Wear-resistant material as well as preparation method and application thereof
By using interlaced laminated structural materials prepared with high wear-resistant and low wear-resistant metal powders in the drill bit, the problems of large contact area and low rock crushing efficiency in deep drilling are solved, and efficient drilling and long life of the drill bit are achieved.
Patent Information
- Application Number
- CN202411134836.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
In deep drilling, the existing diamond drill bits are too flat, resulting in large contact area of rock, low rock crushing efficiency, and the broken rock chips cannot be discharged in time, resulting in short drill bit life.
Using wear-resistant materials composed of high wear-resistant and low wear-resistant metal powders, drill bits with interlaced and stacked high wear-resistant units with arc-shaped or cylindrical structures are prepared through 3D printing technology to reduce the contact area between the drill bit and the rock. , and form grooves or pit structures through the wear of low wear-resistant carcass to improve rock crushing efficiency and cooling effect.
It improves the drilling efficiency and service life of the drill bit, extends the working life of the drill bit, and improves the stress distribution of cutting teeth through special structure, and is suitable for deep solid minerals and ultra-deep well oil and gas exploration.
Smart Images

Figure CN119020650A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wear-resistant materials, and in particular relates to a wear-resistant material and a preparation method and application thereof. Background Art
[0002] The exploration and development of deep oil and gas resources and mineral resources is difficult, and scientific drilling has now advanced to over 10,000 meters. For the drilling of deep wells and ultra-deep wells, the technical level of key drilling equipment and drilling tools directly affects the drilling cycle and cost, and the drill bit in the drilling tool plays a vital role in deep drilling. For deep drilling in hard and highly abrasive formations, conventional diamond drill bits have problems such as slow penetration and short life. The main reason is that the bottom lip surface structure of the drill bit is too flat during rock crushing, and the contact area with the rock is large. The pressure on a single diamond is small, and the rock crushing efficiency is low; in addition, the broken rock cuttings cannot be discharged in time in the hole and are repeatedly worn, resulting in a short drill bit life. Therefore, it is urgent to develop a drill bit with high drilling efficiency and long working life. Summary of the invention
[0003] In view of this, the present invention provides a wear-resistant material and a preparation method and application thereof. The wear-resistant material provided by the present invention, when used as a drill bit, can reduce the contact area between the drill bit lip and the rock, thereby improving the drilling efficiency and extending the service life; at the same time, the groove structure or pit structure generated by the wear-resistant material during use is conducive to chip removal and cooling, further extending the service life of the drill bit.
[0004] In order to solve the above technical problems, the present invention provides a wear-resistant material, including a high wear-resistant carcass and a low wear-resistant carcass; the high wear-resistant carcass is composed of a plurality of high wear-resistant units, the low wear-resistant carcass is composed of a plurality of low wear-resistant units, and any high wear-resistant unit is in direct contact with a low wear-resistant unit;
[0005] The high wear-resistant unit comprises high wear-resistant metal powder and a first diamond, wherein the high wear-resistant metal powder comprises the following components in percentage by mass:
[0006]
[0007] The low wear-resistant unit comprises low wear-resistant metal powder and a second diamond, wherein the low wear-resistant metal powder comprises the following components in percentage by mass:
[0008]
[0009] Preferably, the volume fraction of the highly wear-resistant tire body in the wear-resistant material is 75-90%.
[0010] Preferably, the volume fraction of the first diamond in the high wear-resistant unit is 20-40%; the volume fraction of the second diamond in the low wear-resistant unit is 5-15%.
[0011] Preferably, the average particle size of the first tungsten carbide powder and the second tungsten carbide powder are independently 0.8 to 1.5 μm;
[0012] The average particle sizes of the first cobalt powder and the second cobalt powder are independently 1 to 1.5 μm;
[0013] The average particle sizes of the first nickel powder and the second nickel powder are independently 1 to 3 μm;
[0014] The average particle sizes of the first copper powder and the second copper powder are independently 1 to 5 μm;
[0015] The average particle size of the tin powder is 5 to 15 μm;
[0016] The average particle size of the iron powder is 20 to 30 μm.
[0017] Preferably, the particle size of the first diamond is 300-600 μm; the particle size of the second diamond is 250-425 μm.
[0018] Preferably, the structural composition of the high wear-resistant unit and the low wear-resistant unit in the wear-resistant material includes the first mode, the second mode or the third mode:
[0019] The first mode is: the longitudinal sections of the high wear-resistant unit and the low wear-resistant unit are arc-shaped, and the high wear-resistant unit and the low wear-resistant unit are stacked in sequence along the radial direction;
[0020] The second mode is: the high wear-resistant unit and the low wear-resistant unit are stacked in sequence longitudinally, and the tangent angle between the low wear-resistant unit and the wear-resistant material is 40-50°;
[0021] The third method is: the longitudinal section of the high wear-resistant unit is arc-shaped, and the number of high wear-resistant units is 1; the low wear-resistant unit is cylindrical, and the low wear-resistant unit is radially embedded in the high wear-resistant unit, the height of the cylinder is consistent with the arc thickness of the high wear-resistant unit, and the bottom diameter of the low wear-resistant unit is 1 to 3 mm.
[0022] The present invention also provides a method for preparing the wear-resistant material described in the above technical solution, comprising the following steps:
[0023] Performing a first mixing of a first diamond, a highly wear-resistant metal powder and a first binder to obtain a first slurry;
[0024] The second diamond, the low wear-resistant metal powder and the second binder are mixed for a second time to obtain a second slurry;
[0025] Performing 3D printing using the first slurry and the second slurry to obtain a wear-resistant material blank;
[0026] The wear-resistant material blank is subjected to degreasing treatment and sintering in sequence to obtain the wear-resistant material.
[0027] Preferably, the first binder and the second binder independently include the following components in percentage by weight:
[0028]
[0029] The temperatures of the first mixing and the second mixing are independently 175 to 195° C., and the times of the first mixing and the second mixing are independently 1.5 to 2.5 hours.
[0030] Preferably, the vacuum degree of the degreasing treatment is 1×10 -1 ~1×10 -3 Pa, the degreasing treatment temperature is 350-500°C, the heating rate to the required temperature of the degreasing treatment is 3-5°C / min, and the degreasing treatment time is 0.5-2h;
[0031] The sintering temperature is 900-1000° C., the sintering pressure is 15-40 MPa, and the sintering heat preservation time is 3-5 min.
[0032] The present invention also provides the use of the wear-resistant material described in the above technical solution or the wear-resistant material prepared by the preparation method described in the above technical solution as a drill bit.
[0033] The invention provides a wear-resistant material, comprising a high-wear-resistant matrix and a low-wear-resistant matrix; the high-wear-resistant matrix is composed of a plurality of high-wear-resistant units, the low-wear-resistant matrix is composed of a plurality of low-wear-resistant units, and any high-wear-resistant unit is in direct contact with the low-wear-resistant unit; the high-wear-resistant unit comprises a high-wear-resistant metal powder and a first diamond, the high-wear-resistant metal powder comprises the following components in percentage by mass: 60-70% of a first tungsten carbide powder, 10-20% of a first cobalt powder, 5-15% of a first nickel powder, 5-10% of a first copper powder, and 1-3% of a tin powder; the low-wear-resistant unit comprises a low-wear-resistant metal powder and a second diamond, the low-wear-resistant metal powder comprises the following components in percentage by mass: 10-20% of a second tungsten carbide powder, 15-30% of a second cobalt powder, 5-10% of a second nickel powder, 15-30% of a second copper powder, and 25-40% of an iron powder. The wear-resistant material provided by the present invention is composed of a number of high-wear-resistant units and low-wear-resistant units distributed at intervals. When the wear-resistant material with this special structure is used to prepare diamond cutting teeth, the low-wear-resistant matrix wears out in advance when breaking rocks to form circular or radial grooves or dot-shaped pits, which is beneficial to reduce the contact area between the bottom lip surface of the drill bit and the rock and improve the drilling efficiency; the groove structure or the pit structure is also beneficial to chip removal and cooling. The special structure in the wear-resistant material provided by the present invention also improves the stress distribution of the cutting teeth when the drill bit breaks rocks. When the wear-resistant material provided by the present invention is used as a drill bit, it can be used for deep solid minerals, ultra-deep well oil and gas, and long horizontal well shale gas exploration, and has good wear resistance and thus has a long service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 A schematic diagram of the structure of the wear-resistant material prepared according to an embodiment of the present invention;
[0035] Figure 2 A schematic diagram of the structure of a drill bit prepared according to an embodiment of the present invention;
[0036] Figure 3 This is a schematic diagram of the structure of the wear-resistant material prepared in Example 1;
[0037] Figure 4 This is a schematic diagram of the structure of the wear-resistant material prepared in Example 3;
[0038] Figure 5 This is a schematic diagram of the structure of the wear-resistant material prepared in Example 5;
[0039] Figures 3 to 5 In the middle, 1 is a high wear-resistant unit, and 2 is a low wear-resistant unit. DETAILED DESCRIPTION
[0040] The present invention provides a wear-resistant material, including a high wear-resistant carcass and a low wear-resistant carcass; the high wear-resistant carcass is composed of a plurality of high wear-resistant units, the low wear-resistant carcass is composed of a plurality of low wear-resistant units, and any high wear-resistant unit is in direct contact with a low wear-resistant unit;
[0041] The high wear-resistant unit comprises high wear-resistant metal powder and a first diamond, wherein the high wear-resistant metal powder comprises the following components in percentage by mass:
[0042]
[0043] The low wear-resistant unit comprises low wear-resistant metal powder and a second diamond, wherein the low wear-resistant metal powder comprises the following components in percentage by mass:
[0044]
[0045] The wear-resistant material provided by the present invention comprises a high-wear-resistant carcass and a low-wear-resistant carcass; the volume fraction of the high-wear-resistant carcass in the wear-resistant material is preferably 75-90%, more preferably 80-85%.
[0046] In the present invention, the high wear-resistant matrix is composed of a plurality of high wear-resistant units, and the high wear-resistant units include high wear-resistant metal powder and a first diamond. In the present invention, the particle size of the first diamond is preferably 300-600 μm, more preferably 400-500 μm; the volume fraction of the first diamond in the high wear-resistant unit is preferably 20-40%, more preferably 30-40%. In the present invention, the first diamond is the main rock crushing material, relying on its hardest property in nature to crush the rock, and then the rock is taken out by the rotation of the drill bit.
[0047] In the present invention, the highly wear-resistant metal powder comprises 60-70% of the first tungsten carbide powder, preferably 62-65% by mass. In the present invention, the average particle size of the first tungsten carbide powder is preferably 0.8-1.5 μm, more preferably 1-1.3 μm.
[0048] In terms of mass percentage, the highly wear-resistant metal powder comprises 10-20% of the first cobalt powder, preferably 15-20%. In the present invention, the average particle size of the first cobalt powder is preferably 1-1.5 μm, more preferably 1.2-1.5 μm.
[0049] In terms of mass percentage, the highly wear-resistant metal powder comprises 5-15% of the first nickel powder, preferably 5-10%. In the present invention, the average particle size of the first nickel powder is preferably 1-3 μm, more preferably 1.5-2.5 μm.
[0050] In terms of mass percentage, the highly wear-resistant metal powder includes 5-10% of the first copper powder, preferably 8-10%. In the present invention, the average particle size of the first copper powder is preferably 1-5 μm, more preferably 2-3 μm.
[0051] In terms of mass percentage, the highly wear-resistant metal powder includes 1-3% tin powder, preferably 2-3%. In the present invention, the average particle size of the tin powder is preferably 5-15 μm, more preferably 8-13 μm.
[0052] In the present invention, the first tungsten carbide powder (WC) can improve the wear resistance of the material and extend its service life, the first cobalt powder (Co) can improve the toughness of the matrix and the sharpness of the drill bit, the first nickel powder (Ni) can improve the overall strength of the matrix, the first copper powder (Cu) can improve the cooling effect of the material (drill bit), and the tin powder (Sn) can reduce the sintering temperature and improve the sharpness of the drill bit.
[0053] In the present invention, the low wear-resistant unit comprises low wear-resistant metal powder and second diamond. In the present invention, the particle size of the second diamond is preferably 250-425 μm, more preferably 300-400 μm; the volume fraction of the second diamond in the low wear-resistant unit is preferably 5-15%, more preferably 10-13%.
[0054] In the present invention, the low wear-resistant metal powder includes 10-20% of the second tungsten carbide powder, preferably 15-18% by mass. In the present invention, the average particle size of the second tungsten carbide powder is preferably 0.8-1.5 μm, more preferably 1-1.3 μm.
[0055] In terms of mass percentage, the low wear-resistant metal powder includes 15-30% of the second cobalt powder, preferably 20-25%. In the present invention, the average particle size of the second cobalt powder is preferably 1-1.5 μm, more preferably 1.2-1.5 μm.
[0056] In terms of mass percentage, the low wear-resistant metal powder includes 5-10% of the second nickel powder, preferably 5-8%. In the present invention, the average particle size of the second nickel powder is preferably 1-3 μm, more preferably 1.5-2.5 μm.
[0057] In terms of mass percentage, the low wear-resistant metal powder includes 15-30% of the second copper powder, preferably 20-25%. In the present invention, the average particle size of the second copper powder is preferably 1-5 μm, more preferably 2-3 μm.
[0058] In terms of mass percentage, the low wear-resistant metal powder includes 25-40% iron powder, preferably 30-35%. In the present invention, the average particle size of the iron powder is preferably 20-30 μm, more preferably 23-26 μm.
[0059] In the present invention, the second tungsten carbide powder (WC) can improve the wear resistance of the material and extend its service life, the second cobalt powder (Co) can improve the toughness of the matrix and the sharpness of the drill bit, the second nickel powder (Ni) can improve the overall strength of the matrix, the second copper powder (Cu) can improve the cooling effect of the material (drill bit), and the iron powder (Fe) can increase the toughness of the matrix.
[0060] In the present invention, the structural composition of the high wear-resistant unit and the low wear-resistant unit in the wear-resistant material preferably includes the first mode, the second mode or the third mode.
[0061] In the present invention, the first mode is preferably: the longitudinal sections of the high wear-resistant unit and the low wear-resistant unit are arc-shaped, and the high wear-resistant unit and the low wear-resistant unit are stacked in sequence along the radial direction. In the present invention, the thickness ratio of the high wear-resistant unit and the low wear-resistant unit along the radial direction is preferably 2 to 4:1, and more preferably 3:1. The present invention has no special requirements for the thickness and number of layers of the high wear-resistant unit, and it can be designed according to the thickness size required by the wear-resistant material. In the present invention, when the wear-resistant material is used as a drill bit, taking the outer diameter of the drill bit as 216mm and the inner diameter of 105mm as an example, the radial thickness of the wear-resistant material matrix is preferably 55mm, the number of layers of the high wear-resistant unit is preferably 9 to 13, and the radial thickness of any high wear-resistant unit is preferably 3.3 to 4.8mm; the number of layers of the low wear-resistant unit is preferably one layer less than the number of layers of the high wear-resistant unit, and the radial thickness of any low wear-resistant unit is preferably 1.1 to 1.6mm. Taking the drill bit with an outer diameter of 75mm and an inner diameter of 49mm as an example, the radial thickness of the wear-resistant material matrix is 13mm, the number of layers of the high wear-resistant unit is preferably 3 to 5, and the radial thickness of any high wear-resistant unit is preferably 2.1 to 3.6mm; the number of layers of the low wear-resistant unit is preferably one layer less than the number of layers of the high wear-resistant unit, and the radial thickness of any low wear-resistant unit is preferably 0.7 to 1.2mm.
[0062] In the present invention, the second method is preferably: the high wear-resistant unit and the low wear-resistant unit are stacked longitudinally in sequence, and the tangent angle between the low wear-resistant unit and the wear-resistant material is preferably 40-50°, and more preferably 45°. The present invention has no special requirements on the shapes of the high wear-resistant unit and the low wear-resistant unit. In an embodiment of the present invention, the high wear-resistant unit and the low wear-resistant unit are radial, and the longitudinal cross-sectional shape of the low wear-resistant unit is quasi-square. In the present invention, the number of layers of the low wear-resistant unit is preferably one layer less than the number of layers of the high wear-resistant unit. The present invention has no special requirements on the number of layers of the high wear-resistant unit, and it can be set according to the required size of the wear-resistant material.
[0063] In the present invention, the third mode is preferably: the longitudinal section of the high wear-resistant unit is arc-shaped, and the number of high wear-resistant units is 1; the low wear-resistant unit is cylindrical, and the low wear-resistant unit is radially embedded in the high wear-resistant unit, the height of the cylinder is less than or equal to the arc thickness of the high wear-resistant unit, and the bottom diameter of the low wear-resistant unit is preferably 1 to 3 mm, more preferably 2 mm; the height of the cylinder is preferably 1 to 3 mm smaller than the arc thickness of the high wear-resistant unit, and more preferably 2 to 3 mm smaller. The present invention has no special requirements for the arrangement of the low wear-resistant units, as long as they are evenly distributed in the high wear-resistant units.
[0064] The present invention also provides a method for preparing the wear-resistant material described in the above technical solution, comprising the following steps:
[0065] Performing a first mixing of a first diamond, a highly wear-resistant metal powder and a first binder to obtain a first slurry;
[0066] The second diamond, the low wear-resistant metal powder and the second binder are mixed for a second time to obtain a second slurry;
[0067] Performing 3D printing using the first slurry and the second slurry to obtain a wear-resistant material blank;
[0068] The wear-resistant material blank is subjected to degreasing treatment and sintering in sequence to obtain the wear-resistant material.
[0069] The present invention performs a first mixing of the first diamond, the high wear-resistant metal powder and the first binder to obtain a first slurry. The present invention preferably mixes the high wear-resistant metal powder with raw materials according to a ratio to obtain the high wear-resistant metal powder; the present invention has no special requirements for the mixing as long as it can be mixed evenly. In the present invention, the first binder preferably includes 80-85% polyoxymethylene, more preferably 82-83%, in terms of mass percentage.
[0070] In terms of mass percentage, the first binder preferably comprises 4-6% polyethylene, more preferably 5-6%.
[0071] In terms of mass percentage, the first binder preferably includes 4-10% ethylene vinyl acetate, and more preferably 6-8%.
[0072] In terms of mass percentage, the first binder preferably includes 4-8% stearic acid, and more preferably 5-7%.
[0073] In the present invention, the mass ratio of the first binder to the high wear-resistant metal powder is preferably 2 to 8:100, more preferably 3 to 5:100.
[0074] In the present invention, the temperature of the first mixing is preferably 175 to 195° C., more preferably 180 to 185° C.; the time of the first mixing is preferably 1.5 to 2.5 h, more preferably 2 h.
[0075] The present invention performs a second mixing of the second diamond, the low-wear-resistant metal powder and the second binder to obtain a second slurry. The present invention preferably mixes the low-wear-resistant metal powder with raw materials according to a ratio to obtain the low-wear-resistant metal powder; the present invention has no special requirements for the mixing as long as it can be mixed evenly. In the present invention, the composition of the second binder is preferably consistent with that of the first binder, and will not be repeated here.
[0076] In the present invention, the mass ratio of the second binder to the low wear-resistant metal powder is preferably 2 to 8:100, more preferably 3 to 5:100.
[0077] In the present invention, the temperature of the second mixing is preferably 175 to 195° C., more preferably 180 to 185° C.; the time of the second mixing is preferably 1.5 to 2.5 h, more preferably 2 h.
[0078] After obtaining the first slurry and the second slurry, the present invention uses the first slurry and the second slurry to perform 3D printing to obtain a wear-resistant material blank. The present invention preferably inputs the structural composition parameters of the wear-resistant material into the 3D printing computer before performing 3D printing, and the structural composition parameters preferably include the circumferential distribution spacing and number of the high wear-resistant carcass and the low wear-resistant carcass, the shape and number of the radial structure of the low wear-resistant carcass, or the diameter and number of the point structure of the low wear-resistant carcass. The present invention preferably uses a finite element simulation method to design the structure of the wear-resistant material.
[0079] The present invention adopts a slurry extrusion 3D printing process to design drill bit cutting teeth into various complex structures, and can also realize multi-type design of cutting tooth matrix materials. The present invention improves the rock crushing efficiency and service life of the drill bit by staggered contact of high wear-resistant matrix and low wear-resistant matrix.
[0080] After obtaining the wear-resistant material blank, the wear-resistant material blank is subjected to degreasing treatment and sintering in sequence to obtain the wear-resistant material. In the present invention, the vacuum degree of the degreasing treatment is preferably 1×10 -1 ~1×10 -3 Pa, more preferably 1×10 -3 Pa; the temperature of the degreasing treatment is preferably 350-500°C, more preferably 400-450°C; the heating rate to the temperature required for the degreasing treatment is preferably 3-5°C / min, more preferably 4-5°C / min; the time of the degreasing treatment is preferably 0.5-2h, more preferably 1-2h. The present invention can remove the binder in the wear-resistant material blank through the degreasing treatment, avoiding the formation of carbon elements during high-temperature sintering to have a harmful effect on the matrix.
[0081] In the present invention, the sintering temperature is preferably 900-1000°C, more preferably 960-980°C; the sintering pressure is preferably 15-40MPa; the sintering holding time is preferably 3-5min, more preferably 4-5min. In the present invention, the sintering equipment is preferably a medium frequency hot pressing sintering machine or a resistance hot pressing sintering machine; the present invention preferably places the product to be sintered in a graphite mold and then places it in the sintering equipment. In the present invention, when the sintering is carried out in a resistance hot pressing sintering machine, the sintering pressure is preferably 25-40MPa; the present invention preferably connects the wear-resistant material obtained by sintering with the steel body by welding to form a drill bit. In the present invention, when the sintering is carried out in a medium frequency hot pressing sintering machine, the sintering pressure is preferably 15-30MPa; the present invention preferably places the degreased product and the steel body in a graphite mold at the same time for hot pressing sintering to form a diamond integral drill bit.
[0082] The present invention utilizes the diffusion and deformation characteristics of materials at high temperatures through sintering to cause metallurgical bonding between powder particles, thereby promoting the transformation of mechanical meshing between powder particles into grain boundary bonding between atoms. As the temperature rises or the time increases, the grains gradually grow.
[0083] The present invention also provides the use of the wear-resistant material described in the above technical solution or the wear-resistant material prepared by the preparation method described in the above technical solution as a drill bit. In the present invention, the drill bit is preferably a diamond drill bit for deep oil and gas and solid mineral exploration. When the wear-resistant material is used as a drill bit in the present invention, the low-wear-resistant tire body will form circumferential grooves, radial grooves or dot-shaped pits due to rapid wear, and such grooves or pits exist throughout the life cycle of the drill bit, which is beneficial to improve the efficiency, chip removal and cooling of the drill bit, thereby extending the service life of the drill bit. Figure 1 This is a schematic diagram of the structure of the wear-resistant material prepared in an embodiment of the present invention. Figure 2 It is a schematic structural diagram of a drill bit made of the wear-resistant material provided by an embodiment of the present invention.
[0084] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0085] Example 1
[0086] The high wear-resistant metal powder is composed of the following raw materials by mass percentage: 62% of WC powder with an average particle size of 1.2 μm, 20% of Co powder with an average particle size of 1.3 μm, 5% of Ni powder with an average particle size of 2 μm, 10% of Cu powder with an average particle size of 3 μm, and 3% of Sn powder with an average particle size of 10 μm;
[0087] The low wear-resistant metal powder is composed of the following raw materials by mass percentage: 15% of WC powder with an average particle size of 1.2 μm, 20% of Co powder with an average particle size of 1.3 μm, 5% of Ni powder with an average particle size of 2 μm, 25% of Cu powder with an average particle size of 3 μm, and 35% of Fe powder with an average particle size of 25 μm; the binder is composed of the following components by mass percentage: 83% of polyoxymethylene, 6% of polyethylene, 6% of ethylene-vinyl acetate, and 5% of stearic acid;
[0088] The raw materials of the high wear-resistant metal powders are mixed to obtain the high wear-resistant metal powder, and then mixed with the first diamond and the binder at 180° C. and kneaded for 2 hours to obtain the first slurry; the first diamond particle size is 500 μm, the volume ratio of the first diamond to the high wear-resistant metal powder is 25:75; the mass ratio of the high wear-resistant metal powder to the binder is 96:4;
[0089] The low wear-resistant metal powders were mixed with raw materials to obtain low wear-resistant metal powders, and then mixed with the second diamond and the binder at 180° C. for 2 hours to obtain a second slurry; the second diamond particle size was 300 μm, the volume ratio of the second diamond to the low wear-resistant metal powder was 7:93; the mass ratio of the low wear-resistant metal powder to the binder was 96:4;
[0090] The finite element simulation method is used to design the wear-resistant material structure, specifically: the longitudinal sections of the high wear-resistant unit and the low wear-resistant unit are arc-shaped, the radial thickness ratio of the high wear-resistant unit and the low wear-resistant unit is 3:1 (the thickness of the high wear-resistant unit is 2.1 mm, and the thickness of the low wear-resistant unit is 0.7 mm), the number of layers of the high wear-resistant unit is 5, and the number of layers of the low wear-resistant unit is 4; the first slurry and the second slurry are respectively loaded into two silos of the 3D printer, and the slurry extrusion 3D printing process is used for printing to obtain a wear-resistant material blank (the volume ratio of the high wear-resistant matrix and the low wear-resistant matrix is 4:1);
[0091] The wear-resistant material blank is placed in a vacuum furnace at a vacuum degree of 1×10 -3Pa, degrease treatment was carried out at a temperature of 450°C (heating at a rate of 5°C / min) for 2 hours, then placed in a graphite mold, placed in a resistance hot press sintering machine at a temperature of 960°C and a pressure of 30MPa for 5 minutes to obtain a wear-resistant material; Figure 3 Schematic diagram of the structure of the wear-resistant material prepared in Example 1, wherein 1 is a high wear-resistant unit and 2 is a low wear-resistant unit;
[0092] The wear-resistant material is welded to the drill bit steel body by welding technology to obtain a drill bit with an inner diameter of 49 mm and an outer diameter of 75.6 mm.
[0093] Example 2
[0094] The wear-resistant material blank was prepared according to the method of Example 1, and the wear-resistant material blank was placed in a vacuum furnace at a vacuum degree of 1×10 -3 Pa, degrease treatment is carried out at a temperature of 450°C (heating rate of 5°C / min) for 2 hours and then put into a graphite mold, and then the drill steel body is placed on the upper part of the degreased green body, and put into a medium frequency hot pressing sintering machine at a temperature of 980°C and a pressure of 35MPa for sintering for 5 minutes to obtain an integral drill with an inner diameter of 49mm and an outer diameter of 75.6mm.
[0095] Example 3
[0096] The wear-resistant material is prepared according to the method of Example 1, except that the wear-resistant material structure is designed by a finite element simulation method, specifically: the longitudinal cross-section shape of the low wear-resistant unit is a square, the thickness thereof is 0-1.5 mm, the tangent angle between the low wear-resistant unit and the wear-resistant material is 45°, 4 layers of high wear-resistant units and 3 layers of low wear-resistant units are stacked longitudinally in sequence, and the obtained wear-resistant material blank has a volume ratio of 17:3 between the high wear-resistant carcass and the low wear-resistant carcass;
[0097] A wear-resistant material and a drill bit were prepared according to the method of Example 1. The inner diameter of the drill bit was 49 mm and the outer diameter was 75.6 mm.
[0098] Figure 4 This is a schematic diagram of the structure of the wear-resistant material prepared in Example 3, wherein 1 is a high wear-resistant unit and 2 is a low wear-resistant unit.
[0099] Example 4
[0100] Prepare a wear-resistant material blank according to the method of Example 3;
[0101] A drill bit was prepared according to the method of Example 2 using the wear-resistant material blank prepared in Example 4 as a raw material.
[0102] Example 5
[0103] A wear-resistant material is prepared according to the method of Example 1, except that the structure of the wear-resistant material is designed by a finite element simulation method, specifically: the longitudinal section of the high wear-resistant unit is arc-shaped, the thickness of the high wear-resistant unit is 13 mm, and the number of the high wear-resistant unit is 1; the low wear-resistant unit is cylindrical with a bottom diameter of 2 mm and a height of 10 mm, the number of the low wear-resistant units is 8, and the low wear-resistant units are uniformly embedded in the high wear-resistant units along the radial direction, and the volume ratio of the high wear-resistant carcass to the low wear-resistant carcass is 87:13.
[0104] A wear-resistant material and a drill bit were prepared according to the method of Example 1. The inner diameter of the drill bit was 49 mm and the outer diameter was 75 mm.
[0105] Figure 5 This is a schematic diagram of the structure of the wear-resistant material prepared in Example 5, wherein 1 is a high wear-resistant unit and 2 is a low wear-resistant unit.
[0106] Example 6
[0107] Prepare a wear-resistant material blank according to the method of Example 5;
[0108] A drill bit was prepared according to the method of Example 2 using the wear-resistant material blank prepared in Example 6 as a raw material.
[0109] The drill bits prepared in Examples 1 to 6 were used to drill holes in granite, and the results are listed in Table 1.
[0110] Table 1 Results of drilling holes in granite using the drill bits prepared in Examples 1 to 6
[0111] Example Drilling speed (m / h) Drill bit life (m) Example 1 2 150 Example 2 2 150 Example 3 1.8 165 Example 4 1.8 165 Example 5 2.1 145 Example 6 2.1 145
[0112] It can be seen from the results in Table 1 that the drill bit prepared by using the wear-resistant material provided by the present invention has a faster drilling speed and a longer service life, that is, the wear-resistant material provided by the present invention improves the drilling efficiency and service life of the drill bit.
[0113] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A wear-resistant material, characterized in that: It includes a high-wear-resistant carcass and a low-wear-resistant carcass; the high-wear-resistant carcass is composed of a plurality of high-wear-resistant units, and the low-wear-resistant carcass is composed of a plurality of low-wear-resistant units, and any high-wear-resistant unit is in direct contact with a low-wear-resistant unit; The high wear-resistant unit includes high wear-resistant metal powder and a first diamond, wherein the high wear-resistant metal powder includes the following components in percentage by mass: The low wear-resistant unit includes low wear-resistant metal powder and a second diamond, wherein the low wear-resistant metal powder includes the following components in percentage by mass:
2. The wear-resistant material according to claim 1, characterized in that: The volume fraction of the highly wear-resistant tire body in the wear-resistant material is 75-90%.
3. The wear-resistant material according to claim 1, characterized in that: The volume fraction of the first diamond in the high wear-resistant unit is 20-40%; the volume fraction of the second diamond in the low wear-resistant unit is 5-15%.
4. The wear-resistant material according to any one of claims 1 to 3, characterized in that: The average particle size of the first tungsten carbide powder and the second tungsten carbide powder are independently 0.8 to 1.5 μm; The average particle size of the first cobalt powder and the second cobalt powder are independently 1 to 1.5 μm; The average particle size of the first nickel powder and the second nickel powder are independently 1 to 3 μm; The average particle size of the first copper powder and the second copper powder are independently 1 to 5 μm; The average particle size of the tin powder is 5 to 15 μm; The average particle size of the iron powder is 20 to 30 μm.
5. The wear-resistant material according to claim 1 or 3, characterized in that: The particle size of the first diamond is 300-600 μm; the particle size of the second diamond is 250-425 μm.
6. The wear-resistant material according to claim 1, characterized in that: The structural composition of the high wear-resistant unit and the low wear-resistant unit in the wear-resistant material includes the first, second or third manner: The first mode is: the longitudinal sections of the high wear-resistant unit and the low wear-resistant unit are arc-shaped, and the high wear-resistant unit and the low wear-resistant unit are stacked in sequence along the radial direction; The second method is as follows: the high wear-resistant unit and the low wear-resistant unit are stacked longitudinally in sequence, and the tangent angle between the low wear-resistant unit and the wear-resistant material is 40-50°; The third method is: the longitudinal section of the high wear-resistant unit is arc-shaped, and the number of high wear-resistant units is 1; the low wear-resistant unit is cylindrical, and the low wear-resistant unit is radially embedded in the high wear-resistant unit, the height of the cylinder and the arc thickness of the high wear-resistant unit are consistent, and the bottom diameter of the low wear-resistant unit is 1 to 3 mm.
7. The method for preparing the wear-resistant material according to any one of claims 1 to 6, characterized in that: The following steps are involved: Performing a first mixing of the first diamond, the high wear-resistant metal powder and the first binder to obtain a first slurry; performing a second mixing of the second diamond, the low wear-resistant metal powder and the second binder to obtain a second slurry; Performing 3D printing using the first slurry and the second slurry to obtain a wear-resistant material blank; The wear-resistant material blank is subjected to degreasing treatment and sintering in sequence to obtain the wear-resistant material.
8. The preparation method according to claim 7, characterized in that: The first binder and the second binder independently include the following components in percentage by weight: The temperatures of the first mixing and the second mixing are independently 175 to 195° C., and the times of the first mixing and the second mixing are independently 1.5 to 2.5 hours.
9. The preparation method according to claim 7, characterized in that: The vacuum degree of the degreasing process is 1×10 -1 ~1×10 -3 Pa, the degreasing treatment temperature is 350-500°C, the heating rate to the desired degreasing treatment temperature is 3-5°C / min, and the degreasing treatment time is 0.5-2h; The sintering temperature is 900-1000° C., the sintering pressure is 15-40 MPa, and the sintering holding time is 3-5 minutes.
10. Use of the wear-resistant material according to any one of claims 1 to 6 or the wear-resistant material prepared by the preparation method according to any one of claims 7 to 9 as a drill bit.