Composite slurry as well as preparation method and application thereof
By modifying and reducing the graphene, combining inorganic nanomaterials and epoxy resins, a composite slurry is formed, which solves the problem of poor dispersion of graphene in the coating and significantly improves the corrosion resistance and stability.
Patent Information
- Application Number
- CN202310591798.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
AI Technical Summary
Graphene is prone to agglomeration in the coating system, resulting in poor dispersion and reducing the anti-corrosion effect.
Using graphene oxide, coupling agent, inorganic nanomaterial and epoxy resin, the combination of graphene is improved through modification and reduction treatment, and the lipophilicity and compatibility of graphene are formed to form a composite slurry and enhance its in epoxy resin. Stability and dispersion.
It significantly improves the uniform dispersion and conductivity of graphene in the coating, enhances the anticorrosion performance of the coating, extends the stability of graphene, and avoids agglomeration.
Smart Images

Figure CN119019907A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of anti-corrosion slurries, and in particular to a composite slurry, a method for preparing the composite slurry, and applications containing the composite slurry. Background Art
[0002] Graphene is currently widely used in the coating field because it can improve the anti-corrosion performance of coatings. However, the van der Waals force between graphene sheets makes it easy for graphene to aggregate in the coating system. The aggregated graphene is difficult to exert its excellent performance, thereby reducing the anti-corrosion effect of the coating.
[0003] At present, graphene, epoxy resin and solvent are usually configured to form a slurry, which is then mixed with a base coating to prepare an anti-corrosion coating. In the slurry, due to the poor wettability of graphene itself, it is difficult to disperse in the oily slurry. The existing technology often uses dispersants, modifications and other means to improve the dispersibility of graphene in oily slurries, but in actual use, the graphene slurry needs to be stored at room temperature for more than one year, or stored at 70°C for more than one month. Long-term static storage will still cause graphene to agglomerate, thereby reducing or losing the performance of the slurry.
[0004] The dispersibility of graphene in the slurry still needs to be improved. Summary of the invention
[0005] In view of this, the present application provides a composite slurry and a preparation method and application thereof, aiming to improve the problems of poor dispersion and easy agglomeration of graphene in existing slurries.
[0006] The embodiment of the present application is implemented as follows: a method for preparing a composite slurry comprises the following steps:
[0007] Providing graphene oxide, a coupling agent and a first solvent, mixing and stirring to obtain a dispersion, heating the dispersion to a first temperature, and keeping the temperature for a first time to obtain modified graphene oxide;
[0008] Providing an inorganic nanomaterial and a second solvent, mixing them with the modified graphene oxide, heating them to a second temperature, and keeping the temperature for a second time to obtain oleophilic graphene oxide;
[0009] An epoxy resin and a third solvent are provided, mixed with the oleophilic graphene oxide, heated to a third temperature, and a reducing agent is added to react to obtain a composite slurry.
[0010] Optionally, in some embodiments of the present application, the coupling agent includes one or more of aromatic diisocyanate, toluene diisocyanate, isocyanatepropyltriethoxysilane, polydimethylsiloxane, and 3-aminopropyltriethoxysilane; and / or
[0011] The inorganic nanomaterial includes one or more of titanium dioxide, silicon dioxide, silicon carbide, aluminum oxide, zirconium oxide, and zinc oxide; and / or
[0012] The epoxy resin includes one or more of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, aliphatic epoxy resin, and alicyclic epoxy resin; and / or
[0013] The reducing agent comprises sodium citrate; and / or
[0014] The first solvent includes one or more of toluene, N,N-dimethylformamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, pyridine, tetrahydrofuran, ethylene glycol, acetone, methanol, ethanol, 1-propanol, dichloromethane, o-xylene, and n-hexane; and / or
[0015] The second solvent includes one or more of ethanol, toluene, N,N-dimethylformamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, pyridine, tetrahydrofuran, ethylene glycol, acetone, methanol, 1-propanol, dichloromethane, o-xylene, and n-hexane; and / or
[0016] The third solvent includes one or more of n-butanol and xylene.
[0017] Optionally, in some embodiments of the present application, the mass ratio of the graphene oxide to the coupling agent is 0.2:(1-1.6); and / or
[0018] The mass ratio of the inorganic nanomaterial to the modified graphene oxide is (2.1-4.5):10; and / or
[0019] The mass ratio of the epoxy resin to the oleophilic graphene oxide is (4-8):1; and / or
[0020] The mass ratio of the reducing agent to the oleophilic graphene oxide is (24-40):1; and / or
[0021] The mass ratio of the epoxy resin to the third solvent is (34-64):(8-33).
[0022] Optionally, in some embodiments of the present application, the mixing and stirring time is 15 to 20 minutes;
[0023] The first temperature is 95-115° C.; and / or
[0024] The first time is 2.5 to 3.5 hours; and / or
[0025] The second temperature is 55-75° C.; and / or
[0026] The second time is 1.5 to 2.5 hours; and / or
[0027] The third temperature is 80-100°C.
[0028] Optionally, in some embodiments of the present application, after obtaining the dispersion, the step further includes subjecting the dispersion to a first ultrasonic treatment; and / or
[0029] After the epoxy resin, the third solvent and the oleophilic graphene oxide are mixed, before the heating to the third temperature, a second ultrasonic treatment is further performed; and / or
[0030] After the reducing agent is added, the method further comprises performing a third ultrasonic treatment.
[0031] Optionally, in some embodiments of the present application, the frequency of the first ultrasonic treatment is 10 to 20 kHz; and / or
[0032] The first ultrasonic treatment lasts for 30 to 40 minutes; and / or
[0033] The frequency of the second ultrasonic treatment is 10 to 20 kHz; and / or
[0034] The second ultrasonic treatment time is 1.5 to 2 hours; and / or
[0035] The frequency of the third ultrasonic treatment is 25 to 35 kHz; and / or
[0036] The third ultrasonic treatment lasts for 15 to 17 hours.
[0037] Optionally, in some embodiments of the present application, the adding of the reducing agent reaction further comprises adding a dispersant; and / or
[0038] After the reducing agent is added for reaction, an anti-settling agent is also added.
[0039] Optionally, in some embodiments of the present application, the dispersant includes one or more of polyisobutylene succinate, polyisobutylene thiophosphate, sodium polytetramethylene phenyl sulfonate, sodium polytetramethylene naphthalene sulfonate, sodium polytetramethylene anthracene sulfonate, sodium 4-styrene sulfonate, and sodium cholate; and / or
[0040] In the composite slurry, the concentration of the dispersant is 0.01wt% to 15wt%; and / or
[0041] The anti-settling agent includes one or more of polyethylene wax, bentonite, and polyamide wax; and / or
[0042] In the composite slurry, the concentration of the anti-settling agent is 2wt% to 6wt%.
[0043] Correspondingly, an embodiment of the present application also provides a composite slurry, which is prepared by the above-mentioned preparation method.
[0044] Correspondingly, an embodiment of the present application also provides an anti-corrosion coating, the material of the anti-corrosion coating includes the composite slurry prepared by the above-mentioned preparation method, or the above-mentioned composite slurry.
[0045] Correspondingly, an embodiment of the present application also provides an anti-corrosion coating, the material of the anti-corrosion coating includes the above-mentioned anti-corrosion coating.
[0046] The preparation method of the composite slurry described in the present application can improve the compatibility of graphene oxide and epoxy resin by modifying graphene oxide with a coupling agent, improving the lipophilicity of graphene oxide with inorganic nanomaterials, and realizing the reduction of graphene oxide with a reducing agent, and at the same time establishing an oxygen bridge between unreduced graphene oxide and epoxy resin, and reinforcing the stability of graphene oxide in the epoxy resin system through the newly formed oxygen bridge, controlling the degree of separation of oxygen-containing functional groups on graphene oxide, making the reduced graphene oxide have better solubility and better conductivity in epoxy resin, and improving the uniform dispersion of graphene oxide in epoxy resin slurry. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.
[0048] Figure 1 This is a flow chart of a method for preparing a composite slurry provided in an embodiment of the present application. DETAILED DESCRIPTION
[0049] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.
[0050] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.
[0051] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.
[0052] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0053] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0054] The technical solution of this application is as follows:
[0055] First, as Figure 1 As shown, the present application embodiment provides a method for preparing a composite slurry, comprising the following steps:
[0056] S11, providing graphene oxide, a coupling agent and a first solvent, mixing and stirring to obtain a dispersion, heating the dispersion to a first temperature, and keeping the temperature for a first time to obtain modified graphene oxide;
[0057] S12, providing an inorganic nanomaterial and a second solvent, mixing them with the modified graphene oxide, heating them to a second temperature, and keeping them warm for a second time to obtain oleophilic graphene oxide;
[0058] S13, providing epoxy resin and a third solvent, mixing with the oleophilic graphene oxide, heating to a third temperature, adding a reducing agent, reacting, and obtaining a composite slurry.
[0059] The preparation method of the composite slurry described in the present application can improve the compatibility of graphene oxide and epoxy resin by modifying graphene oxide by coupling agent, improving the lipophilicity of graphene oxide by inorganic nanomaterials, and realizing the reduction of graphene oxide by reducing agent, and at the same time establishing oxygen bridges between unreduced graphene oxide and epoxy resin, and reinforcing the stability of graphene oxide in epoxy resin system through the newly formed oxygen bridges, controlling the degree of separation of oxygen-containing functional groups on graphene oxide, achieving the best balance ratio between solubility and conductivity of reduced graphene oxide in epoxy resin, and improving the uniform dispersion of graphene oxide in epoxy resin slurry.
[0060] In the step S11:
[0061] When the graphene oxide, the coupling agent and the first solvent are heated to react, it can be understood that the graphene oxide has oxygen-containing functional groups such as hydroxyl -OH and carboxyl -COOH, and the oxygen-containing functional groups react with the coupling agent, and the coupling agent modifies the graphene oxide to prepare modified graphene oxide.
[0062] In some embodiments, the coupling agent includes one or more of aromatic diisocyanate, toluene diisocyanate, isocyanatepropyltriethoxysilane, polydimethylsiloxane, and 3-aminopropyltriethoxysilane.
[0063] In some embodiments, the mass ratio of the graphene oxide to the coupling agent is 0.2:(1-1.6), for example, 0.2:1.1, 0.2:1.2, 0.2:1.3, 0.2:1.4, 0.2:1.5, etc. The graphene oxide has oxygen-containing functional groups, namely hydroxyl and carboxyl groups. Within the range of the mass ratio, the hydroxyl and carboxyl groups can fully react with the coupling agent to form modified graphene oxide.
[0064] In some embodiments, the first solvent includes one or more of toluene, N,N-dimethylformamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, pyridine, tetrahydrofuran, ethylene glycol, acetone, methanol, ethanol, 1-propanol, dichloromethane, o-xylene, and n-hexane.
[0065] In some embodiments, the stirring time is 15 to 20 minutes, for example, 15.5 to 19.5 minutes, 16 to 19 minutes, 16.5 to 18.5 minutes, 17 to 18 minutes, 17.5 to 17.8 minutes, etc. Within the stirring time range, the graphene oxide and the coupling agent are conducive to a full reaction.
[0066] In some embodiments, after obtaining the dispersion, the method further includes subjecting the dispersion to a first ultrasonic treatment.
[0067] In some embodiments, the frequency of the first ultrasonic treatment is 10-20 kHz, for example, 11-19 kHz, 12-18 kHz, 13-17 kHz, 14-16 kHz, etc. Within the frequency range of the first ultrasonic treatment, the modification of the graphene oxide is promoted.
[0068] In some embodiments, the first ultrasonic treatment time is 30 to 40 minutes, for example, 31 to 39 minutes, 32 to 38 minutes, 33 to 37 minutes, 34 to 36 minutes, 35 to 35.5 minutes, etc. Within the time range of the first ultrasonic treatment, the graphene oxide is facilitated to be fully modified.
[0069] In some embodiments, the first temperature is 95-115° C. Within the first temperature range, the graphene oxide and the coupling agent are conducive to fully reacting.
[0070] In some embodiments, the first time is 2.5 to 3.5 hours. Within the first time range, the graphene oxide and the coupling agent can fully react.
[0071] In some embodiments, after the first insulation time, the first solvent is removed to obtain modified graphene oxide.
[0072] In step S12:
[0073] When the inorganic nanomaterial, the second solvent and the modified graphene oxide are heated to react, one end of the coupling agent is connected to the oxygen-containing functional group of the graphene oxide, and the other end is connected to the inorganic nanomaterial, forming a bridge bond between the graphene oxide and the inorganic nanomaterial. This bridging structure is relatively stable, so that the graphene oxide is modified into oleophilic graphene oxide.
[0074] In some embodiments, the inorganic nanomaterial includes one or more of titanium dioxide, silicon dioxide, silicon carbide, aluminum oxide, zirconium oxide, and zinc oxide. It is understood that the inorganic nanomaterial can improve the lipophilicity of the modified graphene oxide and play an electrochemical anti-corrosion role.
[0075] In some embodiments, the mass ratio of the inorganic nanomaterial to the modified graphene oxide is (2.1-4.5):10, for example, (2.2-4.4):10, (2.4-4.2):10, (2.6-4):10, (2.8-3.5):10, (2.5-3):10, etc. Within the mass concentration range, the inorganic nanomaterial can effectively improve the lipophilicity of the modified graphene oxide.
[0076] In some embodiments, the second solvent includes one or more of ethanol, toluene, N,N-dimethylformamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, pyridine, tetrahydrofuran, ethylene glycol, acetone, methanol, 1-propanol, dichloromethane, o-xylene, and n-hexane.
[0077] It should be noted that there is no restriction on the mass ratio of the modified graphene oxide to the second solvent, as long as the modified graphene oxide is fully dispersed and dissolved in the second solvent.
[0078] In some embodiments, the second temperature is 55-75°C, for example, 58-73°C, 59-72°C, 60-70°C, 62-68°C, 63-65°C, etc.
[0079] In some embodiments, the second time is 1.5 to 2.5 hours, for example, 1.6 to 2.4 hours, 1.7 to 2.3 hours, 1.8 to 2.2 hours, 1.9 to 2.1 hours, etc.
[0080] Thus, under the conditions of the second temperature and the second time, the coupling agent can serve as a bridge bond to connect the graphene oxide and the inorganic nanomaterial, thereby improving the lipophilicity of the graphene oxide.
[0081] In some embodiments, after the first insulation time, the second solvent is removed to obtain oleophilic graphene oxide.
[0082] In step S13:
[0083] When the epoxy resin and the third solvent, the oleophilic graphene oxide and the reducing agent react, the oxygen-containing functional groups of the graphene oxide are separated from the graphene oxide, and at the same time, the coupling agent is separated from the oxygen-containing functional groups of the graphene oxide. The reducing agent forms a new oxygen bridge between the unreduced graphene oxide and the epoxy resin, thereby reinforcing the stability of the graphene oxide in the epoxy resin system and controlling the degree of separation of the oxygen-containing functional groups of the graphene oxide, so that the graphene oxide has better solubility and better conductivity in the epoxy resin.
[0084] In some embodiments, the epoxy resin includes one or more of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, aliphatic epoxy resin, and alicyclic epoxy resin.
[0085] In some embodiments, the mass ratio of the epoxy resin to the oleophilic graphene oxide is (4-8):1, for example, (4.5-7.5):1, (4.8-7.2):1, (5-7):1, (5.5-6.5):1, (5.8-6):1, etc. Within the mass ratio range, the epoxy resin and the oleophilic graphene oxide can be fully contacted and mixed.
[0086] In some embodiments, the third solvent includes one or more of n-butanol and xylene.
[0087] In some embodiments, the mass ratio of the epoxy resin to the third solvent is (34-64): (8-33), for example, (34-64): (10-30), (34-64): (12-28), (34-64): (14-26), (34-64): (16-24), (34-64): (18-20), etc. Within the mass concentration range, the epoxy resin can be fully dissolved.
[0088] In some embodiments, after the epoxy resin, the third solvent and the oleophilic graphene oxide are mixed, before the heating to the third temperature, a second ultrasonic treatment is further performed.
[0089] In some embodiments, the frequency of the second ultrasonic treatment is 10-20 kHz, for example, 11-19 kHz, 12-18 kHz, 13-17 kHz, 14-16 kHz, 15-15.5 kHz, etc. Within the frequency range of the second ultrasonic treatment, the epoxy resin and the oleophilic graphene oxide are mixed.
[0090] In some embodiments, the second ultrasonic treatment time is 1.5 to 2 hours, for example, 1.52 to 1.98 hours, 1.55 to 1.95 hours, 1.52 to 1.92 hours, 1.6 to 1.9 hours, 1.7 to 1.8 hours, etc. Within the time range of the second ultrasonic treatment, the epoxy resin and the oleophilic graphene oxide are mixed.
[0091] In some embodiments, the third temperature is 80-100° C. Within the third temperature range, the graphene oxide and the coupling agent can react fully.
[0092] In some embodiments, the reducing agent includes sodium citrate. In some embodiments, vitamin C can also be added to act as a reducing agent together with sodium citrate.
[0093] In some embodiments, the mass ratio of the reducing agent to the oleophilic graphene oxide is (24-40):1, for example, (25-38):1, (26-37):1, (27-36):1, (28-35):1, (30-32):1, etc. Within the mass ratio range, the reducing agent can cause the oxygen-containing functional groups of the oleophilic graphene oxide to fall off, reducing the oleophilic graphene oxide, while the coupling agent is separated from the oxygen-containing functional groups of the graphene oxide, and the reducing agent forms a new oxygen bridge between the unreduced graphene oxide and the epoxy resin, effectively preventing the graphene oxide from agglomerating after the oxygen-containing functional groups are removed.
[0094] In some embodiments, after adding the reducing agent, a third ultrasonic treatment is further performed.
[0095] In some embodiments, the frequency of the third ultrasonic treatment is 25-35 kHz, for example, 26-34 kHz, 27-33 kHz, 28-32 kHz, 29-31 kHz, 30-30.5 kHz, etc. Within the frequency range of the third ultrasonic treatment, the reducing agent is conducive to the reduction of the oleophilic graphene oxide.
[0096] In some embodiments, the third ultrasonic treatment lasts for 15 to 17 hours, for example, 15.2 to 16.8 hours, 15.5 to 16.5 hours, 15.8 to 16.2 hours, etc. Within the time range of the third ultrasonic treatment, the reducing agent is conducive to the reduction of the oleophilic graphene oxide.
[0097] In some embodiments, the step of adding the reducing agent to react further includes washing.
[0098] In some embodiments, the cleaning comprises an acid wash.
[0099] In some embodiments, the acid used in the pickling includes one or more of hydrochloric acid, sulfuric acid, and phosphoric acid.
[0100] In some embodiments, the mass fraction of the acid is 1% to 3%, for example, 2%.
[0101] In some embodiments, the cleaning further comprises water washing. It is understood that the water washing can remove the coupling agent, and the remaining trace coupling agent has a beneficial effect of dispersing and bonding the slurry, that is, preventing the graphene oxide in the slurry from agglomerating after reduction, and also enhancing the adhesion of the slurry to the surface of the object to be coated during actual use.
[0102] In some embodiments, the cleaning further includes drying, through which moisture generated during the reduction process of the reducing agent can be removed.
[0103] In some embodiments, the step of adding a dispersant further comprises adding a reducing agent after the reaction.
[0104] In some embodiments, the dispersant includes one or more of polyisobutylene succinate, polyisobutylene thiophosphate, polytetramethylene phenyl sodium sulfonate, polytetramethylene naphthalene sodium sulfonate, polytetramethylene anthracene sodium sulfonate, sodium 4-styrene sulfonate, and sodium cholate. The polyisobutylene succinate can increase the fluidity of the slurry and prevent the graphene oxide from agglomerating.
[0105] In some embodiments, in the composite slurry, the concentration of the dispersant is 0.01wt% to 15wt%, for example, 0.05wt% to 14wt%, 0.1wt% to 13wt%, 1wt% to 12wt%, 2wt% to 10wt%, 5wt% to 8wt%, etc. Within the concentration range, the dispersant can further improve the dispersion stability of graphene oxide in the slurry.
[0106] In some embodiments, the concentration of the polyisobutenyl succinate is 1 wt % to 1.5 wt %.
[0107] In some embodiments, the concentration of the polyisobutylene thiophosphate is 1 wt % to 1.5 wt %.
[0108] In some embodiments, the concentration of the polymeric sodium tetramethylene phenyl sulfonate is 4 wt % to 9 wt %.
[0109] In some embodiments, the concentration of the sodium polytetramethylene naphthalene sulfonate is 4 wt % to 9 wt %.
[0110] In some embodiments, the concentration of the sodium polytetramethylene anthracene sulfonate is 4 wt % to 9 wt %.
[0111] In some embodiments, the concentration of sodium 4-styrenesulfonate is 4.3 wt % to 7.8 wt %.
[0112] In some embodiments, the concentration of sodium cholate is 0.01 wt % to 0.08 wt %.
[0113] In some embodiments, the step of adding an anti-settling agent further comprises adding an anti-settling agent after adding the reducing agent.
[0114] In some embodiments, the anti-settling agent includes one or more of polyethylene wax, bentonite, and polyamide wax.
[0115] In some embodiments, in the composite slurry, the concentration of the anti-settling agent is 2 wt % to 6 wt %.
[0116] In some embodiments, the concentration of the polyethylene wax is 2 wt % to 6 wt %.
[0117] In some embodiments, the concentration of the polyethylene wax is 2 wt % to 4 wt %.
[0118] In a second aspect, an embodiment of the present application further provides a composite slurry prepared by the above-mentioned preparation method.
[0119] The composite slurry described in the present application, the graphene oxide in the composite slurry has been modified by a coupling agent, improved by inorganic nanomaterials and reduced by a reducing agent, so that the solubility and conductivity of the graphene oxide in the composite slurry reach an optimal balance ratio, thereby improving the uniform dispersion of the graphene oxide in the composite slurry.
[0120] In a third aspect, an embodiment of the present application further provides an anti-corrosion coating, which includes the composite slurry prepared by the above-mentioned preparation method.
[0121] In a fourth aspect, an embodiment of the present application also provides an anti-corrosion coating, the material of the anti-corrosion coating includes the above-mentioned anti-corrosion coating.
[0122] The anti-corrosion coating described in the present application uses an anti-corrosion coating including the above-mentioned composite slurry, which can significantly improve the corrosion resistance of the device equipment.
[0123] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and are not limitations of the present application.
[0124] Example 1
[0125] This embodiment provides a composite slurry, and the preparation method thereof is as follows:
[0126] 0.2 g of graphene oxide was dispersed in N,N-dimethylformamide, 1.3 g of aromatic diisocyanate coupling agent was added, stirred for 15 min, ultrasonically treated for 30 min, and then stirred at a constant temperature of 105 ° C for 3 h. After removing N,N-dimethylformamide, modified graphene oxide was obtained;
[0127] Weigh 1 g of modified graphene oxide, disperse it in an ethanol solution, add 0.21 g of titanium dioxide, stir at a constant temperature of 65°C for 2 h, remove the ethanol solvent, and obtain oleophilic graphene oxide;
[0128] Weigh 64 g of epoxy resin and dissolve it in 8 g of n-butanol and 10 g of xylene to obtain an epoxy resin solution, weigh 18 g of oleophilic graphene oxide, slowly add it to the epoxy resin solution, ultrasonically stir at a frequency of 10 kHz for 1.5 h, and after fully mixing, heat to 90 ° C, add 648 g of sodium citrate, increase the ultrasonic frequency to 25 kHz, react for 15 h, slowly cool to room temperature, then use dilute hydrochloric acid to pickle, water wash, dry, and then add 1 wt% of polyisobutylene succinate and 1.5 wt% of polyisobutylene thiophosphate, 2 wt% of polyethylene wax and 2 wt% of bentonite under stirring to obtain a composite slurry.
[0129] Example 2
[0130] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the aromatic diisocyanate coupling agent is replaced by a toluene diisocyanate coupling agent.
[0131] Example 3
[0132] This embodiment is basically the same as Embodiment 1, except that in this embodiment, titanium dioxide is replaced by aluminum oxide.
[0133] Example 4
[0134] This embodiment is substantially the same as Embodiment 3, except that sodium citrate is replaced with vitamin C in this embodiment.
[0135] Example 5
[0136] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the mass of graphene oxide is 0.2 g, and the mass of aromatic diisocyanate coupling agent is 1 g.
[0137] Example 6
[0138] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the mass of graphene oxide is 0.2 g, and the mass of aromatic diisocyanate coupling agent is 1.6 g.
[0139] Example 7
[0140] This embodiment is substantially the same as Embodiment 1, except that the mass of titanium dioxide in this embodiment is 0.3 g.
[0141] Example 8
[0142] This embodiment is substantially the same as Embodiment 1, except that the mass of titanium dioxide in this embodiment is 0.45 g.
[0143] Example 9
[0144] This embodiment is substantially the same as Embodiment 1, except that the mass of the oleophilic graphene oxide in this embodiment is 10 g.
[0145] Example 10
[0146] This embodiment is substantially the same as Embodiment 1, except that the mass of the oleophilic graphene oxide in this embodiment is 8 g.
[0147] Embodiment 11
[0148] This embodiment is substantially the same as Embodiment 1, except that the mass of sodium citrate in this embodiment is 432 g.
[0149] Example 12
[0150] This embodiment is substantially the same as Embodiment 1, except that the mass of sodium citrate in this embodiment is 720 g.
[0151] Embodiment 13
[0152] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the temperature for the reaction of graphene oxide and aromatic diisocyanate coupling agent is 95°C.
[0153] Embodiment 14
[0154] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the temperature for the reaction of graphene oxide and aromatic diisocyanate coupling agent is 115°C.
[0155] Embodiment 15
[0156] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the temperature for the reaction of modified graphene oxide and epoxy resin is 55°C.
[0157] Example 16
[0158] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the temperature for the reaction of modified graphene oxide and epoxy resin is 75°C.
[0159] Embodiment 17
[0160] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the temperature for the reaction of oleophilic graphene oxide and sodium citrate is 80°C.
[0161] Embodiment 18
[0162] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, the temperature for the reaction of oleophilic graphene oxide and sodium citrate is 100°C.
[0163] Embodiment 19
[0164] This embodiment is substantially the same as Embodiment 1, except that, in this embodiment, 1 wt % of polyisobutylene succinate and 1.5 wt % of polyisobutylene thiophosphate are replaced by 4 wt % of sodium polytetramethylene phenyl sulfonate and 9 wt % of sodium polytetramethylene anthracene sulfonate.
[0165] Embodiment 20
[0166] This embodiment is basically the same as Embodiment 4, except that in this embodiment, the polyethylene wax is replaced by polyamide wax.
[0167] Comparative Example 1
[0168] This comparative example is basically the same as Example 1, except that the graphene oxide in the composite slurry in this comparative example is not modified by a coupling agent, an inorganic nanomaterial, and a reducing agent.
[0169] Comparative Example 2
[0170] This comparative example is basically the same as Example 1, except that the graphene oxide in the composite slurry in this comparative example is only modified by a coupling agent, i.e., modified graphene oxide, and is not modified by an inorganic nanomaterial and a reducing agent.
[0171] The particle size tester was used to test the particle size of the composite slurries of Examples 1 to 20 and Comparative Examples 1 to 2, and the average particle size of the substances in the composite slurries was shown in Table 1.
[0172] Table 1
[0173]
[0174]
[0175] It can be seen from Table 1 that the average particle size in the composite slurries of Examples 1 to 20 is significantly lower than the average particle size of the composite slurries of Comparative Examples 1 to 2. This is because the graphene in Comparative Examples 1 to 2 is agglomerated, resulting in an increase in particle size, while the graphene in the composite slurry prepared by this scheme has good dispersion, uniform distribution, and small particle size. This is conducive to exerting the excellent properties of graphene and improving the anti-corrosion performance of the composite slurry.
[0176] Device Examples 1 to 20
[0177] Device Examples 1 to 20 provide a device, provide a zinc substrate, and spray the anti-corrosion coating prepared by the composite slurry of Examples 1 to 19 on the surface of the device to form an anti-corrosion coating.
[0178] Device Comparison Examples 1 to 2
[0179] Device Comparative Examples 1 to 2 are substantially the same as Device Examples 1 to 20, except that the anti-corrosion coating prepared by the composite slurry of Comparative Examples 1 to 2 is sprayed on the surface of the zinc substrate to form an anti-corrosion coating.
[0180] The impact strength tester was used to test the anti-corrosion coatings in device embodiments 1 to 20 and device comparative examples 1 to 2. The salt spray resistance of the anti-corrosion coatings was measured in an artificially simulated salt spray environment, wherein the conditions of the artificially simulated salt spray environment were: 5% sodium chloride saline solution, pH value 6 to 7, sprayed as a spray, the test temperature was 35°C, and the sedimentation rate of the salt spray was 1 to 3 ml / 80 cm 2 The impact strength and salt spray resistance of the anti-corrosion coating are shown in Table 2.
[0181] Table 2
[0182]
[0183]
[0184] It can be seen from Table 2 that the composite slurry prepared by the present scheme is applied to the coating, which can effectively improve the impact resistance and salt spray resistance of the coating; the impact resistance reflects the ability of the anti-corrosion coating to deform rapidly under high-speed gravity without cracking or falling off from the metal substrate. Compared with the anti-corrosion coating of device comparison examples 1 to 2, the impact resistance of the anti-corrosion coating of device embodiments 1 to 20 is significantly improved, indicating that the anti-corrosion coating provided by the present scheme has good flexibility, strong adhesion to the substrate, is not easy to fall off, and has a better anti-corrosion effect; the salt spray resistance can characterize the anti-corrosion effect of the anti-corrosion coating on the metal substrate. Compared with the anti-corrosion coating of device comparison examples 1 to 2, the salt spray resistance of the anti-corrosion coating of device embodiments 1 to 20 is extended, indicating that the anti-corrosion coating provided by the present scheme has an effective anti-corrosion effect on the metal substrate. This is because the graphene in the composite slurry is evenly dispersed and adheres to the metal substrate, thereby avoiding the corrosion of the metal by the salt spray environment.
[0185] The composite slurry provided in the embodiments of the present application and its preparation method and application are introduced in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for technical personnel in this field, according to the idea of the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A method for preparing a composite slurry, characterized in that: The steps include: Providing graphene oxide, a coupling agent and a first solvent, mixing and stirring to obtain a dispersion, heating the dispersion to a first temperature, and keeping the temperature for a first time to obtain modified graphene oxide; Providing an inorganic nanomaterial and a second solvent, mixing them with the modified graphene oxide, heating them to a second temperature, and keeping the temperature for a second time to obtain oleophilic graphene oxide; An epoxy resin and a third solvent are provided, mixed with the oleophilic graphene oxide, heated to a third temperature, and a reducing agent is added to react to obtain a composite slurry.
2. The preparation method according to claim 1, characterized in that The coupling agent includes one or more of aromatic diisocyanate, toluene diisocyanate, isocyanate propyl triethoxysilane, polydimethylsiloxane, 3-aminopropyl triethoxysilane; and / or The inorganic nanomaterial includes one or more of titanium dioxide, silicon dioxide, silicon carbide, aluminum oxide, zirconium oxide, and zinc oxide; and / or The epoxy resin includes one or more of glycidyl ether epoxy resin, glycidyl ester epoxy resin, glycidyl amine epoxy resin, aliphatic epoxy resin, and alicyclic epoxy resin; and / or The reducing agent comprises sodium citrate; and / or The first solvent includes one or more of toluene, N,N-dimethylformamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, pyridine, tetrahydrofuran, ethylene glycol, acetone, methanol, ethanol, 1-propanol, dichloromethane, o-xylene, and n-hexane; and / or The second solvent includes one or more of ethanol, toluene, N,N-dimethylformamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, pyridine, tetrahydrofuran, ethylene glycol, acetone, methanol, 1-propanol, dichloromethane, o-xylene, and n-hexane; and / or The third solvent includes one or more of n-butanol and xylene.
3. The preparation method according to claim 1, characterized in that: The mass ratio of the graphene oxide to the coupling agent is 0.2:(1-1.6); and / or The mass ratio of the inorganic nanomaterial to the modified graphene oxide is (2.1-4.5):10; and / or The mass ratio of the epoxy resin to the oleophilic graphene oxide is (4-8):1; and / or The mass ratio of the reducing agent to the oleophilic graphene oxide is (24-40):1; and / or The mass ratio of the epoxy resin to the third solvent is (34-64):(8-33).
4. The preparation method according to claim 1, characterized in that: The mixing time is 15 to 20 minutes; The first temperature is 95-115° C.; and / or The first time is 2.5 to 3.5 hours; and / or The second temperature is 55-75° C.; and / or The second time is 1.5 to 2.5 hours; and / or The third temperature is 80-100°C.
5. The preparation method according to claim 1, characterized in that: After obtaining the dispersion, the step further includes subjecting the dispersion to a first ultrasonic treatment; and / or After the epoxy resin, the third solvent and the oleophilic graphene oxide are mixed, before the heating to the third temperature, a second ultrasonic treatment is further performed; and / or After the reducing agent is added, the method further comprises performing a third ultrasonic treatment.
6. The preparation method according to claim 5, characterized in that: The frequency of the first ultrasonic treatment is 10 to 20 kHz; and / or The first ultrasonic treatment lasts for 30 to 40 minutes; and / or The frequency of the second ultrasonic treatment is 10 to 20 kHz; and / or The second ultrasonic treatment time is 1.5 to 2 hours; and / or The frequency of the third ultrasonic treatment is 25 to 35 kHz; and / or The third ultrasonic treatment lasts for 15 to 17 hours.
7. The preparation method according to claim 1, characterized in that: After adding the reducing agent to react, the step of adding a dispersant is also followed; and / or After the reducing agent is added for reaction, an anti-settling agent is also added.
8. The preparation method according to claim 7, characterized in that: The dispersant includes one or more of polyisobutylene succinate, polyisobutylene thiophosphate, sodium polytetramethylene phenyl sulfonate, sodium polytetramethylene naphthalene sulfonate, sodium polytetramethylene anthracene sulfonate, sodium 4-styrene sulfonate, and sodium cholate; and / or In the composite slurry, the concentration of the dispersant is 0.01wt% to 15wt%; and / or The anti-settling agent includes one or more of polyethylene wax, bentonite, and polyamide wax; and / or In the composite slurry, the concentration of the anti-settling agent is 2wt% to 6wt%.
9. A composite slurry, characterized in that: The composite slurry is prepared by the preparation method according to any one of claims 1 to 8.
10. An anticorrosive coating, characterized in that: The material of the anti-corrosion coating includes the composite slurry prepared by the preparation method according to any one of claims 1 to 8, or includes the composite slurry according to claim 9.
11. An anti-corrosion coating, characterized in that: The material of the anti-corrosion coating includes the anti-corrosion paint as claimed in claim 10.
Citation Information
Patent Citations
Polypropylene resin-based nano composite material and preparation method thereof
CN104893102A
Flame-retardant graphene anticorrosive paint
CN115109494A