or more of KH-550, KH-560, and KH-792; The titanate coupling agent is one or more of NDZ-105, NDZ-102, and NDZ-201.
[0024] The curing agent is one of bis(2,4-dimethyl-2,5-dimethyl- ... The auxiliary cross-linking agent is one of triallyl isocyanurate, triallyl cyanurate, and N,N′-p-phenylbismaleimide.
[0025] A second aspect of the present invention provides a method for preparing an electromagnetic shielding rubber material that is easy to process and resistant to salt spray, comprising the following steps: Set the mixer speed to 40~60rpm / min; Add rubber, structural control agent, conductive metal powder, conductive reinforcing agent, composite coupling agent and internal lubricant to the internal mixer in sequence, mix for 10-20 minutes, and control the temperature of the mixing chamber to be ≤100°C; take out the rubber material and place it aside to cool to room temperature, then put it into the internal mixer, add vulcanizing agent and auxiliary cross-linking agent, continue mixing for 5-10 minutes, control the temperature of the mixing chamber to be ≤60°C, and let it stand at room temperature for 2-4 hours after mixing to obtain the rubber material; The rubber compound is subjected to a first stage of compression vulcanization molding to obtain a vulcanized rubber compound; the vulcanized rubber compound is then subjected to a second stage of hot air vulcanization to obtain an electromagnetic shielding rubber material.
[0026] Among them, in the first stage of compression vulcanization molding process, the vulcanization temperature is 160~180℃, the vulcanization time is 10~40min, and the vulcanization pressure is 10~20MPa.
[0027] In the two-stage hot air vulcanization process, the vulcanization temperature is 180~200℃ and the vulcanization time is 1~4h.
[0028] In one embodiment, a method for preparing an electromagnetic shielding rubber material that is easy to process and resistant to salt spray comprises the following steps: S1. Weigh the required materials according to the formula.
[0029] S2. Set the mixer speed to 40~60rpm / min.
[0030] S3. Add rubber, structural control agent, conductive metal powder, conductive reinforcing agent, composite coupling agent and internal lubricant into the internal mixer in sequence, mix for 10-20 minutes, and control the temperature of the mixing chamber not to exceed 100°C.
[0031] S4. Take out the rubber material and let it stand to cool to room temperature.
[0032] S5. Put the rubber material back into the internal mixer, add vulcanizing agent and cross-linking agent, mix for 5-10 minutes, and control the temperature of the mixing chamber not to exceed 60℃.
[0033] S6. Leave the rubber at room temperature for 4 hours.
[0034] S7. The rubber compound is subjected to a high-temperature compression molding process, wherein the vulcanization temperature is 160-180°C, the vulcanization time is 10-40 minutes, and the vulcanization pressure is 10-20 MPa.
[0035] S8. Perform two-stage hot air vulcanization on the first-stage vulcanized rubber material. The vulcanization temperature is 180-200°C and the vulcanization time is 1-4 hours to obtain an electromagnetic shielding rubber material.
[0036] A third aspect of the present invention provides an application of a rubber material in electromagnetic shielding.
[0037] It should be noted that the experimental methods used in the present invention are all conventional methods unless otherwise specified; the reagents and materials used are all commercially available unless otherwise specified.
[0038] The following embodiment provides a method for preparing an electromagnetic shielding rubber material that is easy to process and resistant to salt spray, which is specifically as follows: According to the formula in Table 1, the materials were weighed according to the mass ratio, the speed of the internal mixer was set to 50 rpm / min, rubber, structural control agent, conductive metal powder, conductive reinforcing agent, composite coupling agent and internal lubricant were added to the internal mixer in sequence, the temperature of the mixing chamber was controlled to be 80°C, and after mixing for 15 minutes, the rubber was taken out and left to stand for 30 minutes until it reached room temperature, and then put back into the internal mixer and added with vulcanizing agent and auxiliary cross-linking agent, mixed for 10 minutes, and the temperature of the mixing chamber was controlled to be 60°C. After the rubber was left for 4 hours, it was vulcanized and formed according to the vulcanization conditions to obtain the embodiment.
[0039] The proportions of the components added in each embodiment and comparative example are shown in Table 1 below.
[0040] Table 1 Electromagnetic shielding rubber material formula (weight ratio) project Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Silicone rubber kneading glue 100 100 0 0 100 0 Fluorosilicone rubber kneading rubber 0 0 100 100 0 100 Hydroxy silicone oil 3 0 0 0 0 0 Fluorohydroxy silicone oil 0 0 2 3 0 3 Methoxy silicone oil 0 3 0 0 3 0 Silver coated aluminum powder 300 0 300 0 0 0 Silver coated glass beads 0 250 0 250 250 250 Silver powder 10 10 15 15 10 15 Oleamide 4 0 4 0 0 0 Erucamide 0 6 0 6 0 0 Silane coupling agent KH-550 2 0 2 0 0 0 Silane coupling agent KH-792 0 2 0 2 2 2 Titanate coupling agent NDZ-105 2 0 2 4 0 4 Titanate coupling agent NDZ-201 0 3 0 0 3 0 Curing agent DCP 2 0 2 0 0 0 Curing agent double 25 0 2 0 2 2 2 Crosslinking agent TAIC 2 0 2 0 0 0 Crosslinking agent PDM 0 1 0 1 1 1 First stage vulcanization temperature, ℃ 170 160 170 170 160 170 A vulcanization time, min 10 30 10 20 30 20 First stage vulcanization pressure, MPa 10 15 15 15 15 15 Second stage vulcanization temperature, ℃ 190 190 200 200 190 200 Second stage vulcanization time, h 2 2 1 2 2 2 The performance of Examples 1 to 4 and Comparative Examples 1-2 was tested.
[0041] Mooney viscosity is tested according to GB / T 1232.1-2000.
[0042] After the sample was left for 24 hours, the water contact angle was measured using a contact angle meter model SL1000.
[0043] The resistivity was tested using a four-probe resistance tester.
[0044] The electromagnetic shielding performance of the rubber compound is tested according to MIL-G-83528.
[0045] Table 2 Performance of Examples and Comparative Examples project Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Mooney viscosity, [100℃ (1+4)] 68 56 70 60 62 67 Rubber surface hydrophobicity Super hydrophobic Super hydrophobic Super hydrophobic Super hydrophobic Hydrophobic Hydrophobic Shielding effectiveness, 10MHz 72 65 74 70 67 72 Shielding Effectiveness, 10GHz 94 78 98 82 78 81 Shielding Effectiveness, 18GHz 115 88 115 105 90 95 Resistivity, Ω·cm 0.0040 0.0075 0.0042 0.0070 0.0052 0.0048 Resistivity after 400h of acid salt spray, Ω·cm 0.0062 0.0081 0.0065 0.0075 15.25 10.12 As can be seen from Table 2, compared with Comparative Examples 1-2, (1) due to the addition of internal lubricants, the interaction between the rubber macromolecular chains is weakened, the rubber fluidity is increased, and the Mooney viscosity of the rubber material is significantly reduced. (2) Due to the synergistic effect of the internal lubricant and the titanate coupling agent, the internal lubricant is quickly precipitated from the inside of the rubber to the rubber surface. After being parked for 24 hours, a waxy film is formed on the surface of the embodiment, which improves the hydrophobicity of the rubber. (3) The addition of the internal lubricant reduces the interaction between the molecular chains, reduces the friction between the rubber and the filler during the mixing process to a certain extent, and reduces the peeling of the silver shell of the core-shell material such as silver-coated aluminum powder or silver-coated glass microbeads. After 400 hours of acidic salt spray, the volume resistance of the embodiment sample does not change much, while the volume resistance of the comparative sample increases significantly. The presence of the internal lubricant improves the ability of the rubber to resist salt spray corrosion.
[0046] The above is only the best implementation mode of the present invention, but the protection scope of the patent of the present invention is not limited to this. All technicians familiar with this technical field can also make various corresponding changes and modifications to the present invention. Under the premise of not violating the principles of the invention, they should all fall within the protection scope of the claims attached to the present invention.
Claims
1. An electromagnetic shielding rubber material that is easy to process and resistant to salt spray. It is characterized in that The composition comprises the following components by weight: 100 parts of silicone rubber kneaded glue or fluorosilicone rubber kneaded glue, 1-5 parts of structural control agent, 200-500 parts of conductive metal powder, 5-20 parts of conductive reinforcing agent, 4-10 parts of internal lubricant, 3-8 parts of composite coupling agent, 1-4 parts of vulcanizing agent, 1-2 parts of auxiliary cross-linking agent; Wherein, the internal lubricant is one or more of oleamide, erucamide, stearamide, ethylene bisstearamide, and glycerol fatty acid ester.
2. The easily processable, salt-fog resistant electromagnetic shielding rubber material according to claim 1, It is characterized in that The structuring control agent is one or more of methoxy silicone oil, dimethyldiethoxy silicone oil, hydroxy silicone oil, and fluorohydroxy silicone oil.
3. The easily processable, salt-fog resistant electromagnetic shielding rubber material according to claim 1, It is characterized in that The conductive metal powder is one or more of silver-coated aluminum powder, silver-coated nickel powder, and silver-coated glass microbeads, with a particle size of 10 to 60 μm and a spherical particle shape.
4. The easily processable, salt-fog resistant electromagnetic shielding rubber material according to claim 1, It is characterized in that The conductive reinforcing agent is silver powder with a particle size of 1-20 μm.
5. The easily processable, salt-fog resistant electromagnetic shielding rubber material according to claim 1, It is characterized in that The composite coupling agent is a mixture of a silane coupling agent and a titanate coupling agent; The mass ratio of the silane coupling agent to the titanate coupling agent is 1:1-2; Wherein, the silane coupling agent is one or more of KH-550, KH-560, and KH-792; The titanate coupling agent is one or more of NDZ-105, NDZ-102, and NDZ-201.
6. The easily processable, salt-fog resistant electromagnetic shielding rubber material according to claim 1, It is characterized in that The curing agent is one of bis(2,4-dimethyl-2,5-dimethyl- ... The auxiliary cross-linking agent is one of triallyl isocyanurate, triallyl cyanurate, and N,N′-p-phenylbismaleimide.
7. A method for preparing the easy-to-process, salt-fog-resistant electromagnetic shielding rubber material according to any one of claims 1 to 6, It is characterized in that The following steps are involved: Set the mixer speed to 40~60rpm / min; Add rubber, structural control agent, conductive metal powder, conductive reinforcing agent, composite coupling agent and internal lubricant to the internal mixer in sequence, mix for 10-20 minutes, and control the temperature of the mixing chamber to be ≤100°C; take out the rubber material and place it aside to cool to room temperature, then put it into the internal mixer, add vulcanizing agent and auxiliary cross-linking agent, continue mixing for 5-10 minutes, control the temperature of the mixing chamber to be ≤60°C, and let it stand at room temperature for 2-4 hours after mixing to obtain the rubber material; The rubber compound is subjected to a first stage of compression vulcanization molding to obtain a vulcanized rubber compound; the vulcanized rubber compound is then subjected to a second stage of hot air vulcanization to obtain an electromagnetic shielding rubber material.
8. The method for preparing the easily processable and salt-fog resistant electromagnetic shielding rubber material according to claim 7, It is characterized in that In the first stage compression vulcanization molding process, the vulcanization temperature is 160~180℃, the vulcanization time is 10~40min, and the vulcanization pressure is 10~20MPa.
9. The method for preparing the easily processable and salt-fog resistant electromagnetic shielding rubber material according to claim 7, It is characterized in that In the two-stage hot air vulcanization process, the vulcanization temperature is 180~200℃ and the vulcanization time is 1~4h.
10. Use of the rubber material according to any one of claims 1 to 6 in electromagnetic shielding.
Citation Information
Patent Citations
Preparation method for halogen-free flame-retardant rubber composite
CN102617936A
Sealing element for electromagnetic shielding and preparation method thereof
CN115466513A
Silicone rubber composite material with low vacuum mass loss and high electromagnetic shielding effectiveness as well as preparation method and application of silicone rubber composite material
CN117089209A
Conductive resin composition and shield cable
JP2016020463A