High-gloss high-leveling impact-resistant polylactic acid-based powder coating and preparation method thereof

Through the synergistic effect of natural wax and polylactic acid compatible agent, the polylactic acid resin is modified, which solves the brittleness and high melt viscosity of polylactic acid resin, improves the impact resistance and gloss of polylactic acid-based powder coating, and satisfies the Application requirements for high performance coatings.

CN119019919AActive Publication Date: 2024-11-26HEFEI UNIV OF TECH

Patent Information

Application Number
CN202410751967.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-11-26
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

The inherent brittleness and high melt viscosity of unmodified polylactic acid limit its prospects for application as a resin in powder coatings, resulting in defects in appearance and poor fluidity of the coating film, which cannot meet the use requirements.

Method used

Through the synergistic effect of natural wax and polylactic acid compatible agent in the resin modification and powder coating melting and film formation process, the compatibility and interface bonding strength of the resin components are improved, the melt viscosity of the resin is reduced, and the coating is improved. Impact resistance and gloss.

Benefits of technology

It has achieved high gloss, high leveling and impact resistance coatings, meeting the application needs of household appliances, metal furniture and automotive interiors, and expanding the application scope of polylactic acid-based powder coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004888276480000091
    Figure BDA0004888276480000091
Patent Text Reader

Abstract

The invention discloses a high-gloss high-leveling impact-resistant polylactic acid-based powder coating and a preparation method thereof.The powder coating is prepared by the steps that after polylactic resin, polyester resin, natural wax, a polylactic acid compatilizer, an anti-hydrolysis agent and an environment-friendly antioxidant are evenly mixed, extrusion granulation is conducted through a double-screw extruder, drying is conducted, and modified polylactic resin master batches are obtained; mixing the modified master batch with TGIC, a pigment, a filler and an auxiliary agent, tabletting, crushing and sieving to obtain the polylactic acid-based powder coating. Through the synergistic effect of the natural wax and the polylactic acid compatilizer in the resin modification process and the powder coating melting film forming process, the compatibility of all components of the resin is improved, the melting film forming performance of the powder coating is improved, and a coating has good impact resistance and glossiness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and particularly relates to a high-gloss, high-leveling, impact-resistant polylactic acid-based powder coating and a preparation method thereof. Background Art

[0002] Powder coating is a new type of solvent-free 100% solid powder coating, which is made by physical mixing and melt extrusion of specific chemical substances. At present, polyester powder coating is the most widely used type of powder coating product in the market with the highest output. In the formula of polyester resin powder coating, polyester resin is one of the main film-forming substances, and the performance of polyester resin is the key to achieving various properties of powder coating.

[0003] The synthetic raw materials of polyester resin mainly come from fossil resources such as petroleum, coal, and natural gas. However, fossil resources are non-renewable, and the conversion and application of fossil resources cause the "greenhouse effect". The conversion and utilization of biomass resources is an effective way to protect the environment and reduce the greenhouse effect. Polylactic acid is a degradable polymer derived from biomass conversion. It is not only biodegradable, non-toxic, and has good biocompatibility, but also has good mechanical and weather resistance properties. It is a potential raw material for preparing high-performance bio-based powder coatings. However, the inherent brittleness of unmodified polylactic acid limits its prospects for use as a resin in powder coatings; at the same time, polylactic acid has a high melt viscosity, and the coating has poor fluidity during curing. During the resin curing and film-forming process, small molecules such as air and moisture are difficult to overflow from the substrate surface and the melt pores, resulting in defects in the appearance and body of the cured coating, which cannot meet the use requirements. Summary of the invention

[0004] The present invention proposes a high-gloss, high-leveling, impact-resistant polylactic acid-based powder coating and a preparation method thereof, which aims to improve the compatibility between the resin components and improve the melt-film-forming performance of the powder coating through the synergistic effect of natural wax and polylactic acid compatibilizer in the resin modification and powder coating melt film forming process, so that the coating has good impact resistance and gloss.

[0005] To achieve the purpose, the present invention adopts the following technical solution:

[0006] The present invention firstly provides a high-gloss, high-leveling, impact-resistant polylactic acid-based powder coating, which is characterized in that, in terms of weight fraction, the raw materials of the powder coating include: 50-70 parts of modified polylactic acid resin; 3-6 parts of TGIC; 20-25 parts of titanium dioxide; 15-20 parts of filler; 0.5-1 part of leveling agent; 0.5-1 part of brightener; and 0.2-0.5 part of degassing agent.

[0007] In some embodiments of the present invention, the raw materials for preparing the modified polylactic acid resin include, by weight: 10-90 parts of polylactic acid resin; 10-90 parts of polyester resin; 1-3 parts of natural wax; 5-8 parts of polylactic acid compatibilizer; 1-2 parts of anti-hydrolysis agent; and 0.1-0.5 parts of environmentally friendly antioxidant.

[0008] In some embodiments of the present invention, the melt mass flow rate of the polylactic acid resin is 20-50 g / 10 min under the test conditions of a temperature of 190° C. and a load of 2.16 kg, and the notched impact strength is 2-4 kJ / m 2 , tensile strength is 40-60MPa, elongation at break is 4-10%, molecular weight is 20000-80000g / mol, melting point is 155-180℃, density is 1.2-1.3g / cm 3 .

[0009] In some embodiments of the present invention, the melt mass flow rate of the polyester resin is 3-50 g / 10 min under the test conditions of a temperature of 190° C. and a load weight of 2.16 kg, the acid value is 20-50 mg KOH / g, the viscosity is 2000-8000 mPa·s / 200° C., the molecular weight is 2000-8000 g / mol, and the glass transition temperature is ≥60° C.

[0010] In some embodiments of the present invention, the natural wax is selected from a mixture of one or more of beeswax, palm wax, rice bran wax, candelilla wax, soybean wax and coconut wax, all with a molecular weight of 300-1000 g / mol.

[0011] In some embodiments of the present invention, the polylactic acid compatibilizer includes one or both of a polylactic acid grafted glycidyl methacrylate compatibilizer and a polylactic acid grafted maleic anhydride compatibilizer; the grafting rate of the polylactic acid compatibilizer is 1-3%.

[0012] In some embodiments of the present invention, the anti-hydrolysis agent is a polymeric carbodiimide anti-hydrolysis agent, and the carbodiimide content is not less than 12%.

[0013] In some embodiments of the present invention, the environmentally friendly antioxidant includes a primary antioxidant and an auxiliary antioxidant, the primary antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, the auxiliary antioxidant is tris(2,4-di-tert-butylphenyl)phosphite, and the mass ratio of the primary antioxidant to the auxiliary antioxidant is 1:1-2.

[0014] In some embodiments of the present invention, the TGIC is a micronized and modified TGIC, with an average particle size D50 of 50-200 μm, an epoxy equivalent of ≤110 g / mol, and a melting point of 90-115° C.

[0015] In some embodiments of the present invention, the titanium dioxide is one or more of rutile titanium dioxide and anatase titanium dioxide, with an average particle size D50 of 0.2-0.4 μm, a TiO2 content of 94-98%, a pH value of 6.5-8.0, an oil absorption value of 15-20 g / 100 g, and a density of 4.0-4.1 g / cm 3 .

[0016] In some embodiments of the present invention, the filler is one or more of precipitated barium sulfate, matte barium sulfate and light calcium carbonate, with an average particle size D50 of 0.1-2 μm, a pH value of 7.0-9.0, an oil absorption value of 10-22 g / 100 g, a loss on ignition ≤1.50%, and a density of 4.4-4.5 g / cm 3 .

[0017] In some embodiments of the present invention: the leveling agent is one or more of acrylate homopolymer, acrylate copolymer, silicone modified acrylate polymer and polysiloxane. The brightener is acrylate copolymer with a ring and ball softening point of 95-125°C. The degassing agent is benzoin or its modified product with a melting point of 134-138°C and a density of 1.3-1.4 g / cm 3 .

[0018] In some embodiments of the invention, the modified polylactic acid resin is prepared according to the following steps:

[0019] Add polylactic acid resin, polyester resin, natural wax, polylactic acid compatibilizer, anti-hydrolysis agent and environmentally friendly antioxidant into a high-speed mixer in proportion, and mix at a high speed of 1000-1500 r / min for 5-10 minutes to obtain a mixture;

[0020] The mixed material is sheared, mixed and plasticized in a twin-screw extruder with an extrusion temperature of 170-190° C. and a screw speed of 100-300 r / min, and then subjected to water-cooled drawing, air-drying and pelletizing processes to obtain a modified polylactic acid resin masterbatch.

[0021] The present invention further provides a method for preparing the high-gloss, high-leveling, impact-resistant polylactic acid-based powder coating, comprising the following steps:

[0022] The modified polylactic acid resin, TGIC, titanium dioxide, filler, leveling agent, brightener and degassing agent are added to a high-speed mixer in proportion, mixed at a mixing speed of 1000-1500 r / min for 5-10 minutes, and then melt-sheared by a twin-screw extruder at an extrusion temperature of 100-120°C and a screw speed of 400-600 r / min, and then cooled, pressed and roughly crushed to obtain a primary powder coating;

[0023] The primary powder coating is finely ground by an ACM grinder at a main grinder speed of 4000-6000 r / min and a secondary grinder speed of 2000-3000 r / min, and then the particle size is screened by a 100-140 mesh standard test sieve to obtain a high-gloss, high-leveling, and impact-resistant polylactic acid-based powder coating.

[0024] The present invention has the following beneficial effects:

[0025] The present invention firstly prepares a modified polylactic acid resin masterbatch by blending polylactic acid resin, polyester resin, natural wax, polylactic acid compatibilizer and antioxidant, and then mixes the masterbatch with pigment, filler and auxiliary agent to form tablets, and crushes and sieves to obtain a polylactic acid-based powder coating. The present invention improves the interfacial bonding strength and compatibility between polylactic acid and polyester resin through the synergistic effect of natural wax and polylactic acid compatibilizer in the resin modification and powder coating melt film forming process, effectively improves the impact resistance of the coating, and gives the coating good impact resistance. At the same time, the lubricity of natural wax is used to effectively reduce the melt viscosity of the resin, improve the leveling and film-forming properties of the resin melt in the coating film forming process, so that the air on the substrate surface and in the melt pores has enough time to escape the coating, and the coating formed after the melt film forming has high gloss, which can meet the application needs of bio-based powder coating fields such as household appliances, metal furniture and automotive interiors. DETAILED DESCRIPTION

[0026] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0027] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise specified in the present invention, both endpoints of each numerical range and any value between the two endpoints can be selected. Unless otherwise defined, all technical and scientific terms used in the present invention are familiar to those skilled in the art and the description of the present invention, and any methods, equipment and materials of the prior art similar or equivalent to the methods, equipment and materials described in the embodiments of the present invention can also be used to implement the present invention.

[0028] Note that, unless otherwise specified, "%" and "part(s)" shown in the description herein mean "% by mass" and "part(s) by mass", respectively.

[0029] The invention proposes a high-gloss, high-leveling, impact-resistant polylactic acid-based powder coating and a preparation method, which can make the coating after electrostatic spraying have the characteristics of high gloss, high leveling and impact resistance, and can be widely used in the field of bio-based powder coatings such as household appliances, metal furniture and automotive interiors.

[0030] The invention provides a high-gloss, high-leveling, impact-resistant polylactic acid-based powder coating. The powder coating comprises, by weight, 50-70 parts of modified polylactic acid resin, 3-6 parts of TGIC, 20-25 parts of titanium dioxide, 15-20 parts of filler, 0.5-1 part of leveling agent, 0.5-1 part of brightener and 0.2-0.5 part of degassing agent.

[0031] The raw materials for preparing the modified polylactic acid resin include, by weight: 10-90 parts of polylactic acid resin; 10-90 parts of polyester resin; 1-3 parts of natural wax; 5-8 parts of polylactic acid compatibilizer; 1-2 parts of anti-hydrolysis agent; and 0.1-0.5 parts of environmentally friendly antioxidant.

[0032] In the following embodiments of the present invention, the melt mass flow rate of the polylactic acid resin used is 30 g / 10 min under the test conditions of a temperature of 190° C. and a load of 2.16 kg, and the molecular weight of the polylactic acid resin is 20,000 g / mol, and the notched impact strength is 3 kJ / m 2 , tensile strength is 50MPa, elongation at break is 4%, melting point is 175℃, density is 1.24g / cm 3 Specifically, the polylactic acid resin used in the following examples is FY201 produced by Anhui Fengyuan Futailai Polylactic Acid Co., Ltd.

[0033] In the following embodiments of the present invention, the melt mass flow rate of the polyester resin used is 40 g / 10 min under the test conditions of a temperature of 190° C. and a load of 2.16 kg, the acid value is 30-36 mg KOH / g, the viscosity of the polyester resin is 6000-8000 mPa·s / 200° C., the molecular weight of the polyester resin is 2000 g / mol, and the glass transition temperature is ≥65° C. Specifically, the polyester resin used in the following embodiments is YC8600 of Anhui Yongchang New Materials Co., Ltd.

[0034] In the following embodiments of the present invention, the natural wax is refined and purified beeswax with a molecular weight of 300 g / mol.

[0035] In the following embodiments of the present invention, the polylactic acid compatibilizer is polylactic acid grafted glycidyl methacrylate (PLA-g-GMA), and the grafting rate is 2%. Specifically, the polylactic acid compatibilizer used in the following embodiments is V105 produced by Foshan Fanke Chemical Co., Ltd.

[0036] In the following embodiments of the present invention, the anti-hydrolysis agent used is a polymerized carbodiimide anti-hydrolysis agent, and the carbodiimide content is 12.5% ​​and the density is 1.05 g / cm 3 , the melting temperature is 100° C. Specifically, the anti-hydrolysis agent used in the following examples is Hyadimide 100 from Rhein-Schafer, Germany.

[0037] In the following embodiments of the present invention, the environmentally friendly antioxidants used include a primary antioxidant and an auxiliary antioxidant, the primary antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and the auxiliary antioxidant is tris(2,4-di-tert-butylphenyl) phosphite. Further, the mass ratio of the primary antioxidant to the auxiliary antioxidant is 1:1.

[0038] In the following embodiment of the present invention, the TGIC used is a micronized modified TGIC, the average particle size D50 of which is 50 μm, and the epoxy equivalent of the micronized modified TGIC is ≤110 g / mol, and the melting point is 90-115°C. The micronization modification treatment increases the specific surface area of ​​TGIC, which can significantly increase its reaction activity and reduce the activation energy required for the reaction. At the same time, by improving the dispersibility of TGIC in the resin, the purpose of improving the comprehensive performance of the coating is achieved. Specifically, the TGIC used in the following embodiment is T-4005 of Dongguan Long Innovation Materials Technology Co., Ltd.

[0039] In the following embodiments of the present invention, the titanium dioxide used is rutile titanium dioxide, the average particle size D50 of which is 0.3 μm, the TiO2 content is 95%, the pH value is 7.0, the oil absorption value is 20 g / 100 g, and the density is 4.1 g / cm 3 Rutile titanium dioxide as a pigment has good leveling properties for the coating, and has a relatively short gelation time, which is more conducive to curing and film formation. Specifically, the rutile titanium dioxide used in the following examples is NTR-760 from Ningbo Nanhai Chemical Co., Ltd.

[0040] In the following embodiments of the present invention, the filler used is precipitated barium sulfate, the average particle size D50 of which is 0.79 μm, the pH value is 7.0-9.0, the oil absorption value is 14-22 g / 100 g, the ignition loss is ≤1.50%, and the density is 4.5 g / cm 3 The precipitated barium sulfate has the smallest oil absorption, which is beneficial to improving the melt fluidity and glossiness of the coating. Specifically, the precipitated barium sulfate used in the following examples is HY-A03 from Shenzhen Haiyang Powder Technology Co., Ltd.

[0041] In the following examples of the present invention, the leveling agent used is an acrylate homopolymer, which can significantly reduce the surface tension of the powder coating of the present invention and avoid the appearance of orange peel or shrinkage craters in the coating. Specifically, the leveling agent used in the following examples is GLP303 from Ningbo Nanhai Chemical Co., Ltd.

[0042] In the following embodiments of the present invention, the brightener used is a copolymer of butyl acrylate and methyl methacrylate, and the copolymer of butyl acrylate and methyl methacrylate has a ring and ball softening point of 95-125°C. Since it contains a certain number of polar groups, it has a good wetting effect on the pigment, filler and substrate in the powder coating, and can effectively eliminate shrinkage cavities and promote leveling. Specifically, the brightener used in the following embodiments is PLC701 of Ningbo Nanhai Chemical Co., Ltd.

[0043] In the following embodiments of the present invention, the degassing agent used is benzoin, and the melting point of benzoin is 136°C and the density is 1.31 g / cm 3 , which can play the role of a solid solvent in the powder coating of the present invention, so that the air has enough time to escape from the coating film. Specifically, the degassing agent used in the following examples is WK315 from Ningbo Weikai Chemical Co., Ltd.

[0044] Hereinafter, the present invention will be explained in more detail by citing examples, which should not be construed as limiting. Appropriate modifications may be made within the scope consistent with the gist of the present invention, all of which fall within the technical scope of the present invention.

[0045] Example 1

[0046] Step S1, adding 10 parts of polylactic acid resin, 90 parts of polyester resin, 1 part of beeswax, 5 parts of PLA-g-GMA, 2 parts of anti-hydrolysis agent and 0.3 parts of environmentally friendly antioxidant into a high-speed mixer in proportion, and mixing at a high speed of 1000 r / min for 5 minutes to obtain a mixture;

[0047] Step S2, subjecting the mixed material prepared in step S1 to shearing, mixing and plasticizing in a twin-screw extruder at an extrusion temperature of 180° C. and a screw speed of 200 r / min, and then subjecting the mixed material to water-cooling, drawing, air-drying and pelletizing processes to obtain a modified polylactic acid resin masterbatch;

[0048] Step S3, adding 60 parts of the modified polylactic acid resin prepared in step S2, 5 parts of TGIC, 20 parts of titanium dioxide, 15 parts of precipitated barium sulfate, 1 part of a leveling agent, 1 part of a brightener and 0.3 parts of a degassing agent in proportion to a high-speed mixer, mixing at a mixing speed of 1000 r / min for 5 minutes, and then melt-shearing through a twin-screw extruder at an extrusion temperature of 110° C. and a screw speed of 500 r / min, and then cooling, tableting and coarse crushing to obtain a primary powder coating;

[0049] Step S4, the primary powder coating prepared in step S3 is finely ground by an ACM grinder at a main grinder speed of 5000 r / min and a secondary grinder speed of 2500 r / min, and then the particle size is screened by a 120-mesh standard test sieve to obtain a high-gloss, high-leveling, and impact-resistant polylactic acid-based powder coating.

[0050] Example 2

[0051] Step S1, adding 90 parts of polylactic acid resin, 10 parts of polyester resin, 3 parts of beeswax, 8 parts of PLA-g-GMA, 2 parts of anti-hydrolysis agent and 0.3 parts of environmentally friendly antioxidant into a high-speed mixer in proportion, and mixing at a high speed of 1000 r / min for 5 minutes to obtain a mixture;

[0052] Step S2, subjecting the mixed material prepared in step S1 to shearing, mixing and plasticizing in a twin-screw extruder at an extrusion temperature of 180° C. and a screw speed of 200 r / min, and then subjecting the mixed material to water-cooling, drawing, air-drying and pelletizing processes to obtain a modified polylactic acid resin masterbatch;

[0053] Step S3, adding 60 parts of the modified polylactic acid resin prepared in step S2, 5 parts of TGIC, 20 parts of titanium dioxide, 15 parts of precipitated barium sulfate, 1 part of a leveling agent, 1 part of a brightener and 0.3 parts of a degassing agent in proportion to a high-speed mixer, mixing at a mixing speed of 1000 r / min for 5 minutes, and then melt-shearing through a twin-screw extruder at an extrusion temperature of 110° C. and a screw speed of 500 r / min, and then cooling, tableting and coarse crushing to obtain a primary powder coating;

[0054] Step S4, the primary powder coating prepared in step S3 is finely ground by an ACM grinder at a main grinder speed of 5000 r / min and a secondary grinder speed of 2500 r / min, and then the particle size is screened by a 120-mesh standard test sieve to obtain a high-gloss, high-leveling, and impact-resistant polylactic acid-based powder coating.

[0055] Example 3

[0056] Step S1, adding 50 parts of polylactic acid resin, 50 parts of polyester resin, 2 parts of beeswax, 6 parts of PLA-g-GMA, 2 parts of anti-hydrolysis agent and 0.3 parts of environmentally friendly antioxidant into a high-speed mixer in proportion, and mixing at a high speed of 1000 r / min for 5 minutes to obtain a mixture;

[0057] Step S2, subjecting the mixed material prepared in step S1 to shearing, mixing and plasticizing in a twin-screw extruder at an extrusion temperature of 180° C. and a screw speed of 200 r / min, and then subjecting the mixed material to water-cooling, drawing, air-drying and pelletizing processes to obtain a modified polylactic acid resin masterbatch;

[0058] Step S3, adding 60 parts of the modified polylactic acid resin prepared in step S2, 5 parts of TGIC, 20 parts of titanium dioxide, 15 parts of precipitated barium sulfate, 1 part of a leveling agent, 1 part of a brightener and 0.3 parts of a degassing agent in proportion to a high-speed mixer, mixing at a mixing speed of 1000 r / min for 5 minutes, and then melt-shearing through a twin-screw extruder at an extrusion temperature of 110° C. and a screw speed of 500 r / min, and then cooling, tableting and coarse crushing to obtain a primary powder coating;

[0059] Step S4, the primary powder coating prepared in step S3 is finely ground by an ACM grinder at a main grinder speed of 5000 r / min and a secondary grinder speed of 2500 r / min, and then the particle size is screened by a 120-mesh standard test sieve to obtain a high-gloss, high-leveling, and impact-resistant polylactic acid-based powder coating.

[0060] Example 4

[0061] Step S1, adding 50 parts of polylactic acid resin, 50 parts of polyester resin, 2 parts of beeswax, 6 parts of PLA-g-GMA, 2 parts of anti-hydrolysis agent and 0.3 parts of environmentally friendly antioxidant into a high-speed mixer in proportion, and mixing at a high speed of 1000 r / min for 5 minutes to obtain a mixture;

[0062] Step S2, subjecting the mixed material prepared in step S1 to shearing, mixing and plasticizing in a twin-screw extruder at an extrusion temperature of 180° C. and a screw speed of 200 r / min, and then subjecting the mixed material to water-cooling, drawing, air-drying and pelletizing steps to obtain a modified polylactic acid resin masterbatch;

[0063] Step S3, adding 50 parts of the modified polylactic acid resin prepared in step S2, 5 parts of TGIC, 20 parts of titanium dioxide, 15 parts of precipitated barium sulfate, 1 part of a leveling agent, 1 part of a brightener and 0.3 parts of a degassing agent in proportion to a high-speed mixer, mixing at a mixing speed of 1000 r / min for 5 minutes, and then melt-shearing through a twin-screw extruder at an extrusion temperature of 110° C. and a screw speed of 500 r / min, and then cooling, tableting and coarse crushing to obtain a primary powder coating;

[0064] Step S4, the primary powder coating prepared in step S3 is finely ground by an ACM grinder at a main grinder speed of 5000 r / min and a secondary grinder speed of 2500 r / min, and then the particle size is screened by a 120-mesh standard test sieve to obtain a high-gloss, high-leveling, and impact-resistant polylactic acid-based powder coating.

[0065] Example 5

[0066] Step S1, adding 50 parts of polylactic acid resin, 50 parts of polyester resin, 2 parts of beeswax, 6 parts of PLA-g-GMA, 2 parts of anti-hydrolysis agent and 0.3 parts of environmentally friendly antioxidant into a high-speed mixer in proportion, and mixing at a high speed of 1000 r / min for 5 minutes to obtain a mixture;

[0067] Step S2, subjecting the mixed material prepared in step S1 to shearing, mixing and plasticizing in a twin-screw extruder at an extrusion temperature of 180° C. and a screw speed of 200 r / min, and then subjecting the mixed material to water-cooling, drawing, air-drying and pelletizing steps to obtain a modified polylactic acid resin masterbatch;

[0068] Step S3, adding 70 parts of the modified polylactic acid resin prepared in step S2, 5 parts of TGIC, 20 parts of titanium dioxide, 15 parts of precipitated barium sulfate, 1 part of a leveling agent, 1 part of a brightener and 0.3 parts of a degassing agent in proportion to a high-speed mixer, mixing at a mixing speed of 1000 r / min for 5 minutes, and then melt-shearing through a twin-screw extruder at an extrusion temperature of 110° C. and a screw speed of 500 r / min, and then cooling, tableting and coarse crushing to obtain a primary powder coating;

[0069] Step S4, the primary powder coating prepared in step S3 is finely ground by an ACM grinder at a main grinder speed of 5000 r / min and a secondary grinder speed of 2500 r / min, and then the particle size is screened by a 120-mesh standard test sieve to obtain a high-gloss, high-leveling, and impact-resistant polylactic acid-based powder coating.

[0070] Comparative Example 1

[0071] Step S1, adding 50 parts of polylactic acid resin, 50 parts of polyester resin, 6 parts of PLA-g-GMA, 2 parts of anti-hydrolysis agent and 0.3 parts of environmentally friendly antioxidant into a high-speed mixer in proportion, and mixing at a high speed of 1000 r / min for 5 minutes to obtain a mixture;

[0072] Step S2, subjecting the mixed material prepared in step S1 to shearing, mixing and plasticizing in a twin-screw extruder at an extrusion temperature of 180° C. and a screw speed of 200 r / min, and then subjecting the mixed material to water-cooling, drawing, air-drying and pelletizing processes to obtain a modified polylactic acid resin masterbatch;

[0073] Step S3, adding 60 parts of the modified polylactic acid resin prepared in step S2, 5 parts of TGIC, 20 parts of titanium dioxide, 15 parts of precipitated barium sulfate, 1 part of a leveling agent, 1 part of a brightener and 0.3 parts of a degassing agent in proportion to a high-speed mixer, mixing at a mixing speed of 1000 r / min for 5 minutes, and then melt-shearing through a twin-screw extruder at an extrusion temperature of 110° C. and a screw speed of 500 r / min, and then cooling, tableting and coarse crushing to obtain a primary powder coating;

[0074] Step S4, the primary powder coating prepared in step S3 is finely ground by an ACM grinder at a main grinder speed of 5000 r / min and a secondary grinder speed of 2500 r / min, and then the particle size is screened by a 120-mesh standard test sieve to obtain a powder coating.

[0075] Comparative Example 2

[0076] Step S1, adding 50 parts of polylactic acid resin, 50 parts of polyester resin, 2 parts of beeswax, 2 parts of anti-hydrolysis agent and 0.3 parts of environmentally friendly antioxidant into a high-speed mixer in proportion, and mixing at a high speed of 1000 r / min for 5 minutes to obtain a mixture;

[0077] Step S2, subjecting the mixed material prepared in step S1 to shearing, mixing and plasticizing in a twin-screw extruder at an extrusion temperature of 180° C. and a screw speed of 200 r / min, and then subjecting the mixed material to water-cooling, drawing, air-drying and pelletizing processes to obtain a modified polylactic acid resin masterbatch;

[0078] Step S3, adding 60 parts of the modified polylactic acid resin prepared in step S2, 5 parts of TGIC, 20 parts of titanium dioxide, 15 parts of precipitated barium sulfate, 1 part of a leveling agent, 1 part of a brightener and 0.3 parts of a degassing agent in proportion to a high-speed mixer, mixing at a mixing speed of 1000 r / min for 5 minutes, and then melt-shearing through a twin-screw extruder at an extrusion temperature of 110° C. and a screw speed of 500 r / min, and then cooling, tableting and coarse crushing to obtain a primary powder coating;

[0079] Step S4, the primary powder coating prepared in step S3 is finely ground by an ACM grinder at a main grinder speed of 5000 r / min and a secondary grinder speed of 2500 r / min, and then the particle size is screened by a 120-mesh standard test sieve to obtain a powder coating.

[0080] Comparative Example 3

[0081] Step S3, adding 60 parts of polylactic acid resin, 5 parts of TGIC, 20 parts of titanium dioxide, 15 parts of precipitated barium sulfate, 1 part of leveling agent, 1 part of brightener and 0.3 parts of degassing agent in proportion to a high-speed mixer, mixing at a mixing speed of 1000 r / min for 5 minutes, and then melt-shearing through a twin-screw extruder at an extrusion temperature of 110° C. and a screw speed of 500 r / min, and then cooling, tableting and coarse crushing to obtain a primary powder coating;

[0082] Step S4, the primary powder coating prepared in step S3 is finely ground by an ACM grinder at a main grinder speed of 5000 r / min and a secondary grinder speed of 2500 r / min, and then the particle size is screened by a 120-mesh standard test sieve to obtain a powder coating.

[0083] Comparative Example 4

[0084] Step S1, adding 50 parts of polylactic acid resin, 50 parts of polyester resin, 2 parts of beeswax, 6 parts of PLA-g-GMA, 2 parts of anti-hydrolysis agent and 0.3 parts of environmentally friendly antioxidant into a high-speed mixer in proportion, and mixing at a high speed of 1000 r / min for 5 minutes to obtain a mixture;

[0085] Step S2, adding 60 parts of the mixture prepared in step S1, 5 parts of TGIC, 20 parts of titanium dioxide, 15 parts of precipitated barium sulfate, 1 part of leveling agent, 1 part of brightener and 0.3 parts of degassing agent in proportion to a high-speed mixer, mixing at a mixing speed of 1000 r / min for 5 minutes, and then melt shearing through a twin-screw extruder at an extrusion temperature of 110° C. and a screw speed of 500 r / min, and then cooling, tableting and coarse crushing to obtain a primary powder coating;

[0086] Step S3, the primary powder coating prepared in step S2 is finely ground by an ACM grinder at a main grinder speed of 5000 r / min and a secondary grinder speed of 2500 r / min, and then the particle size is screened by a 120-mesh standard test sieve to obtain a powder coating.

[0087] Test Case

[0088] The powder coatings prepared in Examples 1-5 and Comparative Examples 1-4 were used to prepare coating samples by high-voltage electrostatic spraying: first, 200 g of powder coating sample powder was loaded into an electrostatic spray gun, and the spraying pressure was set to 0.38 MPa and the electrostatic high voltage was set to 76 KV. The spray gun was turned on to spray the powder coating evenly on the substrate, and the film thickness was controlled to be 80-90 μm. Then, the sprayed substrate was placed in an oven and cured at 200°C for 10 minutes to form a coating sample. The substrate was a tinplate with a size of 50 mm × 120 mm × 0.3 mm. The surface was polished with sandpaper before spraying to remove the oxide scale.

[0089] The powder coatings prepared in the above comparative examples and embodiments were tested, wherein the performance parameter testing method is as follows:

[0090] Coating appearance: Tested according to GB / T 37356-2019 "Lighting conditions and methods for visual assessment of paint and varnish coatings";

[0091] Impact resistance: tested according to GB / T 1732-2020 "Determination of impact resistance of paint films" standard;

[0092] Gloss: Tested according to GB / T 9754-2007 "Determination of 20°, 60° and 85° specular gloss of paints and varnishes without metallic pigments";

[0093] Leveling grade: According to PCI leveling grading standards;

[0094] Adhesion: Tested according to GB / T 9286-1998 "Paint and Varnish Film Frame Test" standard;

[0095] The coating properties of the powder coatings obtained in the above examples and comparative examples are shown in Table 2 below.

[0096] Table 2. Comparison of the performance of the products after coating in the examples and comparative examples

[0097]

[0098] As shown in Table 2, by comparing the various properties of the coatings in Examples 1-5 and Comparative Examples 1-3, it can be found that the glossiness of the powder coating coatings in Examples 1-5 is significantly higher than that in the comparative examples, indicating that the glossiness of the polylactic acid-based powder coating is improved. The leveling grade in the embodiment is also significantly higher than that in the comparative example, indicating that the leveling property of the material is significantly improved. At the same time, most of the impact resistance of the coating in the embodiment can pass, indicating that the impact resistance of the material is improved. By comparing the various properties of the coatings in Example 3 and Comparative Examples 1-2, it can be seen that after only adding natural wax or polylactic acid compatibilizer to modify the polylactic acid resin / polyester resin blend, the performance difference is large, and the powder coating application requirements cannot be met. The reason is that it is impossible to take into account the compatibility between the resin components and the leveling and film-forming properties of the resin melt. Example 3 has the same formula as Comparative Example 4, but the preparation process is different, and the performance difference is large. The reason is that the traditional method for preparing powder coatings is difficult to achieve effective regulation of the polylactic acid compatibilizer on the interface of the polylactic acid resin / polyester resin blend and the controllable dispersion of natural wax in the matrix, reflecting the superiority of the preparation process.

[0099] Therefore, it can be seen from the glossiness, leveling grade and impact resistance results in each embodiment and the comparative example that the present invention uses a polylactic acid resin / polyester resin blend as a matrix, and improves the interfacial bonding strength and compatibility between the resin components through the synergistic effect of natural wax and polylactic acid compatibilizer in the resin modification and powder coating melt film forming process. At the same time, the lubricity of natural wax is used to effectively reduce the melt viscosity of the resin, thereby improving the leveling and film-forming properties of the resin melt during the coating film forming process, so that the air on the substrate surface and in the melt pores has sufficient time to escape from the coating film. The coating formed after the melt film forming has good impact resistance and gloss, thereby expanding the application scope and field of polylactic acid-based powder coatings, especially in household appliances, metal furniture, and automotive interiors, which have high requirements for appearance gloss and high impact resistance.

[0100] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the inventive concept, such as a technical solution formed by replacing the above-mentioned features with (but not limited to) technical features with similar functions disclosed in this application.

[0101] Except for the technical features described in the specification, the remaining technical features are known technologies to those skilled in the art. In order to highlight the innovative features of the present invention, the remaining technical features will not be described here in detail.

Claims

1. A high-gloss, high-leveling, impact-resistant polylactic acid-based powder coating, characterized in that: The raw materials of the powder coating include, by weight: 50-70 parts of modified polylactic acid resin; 3-6 parts of TGIC; 20-25 parts of titanium dioxide; 15-20 parts of filler; 0.5-1 parts of leveling agent; 0.5-1 parts of brightener; and 0.2-0.5 parts of degassing agent.

2. A high gloss, high leveling, impact-resistant polylactic acid-based powder coating according to claim 1, characterized in that: The raw materials for preparing the modified polylactic acid resin include, by weight: 10-90 parts of polylactic acid resin; 10-90 parts of polyester resin; 1-3 parts of natural wax; 5-8 parts of polylactic acid compatibilizer; 1-2 parts of anti-hydrolysis agent; and 0.1-0.5 parts of environmentally friendly antioxidant.

3. A high gloss, high leveling, impact-resistant polylactic acid-based powder coating according to claim 2, characterized in that: The melt mass flow rate of the polylactic acid resin is 20-50 g / 10 min under the test conditions of a temperature of 190° C. and a load of 2.16 kg.

4. The high-gloss, high-leveling, impact-resistant polylactic acid-based powder coating according to claim 2, characterized in that: The polyester resin has an acid value of 20-50 mg KOH / g, a viscosity of 2000-8000 mPa·s / 200° C., and a molecular weight of 2000-8000 g / mol.

5. The high-gloss, high-leveling, impact-resistant polylactic acid-based powder coating according to claim 2, characterized in that: The natural wax is selected from one or more mixtures of beeswax, palm wax, rice bran wax, candelilla wax, soybean wax and coconut wax, all with molecular weights of 300-1000 g / mol.

6. The high-gloss, high-leveling, impact-resistant polylactic acid-based powder coating according to claim 2, characterized in that: The polylactic acid compatibilizer includes one or two of a polylactic acid grafted glycidyl methacrylate compatibilizer and a polylactic acid grafted maleic anhydride compatibilizer; the grafting rate of the polylactic acid compatibilizer is 1-3%.

7. The high-gloss, high-leveling, impact-resistant polylactic acid-based powder coating according to claim 2, characterized in that: The anti-hydrolysis agent is a polymerized carbodiimide anti-hydrolysis agent, and the carbodiimide content is not less than 12%.

8. The high-gloss, high-leveling, impact-resistant polylactic acid-based powder coating according to claim 2, characterized in that: The environmentally friendly antioxidant comprises a main antioxidant and an auxiliary antioxidant, wherein the main antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and the auxiliary antioxidant is tris(2,4-di-tert-butylphenyl) phosphite, and the mass ratio of the main antioxidant to the auxiliary antioxidant is 1:1-2.

9. The high-gloss, high-leveling, impact-resistant polylactic acid-based powder coating according to claim 2, characterized in that: The modified polylactic acid resin is prepared according to the following steps: Add polylactic acid resin, polyester resin, natural wax, polylactic acid compatibilizer, anti-hydrolysis agent and environmentally friendly antioxidant into a high-speed mixer in proportion, and mix at a high speed of 1000-1500 r / min for 5-10 minutes to obtain a mixture; The mixed material is sheared, mixed and plasticized in a twin-screw extruder with an extrusion temperature of 170-190° C. and a screw speed of 100-300 r / min, and then subjected to water-cooled drawing, air-drying and pelletizing processes to obtain a modified polylactic acid resin masterbatch.

10. A method for preparing the high-gloss, high-leveling, impact-resistant polylactic acid-based powder coating according to any one of claims 1 to 9, characterized in that: The following steps are involved: The modified polylactic acid resin, TGIC, titanium dioxide, filler, leveling agent, brightener and degassing agent are added to a high-speed mixer in proportion, mixed at a mixing speed of 1000-1500 r / min for 5-10 minutes, and then melt-sheared by a twin-screw extruder at an extrusion temperature of 100-120°C and a screw speed of 400-600 r / min, and then cooled, pressed and roughly crushed to obtain a primary powder coating; The primary powder coating is finely ground by an ACM grinder at a main grinder speed of 4000-6000 r / min and a secondary grinder speed of 2000-3000 r / min, and then the particle size is screened by a 100-140 mesh standard test sieve to obtain a high-gloss, high-leveling, and impact-resistant polylactic acid-based powder coating.

Citation Information

Patent Citations

  • Modified poly(lactic acid) and preparation method thereof

    CN102226004A

  • Glycidyl methacrylate grafted polylactic acid copolymer material, preparation method for same and application thereof

    CN102603994A

  • Degradable thermosetting powder coating and preparation method thereof

    CN103773184A

  • Super-leveling mirror powder coating and preparation method thereof

    CN110551441A

  • Super-weather-resistant powder coating material and preparation method thereof

    CN110724444A

Cited By

  • High-leveling impact-resistant bio-based polyester powder coating and preparation method thereof

    CN119752291A

  • Degradable insulating paint and preparation method thereof

    CN120536027A