Preparation method of high-performance alloy sheet using gradient structure and twin composite structure
By annealing and particle micro-forging on the magnesium alloy thin plate, combined with other channel bending deformation, high-performance alloy thin plates with gradient structure and twin composite structure were prepared, which solved the problem of synergistic improvement of magnesium alloy strength and plasticity, and achieved Efficient preparation and performance improvement of materials.
Patent Information
- Application Number
- CN202411034086.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-26
AI Technical Summary
In the prior art, it is difficult to achieve synergistic improvement of strength and plasticity of magnesium alloys, and the preparation process of gradient structures is complex and has poor plasticity.
After the initial thin plate annealing treatment, the particle micro-forging is used to use cold spraying equipment to refine the grains in the surface area, and combine the bending and deformation processing of other channels to introduce gradient structures and twin structures to control process parameters to improve the strength and plasticity of the material .
It realizes the synergistic improvement of plasticity-strength of magnesium alloy thin plates, and flexibly controls the thickness and grain size of the surface of the material. It is suitable for a variety of metal materials, expanding the application field of magnesium alloys.
Smart Images

Figure CN119020708A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal materials, and in particular to a method for preparing a high-performance alloy thin plate using a gradient structure and a twin composite structure. Background Art
[0002] So far, magnesium alloy is one of the lightest structural materials in engineering applications. Due to its low density and good recyclability, it is known as the green metal structural material of the 21st century and is one of the metal materials currently being focused on research and development. Magnesium alloy has low strength, and its close-packed hexagonal structure also greatly limits its plasticity and forming ability. Plasticity is mainly improved through overall strong plastic deformation.
[0003] Commonly used strong plastic deformations such as equal channel extrusion, asynchronous rolling, and cumulative rolling are limited to material size due to processing conditions, and thin plates cannot be processed. Therefore, some scholars have designed an equal channel bending deformation process (patent publication number: CN206104575U) by combining bending deformation and equal channel extrusion. By introducing twins into AZ31 magnesium alloy thin plates (2mm), the elongation of the thin plates was significantly improved, but the yield strength was significantly reduced. How to achieve the synergistic improvement of the strength and plasticity of magnesium alloys and expand their application areas has become a technical problem that urgently needs to be solved. In recent years, the discovery and research of heterogeneous structures have provided methods and approaches for the synergistic improvement of the strength and plasticity of magnesium alloys.
[0004] The synergistic effect between heterogeneous structural organizations can make the material simultaneously obtain high strength and plasticity, improve the comprehensive performance of the material, and gradually develop various heterogeneous magnesium alloys and magnesium-based composite materials (patent publication number: CN115740006A, publication number: CN115807200A) to synergistically improve the strength-plasticity of magnesium alloys. Although the gradient structure has great potential in the preparation of high-strength and toughness materials, its preparation process is relatively complicated, and the prepared gradient grain structure material is generally high in strength but poor in plasticity without post-treatment such as annealing. Summary of the invention
[0005] In view of the above problems and in order to make up for the above deficiencies, the purpose of the present invention is to provide a method for preparing high-performance alloy thin plates using gradient structure and twin composite structure, which can prepare a high-performance alloy thin plate having both fine / coarse grain gradient structure and twin structure, so as to solve the problem of significant decrease in strength when plasticity is improved in the prior art.
[0006] The technical solution of the present invention is:
[0007] A method for preparing a high-performance alloy sheet using a gradient structure and a twin composite structure comprises the following steps:
[0008] 1) Annealing the initial thin plate to obtain a large grain structure without twin structure;
[0009] 2) After annealing, the thin plate is subjected to particle micro-forging by controlling the process parameters of the cold spraying equipment to refine the grains in the surface area and obtain a gradient grain structure;
[0010] 3) Composite processing is performed on the alloy thin plate. The micro-forged alloy thin plate is subjected to equal channel bending deformation processing. By controlling the bending deformation passes and deformation path, different twin numbers and twin types can be introduced into the plate.
[0011] The method for preparing high-performance alloy thin plates using gradient structures and twin composite structures is applicable to magnesium alloy thin plates, zinc alloy thin plates, titanium alloy thin plates, cobalt alloy thin plates or zirconium alloy thin plates having the same hexagonal close-packed structure (HCP).
[0012] The method for preparing a high-performance alloy thin plate using a gradient structure and a twin composite structure, the magnesium alloy thin plate includes a commercial AZ31 magnesium alloy thin plate, and the thickness of the thin plate is less than 3 mm.
[0013] In the method for preparing high-performance alloy thin plates using gradient structures and twin composite structures, in step 1), the annealing temperature of the initial magnesium alloy rolled thin plate is 150-500° C.×0.5-15h.
[0014] In the method for preparing high-performance alloy thin plates using gradient structures and twin composite structures, in step 2), the process parameters for micro-forging by cold spraying equipment include: main gas temperature 25-500°C, main gas pressure 1-5MPa, path spacing 5-10mm, muzzle height from the plate 10-25mm, and steel shot as the granular material with a particle diameter of 0.1-0.5mm.
[0015] In the method for preparing high-performance alloy thin plates using gradient structure and twin composite structure, in step 3), the bending deformation parameters mainly include: bending deformation temperature of 25 to 400°C, bending deformation passes of single or multiple passes, and bending deformation path of the same path, a path rotating around the normal direction (ND) or a path rotating around the rolling direction (RD).
[0016] In the method for preparing high-performance alloy thin plates using gradient structures and twin composite structures, in step 3), the composite processing order of the alloy thin plates is changed, and a micro-forging process is first performed to introduce a gradient grain structure into the alloy thin plates, and then twins are introduced into the alloy thin plates through bending deformation; or, twins are first introduced into the alloy thin plates through bending deformation, and then micro-forging is performed to introduce a gradient grain structure into the alloy thin plates.
[0017] The design concept of the present invention is:
[0018] The present invention can provide a method for effectively preparing high-performance alloy thin plates with gradient structures and twin composite structures on alloy thin plates, which can enable the alloy thin plates to achieve synergistic improvement in plasticity and strength. First, a commercial magnesium alloy rolled thin plate (<3mm) is prepared and the initial alloy thin plate is annealed, and then the front and back sides of the thin plate are subjected to particle micro-forging, and then equal channel bending deformation is performed at different constant temperatures. A high-performance alloy thin plate with a gradient structure and a twin composite structure is prepared by a particle micro-forging and equal channel bending composite process, the gradient structure and twins are combined, the strength of the thin plate is improved by the gradient structure, and then the plasticity of the thin plate is improved by introducing twins, thereby achieving synergistic improvement in strength and plasticity of the magnesium alloy.
[0019] During the particle micro-forging process, the high-speed impact of particles on the thin plate will drive dislocations to occur, significantly refining the grains in the surface area; equal channel bending deformation can introduce twins inside the thin plate. Therefore, the present invention aims to introduce gradient structures through particle micro-forging to improve the strength of the thin plate, further introduce twin structures in combination with equal channel bending deformation to improve the plasticity of the thin plate, and prepare high-performance alloy thin plates in combination with gradient structures and twin composite structures.
[0020] The advantages and beneficial effects of the present invention are:
[0021] 1. The present invention can successfully prepare high-performance alloy thin plates with gradient and twin composite structures, and can achieve synergistic improvement in the plasticity and strength of the alloy thin plates.
[0022] 2. The present invention has flexibility in preparing gradient structures of alloy thin plates. The particle micro-forging process can control the thickness of the fine crystal layer on the surface of the material and the grain size of the fine crystal layer by controlling the process parameters, and can freely control the micro-forging range without restrictions on the shape and size of the material; by changing the micro-end particle material, main gas temperature and pressure, it can be applied to a variety of different metal materials.
[0023] 3. The present invention utilizes equal channel bending to introduce twins into the alloy thin plate, and can significantly improve the elongation of the material after annealing. Different processing passes, processing paths and processing temperatures can introduce different numbers and types of twins.
[0024] 4. The composite process of particle micro-forging and equal channel bending deformation of the present invention can prepare a fine / coarse grain gradient structure in the surface area of the alloy sheet while introducing twins in the center area of the sheet along the thickness direction, changing the grain direction and optimizing the texture. The alloy sheet can enhance the material strength through micro-forging and improve its plasticity through equal channel bending deformation, which can flexibly realize the design and processing of the alloy sheet.
[0025] 5. The present invention is applicable not only to magnesium alloy sheets, but also to zinc (Zn), titanium (Ti), cobalt (Co), zirconium (Zr) and other alloys having the same hexagonal close-packed structure (HCP). BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Schematic diagram of the principle flow of the composite process of particle micro-forging and equal channel bending deformation of magnesium alloy thin plate; in the figure, 1 gas inlet (Gas inlet), 2 steel particle inlet (Steel particles inlet), 3 nozzle (Nozzle), 4 initial magnesium alloy thin plate, 5 steel particles, 6 impact region (Hammered region), 7 intermediate region (Intermediate region), 8 particle micro-forging magnesium alloy thin plate, 9 upper die (Upper die), 10 lower die (Lower die), 11 high performance magnesium alloy thin plate with gradient structure and twin structure, 12 twin (Twin), RD represents rolling direction, ND represents the normal direction of the rolling surface, and Bending represents bending.
[0027] Figure 2 It is the organizational structure diagram of the surface area and the middle area of the RD-ND surface after the composite process of particle micro-forging and equal channel bending deformation in Example 1. Among them, (a) is the OM diagram of the surface area of the RD-ND surface in Example 1, (b) is the OM diagram of the middle area of the RD-ND surface in Example 1, and (c) is the local SEM diagram of the surface area and the middle area of the RD-ND surface in Example 1. In the figure, R1, R2, and R3 correspond to the local scanning positions of Figure (c), respectively, and the distances from the surface of the plate are 0.08mm, 0.12mm, and 0.15mm, respectively, the distance from the surface at 1 / 4 is 0.5mm, and the distance from the surface at 1 / 2 is 1.0mm, and Twin represents twinning.
[0028] Figure 3 The figure compares the mechanical properties of the sheet tensile at room temperature between Example 1 and a sheet subjected to particle micro-forging alone and equal channel bending deformation at 150°C. In the figure, the horizontal axis Engineering strain is the engineering strain, the vertical axis Engineering stress is the engineering stress (MPa), Initial sheet is the initial magnesium alloy sheet, PMF is particle micro-forging alone, ECAB-150 is equal channel angular bending alone at 150°C, PMF-ECAB-150 is a composite process of particle micro-forging and equal channel bending deformation at 150°C, and uniformelongation is the uniform elongation.
[0029] Figure 4The 3-pass bending deformation path is for Example 2. In the figure, RD represents the rolling direction, TD represents the transverse direction of the rolled piece, ND represents the normal direction of the rolling surface, Pass 1 is the first pass, Pass 2 is the second pass, and Pass 3 is the third pass.
[0030] Figure 5 It is a comparison chart of the tensile mechanical properties of Example 2 and the initial magnesium alloy sheet with a thickness of 1 mm at room temperature; in the figure, the horizontal axis Engineering strain is the engineering strain, the vertical axis Engineering stress is the engineering stress (MPa), Initial sheet is the initial magnesium alloy sheet, and PMF-ECAB-200 is a composite process of particle micro-forging and equal channel bending deformation at 200°C. DETAILED DESCRIPTION
[0031] In a specific implementation process, the present invention proposes a method for preparing a high-performance magnesium alloy sheet having a fine / coarse grain gradient structure and a twin structure, comprising the following steps:
[0032] 1) annealing the initial magnesium alloy sheet to obtain a large-grained microstructure without twins;
[0033] The annealing temperature of the initial magnesium alloy rolled sheet is 150-500°C×0.5-15h, in order to obtain a large grain structure (grain size of 0.1-0.5mm) without twin structure. The initial magnesium alloy sheet includes but is not limited to commercial AZ31 magnesium alloy sheet, and the sheet thickness is <3mm.
[0034] 2) The RD-TD front and back sides of the annealed magnesium alloy sheet are subjected to particle micro-forging by cold spraying equipment, and the magnesium alloy sheet after particle micro-forging will obtain a fine / coarse grain gradient structure along the thickness downward on the RD-TD plane;
[0035] Among them, the process parameters for micro-forging by cold spraying equipment include: main gas temperature 25-500°C, main gas pressure 1-5MPa, path spacing 5-10mm, muzzle height from plate 10-25mm, steel shot as particle material, and particle diameter 0.1-0.5mm.
[0036] 3) The micro-forged magnesium alloy sheet is subjected to equal channel bending deformation processing. By controlling the bending deformation passes and deformation path, different twin numbers and twin types can be introduced into the sheet, and the composite processing sequence of the magnesium alloy sheet can be changed. Among them, the bending deformation parameters mainly include: bending deformation temperature 25 ~ 400 ℃, bending deformation passes are single pass, multiple passes (can be processed until the sheet can no longer be processed), bending deformation path is the same path, rotating around the normal direction (ND), rotating around the rolling direction (RD) and other types of different paths.
[0037] like Figure 1 As shown, a gas inlet 1 is provided at the rear end of the nozzle 3 of the cold spraying equipment, a steel particle inlet 2 is provided at the rear side of the nozzle 3, and the front end opening of the nozzle 3 corresponds to the initial magnesium alloy sheet 4. Compressed air carries steel particles 5 through the gas inlet 1 and impacts the surface of the initial magnesium alloy sheet 4 through the steel particle inlet 2 and the nozzle 3 and rebounds, and the initial magnesium alloy sheet 4 is subjected to particle micro-forging to obtain a particle micro-forged magnesium alloy sheet 8. The impact area 6 on the surface of the particle micro-forged magnesium alloy sheet 8 forms fine grains (grain size is 0.2 to 2 μm), and the middle area 7 of the particle micro-forged magnesium alloy sheet 8 forms coarse grains (grain size is 5 to 15 μm), so that the particle micro-forged magnesium alloy sheet 8 has a fine / coarse grain gradient structure.
[0038] The upper die 9 and the lower die 10 are arranged relative to each other to form an equal channel bending deformation die, and the bending deformation channel is composed of the two ends of the inclined section channel and the upper flat section channel and the lower flat section channel respectively. The particle micro-forged magnesium alloy sheet 8 is subjected to equal channel bending deformation (ECAP) under different constant temperature conditions (25-400°C), and the rolled sheet is fed in a certain step length along the set direction. After the particle micro-forged magnesium alloy sheet is subjected to equal channel bending deformation, twins 12 are generated inside the sheet, and a high-performance magnesium alloy sheet 11 with a gradient structure and a twin structure is obtained.
[0039] Main parameters of equal channel bending deformation die: bending deformation angle 2θ=90°~180°, upper die fillet radius R1=0.1~3.0mm, lower die fillet radius R0=0.2~6.0mm, inclined section length L=10~100mm, flat section length: L0=10~100mm, L1=10~100mm, feed step length step is 2mm; equal channel bending deformation process parameters: upper die opening and closing speed V1=V2=50~200mm / min, upper die 9 opening height, upper die 10 pressing height, it is required to ensure that when the die is closed, the distance between the upper die 9 and the lower die 10 is equal to the thickness of the blank to achieve the effect of equal channel deformation.
[0040] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments.
[0041] Example 1
[0042] In this embodiment, a 2 mm thick AZ31 commercial magnesium alloy rolled sheet is cut into long billets of 300 (RD) × 55 (TD) mm.
[0043] The cut long billets were annealed at 250°C for 2h to obtain a twin-free microstructure.
[0044] The initial magnesium alloy sheet after annealing is processed by particle micro-forging process through cold spraying equipment, and the front and back sides of RD-TD are processed twice respectively. The process parameters are selected as follows: main gas temperature 250℃, main gas pressure 1MPa, path spacing 6mm, muzzle height 15mm, steel shot, particle diameter 0.2mm, and main gas compressed air. In this embodiment, the particle micro-forging deformation can form fine grains (average size 0.98μm) in the impact area on the surface of the magnesium alloy sheet, while the middle area of the magnesium alloy sheet is coarse grains (average size 7.98μm).
[0045] The magnesium alloy sheet after micro-forging was subjected to single-pass equal channel bending deformation at a constant temperature of 150°C. The main parameters of the equal channel bending deformation die were: bending deformation angle 2θ=150°, upper die chamfer radius R1=1mm, lower die chamfer radius R0=3mm, inclined section length L=35mm, flat section length: L0=20mm, L1=35mm, upper die opening and closing speed V1=V2=100mm / min, feed direction along RD direction, and feed step length of 2mm.
[0046] like Figure 2 As shown in the figure, the organizational structure diagram of the surface area and the middle area of the RD-ND surface after the composite process of particle micro-forging and equal channel bending deformation in Example 1. Figure 2 It can be seen that the AZ31 magnesium alloy sheet exhibits a gradient grain structure in the surface area and twins exist in the central area.
[0047] like Figure 3 As shown, the mechanical properties of Example 1 (PMF-ECAB-150) and the thin plates subjected to particle micro-forging (PMF) alone and equal channel bending deformation (ECAB-150) alone at 150°C are compared at room temperature. Figure 3 It can be seen that the magnesium alloy sheet processed by the composite process can achieve a synergistic improvement in plasticity and strength.
[0048] In this embodiment, for a 2 mm thick AZ31 magnesium alloy sheet, the uniform elongation of the sheet after micro-forging and 150°C equal channel bending deformation can reach 15.57%, which is 29.1% higher than that of the initial magnesium alloy sheet; the yield strength and tensile strength can reach 234 MPa and 285 MPa, respectively, which are 17.0% and 10.0% higher than those of the initial magnesium alloy sheet.
[0049] Example 2
[0050] In this embodiment, a 1 mm thick AZ31 commercial magnesium alloy rolled sheet is cut into long billets of 300 (RD)×55 (TD) mm.
[0051] The cut long billets were annealed at 250°C for 2h to obtain a twin-free microstructure.
[0052] The initial magnesium alloy sheet after annealing was processed by particle micro-forging process through cold spraying equipment, and the front and back sides of RD-TD were processed in 2 passes respectively. The process parameters were selected as follows: main gas temperature 250℃, main gas pressure 1MPa, path spacing 6mm, gun muzzle height 15mm, steel shot as particles, particle diameter 0.2mm, and main gas compressed air.
[0053] The magnesium alloy sheet after micro-forging was subjected to three equal channel bending deformations at a constant temperature of 200°C. The main parameters of the equal channel bending deformation die were as follows: bending deformation angle 2θ=150°, upper die fillet radius R1=1mm, lower die fillet radius R0=3mm, inclined section length L=35mm, flat section length: L0=20mm, L1=35mm, upper die opening and closing speed V1=V2=100mm / min, feed direction along RD direction, and feed step length of 0.5mm.
[0054] like Figure 4 As shown, the three-pass bending deformation path process of Example 2 is as follows: after the first pass of equal channel bending deformation, the plate is rotated 180° around its rolling direction (RD) axis, followed by the second pass of equal channel bending deformation, and then the plate is rotated 180° around the rolling direction (RD) axis again to perform the third pass of equal channel bending deformation.
[0055] like Figure 5 As shown, the mechanical properties comparison diagram of Example 2 and 1 mm initial magnesium alloy sheet stretched at room temperature. As can be seen from the figure, three equal channel bending deformations after micro-forging can achieve a synergistic improvement in plasticity and strength of magnesium alloy sheet.
[0056] Example 3
[0057] In this embodiment, a 2 mm thick AZ31 commercial magnesium alloy rolled sheet is cut into long billets of 300 (RD) × 55 (TD) mm.
[0058] The cut long billets were annealed at 250°C for 2h to obtain a twin-free microstructure.
[0059] The initial magnesium alloy sheet after annealing was subjected to single-pass equal channel bending deformation at a constant temperature of 150°C. The main parameters of the equal channel bending deformation die were: bending deformation angle 2θ=150°, upper die fillet radius R1=1mm, lower die fillet radius R0=3mm, inclined section length L=35mm, flat section length: L0=20mm, L1=35mm, upper die opening and closing speed V1=V2=100mm / min, feed direction along RD direction, and feed step length of 2mm.
[0060] The magnesium alloy sheet after bending deformation was subjected to particle micro-forging through cold spraying equipment, and two passes were performed on the front and back sides of RD-TD respectively. The process parameters were selected as follows: main gas temperature 250℃, main gas pressure 1MPa, path spacing 6mm, gun muzzle height 15mm, steel shot particles, particle diameter 0.2mm, and main gas compressed air.
[0061] Depend on Figure 3 It can be seen that the uniform elongation of PMF-ECAB-150 sheet is significantly improved, 29.1% higher than that of the initial magnesium alloy sheet, and the elongation at break is not much different from that of the initial magnesium alloy sheet; its yield strength and tensile strength are higher than those of the initial magnesium alloy sheet. Comparing PMF-ECAB-150 sheet with PMF sheet and ECAB-150 sheet, it is found that the uniform elongation of PMF-ECAB-150 sheet is significantly higher than that of PMF sheet and ECAB-150 sheet; and the strength of PMF-ECAB-150 sheet is higher than that of PMF sheet and ECAB-150 sheet.
[0062] Analysis shows that the PMF sheet has large internal residual stress, and severe work hardening will occur during the plastic deformation process, which will reduce the plasticity of the sheet. After 150°C equal channel bending deformation, part of the internal energy of the PMF sheet can be released, reducing the stress concentration of the sheet. The grain gradient structure presented on the surface of the PMF-ECAB-150 sheet will cause completely different flow stress zones due to different grain sizes. The soft zone will bear more plastic strain and easily form dispersed microscopic strain bands, which can significantly improve the uniform elongation of the sheet. The fine-grained layer of the sheet can play a role in fine-grain strengthening to a certain extent and improve the strength of the sheet. The above combined effects significantly increase the uniform elongation of the sheet after composite processing and significantly improve its strength.
Claims
1. A method for preparing a high-performance alloy sheet using a gradient structure and a twin composite structure, characterized in that: The following steps are involved: 1) Annealing the initial thin plate to obtain a large grain structure without twin structure; 2) After annealing, the thin plate is subjected to particle micro-forging by controlling the process parameters of the cold spraying equipment to refine the grains in the surface area and obtain a gradient grain structure; 3) Composite processing is performed on the alloy thin plate. The micro-forged alloy thin plate is subjected to equal channel bending deformation processing. By controlling the bending deformation passes and deformation path, different twin numbers and twin types can be introduced into the plate.
2. The method for preparing a high-performance alloy sheet using a gradient structure and a twin composite structure according to claim 1, characterized in that: The method is applicable to magnesium alloy thin plates, zinc alloy thin plates, titanium alloy thin plates, cobalt alloy thin plates or zirconium alloy thin plates having the same hexagonal close-packed structure (HCP).
3. The method for preparing a high-performance alloy sheet using a gradient structure and a twin composite structure as claimed in claim 2, characterized in that: The magnesium alloy sheet includes a commercial AZ31 magnesium alloy sheet, and the sheet thickness is less than 3 mm.
4. The method for preparing a high performance alloy sheet using a gradient structure and a twin composite structure according to claim 1, characterized in that: In step 1), the initial magnesium alloy rolled sheet is annealed at a temperature of 150-500° C. for 0.5-15 h.
5. The method for preparing a high performance alloy sheet using a gradient structure and a twin composite structure according to claim 1, characterized in that: In step 2), the process parameters for micro-forging by cold spraying equipment include: main gas temperature 25-500°C, main gas pressure 1-5MPa, path spacing 5-10mm, muzzle height from plate 10-25mm, and steel shot as granular material with a granular diameter of 0.1-0.5mm.
6. The method for preparing a high performance alloy sheet using a gradient structure and a twin composite structure according to claim 1, characterized in that: In step 3), the bending deformation parameters mainly include: bending deformation temperature of 25 to 400° C., bending deformation passes of single or multiple passes, and bending deformation paths of the same path, a path rotating around the normal direction (ND) or a path rotating around the rolling direction (RD).
7. The method for preparing a high performance alloy sheet using a gradient structure and a twin composite structure as claimed in claim 1, characterized in that: In step 3), the composite processing sequence of the alloy thin plate is changed, and a micro-forging process is first performed to introduce a gradient grain structure into the alloy thin plate, and then twins are introduced into the alloy thin plate through bending deformation; or, twins are first introduced into the alloy thin plate through bending deformation, and then a micro-forging process is performed to introduce a gradient grain structure into the alloy thin plate.