Nickel-based alloy

By adding Ba and Y to the nickel-based alloy to form a dense oxide layer, the problems of insufficient corrosion resistance and oxidation resistance of existing disc spring materials under high temperature environments are solved, and the nickel-based alloys are realized in petrochemical industry and key areas Widely used in the field of equipment.

CN119020639APending Publication Date: 2024-11-26YANGZHOU JIUWEI PACKAGE PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411143017.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing ordinary disc spring materials (such as 60Si2MnA, 50CrVA) lack rust, corrosion, antimagnetic and heat-resistant properties, which limits their application in petrochemical and key equipment fields, and the oxidation resistance of nickel-based alloys is not excellent enough.

Method used

A nickel-based alloy containing Ba and Y is used to form a dense chromium oxide and aluminum oxide layer by using the deoxygenation of Ba and Y during the alloy smelting process to improve the resistance to dynamic oxidation of the alloy.

Benefits of technology

It significantly improves the oxidation resistance of nickel-based alloys, ensures its stability and corrosion resistance in high temperature environments, and is suitable for petrochemical and key equipment fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005001452640000031
    Figure BDA0005001452640000031
  • Figure BDA0005001452640000032
    Figure BDA0005001452640000032
  • Figure BDA0005001452640000041
    Figure BDA0005001452640000041
Patent Text Reader

Abstract

The invention discloses a nickel-based alloy, and belongs to the technical field of alloys. Comprising less than or equal to 0.02% of C, less than or equal to 0.40% of Si, less than or equal to 0.20% of Mn, less than or equal to 0.02% of P, less than or equal to 0.006% of S, 18.0%-22.0% of Cr, 8.0%-10.0% of Mo, 2%-4% of Cu, less than or equal to 0.25% of Al, less than or equal to 0.20% of Ti, less than or equal to 5.0% of Fe, less than or equal to 0.1% of Y, less than or equal to 0.005% of Sn, less than or equal to 0.01% of Ba, less than or equal to 0.005% of Sb, less than or equal to 0.005% of Bi and the Ba and Y are added into the alloy, the deoxidation effect is achieved during alloy smelting, inclusion spheroidization is facilitated, a chromium oxide layer and an aluminum oxide layer on the surface are more compact, and the dynamic oxidation resistance of the alloy is greatly improved; the optimal content of Ba and Y is less than 0.1%, and when the content is too high, microscopic cracks can be formed at positions where the elements exist.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloys, in particular to a nickel-based alloy. Background Art

[0002] Disc springs are called disc springs for short. They are usually made of metal steel strips, steel plates or forged blanks. They are a kind of truncated cone-shaped spring with high stiffness and variable stiffness characteristics. According to their cross-sections and shapes, they are mainly divided into ordinary disc springs, trapezoidal disc springs, and conical trapezoidal disc springs. At present, ordinary disc springs are widely used in China.

[0003] In the prior art, the common materials for ordinary disc springs are spring steels such as 60Si2MnA and 50CrVA. The main disadvantage of these materials is that they do not have the properties of rust resistance, corrosion resistance, anti-magnetic resistance, and heat resistance. Therefore, disc springs made of these common materials are susceptible to various effects such as thermal expansion and contraction, high temperature, and corrosion, and cannot be widely used in the fields of petrochemicals, key equipment, etc.

[0004] Nickel-based alloys have excellent high-temperature mechanical properties and corrosion resistance, and are widely used in the fields of petrochemicals, key equipment, etc. They are an extremely important material that is indispensable to economic construction and national defense. Nickel-based alloys have a certain range of working conditions. For example, 625 alloy has good resistance to intergranular corrosion, stress corrosion, and pitting corrosion, but its oxidation resistance is not excellent enough. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a nickel-based alloy.

[0006] The present invention is achieved through the following technical solutions:

[0007] A nickel-based alloy comprises, by weight percentage, C≤0.02%, Si≤0.40%, Mn≤0.20%, P≤0.02%, S≤0.006%, Cr 18.0%-22.0%, Mo 8.0%-10.0%, Cu 2%-4%, Al≤0.25%, Ti≤0.20%, Fe≤5.0%, Y≤0.1%, Sn≤0.005%, Ba≤0.01%, Sb≤0.005%, Bi≤0.005%, and the balance is Ni and unavoidable impurities.

[0008] The sum of the Al and Ti contents is Al+Ti≤0.4%.

[0009] The sum of the contents of Ba and Y is Ba+Y≤0.18%.

[0010] Nickel-based alloy, comprising, by weight percentage, C≤0.015%, Si≤0.15%, Mn≤0.1%, P≤0.01%, S≤0.002%, Cr20%-21%, Mo 9%-9.5%, Cu 2.5%-3.5%, Al≤0.20%, Ti≤0.05%, Fe≤3.5%, Y≤0.08%, Sn≤0.002%, Ba≤0.008%, Sb≤0.001%, Bi≤0.002%, and the balance being Ni and unavoidable impurities.

[0011] Compared with the prior art, the present invention has the following beneficial effects:

[0012] The invention adds Ba and Y into the alloy, which plays a deoxidation role during alloy smelting, is beneficial to inclusion spheroidization, makes the chromium oxide layer and aluminum oxide layer on the surface more compact, and greatly improves the dynamic oxidation resistance of the alloy; the content of Ba and Y is preferably less than 0.1%. When the content is too high, micro cracks will form at the position where these elements exist. DETAILED DESCRIPTION

[0013] The present invention is further described below in conjunction with embodiments:

[0014] A nickel-based alloy comprises, by weight percentage, C≤0.02%, Si≤0.40%, Mn≤0.20%, P≤0.02%, S≤0.006%, Cr 18.0%-22.0%, Mo 8.0%-10.0%, Cu 2%-4%, Al≤0.25%, Ti≤0.20%, Fe≤5.0%, Y≤0.1%, Sn≤0.005%, Ba≤0.01%, Sb≤0.005%, Bi≤0.005%, and the balance is Ni and unavoidable impurities.

[0015] The sum of the Al and Ti contents is Al+Ti≤0.4%.

[0016] The sum of the contents of Ba and Y is Ba+Y≤0.18%.

[0017] Example 1

[0018] The nickel-based alloy of the present embodiment includes, by weight percentage, C 0.010%, Si 0.12%, Mn 0.1%, P0.01%, S 0.001%, Cr 20.5, Mo 9.5%, Cu 3%, Al 0.20%, Ti 0.04%, Fe 3%, Y 0.08%, Sn 0.002%, Ba 0.008%, Sb 0.001%, Bi 0.002%, and the balance is Ni and unavoidable impurities.

[0019] The sum of the contents of Al and Ti is Al+Ti=0.24%, and the sum of the contents of Ba and Y is Ba+Y=0.088%.

[0020] Example 2

[0021] The nickel-based alloy of the present embodiment includes, by weight percentage, C 0.015%, Si 0.10%, Mn 0.08%, P 0.08%, S 0.002%, Cr 20%, Mo 9.1%, Cu 2.7%, Al 0.15%, Ti 0.05%, Fe 3.5%, Y 0.05%, Sn 0.001%, Ba 0.008%, Sb 0.001%, Bi 0.001%, and the balance is Ni and unavoidable impurities.

[0022] The sum of the contents of Al and Ti is Al+Ti=0.20%, and the sum of the contents of Ba and Y is Ba+Y=0.058%.

[0023] Example 3

[0024] The nickel-based alloy of the present embodiment includes, by weight percentage, C 0.005%, Si 0.10%, Mn 0.08%, P 0.08%, S 0.002%, Cr22%, Mo 9.1%, Cu 2.7%, Al 0.24%, Ti 0.05%, Fe 4%, Y0.08%, Sn 0.001%, Ba 0.002%, Sb 0.001%, Bi 0.0005%, and the balance is Ni and unavoidable impurities.

[0025] The sum of the contents of Al and Ti is Al+Ti=0.29%, and the sum of the contents of Ba and Y is Ba+Y=0.082%.

[0026] The elastic modulus E and shear modulus G of the alloy obtained in the embodiment at different temperatures are as follows:

[0027]

[0028] The oxidation resistance of the alloys obtained in the examples and the comparative alloys are as follows:

[0029]

[0030]

[0031] In the present invention, the nickel-based alloy obtained in the examples has excellent oxidation resistance.

[0032] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the scope of implementation of the present invention. All equivalent changes and modifications to the shapes, structures, features and spirits described in the claims of the present invention should be included in the scope of the claims of the present invention.

Claims

1. A nickel-based alloy, characterized in that: Calculated in weight percentage, it includes: C≤0.02%, Si≤0.40%, Mn≤0.20%, P≤0.02%, S≤0.006%, Cr 18.0%-22.0%, Mo 8.0%-10.0%, Cu 2%-4%, Al≤0.25%, Ti≤0.20%, Fe≤5.0%, Y≤0.1%, Sn≤0.005%, Ba≤0.01%, Sb≤0.005%, Bi≤0.005%, and the balance is Ni and unavoidable impurities.

2. The nickel-based alloy according to claim 1, characterized in that The sum of the Al and Ti contents is Al+Ti≤0.4%.

3. The nickel-based alloy according to claim 1, characterized in that The sum of the contents of Ba and Y is Ba+Y≤0.1%.

4. The nickel-based alloy according to any one of claims 1 to 3, characterized in that: Measured in weight percentage, it includes: C≤0.015%, Si≤0.15%, Mn≤0.1%, P≤0.01%, S≤0.002%, Cr20%~21%, Mo 9%~9.5%, Cu 2.5%~3.5%, Al≤0.20%, Ti≤0.05%, Fe≤3.5%, Y≤0.08%, Sn≤0.002%, Ba≤0.008%, Sb≤0.001%, Bi≤0.002%, and the balance is Ni and unavoidable impurities.