Preparation method for constructing Pickering emulsion microreactor electrode
By using the preparation method of Pickering emulsion microreactor electrode in cyclohexanone oxime synthesis, the problem of slow reaction efficiency between hydroxylamine and cyclohexanone is solved, the current efficiency and safety are improved, and the efficient synthesis of cyclohexanone oxime is achieved.
Patent Information
- Application Number
- CN202411072862.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-26
AI Technical Summary
In the synthesis of cyclohexanone oxime, the reaction efficiency of hydroxylamine and cyclohexanone is slow, resulting in low current efficiency and safety hazards.
Using the preparation method of Pickering emulsion microreactor electrode, by dissolving metal oxides and conductive polymers in deionized water, adding ammonium persulfate, and reacting in an ice water bath, followed by homogenizer homogenization and carbon felt or carbon fiber cloth , form a conductive polymer-metal oxide catalyst to improve the binding efficiency of hydroxylamine and cyclohexanone.
It significantly improves the synthesis current efficiency and production rate of cyclohexanone oxime, reduces the reaction risk, and has good market promotion prospects.
Smart Images

Figure CN119021003A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical materials, and in particular relates to a preparation method for constructing a Pickering emulsion microreactor electrode. Background Art
[0002] Cyclohexanone oxime is the second most widely used polyamide monomer in the world and is one of the important raw materials in the chemical industry. Since the downstream product of cyclohexanone oxime, ε-caprolactam, is mainly used in the production of nylon-6 by ring-opening polymerization, nylon-6 and its manufacturing make cyclohexanone oxime a highly demanded intermediate, cyclohexanone oxime has good market value.
[0003] The synthesis of cyclohexanone oxime generally adopts the cyclohexanone-hydroxylamine route, but the free hydroxylamine (NH2OH) used in this process is extremely unstable and direct use is prone to safety accidents.
[0004] The nitrate reduction reaction driven by electrical energy can produce adsorbed hydroxylamine species in a solution with water as the hydrogen source, which couples with cyclohexanone adsorbed on the electrode surface to generate cyclohexanone oxime. The process does not involve the accumulation of free hydroxylamine, thus greatly reducing the risk of the reaction. However, as a typical two-phase reaction, it has the problem of slow reaction rate between aqueous phase hydroxylamine and oil phase cyclohexanone, and low current efficiency of cyclohexanone oxime synthesis. Summary of the invention
[0005] The invention aims to provide a preparation method for constructing a Pickering emulsion microreactor electrode, so as to solve the problems of slow reaction efficiency of hydroxylamine and cyclohexanone and low current efficiency of cyclohexanone oxime synthesis in the existing cyclohexanone oxime synthesis technology.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is: a preparation method for constructing a Pickering emulsion microreactor electrode, which is specifically implemented according to the following steps:
[0007] Step 1, adding metal oxide powder into deionized water to dissolve it;
[0008] Step 2, after continuously stirring the product obtained in step 1 in an ice water bath for 10 min-30 min, adding a conductive polymer monomer and stirring again for 5 min-20 min to obtain a solution a, wherein the molar ratio of the metal oxide powder to the conductive polymer monomer in the solution a is 1000-5000:1;
[0009] Step 3, weighing ammonium persulfate, adding it into deionized water to dissolve it, to obtain a solution b, wherein the molar ratio of ammonium persulfate to the conductive polymer monomer in the solution b is 200-2000:1;
[0010] Step 4, adding solution b dropwise into solution a, reacting in an ice water bath for 3h-12h, washing the precipitate with deionized water for multiple times, and then centrifuging and drying to obtain a conductive polymer-metal oxide catalyst;
[0011] Step 5, weighing ammonium persulfate, adding deionized water to dissolve it, then adding the conductive polymer-metal oxide catalyst, and continuously stirring in an ice water bath for 10 min-30 min to obtain a solution c, wherein the molar ratio of ammonium persulfate to the conductive polymer-metal oxide catalyst in the solution c is 0.1-0.8:1;
[0012] Step 6, dissolving the conductive polymer monomer in an organic solvent to prepare a solution d;
[0013] Step 7, adding solution d to solution c to obtain solution e, wherein the molar ratio of ammonium persulfate to the conductive polymer monomer in solution e is 200-2000:1; then solution e is homogenized by a homogenizer at a rate of 8000rpm / min to 20000rpm / min for 5min-20min; then carbon felt or carbon fiber cloth of a set size is cut and placed in the homogenized solution e, and after reacting in an ice water bath for 3h-12h, it is taken out and washed with deionized water to obtain a Pickering emulsion microreactor electrode.
[0014] As a preferred technical solution of the present invention, in step 1: the metal oxide is one or a mixture of silver oxide, copper oxide, titanium oxide and iron oxide.
[0015] As a preferred technical solution of the present invention, in step 2: the conductive polymer is one or a mixture of pyrrole, thiophene, and aniline.
[0016] As a preferred technical solution of the present invention, in step 6, the organic solvent is one or a mixture of benzene, toluene and cyclohexane.
[0017] The beneficial effects of the present invention are as follows: the preparation method of the present invention for constructing a Pickering emulsion microreactor electrode adopts a method in the preparation process that is conducive to the full combination of hydroxylamine and cyclohexanone molecules generated in the reaction process, greatly improving the reaction current efficiency and production rate, and having a good prospect for market promotion and use. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is a morphology picture of a conductive polymer-metal oxide prepared by a preparation method for constructing a Pickering emulsion microreactor electrode according to the present invention;
[0019] Figure 2This is a morphology picture of a Pickering emulsion microreactor electrode prepared by a preparation method for constructing a Pickering emulsion microreactor electrode according to the method of the present invention;
[0020] Figure 3 This is a preparation method for constructing a Pickering emulsion microreactor electrode according to the method of the present invention. The prepared Pickering emulsion microreactor electrode is used to test the current efficiency and stability of cyclohexanone oxime. DETAILED DESCRIPTION
[0021] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0022] Example 1
[0023] The preparation method of constructing a Pickering emulsion microreactor electrode of the present invention is specifically implemented according to the following steps:
[0024] Step 1, adding silver oxide powder into deionized water to dissolve it;
[0025] Step 2, stirring the product obtained in step 1 continuously in an ice water bath for 10 minutes, adding pyrrole and stirring again for 5 minutes to obtain solution a, wherein the molar ratio of silver oxide powder to pyrrole in solution a is 1000:1;
[0026] Step 3, weighing ammonium persulfate, and adding it into deionized water to dissolve it to obtain a solution b, wherein the molar ratio of ammonium persulfate to pyrrole in the solution b is 200:1;
[0027] Step 4, adding solution b dropwise into solution a, reacting in an ice water bath for 3 hours, washing the precipitate with deionized water for multiple times, and then centrifuging and drying to obtain a conductive polymer-metal oxide catalyst;
[0028] Step 5, weighing ammonium persulfate, adding deionized water to dissolve it, then adding the conductive polymer-metal oxide catalyst, and continuously stirring in an ice water bath for 10 minutes to obtain a solution c, wherein the molar ratio of ammonium persulfate to the conductive polymer-metal oxide catalyst in the solution c is 0.1:1;
[0029] Step 6, dissolving pyrrole in an organic solvent to prepare a solution d;
[0030] Step 7, adding solution d to solution c to obtain solution e, wherein the molar ratio of ammonium persulfate to pyrrole in solution e is 200:1; then solution e is homogenized by a homogenizer at a rate of 8000 rpm / min for 5 minutes; then carbon felt or carbon fiber cloth of a set size is cut and placed in the homogenized solution e, and after reacting in an ice water bath for 3 hours, it is taken out and washed with deionized water to obtain a Pickering emulsion microreactor electrode.
[0031] like Figure 1 As shown, the left figure is a macroscopic morphology picture of a conductive polymer-metal oxide, which is obtained by step 4 and presents the morphology of nanoparticles or nanocubes, with a uniform overall morphology and a particle size of about 200 to 400 nanometers. Particles of this particle size are helpful to better construct a Pickering emulsion microreactor (solution e). The right figure is a microscopic morphology picture of a conductive polymer-metal oxide, in which the dark part is the metal oxide core, which presents a nearly spherical morphology and a particle size of about 100 to 200 nanometers. The light part is the conductive polymer coated on the periphery, and the thickness of the polymer is about 30 to 50 nanometers. Its function is to adjust the wettability of the particles, making it easier to form a Pickering emulsion reactor, and to act with the polymer formed in step 7 to act as an adhesive between the electrodes.
[0032] like Figure 2 As shown, the Pickering droplet reactor (solution e) presents a spherical morphology in the figure. The diameter of the spherical droplet is about 60 to 100 microns. The surface of the droplet is wrapped by a conductive polymer-metal oxide, and the interior is an organic solvent. The carbon fiber on the carbon cloth electrode presents a linear morphology. The fiber diameter is about 10 microns. The carbon cloth serves as a connecting circuit and a carrier and electron transfer for the Pickering droplet reactor. It can be seen that the Pickering droplet reactor can be uniformly attached to the carbon fiber. The adhesion is generated by the polymer produced by the polymerization of the polymer monomer in step 7. The polymer monomer added in step 6 will interact with the carbon felt / carbon fiber electrode, and then polymerize in step 7. The generated polymer will bond with the conductive polymer on the surface of the Pickering droplet reactor, so it can play a role in supporting the Pickering droplet reactor.
[0033] like Figure 3As shown, the electrode was used as the working electrode, nickel iron hydroxide supported by nickel foam was used as the counter electrode, an aqueous solution containing 0.5 M sodium nitrite, 0.1 M cyclohexanone, and 0.5 M sodium carbonate was used as the cathode electrolyte, and an aqueous solution containing 1 M sodium hydroxide was used as the anode electrolyte. The reaction efficiency and stability were tested in an H-type reaction cell. The left figure shows the current efficiency of cyclohexanone oxime generated at different current densities. It can be seen from the figure that at 10 mA cm -2 , 20mA cm -2 , 30mA cm -2 , 50mAcm -2 , 100mA cm -2 The current efficiencies of cyclohexanone oxime generation at current densities of 100 mA cm-1 and 100 mA cm-2 are as follows: -2 It can be seen that under this current, the current efficiency of cyclohexanone oxime generation did not decay significantly within 100 hours and remained at around 80%, and the overall electrolytic cell voltage remained at 3 V, proving that the Pickering droplet reactor showed excellent current efficiency and stability in the process of electrochemical synthesis of cyclohexanone oxime.
[0034] Example 2
[0035] The preparation method of constructing a Pickering emulsion microreactor electrode of the present invention is specifically implemented according to the following steps:
[0036] Step 1, adding copper oxide powder into deionized water to dissolve it;
[0037] Step 2, the product obtained in step 1 is continuously stirred in an ice water bath for 20 minutes, thiophene is added and stirred again for 12 minutes to obtain solution a, wherein the molar ratio of copper oxide powder to thiophene in solution a is 3000:1;
[0038] Step 3, weighing ammonium persulfate, adding it into deionized water to dissolve it, to obtain a solution b, wherein the molar ratio of ammonium persulfate to thiophene in the solution b is 1100:1;
[0039] Step 4, adding solution b dropwise into solution a, reacting in an ice water bath for 8 hours, washing the precipitate with deionized water for multiple times, and then centrifuging and drying to obtain a conductive polymer-metal oxide catalyst;
[0040] Step 5, weighing ammonium persulfate, adding deionized water to dissolve it, then adding the conductive polymer-metal oxide catalyst, and continuously stirring in an ice water bath for 20 minutes to obtain a solution c, wherein the molar ratio of ammonium persulfate to the conductive polymer-metal oxide catalyst in the solution c is 0.5:1;
[0041] Step 6, dissolving thiophene in an organic solvent to prepare a solution d;
[0042] Step 7, adding solution d to solution c to obtain solution e, wherein the molar ratio of ammonium persulfate to thiophene in solution e is 1100:1; then solution e is homogenized by a homogenizer at a rate of 14000 rpm / min for 12 min; then carbon felt or carbon fiber cloth of a set size is cut and placed in the homogenized solution e, and after reacting in an ice water bath for 8 h, it is taken out and washed with deionized water to obtain a Pickering emulsion microreactor electrode.
[0043] Example 3
[0044] The preparation method of constructing a Pickering emulsion microreactor electrode of the present invention is specifically implemented according to the following steps:
[0045] Step 1, adding titanium oxide powder into deionized water to dissolve it;
[0046] Step 2, stirring the product obtained in step 1 in an ice water bath for 30 minutes, adding aniline and stirring again for 20 minutes to obtain solution a, wherein the molar ratio of titanium oxide powder to conductive polymer monomer in solution a is 5000:1;
[0047] Step 3, weighing ammonium persulfate, and adding it into deionized water to dissolve it to obtain a solution b, wherein the molar ratio of ammonium persulfate to aniline in the solution b is 2000:1;
[0048] Step 4, adding solution b dropwise into solution a, reacting in an ice water bath for 12 hours, washing the precipitate with deionized water for multiple times, and then centrifuging and drying to obtain a conductive polymer-metal oxide catalyst;
[0049] Step 5, weighing ammonium persulfate, adding deionized water to dissolve it, then adding the conductive polymer-metal oxide catalyst, and continuously stirring in an ice water bath for 30 minutes to obtain a solution c, wherein the molar ratio of ammonium persulfate to the conductive polymer-metal oxide catalyst in the solution c is 0.8:1;
[0050] Step 6, dissolving aniline in an organic solvent to prepare a solution d;
[0051] Step 7, adding solution d to solution c to obtain solution e, wherein the molar ratio of ammonium persulfate to aniline in solution e is 2000:1; then solution e is homogenized by a homogenizer at a rate of 20000 rpm / min for 20 min; then carbon felt or carbon fiber cloth of a set size is cut and placed in the homogenized solution e, and after reacting in an ice water bath for 12 h, it is taken out and washed with deionized water to obtain a Pickering emulsion microreactor electrode.
Claims
1. A method for preparing a Pickering emulsion microreactor electrode, characterized in that: Follow the steps below to implement it: Step 1, adding metal oxide powder into deionized water to dissolve it; Step 2, after continuously stirring the product obtained in step 1 in an ice water bath for 10 min-30 min, adding a conductive polymer monomer and stirring again for 5 min-20 min to obtain a solution a, wherein the molar ratio of the metal oxide powder to the conductive polymer monomer in the solution a is 1000-5000:1; Step 3, weighing ammonium persulfate, adding it into deionized water to dissolve it, to obtain a solution b, wherein the molar ratio of ammonium persulfate to the conductive polymer monomer in the solution b is 200-2000:1; Step 4, adding solution b dropwise into solution a, reacting in an ice water bath for 3h-12h, washing the precipitate with deionized water for multiple times, and then centrifuging and drying to obtain a conductive polymer-metal oxide catalyst; Step 5, weighing ammonium persulfate, adding deionized water to dissolve it, then adding the conductive polymer-metal oxide catalyst, and continuously stirring in an ice water bath for 10 min-30 min to obtain a solution c, wherein the molar ratio of ammonium persulfate to the conductive polymer-metal oxide catalyst in the solution c is 0.1-0.8:1; Step 6, dissolving the conductive polymer monomer in an organic solvent to prepare a solution d; Step 7, adding solution d to solution c to obtain solution e, wherein the molar ratio of ammonium persulfate to the conductive polymer monomer in solution e is 200-2000:1; then solution e is homogenized by a homogenizer at a rate of 8000rpm / min to 20000rpm / min for 5min-20min; then carbon felt or carbon fiber cloth of a set size is cut and placed in the homogenized solution e, and after reacting in an ice water bath for 3h-12h, it is taken out and washed with deionized water to obtain a Pickering emulsion microreactor electrode.
2. The method for preparing a Pickering emulsion microreactor electrode according to claim 1, characterized in that: In the step 1: the metal oxide is one or a mixture of silver oxide, copper oxide, titanium oxide and iron oxide.
3. The method for preparing a Pickering emulsion microreactor electrode according to claim 2, characterized in that: In the step 2: the conductive polymer monomer is one or a mixture of pyrrole, thiophene and aniline.
4. The method for preparing a Pickering emulsion microreactor electrode according to claim 3, characterized in that: In step 6, the organic solvent is one or a mixture of benzene, toluene and cyclohexane.