Cr-Al-N gradient coating for zirconium alloy protection and preparation method thereof

By designing the Cr-Al-N gradient coating, the Al content is regulated to form a gradient structure with high internal and low external conditions, the erosion problem of zirconium alloy in high-temperature water vapor environment is solved, and effective in high-temperature and high-pressure water and accident conditions is achieved. Protection improves the oxidation and corrosion resistance of zirconium alloy.

CN119020724APending Publication Date: 2024-11-26INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202310607280.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Zirconium alloys are prone to violent reactions in high-temperature water vapor environments, resulting in heat and hydrogen release, which may cause explosions, and the existing coatings are insufficiently eroded in high-temperature and high-pressure water, which cannot effectively prevent the leakage of radioactive substances.

Method used

Design a Cr-Al-N gradient coating, and continuously reduces Al content from the inside to the outside, form a gradient structure with high Al in the inner layer and low Al in the outer layer, and is prepared by physical vapor deposition-magnetically controlled sputtering method to ensure that Stable Cr2O3 and Al2O3 oxide layers are formed under high temperature and high pressure water and accident conditions.

Benefits of technology

It achieves good protective effects under normal working conditions and accidental working conditions, improves the oxidation and corrosion resistance of zirconium alloy, reduces the material oxidation rate, and enhances its resistance to water vapor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020724A_ABST
    Figure CN119020724A_ABST
Patent Text Reader

Abstract

The invention relates to the field of nuclear power zirconium alloy cladding protective coatings, in particular to a Cr-Al-N gradient coating for zirconium alloy protection and a preparation method of the Cr-Al-N gradient coating. The content of solid solution Al in the Cr-Al-N coating is continuously reduced from inside to outside to form a Cr < 1-x > Al < x > N gradient coating, the upper limit range x of the solid solution amount of Al in the gradient coating is 0.45-0.7, the lower limit range x of the solid solution amount of Al is 0.02-0.15, and x is atomic percent. The coating is prepared by adopting a physical vapor deposition-magnetron sputtering technology, N2 / Ar mixed gas is taken as working gas, and continuous change of the solid solution Al content of the coating from inside to outside is realized by adjusting the sputtering power of Cr and Al to a target. The inner layer of the coating is high Al, and the outer layer of the coating is low Al, so that a Cr2O3 layer resistant to high-temperature and high-pressure water corrosion is generated on the surface of the coating in a normal service environment, and an Al2O3 layer resistant to water vapor corrosion is generated in an accident condition, and therefore, intelligent response of the coating to different service environments is realized; therefore, good protection can be provided in a high-temperature and high-pressure water environment under a normal working condition and a high-temperature water vapor environment under an accident working condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of nuclear power zirconium alloy cladding protective coatings, in particular to a Cr-Al-N gradient coating for zirconium alloy protection and a preparation method thereof. Background Art

[0002] Zirconium alloys are widely used as fuel cladding materials for light water reactors and are known as the "first safety barrier" to prevent nuclear fuel leakage. However, the core dehydration accident at the Fukushima Nuclear Power Plant in Japan in 2011 exposed the shortcomings of current zirconium alloy cladding materials in resisting severe accidents. Zirconium alloys react violently with water vapor above 800°C, releasing a large amount of heat and hydrogen. The byproduct hydrogen can easily cause an explosion, resulting in damage to the containment building, and causing highly radioactive fission products to leak into the environment, causing serious consequences. Compared with the development of new non-zirconium alloy cladding materials, applying a protective coating on the surface of zirconium alloys can improve the mechanical properties and oxidation resistance of zirconium alloy cladding while retaining the existing nuclear power plant design, and has higher economic benefits. The coating technology has the shortest R&D cycle, which can realize the replacement of nuclear power plants in a short period of time and improve the ability of existing nuclear reactors to resist accidents.

[0003] Domestic and foreign scholars have conducted a large number of studies, showing that coatings can alleviate the damage of high-temperature water vapor to zirconium alloys to a certain extent. At present, the research is mainly focused on metal coatings (Cr, CrAl, FeCrAl, etc.) and ceramic materials (SiC, Cr2AlC, TiAlN, etc.). Studies have found that in the high-temperature and high-pressure water corrosion process under normal working conditions, the Al in the Al-containing CrAl and TiAlN coatings will quickly react with water to form boehmite phase (AlOOH), which cannot prevent the further erosion of the coating by high-temperature and high-pressure water; in the high-temperature water vapor environment, the Al2O3 oxide layer has higher high-temperature stability than the Cr2O3 oxide layer, and therefore has better high-temperature protection effect.

[0004] In summary, designing a gradient coating for zirconium alloy protection that simultaneously meets the requirements of high-temperature and high-pressure water corrosion under normal conditions and high-temperature water vapor oxidation performance under accident conditions has significant advantages among the candidate coatings for zirconium alloys and has practical value. Summary of the invention

[0005] The purpose of the present invention is to provide a Cr-Al-N gradient coating for zirconium alloy protection and a preparation method thereof. The unique composition gradient design of the Al solid solution content in the coating composition enables it to provide effective protection in the high temperature and high pressure water environment under normal working conditions and the high temperature steam under accident conditions.

[0006] In order to achieve the above object, the technical solution of the present invention is as follows:

[0007] A Cr-Al-N gradient coating for zirconium alloy protection is formed by adjusting the Al content of the solid solution in the Cr-Al-N coating to continuously decrease from the inside to the outside. 1-x Al x N gradient coating, the upper limit range of Al solid solubility in the gradient coating is x=0.45-0.7, the lower limit range of Al solid solubility is x=0.02-0.15, and x is atomic percentage.

[0008] The Cr-Al-N gradient coating for zirconium alloy protection has a gradient composition with continuous linear gradient changes, and the inner layer of the gradient coating has high Al and the outer layer has low Al.

[0009] The Cr-Al-N gradient coating for zirconium alloy protection has a thickness of 8 to 16 μm.

[0010] The method for preparing the Cr-Al-N gradient coating for zirconium alloy protection is described. The coating is prepared by physical vapor deposition-magnetron sputtering. The gradient coating is prepared by co-sputtering a Cr target and an Al target in a nitrogen and argon mixed atmosphere. The specific operation steps are as follows:

[0011] 1) Substrate pretreatment: Before coating, the sample surface was coarsely ground, finely ground and polished, and then ultrasonically cleaned with acetone, alcohol and deionized water in sequence;

[0012] 2) Using argon as the working gas, the Cr buffer layer was prepared by magnetron sputtering;

[0013] 3) Magnetron sputtering is used to prepare gradient coatings: the substrate is heated, a N2 / Ar mixed gas is used as the working gas, and the sputtering power of Cr and Al to the target is adjusted to change linearly, thereby achieving a continuous gradient change of the Al content in the coating from the inside to the outside.

[0014] In the preparation method of the Cr-Al-N gradient coating for zirconium alloy protection, in step 2), the thickness of the Cr buffer layer is 1 to 3 μm to alleviate the mismatch problem of thermal expansion coefficients between the Cr-Al-N coating and the substrate, and to improve the adhesion performance between the coating and the substrate.

[0015] In the method for preparing the Cr-Al-N gradient coating for zirconium alloy protection, in step 3), the substrate heating temperature is 200°C to 400°C.

[0016] The method for preparing the Cr-Al-N gradient coating for zirconium alloy protection, in step 3), the Cr-Al-N gradient coating is prepared by co-sputtering Cr and Al, and the change of the Al content gradient is achieved by controlling the relative power of the Cr and Al targets during the sputtering process through a PID program, and the power density of the Cr target is 3.54-5.31 W / cm 2, Al target power density range is 0.7~5.66W / cm 2 , and a negative bias of 20 to 70 V is applied to the substrate, and the thickness of the gradient coating is 8 to 16 μm.

[0017] In the preparation method of the Cr-Al-N gradient coating for zirconium alloy protection, in step 3), the introduction of N element in the coating is obtained by the working gas in the magnetron sputtering process, and a mixed gas of N2 / Ar is used as the working gas, the argon flow range is: 8~30SCCM, and the nitrogen flow range is: 4~15SCCM.

[0018] The design idea of ​​the present invention is:

[0019] Zirconium alloy reacts violently with water vapor above 800℃, releasing a large amount of heat and hydrogen, which can easily cause explosions and leak radioactive products. Applying a protective coating is an effective way to reduce the oxidation rate of the material and reduce the contact between zirconium alloy and water vapor. In addition, the material has been in high temperature and high pressure water environment for a long time, so it should also have good water corrosion resistance. The Gibbs free energy of forming Cr2O3 and Al2O3 at high temperature (1200℃) is:

[0020] 2Cr + 3 / 2O2 → Cr2O3 -750.9 kJ / mol (1)

[0021] 2Al + 3 / 2O2 → Al2O3 -1190.5 kJ / mol (2)

[0022] Stable and dense Al2O3 is easier to form at high temperatures, thus having good antioxidant properties. In high-temperature and high-pressure water, Cr forms a dense Cr2O3 oxide layer, which makes it have good water corrosion resistance, while the Al in the Al-containing coating will quickly react with water to form a boehmite phase (AlOOH), which cannot prevent the high-temperature and high-pressure water from further corroding the coating. Based on the above principles, the present invention designs a Cr-Al-N gradient coating with low Al on the outside and high Al on the inside, so that it can provide good protection in both the high-temperature and high-pressure water environment under normal working conditions and the high-temperature water vapor environment under accident conditions.

[0023] From the perspective of composition design: The primary purpose of designing and preparing gradient coatings is to form a stable and slowly growing surface oxide layer, which plays a certain role in inhibiting atomic diffusion between the coating and the substrate. The Cr and Al elements that form Cr2O3 and Al2O3 are often used to resist high-temperature oxidation and corrosion environments. Therefore, the coating uses Cr and Al elements.

[0024] From the perspective of coating structure: Cr-containing coatings can form a stable and dense Cr2O3 oxide layer in a high-temperature and high-pressure water environment, and coatings with high Al content can form a stable α-Al2O3 oxide layer at high temperatures. Therefore, the coating gradient is designed to be low Al on the outside and high Al on the inside.

[0025] The present invention has the following advantages and beneficial effects:

[0026] The present invention adopts the magnetron sputtering technology of Cr and Al dual targets co-sputtering, and achieves the purpose of composition control by regulating the power density of Cr and Al targets, thereby realizing a continuous gradient change of Al content from the inside to the outside in the coating, and the continuous change of composition is different from the conventional multi-layer coating. In the Cr-Al-N gradient coating, the Al solid solution amount x on the inner side is 0.45-0.7, and the Al solid solution amount x on the outer side is 0.02-0.15. The inner layer of the gradient coating is high Al and the outer layer is low Al. The special composition structure design enables the surface to generate a Cr2O3 layer that is resistant to high temperature and high pressure water corrosion under normal service conditions, and generates an Al2O3 layer that is resistant to water vapor corrosion under accident conditions, thereby realizing the intelligent response of the coating to different service environments, thereby providing good protection effects in both the high temperature and high pressure water environment under normal conditions and the high temperature water vapor environment under accident conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The Cr on the zirconium alloy matrix of the present invention 1-x Al x Schematic diagram of the N gradient coating structure.

[0028] Figure 2 The Cr / Cr 1-x Al x Oxidation kinetics curve of N gradient coating sample oxidized by water vapor at 1200℃ for 1h. In the figure, the horizontal axis Time represents time (s), and the vertical axis Weightgain represents weight gain (mg / cm 2 ).

[0029] Figure 3 The Cr / Cr 1-x Al x XRD spectrum of the N gradient coating sample after water vapor oxidation at 1200℃ for 1h.

[0030] In the figure, the abscissa 2θ represents the diffraction angle (deg.), and the ordinate Intensity represents the relative intensity (au).

[0031] Figure 4 The zirconium alloy matrix (a), Cr / AlN (b), Cr / CrN (c), Cr / Cr 1-x Alx Surface morphology and elemental composition of N(d) gradient coating sample after 24h of high temperature and high pressure water corrosion at 360℃ and 18.6MPa. DETAILED DESCRIPTION

[0032] In the specific implementation process, the present invention adopts magnetron sputtering technology to prepare the Cr-Al-N coating. The specific operation steps of the method are as follows:

[0033] 1) Substrate pretreatment: The sample surface was coarsely ground, finely ground and polished before coating, and then ultrasonically cleaned with acetone, alcohol and deionized water in sequence;

[0034] 2) Preparation of Cr buffer layer by magnetron sputtering;

[0035] 3) Preparation of Cr by magnetron sputtering 1-x Al x N gradient coating: The substrate is heated, and a mixture of N2 / Ar is used as the working gas. By adjusting the sputtering power of Cr and Al on the target, the Al content of the solid solution in the coating can be continuously changed from the inside to the outside.

[0036] The present invention is further described in detail below by examples and drawings. However, these examples shall not be interpreted as limiting the scope of protection of the present invention, and all changes within the basic idea of ​​the technical solution of the present invention or essentially equivalent to the technical solution of the present invention are within the scope of protection of the present invention.

[0037] Example 1

[0038] In this embodiment, a method for preparing a Cr-Al-N gradient coating for zirconium alloy protection is as follows:

[0039] 1) Substrate pretreatment: The sample surface was coarsely ground, finely ground and polished before coating, and then ultrasonically cleaned with acetone, alcohol and deionized water for 15 min each;

[0040] 2) Magnetron sputtering was used to prepare the Cr buffer layer: Cr target was used as the target material, the substrate was heated to 300 °C, and the back vacuum pressure was 2×10 -4 Pa, Ar gas is the working gas, the gas flow rate is 15 SCCM, the sputtering power is 80 W, the sputtering time is 60 min, the working gas pressure is 0.5 Pa, and a Cr buffer layer with a thickness of 2 μm is deposited on the zirconium alloy substrate. Among them, the diameter of the chromium target is 60 mm, and the target distance is 70 mm;

[0041] 3) Preparation of Cr-Al-N gradient coating by magnetron sputtering: The Cr-Al-N gradient coating was deposited on the prepared Cr buffer layer, with a mixed gas of Ar and N2 as the working gas, an Ar gas flow rate of 10 SCCM, a N2 gas flow rate of 10 SCCM, an Al target sputtering power of 160-20 W (power density of 5.66-0.7 W / cm 2 ), the power decreases linearly with the sputtering time, the target distance is 60 mm, the Cr target sputtering power is 100-150 W (power density is 3.54-5.31 W / cm 2 ), the power increased linearly with the sputtering time, the target distance was 70 mm, the power of the two sputtering targets was controlled by a PID program, the working pressure was 0.5 Pa, and the sputtering time was 5 h. In addition, a negative bias of 30 V was applied to the substrate, and the thickness of the gradient coating was 12 μm.

[0042] like Figure 1 As shown, in this embodiment, a Cr buffer layer and a Cr-Al-N gradient coating are sequentially prepared on the surface of Zry-4 zirconium alloy by magnetron sputtering. The bottom layer of the Cr-Al-N gradient coating is Cr. 0.3 Al 0.7 The surface composition of Cr-Al-N gradient coating is Cr 0.9 Al 0.1 N, the inner layer of the gradient coating is high in Al, the outer layer is low in Al, and the Al content is distributed in a gradient from the inside to the outside; at the same time, the inner layer of the gradient coating is low in Cr, the outer layer is high in Cr, and the Cr content is distributed in a gradient from the inside to the outside.

[0043] Depend on Figure 2 and Figure 3 It can be observed that after 1200℃ water vapor oxidation test, the gradient coating sample prepared on the surface of Zry-4 zirconium alloy has a lower oxidation rate than that of Zry-4 bare zirconium alloy, and XRD results show that Cr2O3 and α-Al2O3 oxide layers are generated.

[0044] Example 2

[0045] In this embodiment, a method for preparing a CrN coating for zirconium alloy protection is as follows:

[0046] 1) Substrate pretreatment: The sample surface was coarsely ground, finely ground and polished before coating, and then ultrasonically cleaned with acetone, alcohol and deionized water for 15 min each;

[0047] 2) Magnetron sputtering was used to prepare the Cr buffer layer: Cr target was used as the target material, the substrate was heated to 300 °C, and the back vacuum pressure was 2×10 -4Pa, Ar gas is the working gas, the gas flow rate is 15 SCCM, the sputtering power is 80 W, the sputtering time is 60 min, the working gas pressure is 0.5 Pa, and a Cr buffer layer with a thickness of 2 μm is deposited on the zirconium alloy substrate. Among them, the diameter of the chromium target is 60 mm, and the target distance is 70 mm;

[0048] 3) Preparation of CrN coating by magnetron sputtering: The CrN coating was deposited on the prepared Cr buffer layer, with a mixed gas of Ar and N2 as the working gas, the Ar gas flow rate was 10 SCCM, the N2 gas flow rate was 10 SCCM, the Cr target sputtering power was 80 W, the target distance was 70 mm, the working gas pressure was 0.5 Pa, the sputtering time was 6 h, and the thickness of the CrN coating was 12 μm.

[0049] Depend on Figure 4 It can be seen that after 24h of high temperature and high pressure water corrosion test at 360°C and 18.6MPa, a relatively dense Cr2O3 layer is generated after CrN corrosion. Compared with the Cr-Al-N gradient coating prepared in Example 1, the oxide layer formed on the surface of the Cr-Al-N gradient coating has a few voids, and the outermost oxide layer is relatively loose.

[0050] Example 3

[0051] In this embodiment, a method for preparing an AlN coating for zirconium alloy protection is as follows:

[0052] 1) Substrate pretreatment: The sample surface was coarsely ground, finely ground and polished before coating, and then ultrasonically cleaned with acetone, alcohol and deionized water for 15 min each;

[0053] 2) Magnetron sputtering was used to prepare the Cr buffer layer: Cr target was used as the target material, the substrate was heated to 300 °C, and the back vacuum pressure was 2×10 -4 Pa, Ar gas is the working gas, the gas flow rate is 15 SCCM, the sputtering power is 80 W, the sputtering time is 60 min, the working gas pressure is 0.5 Pa, and a Cr buffer layer with a thickness of 2 μm is deposited on the zirconium alloy substrate. The diameter of the chromium target is 60 mm, and the target distance is 70 mm.

[0054] 3) Preparation of AlN coating by magnetron sputtering: AlN coating was deposited on the prepared Cr buffer layer, with a mixed gas of Ar and N2 as the working gas, an Ar gas flow rate of 10 SCCM, an N2 gas flow rate of 10 SCCM, a Cr target sputtering power of 80 W, a target distance of 70 mm, a working gas pressure of 0.5 Pa, a sputtering time of 7.5 h, and a CrN coating with a thickness of 12 μm.

[0055] Depend on Figure 4It can be seen that after 24h of high temperature and high pressure water corrosion test at 360℃ and 18.6MPa, the AlN on the coating surface is almost completely consumed. This is because AlN reacts with H2O to generate water-soluble boehmite AlO(OH) in the high temperature and high pressure water environment.

[0056] The results of the embodiments show that the present invention shows that CrN can generate a dense protective oxide layer in a high-temperature and high-pressure water environment, and has a significant protective effect; while the high-Al Cr-Al-N gradient coating forms a loose coating surface and has no protective properties due to the formation of water-soluble boehmite AlO(OH). However, in a high-temperature water vapor environment of 1200°C, the high-Al Cr-Al-N gradient coating generates Cr2O3 and α-Al2O3 oxide layers, which have good protective properties. The Cr-Al-N gradient coating designed by the present invention has low Al on the outside and high Al on the inside, so that it can provide good protection in both the high-temperature and high-pressure water environment of normal working conditions and the high-temperature water vapor environment of accident conditions.

Claims

1. A Cr-Al-N gradient coating for zirconium alloy protection, characterized in that: By adjusting the Al content of solid solution in the Cr-Al-N coating, the Cr 1-x Al x N gradient coating, the upper limit range of Al solid solubility in the gradient coating is x=0.45-0.7, the lower limit range of Al solid solubility is x=0.02-0.15, and x is atomic percentage.

2. The Cr-Al-N gradient coating for zirconium alloy protection according to claim 1, characterized in that: The composition of the gradient coating changes continuously and linearly, with the inner layer of the gradient coating having high Al and the outer layer having low Al.

3. The Cr-Al-N gradient coating for zirconium alloy protection according to claim 1, characterized in that: The thickness of the gradient coating is 8 to 16 μm.

4. A method for preparing a Cr-Al-N gradient coating for zirconium alloy protection according to any one of claims 1 to 3, characterized in that: The coating is prepared by physical vapor deposition-magnetron sputtering method, and the gradient coating is prepared by co-sputtering of Cr target and Al target in a mixed atmosphere of nitrogen and argon. The specific operation steps are as follows: 1) Substrate pretreatment: Before coating, the sample surface was coarsely ground, finely ground and polished, and then ultrasonically cleaned with acetone, alcohol and deionized water in sequence; 2) Using argon as the working gas, the Cr buffer layer was prepared by magnetron sputtering; 3) Magnetron sputtering is used to prepare gradient coatings: the substrate is heated, a N2 / Ar mixed gas is used as the working gas, and the sputtering power of Cr and Al to the target is adjusted to change linearly, thereby achieving a continuous gradient change of the Al content in the coating from the inside to the outside.

5. The method for preparing the Cr-Al-N gradient coating for zirconium alloy protection according to claim 4, characterized in that: In step 2), the thickness of the Cr buffer layer is 1-3 μm to alleviate the mismatch problem of thermal expansion coefficients between the Cr-Al-N coating and the substrate, and to improve the adhesion between the coating and the substrate.

6. The method for preparing a Cr-Al-N gradient coating for zirconium alloy protection according to claim 4, characterized in that: In step 3), the substrate is heated to a temperature of 200°C to 400°C.

7. The method for preparing a Cr-Al-N gradient coating for zirconium alloy protection according to claim 4, characterized in that: In step 3), the Cr-Al-N gradient coating is prepared by co-sputtering of Cr and Al. The change of the Al content gradient is achieved by controlling the relative power of the Cr and Al targets during the sputtering process through a PID program. The power density of the Cr target is 3.54-5.31 W / cm 2 , Al target power density range is 0.7~5.66W / cm 2 , and a negative bias of 20 to 70 V is applied to the substrate, and the thickness of the gradient coating is 8 to 16 μm.

8. The method for preparing a Cr-Al-N gradient coating for zirconium alloy protection according to claim 4, characterized in that: In step 3), the introduction of N element in the coating is obtained by the working gas in the magnetron sputtering process, with a mixed gas of N2 / Ar as the working gas, an argon flow rate range of 8 to 30 SCCM, and a nitrogen flow rate range of 4 to 15 SCCM.

Citation Information

Cited By

  • Multi-layer composite (Cr, Al) Nx / Cr protective coating for zirconium alloy cladding of nuclear reactor and preparation method of multi-layer composite (Cr, Al) Nx / Cr protective coating

    CN121087423A

  • A multilayer composite (Cr, Al)N for zirconium alloy cladding of nuclear reactors x / Cr protective coating and method of manufacture

    CN121087423B

  • Continuous gradient Cr-Al coating of zirconium alloy cladding and preparation method of continuous gradient Cr-Al coating