Shrink-resistant warm-keeping fabric and preparation method thereof

Through enzyme pretreatment and post-organization of cashmere and bamboo fibers, a continuous film is formed, which solves the problem of shrinkage of the fabric under humid and heat conditions, and improves the anti-shrinkage performance and warmth effect.

CN119020995APending Publication Date: 2024-11-26SHENZHEN WANQI APPAREL LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411093819.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the prior art, the fabric containing cashmere and bamboo fiber has poor anti-shrinkage properties, resulting in the fabric being prone to shrink under humid and hot conditions.

Method used

Pretreatment of enzymes such as D-arabinose and papain is adopted, and then sorted out after combining to form a continuous film, reducing the shrinkage and water absorption capacity of the fibers, and improving the anti-shrinkage performance of the fabric.

Benefits of technology

It significantly improves the anti-shrinkage properties of cashmere and bamboo fiber blended fabrics, enhances the warmth and reduces the shrinkage and water absorption of fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020995A_ABST
    Figure CN119020995A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of fabrics, in particular to a shrink-resistant warm-keeping fabric and a preparation method thereof. The shrink-resistant warm-keeping fabric is prepared from the cashmere and the bamboo fibers as raw materials, and has excellent warm-keeping performance; wherein the cashmere is pretreated, so that the shrinkage resistance of the fabric can be effectively improved, and the prepared fabric base cloth can hydrolyze scale surface protein and weaken a directional friction effect through after-finishing treatment, so that the shrinkage of a cashmere fiber body is reduced; scales on the surface of the cashmere are covered through after-finishing treatment, a continuous film is formed, and shrinkage of cashmere fiber bodies is further reduced; through after-finishing treatment, a film layer can be formed on the surface of the bamboo fiber, the water absorption capacity of the bamboo fiber is reduced, and then the shrinkage resistance of the bamboo fiber is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fabrics, and in particular to an anti-shrinkage warm-keeping fabric and a preparation method thereof. Background Art

[0002] In the cold winter, clothing made of warm fabrics is widely loved. Fabrics made of chemical fibers such as polyacrylonitrile fibers (acrylic fibers) have good warming effects, but they are prone to static electricity and are not comfortable to wear. Natural fibers such as cashmere and bamboo fibers not only have good warming properties, but also do not generate static electricity. However, the surface of cashmere contains a scale structure. When it is wet and hot, the scales expand. When it is subjected to mechanical external forces, the scales have a directional friction effect, which causes the fibers to move in a directional manner, causing the fiber aggregate to gradually shrink and become tight, making the cashmere fabric easy to shrink. Bamboo fibers, however, are full of pores in their cross-sections and can absorb a large amount of water in an instant, causing the volume to expand and shrink after drying.

[0003] Chinese patent CN106884258B discloses an antistatic silk cashmere knitted fabric suitable for spring and summer wear and a preparation method thereof, which reduces the shrinkage resistance of the fabric by enzyme treatment. However, for cashmere and bamboo fiber blended fabrics, it can only improve the shrinkage resistance of the cashmere fiber to a certain extent, and has no effect on improving the shrinkage resistance of the bamboo fiber. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a shrinkage-resistant thermal insulation fabric and a preparation method thereof, so as to solve the problem that the fabric containing cashmere and bamboo fiber in the prior art has poor shrinkage-resistant performance.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0006] A method for preparing a shrinkage-resistant thermal insulation fabric comprises the following steps:

[0007] Step 1, dissolving D-arabinose in a glycerol aqueous solution to obtain a D-arabinose solution, placing cashmere in the D-arabinose solution for a primary soaking treatment, and after the soaking is completed, draining and drying to obtain cashmere after the primary soaking treatment;

[0008] Step 2, dissolving papain in a sodium bisulfite aqueous solution, adjusting the pH value to 7, obtaining a papain solution, placing the cashmere treated by the primary immersion treatment in the papain solution for a secondary immersion treatment, draining and washing after the immersion is completed, and obtaining the cashmere treated by the secondary immersion treatment;

[0009] Step 3, dissolving saccharifying enzyme and alkaline pectinase in deionized water, adjusting the pH value to 7-8, obtaining a mixed enzyme solution, placing the cashmere yarn after the secondary immersion treatment in the mixed enzyme solution for a third immersion treatment, and after the immersion is completed, draining, cleaning, inactivating, washing, and drying to obtain modified cashmere;

[0010] Step 4: blending the modified cashmere with bamboo fiber to obtain blended yarn, and knitting the blended yarn into a fabric base cloth;

[0011] Step 5: Perform post-finishing treatment on the fabric base fabric to obtain shrinkage-resistant and warm-keeping fabric.

[0012] Preferably, in step 1, when preparing the D-arabinose solution, the mass ratio of D-arabinose to the glycerol aqueous solution is (0.5-1):100, and the glycerol aqueous solution is a 0.5 wt % glycerol aqueous solution.

[0013] Preferably, in the step 1, during the initial soaking treatment, the bath ratio is 1:10, and the soaking condition is soaking at room temperature for 1-3 hours.

[0014] Preferably, in step 2, when preparing the papain solution, the mass ratio of papain to sodium bisulfite aqueous solution is (1.5-2):100, and the sodium bisulfite aqueous solution is 1wt% sodium bisulfite aqueous solution.

[0015] Preferably, in the step 2, during the secondary immersion treatment, the bath ratio is 1:10, and the immersion condition is immersion at room temperature for 35 minutes.

[0016] Preferably, in step 3, when preparing the mixed enzyme solution, the mass ratio of saccharifying enzyme, alkaline pectinase and deionized water is (1-1.5):(1.5-2):100.

[0017] Preferably, in step three, during the third immersion, the bath ratio is 1:10, and the immersion condition is immersion at room temperature for 15 minutes.

[0018] Preferably, in step three, the inactivation condition is to perform enzyme inactivation treatment in 90° C. hot water for 5 minutes.

[0019] Preferably, in step 4, the mass ratio of modified cashmere to bamboo fiber is (1-2):1, the count of the blended yarn is 20-30S (English count), and the gram weight of the fabric base fabric is 150-200g / m 2 .

[0020] Preferably, in step 5, the post-processing process includes:

[0021] Place the fabric base in a dihydroxymethyl dihydroxyethylene urea solution with a bath ratio of 1:10, double immersion and double rolling, with a rolling rate of 60%, dry at 60°C for 5 hours, and bake at 100°C for 30 minutes. Then place it in a silicone softener solution with a bath ratio of 1:10, double immersion and double rolling, with a rolling rate of 60%, dry at 60°C for 5 hours, and bake at 100°C for 30 minutes.

[0022] The invention also discloses a shrinkage-resistant thermal insulation fabric prepared by adopting the shrinkage-resistant thermal insulation fabric preparation method.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] In the present invention, cashmere and bamboo fiber are used as raw materials to prepare fabrics, which have excellent warmth retention performance; wherein, pre-treating the cashmere can effectively improve the anti-shrinkage performance of the fabric, and the obtained fabric base cloth can further improve the anti-shrinkage performance of the fabric through post-finishing treatment;

[0025] When the scale structure on the surface of cashmere is soaked by moisture and heat, the scale expands. When subjected to mechanical external force, the scale has a directional friction effect, causing the fiber to move in a directional manner, resulting in the gradual contraction and compaction of the fiber aggregate. Through enzyme pretreatment, the protein on the surface of the scale can be hydrolyzed to weaken the directional friction effect, thereby reducing the shrinkage of the cashmere fiber body; through post-finishing treatment, the scales on the surface of the cashmere are covered to form a continuous film, further reducing the shrinkage of the cashmere fiber body;

[0026] Because the cross-section of bamboo fiber is full of pores, it can absorb a large amount of water in an instant, causing its volume to expand. After drying, it will shrink. Through post-finishing treatment, a film layer can be formed on the surface of the bamboo fiber, reducing the water absorption capacity of the bamboo fiber, thereby reducing the bamboo fiber's anti-shrinkage performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The present invention is a flow chart of the preparation process of the shrinkage-resistant thermal insulation fabric;

[0028] Figure 2 It is a bar chart showing the test results of the anti-shrinkage performance of the anti-shrinkage thermal insulation fabrics prepared in Examples 1-6 of the present invention and Comparative Examples 1-2. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] This embodiment discloses a method for preparing a shrinkage-resistant thermal insulation fabric, comprising the following steps:

[0032] Step 1, dissolving D-arabinose in a 0.5wt% glycerol aqueous solution, the mass ratio of D-arabinose to the 0.5wt% glycerol aqueous solution is 0.5:100, to obtain a D-arabinose solution, placing cashmere in the D-arabinose solution for a primary soaking treatment, the bath ratio is 1:10, soaking for 1h at room temperature, after the soaking is completed, draining, and drying at 60°C for 5h to obtain cashmere after the primary soaking treatment;

[0033] Step 2, dissolving papain in a 1wt% sodium bisulfite aqueous solution, the mass ratio of papain to the 1wt% sodium bisulfite aqueous solution is 1.5:100, adjusting the pH value to 7, obtaining a papain solution, placing the cashmere treated by the primary immersion treatment in the papain solution for a secondary immersion treatment, the bath ratio is 1:10, soaking at room temperature for 35 minutes, after the immersion is completed, draining, washing with deionized water 3 times, obtaining the cashmere treated by the secondary immersion treatment;

[0034] Step 3, dissolving saccharifying enzyme and alkaline pectinase in deionized water, the mass ratio of saccharifying enzyme, alkaline pectinase and deionized water is 1:1.5:100, adjusting the pH value to 7, obtaining a mixed enzyme solution, placing the cashmere yarn after the secondary impregnation treatment in the mixed enzyme solution for a third immersion treatment, the bath ratio is 1:10, soaking at room temperature for 15 minutes, after the immersion is completed, draining, washing with deionized water 3 times, placing in 90°C hot water for enzyme inactivation treatment for 5 minutes, washing with deionized water 3 times, and drying at 60°C for 5 hours to obtain modified cashmere;

[0035] Step 4: Blend the modified cashmere with bamboo fiber, the mass ratio of the modified cashmere to the bamboo fiber is 1:1, and obtain blended yarn, the count of the blended yarn is 20S, and the blended yarn is made into a fabric base fabric through a knitting process, and the gram weight of the fabric base fabric is 200g / m 2 ;

[0036] Step 5: Perform post-finishing treatment on the fabric base fabric to obtain shrinkage-resistant and warm-keeping fabric;

[0037] Among them, the post-processing process includes:

[0038] The fabric base is placed in a dihydroxymethyl dihydroxyethylene urea aqueous solution with a bath ratio of 1:10, two dips and two rolls, the roll ratio is 60%, dried at 60°C for 5 hours, and baked at 100°C for 30 minutes. Then, it is placed in a silicone softener solution with a bath ratio of 1:10, two dips and two rolls, the roll ratio is 60%, dried at 60°C for 5 hours, and baked at 100°C for 30 minutes;

[0039] The dimethylol dihydroxy ethylene urea aqueous solution is prepared by mixing dimethylol dihydroxy ethylene urea with deionized water, and the concentration of the dimethylol dihydroxy ethylene urea aqueous solution is 50 g / L;

[0040] The organic silicon softener solution is prepared from hydrophilic and skin-friendly silicone oil and deionized water. The mass percentage of the organic silicon softener in the organic silicon softener solution is 10%.

[0041] Example 2

[0042] This embodiment discloses a method for preparing a shrinkage-resistant thermal insulation fabric, comprising the following steps:

[0043] Step 1, dissolving D-arabinose in a 0.5wt% glycerol aqueous solution, the mass ratio of D-arabinose to the 0.5wt% glycerol aqueous solution is 1:100, to obtain a D-arabinose solution, placing cashmere in the D-arabinose solution for a primary soaking treatment, the bath ratio is 1:10, soaking for 1h at room temperature, after the soaking is completed, draining, and drying at 60°C for 5h to obtain cashmere after the primary soaking treatment;

[0044] Step 2, dissolving papain in a 1wt% sodium bisulfite aqueous solution, the mass ratio of papain to the 1wt% sodium bisulfite aqueous solution is 2:100, adjusting the pH value to 7, obtaining a papain solution, placing the cashmere treated by the primary immersion treatment in the papain solution for a secondary immersion treatment, the bath ratio is 1:10, and soaking for 35 minutes at room temperature. After the immersion is completed, draining, washing with deionized water 3 times, and obtaining the cashmere treated by the secondary immersion treatment;

[0045] Step 3, dissolving saccharifying enzyme and alkaline pectinase in deionized water, the mass ratio of saccharifying enzyme, alkaline pectinase and deionized water is 1.5:2:100, adjusting the pH value to 8, obtaining a mixed enzyme solution, placing the cashmere yarn after the secondary impregnation treatment in the mixed enzyme solution for a third immersion treatment, the bath ratio is 1:10, soaking at room temperature for 15 minutes, after the immersion is completed, draining, washing with deionized water 3 times, placing in 90°C hot water for enzyme inactivation treatment for 5 minutes, washing with deionized water 3 times, and drying at 60°C for 5 hours to obtain modified cashmere;

[0046] Step 4: Blend the modified cashmere with bamboo fiber, the mass ratio of the modified cashmere to bamboo fiber is 2:1, and obtain blended yarn, the count of the blended yarn is 30S, and the blended yarn is made into a fabric base fabric through a knitting process, and the weight of the fabric base fabric is 200g / m 2 ;

[0047] Step 5: Perform post-finishing treatment on the fabric base fabric to obtain shrinkage-resistant and warm-keeping fabric;

[0048] Among them, the post-processing process includes:

[0049] The fabric base is placed in a dimethylol dihydroxyethylene urea solution with a bath ratio of 1:10, two dips and two rolls, the roll ratio is 60%, dried at 60°C for 5 hours, and baked at 100°C for 30 minutes. Then, it is placed in a silicone softener solution with a bath ratio of 1:10, two dips and two rolls, the roll ratio is 60%, dried at 60°C for 5 hours, and baked at 100°C for 30 minutes;

[0050] The dimethylol dihydroxy ethylene urea aqueous solution is prepared by mixing dimethylol dihydroxy ethylene urea with deionized water, and the concentration of the dimethylol dihydroxy ethylene urea aqueous solution is 50 g / L;

[0051] The organic silicon softener solution is prepared from hydrophilic and skin-friendly silicone oil and deionized water. The mass percentage of the organic silicon softener in the organic silicon softener solution is 10%.

[0052] Example 3

[0053] This embodiment discloses a method for preparing a shrinkage-resistant thermal insulation fabric, comprising the following steps:

[0054] Step 1, dissolving D-arabinose in a 0.5wt% glycerol aqueous solution, the mass ratio of D-arabinose to the 0.5wt% glycerol aqueous solution is 0.6:100, to obtain a D-arabinose solution, placing cashmere in the D-arabinose solution for a primary soaking treatment, the bath ratio is 1:10, soaking for 1h at room temperature, after the soaking is completed, draining, and drying at 60°C for 5h to obtain cashmere after the primary soaking treatment;

[0055] Step 2, dissolving papain in a 1wt% sodium bisulfite aqueous solution, the mass ratio of papain to the 1wt% sodium bisulfite aqueous solution is 1.6:100, adjusting the pH value to 7, obtaining a papain solution, placing the cashmere treated by the primary immersion treatment in the papain solution for a secondary immersion treatment, the bath ratio is 1:10, and soaking for 35 minutes at room temperature. After the immersion is completed, draining, washing with deionized water 3 times, and obtaining the cashmere treated by the secondary immersion treatment;

[0056] Step 3, dissolving saccharifying enzyme and alkaline pectinase in deionized water, the mass ratio of saccharifying enzyme, alkaline pectinase and deionized water is 1.1:1.6:100, adjusting the pH value to 7.5, obtaining a mixed enzyme solution, placing the cashmere yarn after the secondary impregnation treatment in the mixed enzyme solution for a third immersion treatment, the bath ratio is 1:10, soaking at room temperature for 15 minutes, after the immersion is completed, draining, washing with deionized water 3 times, placing in 90°C hot water for enzyme inactivation treatment for 5 minutes, washing with deionized water 3 times, and drying at 60°C for 5 hours to obtain modified cashmere;

[0057] Step 4: Blend the modified cashmere with bamboo fiber, the mass ratio of the modified cashmere to bamboo fiber is 1.2:1, and obtain blended yarn, the count of the blended yarn is 30S, and the blended yarn is made into a fabric base fabric through a knitting process, and the weight of the fabric base fabric is 200g / m 2 ;

[0058] Step 5: Perform post-finishing treatment on the fabric base fabric to obtain shrinkage-resistant and warm-keeping fabric;

[0059] Among them, the post-processing process includes:

[0060] The fabric base is placed in a dimethylol dihydroxyethylene urea solution with a bath ratio of 1:10, two dips and two rolls, the roll ratio is 60%, dried at 60°C for 5 hours, and baked at 100°C for 30 minutes. Then, it is placed in a silicone softener solution with a bath ratio of 1:10, two dips and two rolls, the roll ratio is 60%, dried at 60°C for 5 hours, and baked at 100°C for 30 minutes;

[0061] The dimethylol dihydroxy ethylene urea aqueous solution is prepared by mixing dimethylol dihydroxy ethylene urea with deionized water, and the concentration of the dimethylol dihydroxy ethylene urea aqueous solution is 50 g / L;

[0062] The organic silicon softener solution is prepared from hydrophilic and skin-friendly silicone oil and deionized water. The mass percentage of the organic silicon softener in the organic silicon softener solution is 10%.

[0063] Example 4

[0064] This embodiment discloses a method for preparing a shrinkage-resistant thermal insulation fabric, comprising the following steps:

[0065] Step 1, dissolving D-arabinose in a 0.5wt% glycerol aqueous solution, the mass ratio of D-arabinose to the 0.5wt% glycerol aqueous solution is 0.7:100, to obtain a D-arabinose solution, placing cashmere in the D-arabinose solution for a primary soaking treatment, the bath ratio is 1:10, soaking for 1h at room temperature, after the soaking is completed, draining, and drying at 60°C for 5h to obtain cashmere after the primary soaking treatment;

[0066] Step 2, dissolving papain in a 1wt% sodium bisulfite aqueous solution, the mass ratio of papain to the 1wt% sodium bisulfite aqueous solution is 1.7:100, adjusting the pH value to 7, obtaining a papain solution, placing the cashmere treated by the primary immersion treatment in the papain solution for a secondary immersion treatment, the bath ratio is 1:10, soaking at room temperature for 35 minutes, after the immersion is completed, draining, washing with deionized water 3 times, obtaining the cashmere treated by the secondary immersion treatment;

[0067] Step 3, dissolving saccharifying enzyme and alkaline pectinase in deionized water, the mass ratio of saccharifying enzyme, alkaline pectinase and deionized water is 1.2:1.7:100, adjusting the pH value to 7.5, obtaining a mixed enzyme solution, placing the cashmere yarn after the secondary impregnation treatment in the mixed enzyme solution for a third immersion treatment, the bath ratio is 1:10, soaking at room temperature for 15 minutes, after the immersion is completed, draining, washing with deionized water 3 times, placing in 90°C hot water for enzyme inactivation treatment for 5 minutes, washing with deionized water 3 times, and drying at 60°C for 5 hours to obtain modified cashmere;

[0068] Step 4: Blend the modified cashmere with bamboo fiber, the mass ratio of the modified cashmere to bamboo fiber is 1.4:1, and obtain blended yarn, the count of the blended yarn is 30S, and the blended yarn is made into a fabric base fabric through a knitting process, and the weight of the fabric base fabric is 200g / m 2 ;

[0069] Step 5: Perform post-finishing treatment on the fabric base fabric to obtain shrinkage-resistant and warm-keeping fabric;

[0070] Among them, the post-processing process includes:

[0071] The fabric base is placed in a dimethylol dihydroxyethylene urea solution with a bath ratio of 1:10, two dips and two rolls, the roll ratio is 60%, dried at 60°C for 5 hours, and baked at 100°C for 30 minutes. Then, it is placed in a silicone softener solution with a bath ratio of 1:10, two dips and two rolls, the roll ratio is 60%, dried at 60°C for 5 hours, and baked at 100°C for 30 minutes;

[0072] The dimethylol dihydroxy ethylene urea aqueous solution is prepared by mixing dimethylol dihydroxy ethylene urea with deionized water, and the concentration of the dimethylol dihydroxy ethylene urea aqueous solution is 50 g / L;

[0073] The organic silicon softener solution is prepared from hydrophilic and skin-friendly silicone oil and deionized water. The mass percentage of the organic silicon softener in the organic silicon softener solution is 10%.

[0074] Example 5

[0075] This embodiment discloses a method for preparing a shrinkage-resistant thermal insulation fabric, comprising the following steps:

[0076] Step 1, dissolving D-arabinose in a 0.5wt% glycerol aqueous solution, the mass ratio of D-arabinose to the 0.5wt% glycerol aqueous solution is 0.8:100, to obtain a D-arabinose solution, placing cashmere in the D-arabinose solution for a primary soaking treatment, the bath ratio is 1:10, soaking for 1h at room temperature, after the soaking is completed, draining, and drying at 60°C for 5h to obtain cashmere after the primary soaking treatment;

[0077] Step 2, dissolving papain in a 1wt% sodium bisulfite aqueous solution, the mass ratio of papain to the 1wt% sodium bisulfite aqueous solution is 1.8:100, adjusting the pH value to 7, obtaining a papain solution, placing the cashmere treated by the primary immersion treatment in the papain solution for a secondary immersion treatment, the bath ratio is 1:10, soaking at room temperature for 35 minutes, after the immersion is completed, draining, washing with deionized water 3 times, obtaining the cashmere treated by the secondary immersion treatment;

[0078] Step 3, dissolving saccharifying enzyme and alkaline pectinase in deionized water, the mass ratio of saccharifying enzyme, alkaline pectinase and deionized water is 1.3:1.8:100, adjusting the pH value to 7.5, obtaining a mixed enzyme solution, placing the cashmere yarn after the secondary impregnation treatment in the mixed enzyme solution for a third immersion treatment, the bath ratio is 1:10, soaking at room temperature for 15 minutes, after the immersion is completed, draining, washing with deionized water 3 times, placing in 90°C hot water for enzyme inactivation treatment for 5 minutes, washing with deionized water 3 times, and drying at 60°C for 5 hours to obtain modified cashmere;

[0079] Step 4: Blend the modified cashmere with bamboo fiber, the mass ratio of the modified cashmere to bamboo fiber is 1.6:1, and obtain blended yarn, the count of the blended yarn is 30S, and the blended yarn is made into a fabric base fabric through a knitting process, and the gram weight of the fabric base fabric is 200g / m 2 ;

[0080] Step 5: Perform post-finishing treatment on the fabric base fabric to obtain shrinkage-resistant and warm-keeping fabric;

[0081] Among them, the post-processing process includes:

[0082] The fabric base is placed in a dimethylol dihydroxyethylene urea solution with a bath ratio of 1:10, two dips and two rolls, the roll ratio is 60%, dried at 60°C for 5 hours, and baked at 100°C for 30 minutes. Then, it is placed in a silicone softener solution with a bath ratio of 1:10, two dips and two rolls, the roll ratio is 60%, dried at 60°C for 5 hours, and baked at 100°C for 30 minutes;

[0083] The dimethylol dihydroxy ethylene urea aqueous solution is prepared by mixing dimethylol dihydroxy ethylene urea with deionized water, and the concentration of the dimethylol dihydroxy ethylene urea aqueous solution is 50 g / L;

[0084] The organic silicon softener solution is prepared from hydrophilic and skin-friendly silicone oil and deionized water. The mass percentage of the organic silicon softener in the organic silicon softener solution is 10%.

[0085] Example 6

[0086] This embodiment discloses a method for preparing a shrinkage-resistant thermal insulation fabric, comprising the following steps:

[0087] Step 1, dissolving D-arabinose in a 0.5wt% glycerol aqueous solution, the mass ratio of D-arabinose to the 0.5wt% glycerol aqueous solution is 0.9:100, to obtain a D-arabinose solution, placing cashmere in the D-arabinose solution for a primary soaking treatment, the bath ratio is 1:10, soaking for 1h at room temperature, after the soaking is completed, draining, and drying at 60°C for 5h to obtain cashmere after the primary soaking treatment;

[0088] Step 2, dissolving papain in a 1wt% sodium bisulfite aqueous solution, the mass ratio of papain to the 1wt% sodium bisulfite aqueous solution is 1.9:100, adjusting the pH value to 7, obtaining a papain solution, placing the cashmere treated by the primary immersion treatment in the papain solution for a secondary immersion treatment, the bath ratio is 1:10, soaking at room temperature for 35 minutes, after the immersion is completed, draining, washing with deionized water 3 times, obtaining the cashmere treated by the secondary immersion treatment;

[0089] Step 3, dissolving saccharifying enzyme and alkaline pectinase in deionized water, the mass ratio of saccharifying enzyme, alkaline pectinase and deionized water is 1.4:1.9:100, adjusting the pH value to 7.5, obtaining a mixed enzyme solution, placing the cashmere yarn after the secondary impregnation treatment in the mixed enzyme solution for a third immersion treatment, the bath ratio is 1:10, soaking at room temperature for 15 minutes, after the immersion is completed, draining, washing with deionized water 3 times, placing in 90°C hot water for enzyme inactivation treatment for 5 minutes, washing with deionized water 3 times, and drying at 60°C for 5 hours to obtain modified cashmere;

[0090] Step 4: Blend the modified cashmere with bamboo fiber, the mass ratio of the modified cashmere to bamboo fiber is 1.8:1, and obtain blended yarn, the count of the blended yarn is 30S, and the blended yarn is made into a fabric base fabric through a knitting process, and the weight of the fabric base fabric is 200g / m 2 ;

[0091] Step 5: Perform post-finishing treatment on the fabric base fabric to obtain shrinkage-resistant and warm-keeping fabric;

[0092] Among them, the post-processing process includes:

[0093] The fabric base is placed in a dimethylol dihydroxyethylene urea solution with a bath ratio of 1:10, two dips and two rolls, the roll ratio is 60%, dried at 60°C for 5 hours, and baked at 100°C for 30 minutes. Then, it is placed in a silicone softener solution with a bath ratio of 1:10, two dips and two rolls, the roll ratio is 60%, dried at 60°C for 5 hours, and baked at 100°C for 30 minutes;

[0094] The dimethylol dihydroxy ethylene urea aqueous solution is prepared by mixing dimethylol dihydroxy ethylene urea with deionized water, and the concentration of the dimethylol dihydroxy ethylene urea aqueous solution is 50 g / L;

[0095] The organic silicon softener solution is prepared from hydrophilic and skin-friendly silicone oil and deionized water. The mass percentage of the organic silicon softener in the organic silicon softener solution is 10%.

[0096] Comparative Example 1

[0097] This comparative example discloses a method for preparing a shrinkage-resistant thermal insulation fabric, comprising the following steps:

[0098] Step 1: Blend cashmere and bamboo fiber, the mass ratio of cashmere to bamboo fiber is 1:1, and obtain blended yarn, the count of the blended yarn is 20S, and the blended yarn is made into a fabric base fabric through a knitting process, and the weight of the fabric base fabric is 200g / m 2 ;

[0099] Step 2: Perform post-finishing treatment on the fabric base fabric to obtain shrinkage-resistant and warm-keeping fabric;

[0100] Among them, the post-processing process includes:

[0101] The fabric base is placed in a dimethylol dihydroxyethylene urea solution with a bath ratio of 1:10, two dips and two rolls, the roll ratio is 60%, dried at 60°C for 5 hours, and baked at 100°C for 30 minutes. Then, it is placed in a silicone softener solution with a bath ratio of 1:10, two dips and two rolls, the roll ratio is 60%, dried at 60°C for 5 hours, and baked at 100°C for 30 minutes;

[0102] The dimethylol dihydroxy ethylene urea aqueous solution is prepared by mixing dimethylol dihydroxy ethylene urea with deionized water, and the concentration of the dimethylol dihydroxy ethylene urea aqueous solution is 50 g / L;

[0103] The organic silicon softener solution is prepared from hydrophilic and skin-friendly silicone oil and deionized water. The mass percentage of the organic silicon softener in the organic silicon softener solution is 10%.

[0104] Comparative Example 2

[0105] This comparative example discloses a method for preparing a shrinkage-resistant thermal insulation fabric, comprising the following steps:

[0106] Step 1, dissolving D-arabinose in a 0.5wt% glycerol aqueous solution, the mass ratio of D-arabinose to the 0.5wt% glycerol aqueous solution is 0.5:100, to obtain a D-arabinose solution, placing cashmere in the D-arabinose solution for a primary soaking treatment, the bath ratio is 1:10, soaking for 1h at room temperature, after the soaking is completed, draining, and drying at 60°C for 5h to obtain cashmere after the primary soaking treatment;

[0107] Step 2, dissolving papain in a 1wt% sodium bisulfite aqueous solution, the mass ratio of papain to the 1wt% sodium bisulfite aqueous solution is 1.5:100, adjusting the pH value to 7, obtaining a papain solution, placing the cashmere treated by the primary immersion treatment in the papain solution for a secondary immersion treatment, the bath ratio is 1:10, soaking at room temperature for 35 minutes, after the immersion is completed, draining, washing with deionized water 3 times, obtaining the cashmere treated by the secondary immersion treatment;

[0108] Step 3, dissolving saccharifying enzyme and alkaline pectinase in deionized water, the mass ratio of saccharifying enzyme, alkaline pectinase and deionized water is 1:1.5:100, adjusting the pH value to 7, obtaining a mixed enzyme solution, placing the cashmere yarn after the secondary impregnation treatment in the mixed enzyme solution for a third immersion treatment, the bath ratio is 1:10, soaking at room temperature for 15 minutes, after the immersion is completed, draining, washing with deionized water 3 times, placing in 90°C hot water for enzyme inactivation treatment for 5 minutes, washing with deionized water 3 times, and drying at 60°C for 5 hours to obtain modified cashmere;

[0109] Step 4: blending the modified cashmere with bamboo fiber, wherein the mass ratio of the modified cashmere to the bamboo fiber is 1:1, to obtain a blended yarn, wherein the count of the blended yarn is 20S, and the blended yarn is knitted into a fabric base fabric, i.e., an anti-shrinkage warm fabric;

[0110] The weight of shrink-resistant warm fabric is 200g / m 2 .

[0111] In the above embodiments and comparative examples: D-arabinose was purchased from Sichuan Weikeqi Biotechnology Co., Ltd., CAS No.: 10323-20-3; papain was purchased from Shandong Zhongsen Biotechnology Co., Ltd., product specification: 500,000 u / g; saccharifying enzyme was purchased from Jiangsu Ruiyang Biotechnology Co., Ltd., product specification: 300,000 u / g; alkaline pectinase was purchased from Ningxia Heshibi Biotechnology Co., Ltd., 100,000 u / g; cashmere was purchased from Hebei Linwo Wool Products Co., Ltd., length: 50 mm; bamboo fiber was purchased from Shandong Aorong Garment Co., Ltd., length: 38 mm; dihydroxymethyl dihydroxyethylene urea was purchased from Wuhan Haorong Biotechnology Co., Ltd., CAS No.: 1854-26-8; hydrophilic and skin-friendly silicone oil was purchased from Dongguan Zhongsheng Environmental Protection Materials Co., Ltd., item number: ZSH-1353, effective substance content: 30%.

[0112] Test example

[0113] The fabrics prepared in the above embodiments and comparative examples were tested for performance:

[0114] Shrinkage resistance: Referring to the standard FZ / T20010-2012 "Determination of Dimensional Change of Wool Fabrics - Mild Household Washing Method", the dimensions of the shrinkage-resistant thermal insulation fabrics prepared in Examples 1-6 and Comparative Examples 1-2 before and after washing were measured, and the shrinkage of the fabrics was calculated. The test results are shown in Table 1:

[0115] Table 1

[0116]

[0117] It can be seen from Table 1 that the fabric prepared by the present invention has good anti-shrinkage performance.

[0118] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a shrinkage-resistant thermal insulation fabric, characterized in that: The following steps are involved: Step 1, dissolving D-arabinose in a glycerol aqueous solution to obtain a D-arabinose solution, placing cashmere in the D-arabinose solution for a primary soaking treatment, and after the soaking is completed, draining and drying to obtain cashmere after the primary soaking treatment; Step 2, dissolving papain in a sodium bisulfite aqueous solution, adjusting the pH value to 7, obtaining a papain solution, placing the cashmere treated by the primary immersion treatment in the papain solution for a secondary immersion treatment, draining and washing after the immersion is completed, and obtaining the cashmere treated by the secondary immersion treatment; Step 3, dissolving saccharifying enzyme and alkaline pectinase in deionized water, adjusting the pH value to 7-8, obtaining a mixed enzyme solution, placing the cashmere yarn after the secondary immersion treatment in the mixed enzyme solution for a third immersion treatment, and after the immersion is completed, draining, cleaning, inactivating, washing, and drying to obtain modified cashmere; Step 4: blending the modified cashmere with bamboo fiber to obtain blended yarn, and knitting the blended yarn into a fabric base cloth; Step 5: Perform post-finishing treatment on the fabric base fabric to obtain shrinkage-resistant and warm-keeping fabric.

2. The method for preparing a shrinkage-resistant thermal insulation fabric according to claim 1, characterized in that: In the step 1, when preparing the D-arabinose solution, the mass ratio of D-arabinose to the glycerol aqueous solution is (0.5-1):100, and the glycerol aqueous solution is a 0.5 wt % glycerol aqueous solution.

3. The method for preparing a shrinkage-resistant thermal insulation fabric according to claim 1, characterized in that: In the step 1, during the initial immersion treatment, the bath ratio is 1:10, and the immersion condition is immersion at room temperature for 1-3 hours.

4. The method for preparing a shrinkage-resistant thermal insulation fabric according to claim 1, characterized in that: In the step 2, when preparing the papain solution, the mass ratio of papain to sodium bisulfite aqueous solution is (1.5-2):100, and the sodium bisulfite aqueous solution is 1wt% sodium bisulfite aqueous solution.

5. The method for preparing a shrinkage-resistant thermal insulation fabric according to claim 1, characterized in that: In the step 2, during the secondary immersion treatment, the bath ratio is 1:10, and the immersion condition is immersion at room temperature for 35 minutes.

6. The method for preparing a shrinkage-resistant thermal insulation fabric according to claim 1, characterized in that: In the step 3, when preparing the mixed enzyme solution, the mass ratio of saccharifying enzyme, alkaline pectinase and deionized water is (1-1.5):(1.5-2):

100.

7. The method for preparing a shrinkage-resistant thermal insulation fabric according to claim 1, characterized in that: In the step 3, during the third immersion, the bath ratio is 1:10, and the immersion condition is immersion at room temperature for 15 minutes.

8. The method for preparing a shrinkage-resistant thermal insulation fabric according to claim 1, characterized in that: In the step 4, the mass ratio of modified cashmere to bamboo fiber is (1-2):1, the count of the blended yarn is 20-30S, and the weight of the fabric base fabric is 150-200g / m 2 .

9. The method for preparing a shrinkage-resistant thermal insulation fabric according to claim 1, characterized in that: In the step 5, the post-processing process includes: Place the fabric base in a dihydroxymethyl dihydroxyethylene urea solution with a bath ratio of 1:10, double immersion and double rolling, with a rolling rate of 60%, dry at 60°C for 5 hours, and bake at 100°C for 30 minutes. Then place it in a silicone softener solution with a bath ratio of 1:10, double immersion and double rolling, with a rolling rate of 60%, dry at 60°C for 5 hours, and bake at 100°C for 30 minutes.