Resin composition, prepreg, laminate, printed wiring board, and semiconductor package

The melt viscosity of resin in printed wiring boards is solved by using fused ring groups of aromatic rings and aliphatic rings and maleimide resins and phosphate compounds of N-substituted maleimide groups in the resin composition. The high problem achieves lower minimum melt viscosity and higher insulating layer density, meeting the heat resistance and conductor adhesion requirements of electronic equipment.

CN119095891APending Publication Date: 2024-12-06RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380036569.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-10-19
Filing Date
2023-10-11
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The maleimide resin used in existing printed wiring boards has a high minimum melt viscosity, which leads to voids that may be generated in the insulating layer, making it difficult to meet the requirements of electronic equipment for heat resistance and conductor adhesion.

Method used

The resin composition of the maleimide resin and the phosphate compound containing a fused ring group of an aromatic ring and an aliphatic ring and an N-substituted maleimide group is captured by the phosphate compound. Free radicals inhibit curing reaction and reduce minimum melt viscosity.

Benefits of technology

While maintaining the heat resistance and conductor adhesion of the maleimide resin, it is achieved, and the minimum melt viscosity of the resin composition is significantly reduced, thereby improving the density and performance of the insulating layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005102524410000021
    Figure BDA0005102524410000021
  • Figure BDA0005102524410000031
    Figure BDA0005102524410000031
  • Figure BDA0005102524410000061
    Figure BDA0005102524410000061
Patent Text Reader

Abstract

The present invention relates to: a resin composition containing: (A) one or more substances selected from the group consisting of maleimide resins having one or more N-substituted maleimide groups and derivatives of the maleimide resins; and a prepreg, a laminate, a resin film, a printed wiring board, and a semiconductor package using the resin composition, the resin composition containing: (A) one or more substances selected from the group consisting of maleimide resins having one or more N-substituted maleimide groups; and (B) a phosphate ester compound having two or more phosphorus atoms, the group connecting at least two phosphorus atoms to each other including two or more aromatic rings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present embodiment relates to a resin composition, a prepreg, a laminate, a printed wiring board, and a semiconductor package. Background Art

[0002] In recent years, there has been a growing demand for miniaturization, weight reduction, higher wiring density, and faster processing speeds of printed wiring boards used in electronic devices, communication devices, etc. In response, higher reliability than ever is required for the insulation layer of the printed wiring board.

[0003] Conventionally, thermosetting resins have been used as insulating materials for printed wiring boards.

[0004] As thermosetting resins used in insulating materials, epoxy resins are generally used, which have an excellent balance among insulation, heat resistance, cost, etc. However, epoxy resins have difficulty in satisfying the level of performance required in recent years in terms of heat resistance.

[0005] Therefore, maleimide resins are used as insulating materials for printed wiring boards as thermosetting resins having better heat resistance (for example, Patent Document 1).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2022-013142 Summary of the invention

[0009] Problems to be solved by the invention

[0010] However, as described above, the progress of fine wiring in electronic devices and the like is remarkable, and if the melt viscosity of the insulating material used for embedding the fine wiring pattern is high, voids may be generated in the insulating layer, etc. Maleimide resins are excellent in heat resistance, conductor adhesion, etc., but on the other hand, tend to have a high minimum melt viscosity, so it is desired to reduce the melt viscosity of the insulating material while effectively utilizing the characteristics of maleimide resins.

[0011] In view of such a situation, the present embodiment aims to provide a resin composition having a low minimum melt viscosity even though a maleimide resin is used as a thermosetting resin, and a prepreg, a laminate, a resin film, a printed wiring board, and a semiconductor package using the resin composition.

[0012] Means for solving problems

[0013] That is, this embodiment provides the following [1] to

[11] .

[0014] [1] A resin composition comprising:

[0015] (A) at least one selected from a maleimide resin and a derivative of the maleimide resin, wherein the maleimide resin has a group including a condensed ring of an aromatic ring and an aliphatic ring and two or more N-substituted maleimide groups; and

[0016] (B) A phosphoric acid ester compound having two or more phosphorus atoms, wherein a group connecting at least two phosphorus atoms to each other includes two or more aromatic rings.

[0017] [2] The resin composition according to [1] above, wherein the group containing a condensed ring of an aromatic ring and an aliphatic ring contained in the component (A) is a group containing an indane ring as the condensed ring.

[0018] [3] The resin composition according to [2] above, wherein the group containing an indane ring is a divalent group represented by the following general formula (A-1).

[0019] [Chemical formula 1]

[0020]

[0021] (Where R A1 It is an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a hydroxyl group or a mercapto group. A1 is an integer from 0 to 3. A2 ~R A4 Each independently represents an alkyl group having 1 to 10 carbon atoms. * represents a bonding site. )

[0022] [4] The resin composition according to any one of [1] to [3], wherein the component (B) is a compound represented by the following general formula (B-1).

[0023] [Chemical formula 2]

[0024]

[0025] (Where R B1 ~R B4 Each independently represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. B1 It is a divalent group containing two or more aromatic rings. B1 ~n B4 Each independently represents an integer from 0 to 5, and n B5 is an integer from 1 to 5.)

[0026] [5] The resin composition according to any one of [1] to [4], wherein the content of the component (B) is 0.1 to 10 parts by mass relative to the total amount (100 parts by mass) of the resin components in the resin composition.

[0027] [6] The resin composition according to any one of [1] to [5], further comprising (C) a compound having two or more functional groups containing ethylenically unsaturated bonds.

[0028] [7] A prepreg comprising the resin composition according to any one of [1] to [6] above or a semi-cured product of the resin composition.

[0029] [8] A laminate comprising a cured product of the resin composition according to any one of [1] to [6] above and a metal foil.

[0030] [9] A resin film comprising the resin composition according to any one of [1] to [6] above or a semi-cured product of the resin composition.

[0031]

[10] A printed wiring board comprising a cured product of the resin composition according to any one of [1] to [6].

[0032]

[11] A semiconductor package comprising the printed wiring board described in

[10] above and a semiconductor element.

[0033] Effects of the Invention

[0034] According to the present embodiment, a resin composition having a low minimum melt viscosity even though a maleimide resin is used as a thermosetting resin, and a prepreg, a laminate, a resin film, a printed wiring board, and a semiconductor package using the resin composition can be provided. DETAILED DESCRIPTION

[0035] In the present specification, a numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the minimum value and the maximum value, respectively.

[0036] For example, a numerical range such as "X to Y" (X, Y are real numbers) refers to a numerical range greater than X and less than Y. Also, a description such as "greater than X" in this specification refers to X and a numerical value greater than X. In addition, a description such as "less than Y" in this specification refers to Y and a numerical value less than Y.

[0037] The lower limit and upper limit of the numerical range described in the present specification may be arbitrarily combined with the lower limit or upper limit of other numerical ranges, respectively.

[0038] In the numerical range described in the present specification, the lower limit value or the upper limit value of the numerical range may be replaced with the value shown in the Examples.

[0039] Unless otherwise specified, each component and material exemplified in the present specification may be used alone or in combination of two or more.

[0040] In this specification, when a plurality of substances corresponding to each component are present in the resin composition, the content of each component in the resin composition refers to the total amount of the plurality of substances present in the resin composition unless otherwise specified.

[0041] In this specification, "solid content" refers to components other than solvents, and also includes substances that are liquid, syrupy, and waxy at room temperature. Here, in this specification, room temperature refers to 25°C.

[0042] The number average molecular weight (Mn) and weight average molecular weight (Mw) in this specification refer to the values ​​measured by gel permeation chromatography (GPC) and converted to polystyrene. Specifically, the number average molecular weight (Mn) and weight average molecular weight (Mw) in this specification can be measured by the method described in the Examples.

[0043] The "semi-cured product" in this specification has the same meaning as the resin composition in a B-stage state in JIS K 6800 (1985), and the "cured product" has the same meaning as the resin composition in a C-stage state in JIS K 6800 (1985).

[0044] The mechanism of action described in this specification is a speculation and does not limit the mechanism by which the effects of the present embodiment are achieved.

[0045] Arbitrary combinations of the matters described in this specification are also included in this embodiment.

[0046] [Resin composition]

[0047] The resin composition of this embodiment contains:

[0048] (A) at least one selected from a maleimide resin and a derivative of the maleimide resin, wherein the maleimide resin has a group including a condensed ring of an aromatic ring and an aliphatic ring and two or more N-substituted maleimide groups,

[0049] (B) A phosphoric acid ester compound having two or more phosphorus atoms, wherein a group connecting at least two phosphorus atoms to each other includes two or more aromatic rings (hereinafter, also referred to as "(B) phosphoric acid ester compound").

[0050] In addition, in this specification, each component may be abbreviated as (A) component, (B) component, etc., and the same abbreviation may be used for other components.

[0051] Hereinafter, each component which the resin composition of this embodiment may contain is demonstrated sequentially.

[0052] <(A)Component>

[0053] The component (A) is at least one selected from a maleimide resin and a derivative of the maleimide resin, wherein the maleimide resin has a group including a condensed ring of an aromatic ring and an aliphatic ring and two or more N-substituted maleimide groups.

[0054] (A) The component may be used alone or in combination of two or more.

[0055] From the viewpoints of dielectric properties, conductor adhesion and heat resistance, component (A) is preferably an aromatic maleimide resin having a group including a condensed ring of an aromatic ring and an aliphatic ring, and two or more N-substituted maleimide groups directly bonded to the aromatic ring, and more preferably an aromatic bismaleimide resin having a group including a condensed ring of an aromatic ring and an aliphatic ring, and two N-substituted maleimide groups directly bonded to the aromatic ring.

[0056] From the viewpoint of dielectric properties, conductor adhesion and ease of manufacture, the group containing a condensed ring of an aromatic ring and an aliphatic ring contained in the component (A) is preferably a group containing a condensed bicyclic structure as a condensed ring, more preferably a group containing a condensed ring of a benzene ring and an aliphatic ring, and further preferably a group containing an indane ring. That is, the component (A) is preferably a maleimide resin containing a group containing an indane ring and two or more N-substituted maleimide groups.

[0057] The group containing an indane ring is preferably a divalent group represented by the following general formula (A-1).

[0058] [Chemical formula 3]

[0059]

[0060] (Where R A1 It is an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a hydroxyl group or a mercapto group. A1 is an integer from 0 to 3. A2 ~R A4 Each independently represents an alkyl group having 1 to 10 carbon atoms. * represents a bonding site. )

[0061] As R in the above general formula (A-1) A1 Examples of the alkyl group having 1 to 10 carbon atoms include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, etc. These alkyl groups may be linear or branched.

[0062] As R A1 Examples of the alkyl group contained in the alkoxy group having 1 to 10 carbon atoms and the alkylthio group having 1 to 10 carbon atoms shown in the above-mentioned group include the same alkyl groups as those described above for the alkyl group having 1 to 10 carbon atoms.

[0063] As R A1 Examples of the aryl group having 6 to 10 carbon atoms include phenyl and naphthyl.

[0064] As R A1 Examples of the aryl group contained in the aryloxy group having 6 to 10 carbon atoms and the arylthio group having 6 to 10 carbon atoms shown in the above-mentioned example include the same aryl groups as those described above for the aryl group having 6 to 10 carbon atoms.

[0065] As R A1 Examples of the cycloalkyl group having 3 to 10 carbon atoms include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl and cyclodecyl.

[0066] In the above general formula (A-1), n A1 When R is an integer of 1 to 3, from the viewpoint of solvent solubility and reactivity, A1 An alkyl group having 1 to 4 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms is preferred, and an alkyl group having 1 to 4 carbon atoms is more preferred.

[0067] As R A2 ~R A4 The alkyl group having 1 to 10 carbon atoms shown in , for example, methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, etc. These alkyl groups may be straight chain or branched. A2 ~R A4 An alkyl group having 1 to 4 carbon atoms is preferred, a methyl group and an ethyl group are more preferred, and a methyl group is further preferred.

[0068] In the above general formula (A-1), n A1 is an integer from 0 to 3, where n A1 If the value is 2 or 3, multiple R A1 They can be the same or different from each other.

[0069] Among the above, from the viewpoint of ease of production, the divalent group represented by the general formula (A-1) is preferably nA1 0, R A2 ~R A4 The divalent group represented by the following formula (A-1a) which is a methyl group is more preferably a divalent group represented by the following formula (A-1a′) or a divalent group represented by the following formula (A-1a″).

[0070] [Chemical formula 4]

[0071]

[0072] (Wherein, * indicates the bonding site.)

[0073] As the component (A) containing a divalent group represented by the general formula (A-1), a component represented by the following general formula (A-2) is preferred from the viewpoints of dielectric properties, conductor adhesion, heat resistance and ease of production.

[0074] [Chemical formula 5]

[0075]

[0076] (Where R A1 ~R A4 and n A1 and R in the above general formula (A-1) A1 ~R A4 and n A1 Same. A5 Each is independently an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a nitro group, a hydroxyl group or a mercapto group. A2 Each independently represents an integer from 0 to 4. A3 A number between 0.95 and 10.0.)

[0077] In the above general formula (A-2), a plurality of R A1 Each other, multiple n A1 Each other, multiple R A5 Each other, multiple n A2 They may be the same as or different from each other.

[0078] In n A3 If more than 1, multiple R A2 Each other, multiple R A3 Each other and multiple R A4 They may be the same as or different from each other.

[0079] As R in the above general formula (A-2) A5Examples of the alkyl group having 1 to 10 carbon atoms include methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, etc. These alkyl groups may be linear or branched.

[0080] As R A5 Examples of the alkyl group contained in the alkoxy group having 1 to 10 carbon atoms and the alkylthio group having 1 to 10 carbon atoms shown in the above-mentioned group include the same alkyl groups as those described above for the alkyl group having 1 to 10 carbon atoms.

[0081] As R A5 Examples of the aryl group having 6 to 10 carbon atoms include phenyl and naphthyl.

[0082] As R A5 Examples of the aryl group contained in the aryloxy group having 6 to 10 carbon atoms and the arylthio group having 6 to 10 carbon atoms shown in the above-mentioned example include the same aryl groups as those described above for the aryl group having 6 to 10 carbon atoms.

[0083] As R A5 Examples of the cycloalkyl group having 3 to 10 carbon atoms include cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl and cyclodecyl.

[0084] Among them, from the viewpoint of solvent solubility and ease of production, R A5 An alkyl group having 1 to 4 carbon atoms, a cycloalkyl group having 3 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms is preferred, an alkyl group having 1 to 3 carbon atoms is more preferred, and a methyl group is further preferred.

[0085] In the above general formula (A-2), n A2 It is an integer of 0 to 4, and is preferably an integer of 1 to 3, more preferably 2 or 3, and even more preferably 2, from the viewpoint of compatibility with other resins, dielectric properties, conductor adhesion, and ease of production.

[0086] It should be noted that by making n A2 When n is 1 or more, the benzene ring and the N-substituted maleimide group have a distorted conformation, and the intermolecular stacking is suppressed, thereby tending to further improve the solvent solubility. A2 When R is greater than 1, A5 The substitution position of is preferably the ortho position relative to the substitution position of the N-substituted maleimide group.

[0087] From the viewpoints of dielectric properties, conductor adhesion, solvent solubility, handling properties, and heat resistance, n in the general formula (A-2) is A3 It is preferably a number of 0.98 to 8.0, more preferably a number of 1.0 to 7.0, and still more preferably a number of 1.1 to 6.0.A3 The average value of the number of structures containing indane rings is shown.

[0088] From the viewpoints of dielectric properties, conductor adhesion, solvent solubility and ease of production, the component (A) represented by the general formula (A-2) is more preferably a component represented by the following general formula (A-3) or a component represented by the following general formula (A-4).

[0089] [Chemical formula 6]

[0090]

[0091] (Where R A1 ~R A5 and n A1 and n A3 and R in the above general formula (A-2) A1 ~R A5 and n A1 and n A3 same.)

[0092] [Chemical formula 7]

[0093]

[0094] (Where R A1 ~R A4 and n A1 and n A3 and R in the above general formula (A-2) A1 ~R A4 and n A1 and n A3 same.)

[0095] Examples of the component (A) represented by the general formula (A-3) include a maleimide resin represented by the following general formula (A-3-1).

[0096] [Chemical formula 8]

[0097]

[0098] (Where R A6 Each is independently methyl, ethyl or isopropyl. A3 and n in the above general formula (A-2) A3 same.)

[0099] The component (A) represented by the general formula (A-4) is more preferably a component represented by the following general formula (A-4-1) from the viewpoints of dielectric properties, conductor adhesion, solvent solubility, and ease of production.

[0100] [Chemical formula 9]

[0101]

[0102] (where n A3 and n in the above general formula (A-2) A3 same.)

[0103] As the derivative of the maleimide resin having a group including a condensed ring of an aromatic ring and an aliphatic ring and two or more N-substituted maleimide groups, for example, an aminomaleimide resin containing a structure derived from the maleimide resin exemplified as the component (A) and a structure derived from a diamine compound is preferred.

[0104] The aminomaleimide resin can be produced, for example, by subjecting the maleimide resin listed as the component (A) to a Michael addition reaction with a diamine compound.

[0105] Examples of the diamine compound include aromatic diamine compounds having two amino groups directly bonded to an aromatic ring, such as 4,4'-diaminodiphenylmethane, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-diethyl-4,4'-diaminodiphenylmethane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-[1,3-phenylenebis(1-methylethylidene)]dianiline, and 4,4'-[1,4-phenylenebis(1-methylethylidene)]dianiline; and organosilicon compounds having two primary amino groups.

[0106] The number average molecular weight (Mn) of the component (A) is not particularly limited, but is preferably 600 to 3000, more preferably 800 to 2000, and even more preferably 1000 to 1500 from the viewpoint of compatibility with other resins, conductor adhesion, and heat resistance.

[0107] The content of the component (A) in the resin composition of the present embodiment is not particularly limited, but is preferably 10 to 80% by mass, more preferably 30 to 75% by mass, and further preferably 50 to 70% by mass, relative to the total amount (100% by mass) of the resin components in the resin composition of the present embodiment.

[0108] If the content of component (A) is above the lower limit, heat resistance, formability, processability and conductor adhesion tend to be better. In addition, if the content of component (A) is below the upper limit, dielectric properties tend to be better.

[0109] <(A')Component>

[0110] The resin composition of the present embodiment may further contain (A′) other than the above-mentioned component (A) at least one selected from a maleimide resin having one or more N-substituted maleimide groups and a derivative of the maleimide resin.

[0111] As the component (A'), a maleimide resin represented by the following general formula (A'-1) is preferred.

[0112] [Chemical formula 10]

[0113]

[0114] (Where X Ad1 It is a divalent organic group that does not contain a fused ring of an aromatic ring and an aliphatic ring.)

[0115] X in the above general formula (A'-1) Ad1 It is a divalent organic group not containing a condensed ring of an aromatic ring and an aliphatic ring.

[0116] As X in the above general formula (A'-1) Ad1 The divalent organic group represented by the following general formula (A'-2) can be exemplified by a divalent group represented by the following general formula (A'-3) , a divalent group represented by the following general formula (A'-4) , a divalent group represented by the following general formula (A'-5) , a divalent group represented by the following general formula (A'-6) and the like.

[0117] [Chemical formula 11]

[0118]

[0119] (Where R Ad1 It is an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. Ad1 is an integer from 0 to 4. * indicates a bonding site. )

[0120] As R in the above general formula (A'-2) Ad1 The aliphatic hydrocarbon group having 1 to 5 carbon atoms shown in the formula (a) may include, for example, alkyl groups having 1 to 5 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, and n-pentyl; alkenyl groups having 2 to 5 carbon atoms; and alkynyl groups having 2 to 5 carbon atoms. The aliphatic hydrocarbon group having 1 to 5 carbon atoms may be straight-chain or branched.

[0121] Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.

[0122] In n Ad1 When the integer is 2 or more, multiple R Ad1 They can be the same or different from each other.

[0123] [Chemical formula 12]

[0124]

[0125] (Where R Ad2 and R Ad3 Each independently represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. Ad2 It is an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a thioether group, a sulfonyl group, a carbonyloxy group, a keto group, a single bond, or a divalent group represented by the following general formula (A'-3-1). Ad2 and n Ad3 Each independently represents an integer of 0 to 4. * represents a bonding site. )

[0126] In the above general formula (A'-3), R Ad2 and R Ad3 The aliphatic hydrocarbon group or halogen atom having 1 to 5 carbon atoms represented by the above general formula (A'-2) and R Ad1 The groups shown are explained in the same manner.

[0127] As X in the above general formula (A'-3) Ad2 Examples of the alkylene group having 1 to 5 carbon atoms include a methylene group, a 1,2-ethylene group, a 1,3-propylene group, a 1,4-butylene group, and a 1,5-pentylene group.

[0128] As X in the above general formula (A'-3) Ad2 Examples of the alkylidene group having 2 to 5 carbon atoms include ethylidene, propylidene, isopropylidene, butylidene, isobutylidene, pentylidene and isopentylidene.

[0129] In n Ad2 or Ad3 When the integer is 2 or more, multiple R Ad2 Each other or multiple R Ad3 They may be the same as or different from each other.

[0130] X in the above general formula (A'-3) Ad2 The divalent group represented by the general formula (A'-3-1) is as follows.

[0131] [Chemical formula 13]

[0132]

[0133] (Where R Ad4 and R Ad5 Each independently represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. Ad3It is an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a thioether group, a sulfonyl group, a carbonyloxy group, a keto group or a single bond. Ad4 and n Ad5 Each independently represents an integer of 0 to 4. * represents a bonding site. )

[0134] In the above general formula (A'-3-1), R Ad4 and R Ad5 The aliphatic hydrocarbon group or halogen atom having 1 to 5 carbon atoms represented by the above general formula (A'-2) and R Ad1 The groups shown are explained in the same manner.

[0135] X in the above general formula (A'-3-1) Ad3 The alkylene group having 1 to 5 carbon atoms and the alkylidene group having 2 to 5 carbon atoms and X in the above general formula (A'-3) Ad2 The groups shown are explained in the same manner.

[0136] In n Ad4 or Ad5 When the integer is 2 or more, multiple R Ad4 Each other or multiple R Ad5 They may be the same as or different from each other.

[0137] [Chemical formula 14]

[0138]

[0139] (where n Ad6 is an integer from 0 to 10. * indicates a bonding site. )

[0140] [Chemical formula 15]

[0141]

[0142] (where n Ad7 It is a number from 0 to 5. * indicates a bonding site. )

[0143] [Chemical formula 16]

[0144]

[0145] (Where R Ad6 and R Ad7 Each independently represents a hydrogen atom or an aliphatic hydrocarbon group having 1 to 5 carbon atoms. Ad8 is an integer from 1 to 8. * represents a bonding site. )

[0146] In the above general formula (A'-6), R Ad6 and R Ad7The aliphatic hydrocarbon group having 1 to 5 carbon atoms represented by Ad1 The groups shown are explained in the same manner.

[0147] In n Ad8 When the integer is 2 or more, multiple R Ad6 Each other or multiple R Ad7 They may be the same as or different from each other.

[0148] Examples of the component (A') include aromatic bismaleimide resins, aromatic polymaleimide resins, aliphatic maleimide resins, etc. Among them, the component (A') is preferably an aromatic polymaleimide resin, and more preferably a biphenyl aralkyl maleimide resin.

[0149] The derivative of the maleimide resin having one or more N-substituted maleimide groups as the component (A') is preferably an aminomaleimide resin containing a structure derived from the maleimide resin exemplified as the component (A') and a structure derived from a diamine compound.

[0150] The aminomaleimide resin can be produced, for example, by subjecting the maleimide resin listed as the component (A') to a Michael addition reaction with a diamine compound.

[0151] Examples of the diamine compound include the same diamine compounds as those mentioned as the raw material components of the derivative of the maleimide resin described as the (A) component, which has a group including a condensed ring of an aromatic ring and an aliphatic ring and two or more N-substituted maleimide groups.

[0152] When the components (A) and (A') are used in combination, the content of the component (A) is not particularly limited relative to 100% by mass of the total amount of the components (A) and (A'), but is preferably 20% by mass or more, more preferably 50% by mass or more, and even more preferably 70% by mass or more.

[0153] If the content of component (A) is above the above lower limit, there is a tendency to easily obtain a lower minimum melt viscosity. In addition, the upper limit of the content of component (A) may be 99% by mass or less, 90% by mass or less, 85% by mass or less, or 80% by mass or less, relative to 100% by mass of the total amount of component (A) and component (A').

[0154] The content of the component (A') is not particularly limited, but is preferably 5 to 80% by mass, more preferably 10 to 50% by mass, and further preferably 20 to 30% by mass, relative to 100% by mass of the total amount of the components (A) and (A').

[0155] When the content of the component (A') is within the above range, the characteristics of the components (A) and (A') tend to be more readily expressed.

[0156] (Total content of component (A) and component (A'))

[0157] In the resin composition of the present embodiment, the total content of component (A) and component (A') is not particularly limited, but is preferably 20 to 97% by mass, more preferably 50 to 95% by mass, and further preferably 70 to 90% by mass, relative to the total amount (100% by mass) of the resin components in the resin composition of the present embodiment.

[0158] If the total content of components (A) and (A') is above the above lower limit, the heat resistance, formability, processability and conductor adhesion tend to be better. In addition, if the total content of components (A) and (A') is below the above upper limit, the dielectric properties tend to be better.

[0159] Here, in this specification, the "resin component" refers to a resin and a compound that forms a resin by a curing reaction.

[0160] For example, in the resin composition of the present embodiment, the component (A), the component (A′), the component (C), and the component (D) correspond to the resin component.

[0161] When the resin composition of the present embodiment contains a resin or a compound that forms a resin by a curing reaction as an arbitrary component in addition to the above-mentioned components, these arbitrary components are also included in the resin component.

[0162] However, the components (B), (E) and (F) are not included in the resin component.

[0163] The content of the resin component in the resin composition of the present embodiment is not particularly limited, but is preferably 20 to 95% by mass, more preferably 40 to 92% by mass, and further preferably 70 to 90% by mass, relative to the total solid content (100% by mass) of the resin composition of the present embodiment.

[0164] If the content of the resin component is above the above lower limit, heat resistance, formability, processability and conductor adhesion tend to become better. In addition, if the content of the resin component is below the above upper limit, low thermal expansion tends to become better.

[0165] <(B) Phosphate ester compound>

[0166] (B) The phosphoric acid ester compound is a phosphoric acid ester compound having two or more phosphorus atoms, wherein a group connecting at least two phosphorus atoms to each other includes two or more aromatic rings.

[0167] (B) The phosphoric acid ester compound may be used alone or in combination of two or more.

[0168] The resin composition of the present embodiment contains the (B) phosphate ester compound, and thus has a low minimum melt viscosity even when a maleimide resin is used as a thermosetting resin.

[0169] The reason for this is not clear, but one possible reason is that the (B) phosphate compound captures free radicals present in the system when the resin composition is melted, thereby inhibiting the curing reaction of the (A) component.

[0170] The number of phosphorus atoms contained in the (B) phosphate ester compound is 2 or more, preferably 2 to 10, more preferably 2 to 5, and even more preferably 2 or 3.

[0171] Among the phosphorus atoms in the (B) phosphate ester compound, at least one phosphorus atom forms a phosphate ester bond, and preferably all the phosphorus atoms form a phosphate ester bond.

[0172] Here, in the present specification, "phosphate bond" refers to a bond represented by any one of the following formulas (B-3) to (B-5). Among them, it is preferred to form a phosphate bond represented by the following formula (B-5).

[0173] [Chemical formula 17]

[0174]

[0175] (In the formula, * is the site that bonds to the organic group.)

[0176] Examples of the organic group bonded to the phosphate ester bond include aliphatic hydrocarbon groups and aromatic hydrocarbon groups. Among them, aromatic hydrocarbon groups are preferred. That is, the (B) phosphate ester compound is preferably an aromatic phosphate ester compound.

[0177] Examples of the aromatic hydrocarbon group bonded to the phosphate ester bond include substituted or unsubstituted phenyl, substituted or unsubstituted naphthyl, etc. Examples of the substituent include hydrocarbon groups having 1 to 5 carbon atoms such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, and n-pentyl; and halogen atoms. Among them, unsubstituted phenyl or 2,5-dimethylphenyl is preferred.

[0178] In the component (B), the group linking two phosphorus atoms to each other includes two or more aromatic rings.

[0179] From the viewpoint of the minimum melt viscosity, the above-mentioned two or more aromatic rings preferably form: a divalent aromatic hydrocarbon group having a structure in which two or more aromatic rings are bonded by a single bond or a connecting group having less than 5 carbon atoms (hereinafter also referred to as "aromatic hydrocarbon group (Z1)"), or a divalent condensed polycyclic aromatic hydrocarbon group containing two or more aromatic rings (hereinafter also referred to as "aromatic hydrocarbon group (Z2)"), and more preferably form an aromatic hydrocarbon group (Z1).

[0180] (Aromatic hydrocarbon group (Z1))

[0181] Examples of the two or more aromatic rings contained in the aromatic hydrocarbon group (Z1) include a benzene ring, a naphthalene ring, an anthracene ring, and the like. Among them, a benzene ring is preferred.

[0182] Examples of the linking group having 5 or less carbon atoms that the aromatic hydrocarbon group (Z1) may contain include a divalent hydrocarbon group having 1 to 5 carbon atoms, a divalent heteroatom-containing group having 5 or less carbon atoms, and a divalent group having 1 to 5 carbon atoms formed by linking a hydrocarbon group and a heteroatom-containing group. It should be noted that "5 or less carbon atoms" herein also includes the case where the carbon number is 0.

[0183] Examples of the divalent hydrocarbon group having 1 to 5 carbon atoms include alkylidene groups having 1 to 5 carbon atoms such as methylene, 1,2-ethylene, 1,3-propylene, 1,4-butylene, and 1,5-pentylene; and alkylidene groups having 2 to 5 carbon atoms such as ethylidene, propylidene, isopropylidene, butylidene, isobutylidene, pentylidene, and isopentylidene. Examples of the divalent heteroatom-containing group having 5 or less carbon atoms include ether groups, thioether groups, sulfonyl groups, carbonyloxy groups, and keto groups.

[0184] From the viewpoint of the minimum melt viscosity, the aromatic hydrocarbon group (Z1) is preferably a divalent group represented by the following general formula (B-2).

[0185] [Chemical formula 18]

[0186]

[0187] (Where R B5 and R B6 Each independently represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. B2 It is an alkylene group having 1 to 5 carbon atoms, an alkylidene group having 2 to 5 carbon atoms, an ether group, a thioether group, a sulfonyl group, a carbonyloxy group, a keto group or a single bond. B6 and n B7 Each independently represents an integer from 0 to 4. B8 is an integer from 1 to 3. * indicates a bonding site. )

[0188] As X in the above general formula (B-2)B2 Examples of the alkylene group having 1 to 5 carbon atoms include a methylene group, a 1,2-ethylene group, a 1,3-propylene group, a 1,4-butylene group, and a 1,5-pentylene group.

[0189] As X B2 Examples of the alkylidene group having 2 to 5 carbon atoms include ethylidene, propylidene, isopropylidene, butylidene, isobutylidene, pentylidene and isopentylidene.

[0190] X B2 Among the groups shown, a methylene group, an isopropylidene group, and a single bond are preferred, and a single bond is more preferred.

[0191] As R in the above general formula (B-2) B5 and R B6 Examples of the aliphatic hydrocarbon group having 1 to 5 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl and n-pentyl.

[0192] In the above general formula (B-2), n B6 and n B7 It is preferably an integer of 0 to 3, more preferably 0 or 1, and even more preferably 0.

[0193] In n B6 or B7 When the integer is 2 or more, multiple R B5 Each other or multiple R B6 They may be the same as or different from each other.

[0194] In the above general formula (B-2), n B8 It is preferably 1 or 2, and more preferably 1.

[0195] In n B8 When X is an integer greater than 2, multiple B2 Each other and multiple n B7 They may be the same as or different from each other.

[0196] The divalent group represented by the general formula (B-2) is preferably a divalent group represented by the following formula (B-2-1) or a divalent group represented by the following formula (B-2-2), and more preferably a divalent group represented by the following formula (B-2-2).

[0197] [Chemical formula 19]

[0198]

[0199] (Wherein, * indicates the bonding site.)

[0200] (Aromatic hydrocarbon group (Z2))

[0201] Aromatic hydrocarbon group (Z2) is a divalent condensed polycyclic aromatic hydrocarbon group containing two or more aromatic rings. In the present embodiment, "condensed polycyclic aromatic hydrocarbon" refers to an aromatic hydrocarbon having two or more ring structures and having condensed rings with two or more rings having two or more atoms, for example, naphthalene, anthracene, pyrene, etc. Therefore, as aromatic hydrocarbon group (Z2), divalent groups formed by removing two hydrogen atoms from these condensed polycyclic aromatic hydrocarbons can be cited. These condensed polycyclic aromatic hydrocarbons may be substituted with substituents or may not be substituted. As substituents, substituents identical to the substituents that the aromatic rings contained in the aromatic hydrocarbon group (Z1) may have can be cited.

[0202] (B) The phosphoric acid ester compound is preferably a compound represented by the following general formula (B-1).

[0203] [Chemical formula 20]

[0204]

[0205] (Where R B1 ~R B4 Each independently represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom. B1 It is a divalent group containing two or more aromatic rings. B1 ~n B4 Each independently represents an integer from 0 to 5, and n B5 is an integer from 1 to 5.)

[0206] As R in the above general formula (B-1) B1 ~R B4 The aliphatic hydrocarbon group having 1 to 5 carbon atoms shown in the above formula (a) includes, for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, etc. As the aliphatic hydrocarbon group, an aliphatic hydrocarbon group having 1 to 3 carbon atoms is preferred, an alkyl group having 1 to 3 carbon atoms is more preferred, and a methyl group is further preferred.

[0207] In the above general formula (B-1), n B1 ~n B4 It is preferably 0 to 2, and more preferably 0 or 2. B1 ~n B4 When the integer is 2 or more, multiple R B1 Each other, R B2 Each other, R B3 Each other or R B4 They may be the same as or different from each other.

[0208] In the above general formula (B-1), n B5 represents an integer of 1 to 5, preferably an integer of 1 to 3, more preferably 1 or 2, and further preferably 1. B5When X is an integer greater than 2, multiple B1 Each other and multiple n B4 They may be the same as or different from each other.

[0209] As X in the above general formula (B-1) B1 The divalent group containing two or more aromatic rings shown in the formula (Z) may include the above-mentioned aromatic hydrocarbon group (Z1) and aromatic hydrocarbon group (Z2). B1 It is preferably an aromatic hydrocarbon group (Z1), more preferably a divalent group represented by the above-mentioned general formula (B-2), and still more preferably a divalent group represented by the above-mentioned formula (B-2-2).

[0210] Examples of the phosphate compound (B) include 4,4'-biphenol-diphenyl phosphate, bisphenol A-diphenyl phosphate, 4,4'-biphenol-xylyl phosphate, bisphenol A-xylyl phosphate, 4,4'-biphenol-di(2,6-xylyl phosphate), bisphenol A-di(2,6-xylyl phosphate), 4,4'-biphenol-polyphosphate, bisphenol A-polyphenyl phosphate, 4,4'-biphenol-polycresyl phosphate, bisphenol A-polycresyl phosphate, 4,4'-biphenol-poly(2,6-xylyl phosphate), and bisphenol A-poly(2,6-xylyl phosphate). Among them, 4,4'-biphenol-di(2,6-xylyl phosphate) is preferred.

[0211] It should be noted that the "poly" in the above-mentioned exemplary compounds refers to a repeating unit containing a structure derived from a divalent phenol compound constituting a phosphate ester compound and a structure derived from phosphoric acid (for example, the structure consisting of n B5 A compound having a number of structural units (i.e., a structural unit number indicating the number of structural units) of 2 or more may also refer to a compound in which the average value of the above-mentioned repeating units exceeds 1 due to the inclusion of this compound.

[0212] (B) Average particle size of the phosphate ester compound (D 50 ) is not particularly limited, but is preferably 0.1 to 10 μm, more preferably 0.3 to 5 μm, and still more preferably 0.5 to 3 μm from the viewpoint of dispersibility and handling properties.

[0213] Here, the average particle size (D 50 ) refers to the particle diameter corresponding to the point at which the volume accounts for 50% when the cumulative frequency distribution curve based on the particle diameter is obtained, with the total volume of the particles being 100%.

[0214] ((B) Content of Phosphate Ester Compound)

[0215] In the resin composition of the present embodiment, the content of the (B) phosphate compound is not particularly limited, but is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 7 parts by mass, and further preferably 0.3 to 4 parts by mass, relative to the total amount (100 parts by mass) of the resin components in the resin composition of the present embodiment.

[0216] When the content of the (B) phosphate ester compound is at least the above lower limit, the minimum melt viscosity tends to be better. When the content of the (B) phosphate ester compound is at most the above upper limit, the conductor adhesion tends to be better.

[0217] <(C) Compound having two or more ethylenically unsaturated bond-containing functional groups>

[0218] The resin composition of the present embodiment preferably further contains (C) a compound having two or more ethylenically unsaturated bond-containing functional groups.

[0219] There is a tendency that more excellent dielectric properties are easily obtained by the resin composition of the present embodiment containing the component (C).

[0220] It should be noted that, in the present specification, the "ethylenically unsaturated bond" refers to a carbon-carbon double bond capable of an addition reaction, and does not include a double bond of an aromatic ring.

[0221] Hereinafter, a functional group containing an ethylenically unsaturated bond may be referred to as an "ethylenically unsaturated group".

[0222] Examples of the ethylenically unsaturated group include a vinyl group, an allyl group, a 1-methallyl group, an isopropenyl group, a 2-butenyl group, a 3-butenyl group, a styryl group, a maleimide group, and a (meth)acryloyl group.

[0223] (C) The component may be used alone or in combination of two or more.

[0224] From the viewpoint of obtaining more excellent dielectric properties, the component (C) is preferably a polymer having two or more functional groups containing an ethylenically unsaturated bond.

[0225] Examples of polymers having two or more functional groups containing ethylenically unsaturated bonds include: (C1) a conjugated diene polymer having two or more ethylenically unsaturated groups (hereinafter, also simply referred to as "(C1) conjugated diene polymer"); (C2) a modified conjugated diene polymer having two or more ethylenically unsaturated groups (hereinafter, also simply referred to as "(C2) modified conjugated diene polymer"); (C3) a polyphenylene ether having two or more ethylenically unsaturated groups (hereinafter, also simply referred to as "(C3) modified polyphenylene ether"); and the like.

[0226] In addition, in this specification, "conjugated diene polymer" means a polymer of a conjugated diene compound.

[0227] Hereinafter, components (C1) to (C3) will be described.

[0228] ((C1) conjugated diene polymer)

[0229] The (C1) conjugated diene polymer is a conjugated diene polymer having two or more ethylenically unsaturated groups.

[0230] The (C1) conjugated diene polymer preferably has a vinyl group as an ethylenically unsaturated group in a side chain from the viewpoint of compatibility with other resins and dielectric properties.

[0231] The number of side chain vinyl groups in one molecule of the (C1) conjugated diene polymer is not particularly limited. From the viewpoint of compatibility with other resins and dielectric properties, it is preferably 2 or more, more preferably 5 or more, and further preferably 10 or more. It may be 100 or less, 80 or less, or even 60 or less.

[0232] As (C1) conjugated diene polymer, for example, polybutadiene having 1,2-vinyl group, butadiene-styrene copolymer having 1,2-vinyl group, polyisoprene having 1,2-vinyl group, etc. can be mentioned. Among them, polybutadiene having 1,2-vinyl group is preferred from the viewpoint of dielectric properties and heat resistance. In addition, as polybutadiene having 1,2-vinyl group, polybutadiene homopolymer having 1,2-vinyl group is preferred.

[0233] The 1,2-vinyl group derived from butadiene in the conjugated diene polymer (C1) refers to a vinyl group contained in the structural unit derived from 1,3-butadiene represented by the following formula (C1-1).

[0234] [Chemical formula 21]

[0235]

[0236] In the case where the (C1) conjugated diene polymer is a polybutadiene having 1,2-vinyl, the content of the structural unit having 1,2-vinyl relative to all structural units of butadiene constituting the polybutadiene (hereinafter, also referred to as "vinyl content") is not particularly limited, and is preferably 50 mol% or more, more preferably 70 mol% or more, and further preferably 85 mol% or more from the viewpoint of compatibility with other resins, dielectric properties and heat resistance. In addition, the upper limit of the vinyl content is not particularly limited, and may be 100 mol% or less, 95 mol% or less, or 90 mol% or less.

[0237] The number average molecular weight (Mn) of the conjugated diene polymer (C1) is not particularly limited, but is preferably 400 to 3,000, more preferably 600 to 2,000, and even more preferably 800 to 1,500 from the viewpoint of compatibility with other resins, dielectric properties, and heat resistance.

[0238] ((C2) Modified conjugated diene polymer)

[0239] (C2) The modified conjugated diene polymer is a modified conjugated diene polymer having two or more ethylenically unsaturated groups.

[0240] The (C2) modified conjugated diene polymer is preferably a polymer obtained by modifying the (C1) conjugated diene polymer with a maleimide resin having two or more N-substituted maleimide groups (hereinafter, also simply referred to as “maleimide resin”).

[0241] The (C1) conjugated diene polymer as a raw material of the (C2) modified conjugated diene polymer is preferably a conjugated diene polymer having a vinyl group in a side chain.

[0242] As the maleimide resin as a raw material of the (C2) modified conjugated diene polymer, those exemplified as the (A) component and the (A′) component can be used, and preferred embodiments are also the same.

[0243] The (C2) modified conjugated diene polymer preferably has a substituent in the side chain: a substituent formed by the reaction of a side chain vinyl group possessed by a conjugated diene polymer having a vinyl group in the side chain with an N-substituted maleimide group possessed by a maleimide resin [hereinafter sometimes referred to as a "substituent derived from a maleimide resin"]. More preferably, it has a substituent derived from a maleimide resin and a vinyl group in the side chain.

[0244] From the viewpoint of compatibility with other resins, dielectric properties, low thermal expansion and heat resistance, the substituent derived from the maleimide resin is preferably a group including a structure represented by the following general formula (C2-1) or (C2-2) as a structure derived from the maleimide resin.

[0245] [Chemical formula 22]

[0246]

[0247] (Where X C1 A divalent group formed by removing two N-substituted maleimide groups from a maleimide resin. C1 This is the site that bonds to the carbon atom derived from the side chain vinyl group of a conjugated diene polymer having a side chain vinyl group.* C2 The site where atoms bond to other atoms.)

[0248] The number average molecular weight (Mn) of the modified conjugated diene polymer (C2) is not particularly limited, but is preferably 700 to 6,000, more preferably 800 to 5,000, and even more preferably 1,000 to 2,500.

[0249] The reaction conditions of the conjugated diene polymer (C1) and the maleimide resin are not particularly limited. For example, the raw materials and the organic solvent are placed in a reaction vessel and reacted with heating and stirring as necessary to obtain the modified conjugated diene polymer (C2).

[0250] When the reaction is carried out, the molar number (M) of the N-substituted maleimide group of the maleimide resin is m ) relative to the molar number of the side chain vinyl groups of the conjugated diene polymer having the side chain vinyl groups (M v ) ratio (M m / M v ) is not particularly limited, but is preferably 0.001 to 0.5, more preferably 0.005 to 0.1, and further preferably 0.008 to 0.05, from the viewpoint of compatibility of the obtained (C2) modified conjugated diene polymer with other resins and suppression of gelation of the product during the reaction.

[0251] ((C3) Modified polyphenylene ether)

[0252] (C3) The modified polyphenylene ether is a polyphenylene ether having two or more ethylenically unsaturated groups.

[0253] The modified polyphenylene ether (C3) is not particularly limited, but preferably has a structural unit represented by the following general formula (C3-1).

[0254] [Chemical formula 23]

[0255]

[0256] The ethylenically unsaturated group contained in the (C3) modified polyphenylene ether is preferably a (meth)acryloyl group, and more preferably a methacryloyl group.

[0257] The number of ethylenically unsaturated groups in the (C3) modified polyphenylene ether is not particularly limited, but is preferably 1 to 5, more preferably 2 to 3, and even more preferably 2, from the viewpoint of heat resistance and fluidity.

[0258] The (C3) modified polyphenylene ether preferably has an ethylenically unsaturated group at at least one terminal, more preferably has an ethylenically unsaturated group at both terminals, and further preferably has an ethylenically unsaturated group only at both terminals.

[0259] The weight average molecular weight (Mw) of the modified polyphenylene ether (C3) is not particularly limited, but is preferably 500 to 7,000, more preferably 800 to 5,000, further preferably 1,000 to 3,000, and particularly preferably 1,200 to 2,500.

[0260] (Content of component (C))

[0261] In the resin composition of the present embodiment, the content of the component (C) is not particularly limited, but is preferably 1 to 50% by mass, more preferably 5 to 30% by mass, and further preferably 8 to 20% by mass, relative to the total amount (100% by mass) of the resin components in the resin composition of the present embodiment.

[0262] If the content of the component (C) is above the lower limit, the dielectric properties tend to be better. If the content of the component (C) is below the upper limit, the heat resistance, formability, processability and conductor adhesion tend to be better.

[0263] <(D) Styrene-based thermoplastic resin>

[0264] The resin composition of the present embodiment preferably further contains (D) a styrene-based thermoplastic resin.

[0265] The resin composition of the present embodiment tends to easily obtain more excellent dielectric properties by containing the (D) styrene-based thermoplastic resin.

[0266] (D) The styrene-based thermoplastic resin may be used alone or in combination of two or more.

[0267] (D) Styrene-based thermoplastic resin has a structural unit derived from a styrene-based compound. Examples of styrene-based compounds include styrene, alkyl-substituted styrenes such as α-methylstyrene, o-methylstyrene, m-methylstyrene, and p-methylstyrene. The number of carbon atoms in the alkyl group of the alkyl-substituted styrene is not particularly limited, but is preferably 1 to 5, more preferably 1 to 3, and even more preferably 1 or 2.

[0268] In the (D) styrene-based thermoplastic resin, the content of the structural unit derived from the styrene-based compound [hereinafter sometimes referred to as "styrene content"] is not particularly limited, but is preferably 5 to 60% by mass, more preferably 7 to 40% by mass, and further preferably 10 to 20% by mass from the viewpoint of dielectric properties, conductor adhesion, heat resistance, glass transition temperature and low thermal expansion.

[0269] Examples of the structural unit other than the structural unit derived from the styrene-based compound that the (D) styrene-based thermoplastic resin has include a structural unit derived from butadiene, a structural unit derived from isoprene, a structural unit derived from maleic acid, and a structural unit derived from maleic anhydride.

[0270] (D) Styrene-based thermoplastic resins include, for example, hydrogenated styrene-butadiene-styrene block copolymers (SEBS, SBBS), hydrogenated styrene-isoprene-styrene block copolymers (SEPS), and styrene-maleic anhydride copolymers (SMA). Among them, hydrogenated styrene-butadiene-styrene block copolymers (SEBS) are preferred.

[0271] (D) The number average molecular weight (Mn) of the styrene-based thermoplastic resin is not particularly limited, but is preferably 10,000 to 500,000, more preferably 50,000 to 350,000, and even more preferably 100,000 to 200,000.

[0272] ((D) Content of Styrene-Based Thermoplastic Resin)

[0273] In the resin composition of the present embodiment, the content of (D) styrene-based thermoplastic resin is not particularly limited, but is preferably 1 to 50% by mass, more preferably 5 to 30% by mass, and further preferably 8 to 20% by mass, relative to the total amount (100% by mass) of the resin components in the resin composition of the present embodiment.

[0274] If the content of the (D) styrene-based thermoplastic resin is above the above lower limit, the dielectric properties tend to be better. In addition, if the content of the (D) styrene-based thermoplastic resin is below the above upper limit, the heat resistance, formability, processability and conductor adhesion tend to be better.

[0275] <(E) Inorganic fillers>

[0276] The resin composition of the present embodiment preferably further contains (E) an inorganic filler.

[0277] The resin composition of the present embodiment tends to easily obtain more excellent low thermal expansion property and heat resistance by containing the (E) inorganic filler.

[0278] (E) The inorganic filler may be used alone or in combination of two or more.

[0279] (E) Inorganic fillers include, for example, silica, alumina, titanium oxide, mica, beryllium oxide, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay, talc, aluminum borate, silicon carbide, etc. Among them, from the viewpoint of low thermal expansion, heat resistance and flame retardancy, silica, alumina, mica and talc are preferred, silica and alumina are more preferred, and silica is further preferred.

[0280] Examples of silica include crushed silica, fumed silica, and fused silica. Among them, fused silica is preferred from the viewpoint of dispersibility and moldability.

[0281] Examples of the shape of the (E) inorganic filler include spherical shapes and crushed shapes, and a spherical shape is preferred.

[0282] (E) The inorganic filler may be an inorganic filler surface-treated with a coupling agent such as a silane coupling agent, for example.

[0283] (E) Average particle size of inorganic filler (D 50 ) is not particularly limited, but from the viewpoint of the dispersibility and fine wiring properties of the (E) inorganic filler, it is preferably 0.01 to 20 μm, more preferably 0.1 to 10 μm, further preferably 0.2 to 1 μm, and particularly preferably 0.3 to 0.8 μm.

[0284] ((E) Content of inorganic filler)

[0285] When the resin composition of the present embodiment contains (E) an inorganic filler, the content of the (E) inorganic filler in the resin composition of the present embodiment is not particularly limited, and is preferably 5 to 80% by mass, more preferably 7 to 50% by mass, and further preferably 10 to 30% by mass, relative to the total solid content (100% by mass) of the resin composition.

[0286] If the content of the (E) inorganic filler is above the above lower limit, low thermal expansion and heat resistance tend to be better. In addition, if the content of the (E) inorganic filler is below the above upper limit, formability and conductor adhesion tend to be better.

[0287] <(F) Curing accelerator>

[0288] The resin composition of the present embodiment preferably further contains (F) a curing accelerator.

[0289] The resin composition of the present embodiment contains the (F) curing accelerator, whereby curability is improved, and there is a tendency that more excellent dielectric properties, heat resistance, and conductor adhesion are easily obtained.

[0290] (F) The curing accelerator may be used alone or in combination of two or more.

[0291] Examples of the curing accelerator (F) include acidic catalysts such as p-toluenesulfonic acid; amine compounds such as triethylamine, tributylamine, pyridine, and dicyandiamide; imidazole compounds such as methylimidazole, phenylimidazole, 1-cyanoethyl-2-phenylimidazole, and 1-cyanoethyl-2-phenyltrimellitate imidazole; isocyanate-masked imidazoles such as an addition reaction product of hexamethylene diisocyanate resin and 2-ethyl-4-methylimidazole; tert-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, tert-butylperoxyisopropyl monocarbonate, α,α'-bis(tert-butylperoxy)diisopropylbenzene, carboxylates of manganese, cobalt, zinc, etc. Among them, imidazole compounds and organic peroxides are preferred.

[0292] ((F) Content of curing accelerator)

[0293] When the resin composition of the present embodiment contains (F) a curing accelerator, the content of the (F) curing accelerator is not particularly limited, and is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 7 parts by mass, and further preferably 0.5 to 5 parts by mass, relative to the total amount (100 parts by mass) of the resin components in the resin composition of the present embodiment.

[0294] When the content of the curing accelerator (F) is at least the above lower limit, a sufficient curing acceleration effect tends to be easily obtained. On the other hand, when the content of the curing accelerator (F) is at most the above upper limit, storage stability tends to be more favorable.

[0295] <Other ingredients>

[0296] The resin combination of the present embodiment may further contain as required: one or more of the resin material, antioxidant, heat stabilizer, antistatic agent, ultraviolet absorber, pigment, colorant, lubricant, flame retardant, organic solvent and additives other than the above-mentioned components. They can each be used alone or in combination of two or more. In addition, their usage is not particularly limited, and can be used as required within the scope of not hindering the effect of the present embodiment.

[0297] (Organic Solvent)

[0298] The resin composition of the present embodiment may contain an organic solvent from the viewpoint of easy handling and easy production of a prepreg described later.

[0299] The organic solvent may be used alone or in combination of two or more.

[0300] In addition, in this specification, the resin composition containing an organic solvent may be referred to as a resin varnish.

[0301] Examples of the organic solvent include alcohol solvents such as ethanol, propanol, butanol, methyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ether solvents such as tetrahydrofuran; aromatic hydrocarbon solvents such as toluene, xylene, and mesitylene; nitrogen atom-containing solvents such as dimethylformamide, dimethylacetamide, and N-methylpyrrolidone; sulfur atom-containing solvents such as dimethyl sulfoxide; ester solvents such as γ-butyrolactone, and the like.

[0302] Among them, alcohol solvents, ketone solvents, nitrogen atom-containing solvents, and aromatic hydrocarbon solvents are preferred from the viewpoint of solubility, aromatic hydrocarbon solvents are more preferred, and toluene is further preferred.

[0303] <Method for producing resin composition>

[0304] The resin composition of the present embodiment can be produced by mixing the above-mentioned components.

[0305] When mixing the components, the components may be dissolved or dispersed while being stirred. In addition, the order of mixing the raw materials, the mixing temperature, the mixing time and other conditions are not particularly limited and may be arbitrarily set according to the types of raw materials.

[0306] [Prepreg]

[0307] The prepreg of the present embodiment is a prepreg containing the resin composition of the present embodiment or a semi-cured product of the resin composition.

[0308] The prepreg of the present embodiment contains, for example, the resin composition of the present embodiment or a semi-cured product of the resin composition, and a sheet-like fiber base material.

[0309] As the sheet-like fiber base material contained in the prepreg of the present embodiment, for example, a known sheet-like fiber base material used in various laminated plates for electrical insulating materials can be used.

[0310] Examples of the material of the sheet-like fiber substrate include inorganic fibers such as E glass, D glass, S glass, and Q glass; organic fibers such as polyimide, polyester, and tetrafluoroethylene; and mixtures thereof. These sheet-like fiber substrates have shapes such as woven fabrics, nonwoven fabrics, rovings, chopped strand mats, and surface mats.

[0311] The prepreg of the present embodiment can be produced, for example, by impregnating or applying the resin composition of the present embodiment to a sheet-like fiber base material, and then heating and drying the sheet-like fiber base material to bring the sheet-like fiber base material to a B-stage.

[0312] The temperature and time of heat drying are not particularly limited, and can be, for example, 50 to 200° C. and 1 to 30 minutes from the viewpoint of productivity and appropriately bringing the resin composition of the present embodiment to a B-stage.

[0313] The solid content concentration derived from the resin composition in the prepreg of the present embodiment is not particularly limited, but is preferably 20 to 90% by mass, more preferably 25 to 80% by mass, and still more preferably 30 to 75% by mass, from the viewpoint of obtaining better formability when forming a laminate.

[0314] [Resin film]

[0315] The resin film of the present embodiment is a resin film containing the resin composition of the present embodiment or a semi-cured product of the resin composition.

[0316] The resin film of the present embodiment can be produced by, for example, applying the resin composition of the present embodiment containing an organic solvent, that is, a resin varnish, to a support, and then heating and drying the coating.

[0317] Examples of the support include plastic films, metal foils, and release papers.

[0318] The temperature and time of heat drying are not particularly limited, but can be set to 50 to 200° C. and 1 to 30 minutes from the viewpoint of productivity and appropriately bringing the resin composition of the present embodiment to a B-stage.

[0319] The resin film of the present embodiment is preferably used to form an insulating layer when a printed wiring board is produced.

[0320] [Laminated board]

[0321] The laminated plate of the present embodiment is a laminated plate including a cured product of the resin composition of the present embodiment and a metal foil.

[0322] In addition, the laminated plate having a metal foil is sometimes also referred to as a metal-clad laminated plate.

[0323] The metal of the metal foil is not particularly limited, and examples thereof include copper, gold, silver, nickel, platinum, molybdenum, ruthenium, aluminum, tungsten, iron, titanium, chromium, and alloys containing one or more of these metal elements.

[0324] The laminated plate of the present embodiment can be produced, for example, by placing a metal foil on one or both surfaces of the prepreg of the present embodiment and then performing heat and pressure molding.

[0325] Usually, the prepreg after B-stage is cured by this heat and pressure molding, thereby obtaining the laminated plate of the present embodiment.

[0326] In the case of heat and pressure molding, only one prepreg may be used, or two or more prepregs may be stacked and used.

[0327] For the heat and pressure molding, for example, a multi-stage press, a multi-stage vacuum press, a continuous molding machine, an autoclave molding machine, etc. can be used.

[0328] The conditions for the heat-press molding are not particularly limited, and for example, the conditions may be a temperature of 100 to 300° C., a time of 10 to 300 minutes, and a pressure of 1.5 to 5 MPa.

[0329] [Printed wiring board]

[0330] The printed wiring board of the present embodiment is a printed wiring board having a cured product of the resin composition of the present embodiment.

[0331] The printed wiring board of the present embodiment can be manufactured by, for example, forming a conductor circuit on one or more of the cured product of the prepreg of the present embodiment, the cured product of the resin film of the present embodiment, and the laminate using a known method. In addition, by further performing a multilayer bonding process as required, a multilayer printed wiring board can also be manufactured. The conductor circuit can be formed by, for example, appropriately performing a hole opening process, a metal plating process, an etching of a metal foil, etc.

[0332] [Semiconductor package]

[0333] The semiconductor package of the present embodiment includes the printed wiring board of the present embodiment and a semiconductor element.

[0334] The semiconductor package of the present embodiment can be manufactured by, for example, mounting a semiconductor chip, a memory, and the like on a printed wiring board of the present embodiment by a known method.

[0335] Example

[0336] Hereinafter, the present embodiment will be described in detail with reference to examples, but the present embodiment is not limited to the following examples.

[0337] In addition, in each example, the number average molecular weight (Mn) and the weight average molecular weight (Mw) were measured by the following method.

[0338] The conversion was performed by gel permeation chromatography (GPC) based on a calibration curve using standard polystyrene. The calibration curve used standard polystyrene: TSK standard POLYSTYRENE (models; A-2500, A-5000, F-1, F-2, F-4, F-10, F-20, F-40) [manufactured by Tosoh Corporation, trade name], and was approximated by a cubic equation. The measurement conditions of GPC are shown below.

[0339] Device:

[0340] Pump: L-6200 model [manufactured by Hitachi High-Technologies Co., Ltd.]

[0341] Detector: L-3300 RI [manufactured by Hitachi High-Technologies Co., Ltd.]

[0342] Column oven: L-655A-52 [manufactured by Hitachi High-Technologies Co., Ltd.]

[0343] Column: Guard column; TSK Guardcolumn HHR-L + column; TSKgel G4000HHR + TSKgel G2000HHR (all manufactured by Tosoh Corporation, trade names)

[0344] Column size: 6.0×40mm (guard column), 7.8×300mm (column)

[0345] Eluent: Tetrahydrofuran

[0346] Sample concentration: 30mg / 5mL

[0347] Injection volume: 20 μL

[0348] Flow rate: 1.00mL / min

[0349] Measurement temperature: 40℃

[0350] [Manufacturing of modified conjugated diene polymer]

[0351] Production Example 1

[0352] In a 2L glass flask container capable of heating and cooling and equipped with a thermometer, a reflux condenser and a stirring device, 33.8 parts by mass of polybutadiene (1,2-polybutadiene homopolymer, number average molecular weight (Mn) 1200, vinyl content = 85 mol% or more), 1.43 parts by mass of bismaleimide resin (aromatic bismaleimide resin having a group containing an indane ring: number average molecular weight (Mn) 1300, the same as maleimide resin 1 described later), 0.0035 parts by mass of α,α'-bis(tert-butylperoxy)diisopropylbenzene, and toluene as an organic solvent were added. Next, under a nitrogen atmosphere, the mixture was reacted at 90 to 100°C while stirring for 5 hours, thereby obtaining a solution of a modified conjugated diene polymer (solid content concentration: 35% by mass). The number average molecular weight (Mn) of the obtained modified conjugated diene polymer was 2000.

[0353] In addition, for the solution comprising polybutadiene and bismaleimide resin before the reaction starts and the reacted solution, GPC is measured by the above method, the peak area from bismaleimide resin before and after the reaction is obtained. Next, the vinyl modification rate of bismaleimide resin is calculated by following formula. It should be noted that the vinyl modification rate is equivalent to the reduction rate of the peak area from bismaleimide resin caused by the reaction.

[0354] Vinyl modification rate (%) = [(peak area derived from bismaleimide resin before the reaction) - (peak area derived from bismaleimide resin after the reaction)] × 100 / (peak area derived from bismaleimide resin before the reaction)

[0355] The vinyl modification ratio determined from the above formula was 40%.

[0356] [Manufacturing of resin composition]

[0357] Examples 1 to 6, Comparative Examples 1 to 4

[0358] The components listed in Table 1 were blended with toluene and methyl ethyl ketone in the amounts listed in Table 1, stirred and mixed at 25° C. to prepare a varnish-like resin composition having a solid content concentration of about 60% by mass. It should be noted that in Table 1, the unit of the amount of each component is part by mass, and in the case of a solution, it refers to part by mass converted to solid content.

[0359] (Manufacturing of resin film)

[0360] The varnish-like resin composition obtained above was applied onto a 38 μm-thick PET film (manufactured by Teijin Limited, trade name “G2-38”), and then heated and dried at 170° C. for 5 minutes to prepare a resin film in a B-stage state.

[0361] (Manufacturing of resin sheets with copper foil on both sides)

[0362] After the resin film obtained above is peeled off from the PET film, it is crushed to make a resin powder in a B-stage state. The resin powder is put into a Teflon (registered trademark) sheet punched into a size of 0.5 mm thick × 50 mm long × 35 mm wide, and a low-profile copper foil with a thickness of 18 μm (Mitsui Mining and Smelting Co., Ltd., trade name "3EC-VLP-18") is arranged on the upper and lower sides. It should be noted that the low-profile copper foil is arranged in a manner that the M side (roughened side) is on the resin powder side. Next, the laminate before heat and pressure forming is heat and press formed under the conditions of a temperature of 230°C, a pressure of 2.0 MPa, and a time of 120 minutes, and the resin powder is formed into a resin plate while being cured, thereby making a resin plate with copper foil on both sides. The thickness of the resin plate part of the obtained resin plate with copper foil on both sides is 0.5 mm.

[0363] (Manufacturing of prepreg)

[0364] The varnish-like resin composition obtained above was impregnated into E glass cloth having a thickness of 0.1 mm, and heated and dried at 110° C. for 3 minutes to obtain a prepreg having a content of the resin composition of 48% by mass.

[0365] [Evaluation method]

[0366] Each evaluation was performed according to the following method. The results are shown in Table 1.

[0367] (Method for determining minimum melt viscosity and minimum melt viscosity temperature)

[0368] About 0.6 g of the resin powder in the B-stage state obtained by crushing the resin film prepared in each example was weighed and formed into a disc-shaped tablet with a diameter of 20 mm using a tablet forming machine. The tablet was used as a measurement sample, and the viscosity was measured using a rheometer (manufactured by Rheometric Company, trade name "ARES-2K STD-FCO-STD") under the conditions of a heating rate of 3°C / min, a load of 0.2N, and a measurement temperature range of 50 to 200°C, and the minimum melt viscosity and the minimum melt viscosity temperature were measured. It should be noted that the minimum melt viscosity temperature refers to the temperature at which the minimum melt viscosity is exhibited.

[0369] (Evaluation method of non-adhesion between prepregs)

[0370] Fifteen prepregs prepared in each example were stacked and placed in an aluminum vapor deposition bag, and allowed to stand for one week in a state of being pressed at 1 MPa. After the pressing was released, the non-adhesion between the prepregs was evaluated according to the following evaluation criteria.

[0371] A: The prepregs can be easily peeled off by hand without causing cracks in the prepregs.

[0372] B: When the prepregs were peeled off by hand, cracks occurred in part of the prepreg.

[0373] C: The overlapped prepregs were integrated with each other and could not be separated by hand.

[0374] (Measurement method of relative dielectric constant (Dk) and dielectric loss tangent (Df))

[0375] The resin plate with copper foil on both sides prepared in each example was immersed in a 10 mass % solution of ammonium persulfate (manufactured by Mitsubishi Gas Chemical Co., Ltd.) as a copper etching solution to remove the copper foil. The obtained resin plate was cut into 2 mm × 50 mm pieces, dried at 105°C for 1 hour, and the obtained pieces were used as test pieces. Next, the relative dielectric constant (Dk) and dielectric loss tangent (Df) of the above test pieces were measured under the conditions of an atmosphere temperature of 25°C and a frequency band of 10 GHz according to the cavity resonator perturbation method.

[0376] (Flame retardancy)

[0377] The resin plate with copper foil on both sides prepared in each example was immersed in a 10 mass % solution of ammonium persulfate (manufactured by Mitsubishi Gas Chemical Co., Ltd.) as a copper etching solution to remove the copper foil. The obtained resin plate was cut into 200 mm in length and 50 mm in width, and the obtained product was used as a test piece and subjected to a flammability test according to the UL standard (UL94VTM).

[0378] [Table 1]

[0379] surface

[0380]

[0381] ※In the table, “-” means not measured.

[0382] The details of each component described in Table 1 are as follows.

[0383] [(A) ingredient]

[0384] Maleimide resin 1: an aromatic bismaleimide resin having an indane ring-containing group represented by the general formula (A-2): number average molecular weight (Mn) 1300

[0385] [(A')Component]

[0386] Maleimide resin 2: biphenyl aralkyl type maleimide (manufactured by Nippon Kayaku Co., Ltd., trade name "MIR-3000")

[0387] [(B) ingredient]

[0388] Phosphate compound: 4,4'-biphenol-bis(di-2,6-xylyl phosphate) represented by the following formula (B-6)

[0389] [Chemical formula 24]

[0390]

[0391] [(C) ingredient]

[0392] Modified polyphenylene ether: polyphenylene ether having methacryloyl groups at both ends, weight average molecular weight (Mw) 1700

[0393] Modified conjugated diene polymer: the modified conjugated diene polymer obtained in Production Example 1

[0394] [(D) ingredient]

[0395] Styrene-based thermoplastic resin: styrene-ethylene-butylene-styrene (SEBS) copolymer (manufactured by Kraton Polymer Japan Co., Ltd., trade name "Kraton (registered trademark) MD1653", melt flow rate 5.0 g / 10 min, styrene content 30% by mass, hydrogenation rate 100%)

[0396] [(E) ingredient]

[0397] ·Silica: Spherical fused silica, average particle size (D 50 )0.5μm

[0398] [(F)INGREDIENT]

[0399] Organic peroxide: α,α'-bis(tert-butylperoxy)diisopropylbenzene

[0400] Imidazole curing accelerator: isocyanate-masked imidazole (addition reaction product of hexamethylene diisocyanate resin and 2-ethyl-4-methylimidazole) (manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd., trade name "G-8009L")

[0401] The results shown in Table 1 show that when Examples 1 and 2 and Comparative Example 1 are compared, in which the same components other than the component (B) are used, the resin compositions of Examples 1 and 2 have lower minimum melt viscosities than the resin composition of Comparative Example 1.

[0402] Similarly, when Examples 3 to 5 and Comparative Example 2 are compared in which the same components other than the component (B) are used, it is found that the resin compositions of Examples 3 to 5 have lower minimum melt viscosities than the resin composition of Comparative Example 2.

[0403] Industrial Applicability

[0404] The resin composition of the present embodiment uses a maleimide resin as a thermosetting resin but has a low minimum melt viscosity. Therefore, a prepreg, a laminate, a printed wiring board, a semiconductor package, etc. obtained using the resin composition are suitable for electronic component applications.

Claims

1. A resin composition comprising: (A) at least one selected from a maleimide resin and a derivative of the maleimide resin, wherein the maleimide resin has a group including a condensed ring of an aromatic ring and an aliphatic ring and two or more N-substituted maleimide groups; and (B) A phosphoric acid ester compound having two or more phosphorus atoms, wherein a group connecting at least two phosphorus atoms to each other includes two or more aromatic rings.

2. The resin composition according to claim 1, wherein The group containing a condensed ring of an aromatic ring and an aliphatic ring contained in the component (A) is a group containing an indane ring as the condensed ring.

3. The resin composition according to claim 2, wherein The group containing an indane ring is a divalent group represented by the following general formula (A-1), In the general formula (A-1), R A1 is an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aryloxy group having 6 to 10 carbon atoms, an arylthio group having 6 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, a halogen atom, a hydroxyl group or a mercapto group; A1 is an integer from 0 to 3; R A2 ~R A4 Each independently represents an alkyl group having 1 to 10 carbon atoms; * represents a bonding site.

4. The resin composition according to any one of claims 1 to 3, wherein The component (B) is a compound represented by the following general formula (B-1), In the general formula (B-1), R B1 ~R B4 Each independently represents an aliphatic hydrocarbon group having 1 to 5 carbon atoms or a halogen atom; X B1 is a divalent group containing two or more aromatic rings; n B1 ~n B4 Each independently represents an integer from 0 to 5, and n B5 It is an integer from 1 to 5.

5. The resin composition according to any one of claims 1 to 3, wherein The content of the component (B) is 0.1 to 10 parts by mass based on 100 parts by mass, which is the total amount of the resin components in the resin composition. 6 . The resin composition according to claim 1 , further comprising (C) a compound having two or more ethylenically unsaturated bond-containing functional groups. 7 . A prepreg comprising the resin composition according to claim 1 or a semi-cured product of the resin composition. 8 . A laminate comprising a cured product of the resin composition according to claim 1 and a metal foil. 9 . A resin film comprising the resin composition according to claim 1 or a semi-cured product of the resin composition. 10 . A printed wiring board comprising a cured product of the resin composition according to claim 1 . 11 . A semiconductor package comprising the printed wiring board according to claim 10 and a semiconductor element.