Cotton-like carpet and preparation method thereof
Through twisting and shaping and process processing of imitation cotton filaments, the problem of chemical fiber carpet lacking natural touch and hygroscopicity and environmental impact of all cotton carpets is solved, and the simulation, hygroscopicity and durability are improved, which is suitable for industrial production.
Patent Information
- Application Number
- CN202411146498.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
AI Technical Summary
Chemical fiber carpets lack the soft, natural touch and moisture absorption of all cotton carpets. At the same time, all cotton carpets have a great impact on the environment during the production process, and there are problems such as hair loss, shrinkage, and fading.
The velvet layer is formed by twisting, tufting, knitting/wovening processes, and is subjected to solidifying and glueing to simulate the characteristics of cotton carpets and improve the simulation, moisture absorption and durability of the carpet.
It significantly improves the aesthetics, comfort and practical value of the carpet, extends the service life, and simplifies the production process, reduces costs, and is suitable for large-scale industrial production.
Smart Images

Figure CN119021013A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a cotton-like carpet and a preparation method thereof, belonging to the technical field of textiles. Background Art
[0002] As an alternative, chemical fiber carpets, especially those made of chemical fibers such as polyester and nylon, are becoming more and more popular in the market due to their durability, dimensional stability and easy maintenance. The common problem of chemical fiber carpets is that they lack the soft, natural touch and moisture absorption of pure cotton carpets.
[0003] However, traditional cotton carpets are highly favored for their excellent moisture absorption and natural skin-friendliness. However, due to the characteristics of natural cotton fibers, they will lose hair, shrink, fade, and cause bacteria and mildew due to the difficulty in drying quickly after absorbing moisture. In addition, cotton carpets have a great impact on the environment during the production process. For example, the spinning process consumes a lot of water resources and energy, and the wastewater generated during the dyeing process is difficult to treat, which does not conform to the development trend of modern green environmental protection.
[0004] For this reason, it is necessary to provide a kind of imitation cotton carpet to solve the above problems. Summary of the invention
[0005] The purpose of the present invention is to provide a cotton-like carpet and a preparation method thereof, which can simulate the characteristics of a cotton carpet on a chemical fiber material and have the effects of being not easy to shed, durable, dimensionally stable and low in cost.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] In a first aspect, the present application provides a method for preparing a cotton-like carpet, which comprises the following steps:
[0008] S1. Providing imitation cotton filaments, wherein the imitation cotton filaments are made of any one or more filament raw materials of DTY, ATY, FDY or POY;
[0009] S2, performing twisting and shaping treatment on the cotton-like filaments;
[0010] S3, processing the twisted and shaped cotton-like filaments into a blanket having a blanket surface and a back surface;
[0011] S4, performing post-finishing treatment on the blank blanket to form a fluff layer on the blanket surface;
[0012] S5, performing a pile fixing treatment on the pile layer and performing a back adhesive treatment on the back side to obtain the imitation cotton carpet.
[0013] In one or more possible implementations, in step S1, the raw material of the filament is polyester or nylon, and the imitation cotton filament is made of DTY or ATY;
[0014] Alternatively, the cotton-like filament is made by stretching FDY and POY in parallel.
[0015] In one or more possible implementations, before performing the twisting and shaping process, the method further includes:
[0016] Performing a sanding treatment on the cotton-like filaments;
[0017] or,
[0018] A plurality of the filament raw materials are paralleled and then subjected to a grinding process.
[0019] In one or more possible embodiments, the cotton-like filaments may be white and may be tufted, knitted and woven before being dyed; or, colored cotton-like filaments may be directly tufted, knitted and woven to form a blanket.
[0020] In one or more possible implementations, in step S2, during the twisting and setting process, the twist is 100-900 TPM and the setting temperature is 60-180° C. to enhance the three-dimensional effect of the fluff.
[0021] In one or more possible implementations, in step S3, processing the twisted and shaped cotton-like filaments into a blanket includes:
[0022] The texture and pattern of the loops are manufactured by tufting, knitting or weaving to obtain the blank blanket, which is loop pile and / or cut pile.
[0023] In one or more possible embodiments, during the tufting process, the base fabric layer is selected from any one of needle-punched nonwoven fabrics, PP base fabrics or cationic base fabrics, the needle pitch of the tufting machine is 2.54-9.525 mm, and the pile height is 1.5-20 mm.
[0024] In one or more possible implementations, during the weaving process and the knitting process, the weight of the blanket obtained is 200-2000 GSM.
[0025] In one or more possible embodiments, the weaving process includes but is not limited to a grey blanket made by a weaving towel machine.
[0026] In one or more possible embodiments, the knitting process includes but is not limited to a grey carpet made by a single-needle bed warp knitting machine, a double-needle bed fine knitting machine, a weft knitting circular machine, a flat knitting machine, and a carpet flat knitting machine.
[0027] In one or more possible implementations, in step S4, the post-processing is a water drop treatment or a ball rolling treatment;
[0028] Wherein, during the ball rolling process, the temperature of the rolling machine is 80-150°C, and the processing time is 3-30 minutes.
[0029] In one or more possible implementations, step S4 further includes performing a velvet fixing treatment on the carpet surface, the velvet fixing treatment being before or after the post-finishing treatment, and the velvet fixing treatment includes:
[0030] The fluff layer is heated and treated with a fluff fixing agent, wherein the fluff fixing agent has a viscosity of 1500-2000 mPa.s and a glue amount of 40-60 g / m 2 The heating temperature is 135-145℃ to enhance the pulling force of the blanket yarn.
[0031] In one or more possible implementations, the velvet fixing agent is selected from a mixture of any two of EVA glue, stone powder, water, a thickener or a foaming agent.
[0032] In one or more possible embodiments, during the adhesive backing treatment process, the adhesive backing is selected from any one or more of latex, TPE, hot melt adhesive, non-woven point plastic anti-slip layer, EVA, polyurethane reactive adhesive or modified silicone.
[0033] In a second aspect, the present application provides a cotton-like carpet prepared according to the method for preparing the cotton-like carpet according to the first aspect, wherein the specification of the cotton-like filaments is 75-2500D; the cotton-like carpet comprises a carpet surface and a back surface, the surface of the carpet surface is provided with a fluff layer, and the back surface is provided with a backing adhesive.
[0034] Compared with the prior art, the beneficial effects of this application are:
[0035] The present application provides a method for making a cotton-like carpet using chemical fiber filaments. By flexibly selecting and processing polyester / nylon cotton-like filaments, the appearance and feel of cotton yarn are effectively simulated, the simulation degree of the carpet is significantly improved, and the market demand for cotton-like carpets is met. And through twisting and shaping and subsequent tufting, knitting / weaving processes, the pile layer of the carpet has a rich three-dimensional sense and delicate texture, which enhances the aesthetics and comfort of the carpet. At the same time, through reasonable water drop and rolling ball treatment, a more subtle and uniform pile is formed on the surface of the carpet, which enhances the hygroscopicity of the carpet and the effect of imitating a towel floor towel, and improves the practical value of the carpet. Furthermore, through specific pile solid treatment and adhesive backing technology, the durability and stability of the carpet are significantly improved, the problem of pile shedding caused by wear and cleaning during use of the carpet is reduced, and the service life of the carpet is extended.
[0036] In summary, the preparation method of the cotton-like carpet of the present application simplifies the production process, reduces the production cost, and improves the production efficiency, which is conducive to large-scale industrial production and has broad market application prospects and economic benefits.
[0037] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a process step diagram of a method for preparing a cotton-like carpet shown in an embodiment of the present application;
[0039] Figure 2 This is a schematic diagram of the overall structure of a cotton-like carpet shown in one embodiment of the present application;
[0040] Figures 3 to 5 This is a partial structural schematic diagram of a cotton-like carpet shown in an embodiment of the present application. DETAILED DESCRIPTION
[0041] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the following embodiments and features in the embodiments can be combined with each other without conflict.
[0042] While some exemplary embodiments of the present invention have been described for the purpose of illustration, it should be understood that the present invention may be implemented in other ways not specifically shown in the drawings.
[0043] Figure 1 A method for preparing a cotton-like carpet according to an embodiment of the present application is shown, which comprises the following steps:
[0044] S1. Providing imitation cotton filaments, wherein the imitation cotton filaments are made of any one or more filament raw materials of DTY, ATY, FDY or POY;
[0045] S2, performing twisting and shaping treatment on the cotton-like filaments;
[0046] S3, processing the twisted and shaped cotton-like filaments into a blanket having a blanket surface and a back surface;
[0047] S4, performing post-finishing treatment on the blank blanket to form a fluff layer on the blanket surface;
[0048] S5, performing a pile fixing treatment on the pile layer and performing a back adhesive treatment on the back side to obtain the imitation cotton carpet.
[0049] Specifically, in step S1, the raw material of the filament is polyester or nylon, and the imitation cotton filament is made of DTY or ATY; or, the imitation cotton filament is made of FDY and POY by paralleling and stretching; or, multiple filament raw materials are selected to parallel the cotton filament.
[0050] Optionally, before the twisting and shaping process is performed, the method further comprises:
[0051] The imitation cotton filaments are subjected to a sanding treatment; or, a plurality of the filament raw materials are subjected to a sanding treatment after being paralleled, so that the obtained imitation cotton filaments have an appearance very close to that of pure cotton yarns, and at the same time have excellent water absorption, softness, stable size and are not easy to shed.
[0052] It is also possible to combine multiple imitation cotton filaments and then twist them to shape them, with each strand containing 1 to 15 imitation cotton filaments.
[0053] As an example but not a limitation, the imitation cotton filaments may be white, and may be tufted, knitted and woven before being dyed; or, colored imitation cotton filaments may be directly tufted, knitted and woven to form a blanket.
[0054] Specifically, in step S2, during the twisting and setting process, the twist is 100-900 TPM and the setting temperature is 60-180° C. to enhance the three-dimensional sense of the fluff.
[0055] Specifically, in step S3, processing the twisted and shaped cotton-like filaments into a blanket includes:
[0056] The texture and pattern of the loops are manufactured by tufting, knitting or weaving to obtain the blank blanket, which is loop pile and / or cut pile.
[0057] Wherein, in the tufting process, the base fabric layer is selected from any one of needle-punched nonwoven fabric, PP base fabric or cationic base fabric, the needle pitch of the tufting machine is 2.54-9.525 mm, and the pile height is 1.5-20 mm.
[0058] Wherein, in the weaving process and the knitting process, the weight of the obtained blanket is 200-2000GSM.
[0059] Among them, the weaving process includes but is not limited to the blank blanket made by the weaving towel machine.
[0060] Among them, the knitting process includes but is not limited to blank carpets made by single-needle bed warp knitting machines, double-needle bed fine knitting machines, weft knitting circular machines, flat knitting machines and carpet flat knitting machines.
[0061] Specifically, in step S4, the post-finishing treatment is a water drop treatment or a ball rolling treatment, which further forms fine fluff on the suede surface and increases its towel-like floor towel effect. In the ball rolling treatment process, the temperature of the rolling machine is 80-150° C. and the treatment time is 3-30 minutes.
[0062] Specifically, step S5 further includes performing a pile fixing treatment on the carpet surface, the pile fixing treatment being performed before or after the post-finishing treatment, and the pile fixing treatment includes:
[0063] The fluff layer is heated and treated with a fluff fixing agent, wherein the fluff fixing agent has a viscosity of 1500-2000 mPa.s and a glue amount of 40-60 g / m 2 The heating temperature is 135-145℃ to enhance the pulling force of the blanket yarn.
[0064] Optionally, the velvet fixing agent is selected from a mixture of any two of EVA glue, stone powder, water, a thickener or a foaming agent.
[0065] Optionally, during the adhesive treatment process, the adhesive is selected from any one or more of latex, TPE, hot melt adhesive, non-woven point plastic anti-slip layer, EVA, polyurethane reactive adhesive or modified silicone.
[0066] Specifically, the latex may be in the form of polymer particles in aqueous solution, for example, based on polymers and copolymers of polystyrene / butadiene, polyacrylate, polystyrene / acrylate, polyvinyl acetate and acrylonitrile / butadiene. As for hot melt adhesives, they are thermoplastic materials dispersed in a suspension to form a slurry, for example, based on polymers and copolymers of polyolefins, polyesters, polyamides, etc.
[0067] The adhesive backing can also be in the form of pure thermoplastics of 100% polyolefins, polyesters and polyamide polymers and copolymers. The thermoplastic is applied in a dry state to the semi-finished material and the fiber structure of the second backing layer. Various coating and lamination methods can be used, such as powder coating or melt coating (hot melt).
[0068] The cotton-like filaments produced by the above process have specifications ranging from 75 to 2500D. Figure 2 , Figure 2 A cotton-like carpet shown in an embodiment of the present application is shown, which includes a carpet surface 1, a base fabric layer 2 and a back surface 3. The surface of the carpet surface 1 is provided with a fluff layer, and the back surface 3 is provided with adhesive.
[0069] Please combine Figures 3 to 5 , respectively showing three types of fluff layer structures of the present application, wherein, Figure 3 For loop velvet, Figure 4 For cutting velvet, Figure 5 It is a combination of loop pile and cut pile.
[0070] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0071] Embodiment 1
[0072] Step 1: Select polyester 820D imitation cotton filament, which is made of 420D FDY and 400D POY filament raw materials, and perform sanding treatment on the imitation cotton filament to form fine fluff on its surface. Then the hank yarn is dyed, which specifically includes: pre-treatment of the original yarn - whitening at 130℃ for 40 minutes - post-treatment - drying - rewinding.
[0073] Step 2: Use three 820D imitation cotton filaments to make one strand.
[0074] Step 3: Twist and shape the paralleled material, with a twist of 300 TPM and a shaping temperature of 135°C.
[0075] Step 4: Tuft the twisted and shaped material, and select the 1 / 4 model for tufting machine. Hang the yarn of the inverted bobbin according to the weaving process, then thread the yarn, and put on the white PP woven base fabric to get the blanket. Among them, the PP base fabric is 110X71 weft, the process parameters are set to 6.35mm needle pitch, 28 needles / 10cm, 6.5mm pile height, and 730G / M2 weight.
[0076] Step 5: The blanket is subjected to a rolling process to further form fine fluff on the suede surface to increase its towel-like effect. The temperature of the rolling machine is 80°C, the time is 30 minutes, and the rolling volume rate is 10 kg fabric / M3.
[0077] Step 6: Fix the fleece layer. Fix the fleece layer with a fixer made of EVA glue, stone powder and water to enhance its fastness. The viscosity of the fixer is 1750mPa.s and the amount of glue is 50g / m 2 , the drying temperature is 135℃. The tufting force of the finished blanket is greater than 10N.
[0078] Step 7: Use latex to make anti-slip treatment on the back, then cut and wrap the edges, and package and ship as needed.
[0079] Embodiment 2
[0080] Step 1: Select fixed-spinning polyester ATY620D filament, which has a fiber length similar to cotton fiber and has fine fluff on the surface. Then dye the hank yarn, which includes: pre-treatment of the raw yarn - whitening at 135℃ for 30 minutes - post-treatment - drying - rewinding.
[0081] Step 2: Combine 11 620D yarns into one strand, twist them 40 times, and then sand the combined cotton-like filaments.
[0082] Step 3: Twist and shape the ground cotton-like filaments, with a twist of 350 TPM and a shaping temperature of 135°C.
[0083] Step 4: Tuft the twisted and shaped material, and select the 3 / 8 model tufting machine for production. Hang the yarn of the inverted bobbin according to the weaving process, then thread the yarn, and at the same time, apply the white PP woven base fabric. Among them, the process parameters are set to 9.525mm needle length, 55 needles / 10cm, 7mm pile height, and 700G / M2 weight.
[0084] Step 5: The blank blanket is subjected to a ball rolling process to further form fine pile on the suede surface, and the tufting rings are twisted tightly to present a mop yarn effect. The temperature of the rolling machine is 140°C, the time is 20 minutes, and the rolling volume rate is 10 kg fabric / M3.
[0085] Step 6: Use hot melt adhesive to make anti-slip treatment on the back, then cut and wrap the edges, and package and ship as needed.
[0086] Embodiment 3
[0087] Step 1: Select the colored spun polyester DTY620D / 576F imitation cotton filament, twist each filament 130 times, twist direction Z.
[0088] Step 2: Align 4 black filaments and 2 white filaments.
[0089] Step 3: Twist and shape the paralleled cotton-like filaments, with a twist of 30 TPM and a shaping temperature of 135°C.
[0090] Step 4: Tuft the twisted and shaped material, and the tufting machine selects 1 / 4 needle pitch flat cutting. Hang the yarn of the inverted bobbin according to the weaving process, then thread the yarn, and at the same time, apply the white PP woven base fabric. Among them, the process parameters are set to a needle pitch of 6.35mm, a stitch of 55 needles / 10cm, a pile height of 15mm, and a weight of 750G / M2.
[0091] Step 5: Then the fluff layer is treated with a fluff fixation treatment. The fluff fixation treatment uses a yarn fixation agent mixed with water, a thickener and a foaming agent to heat the fluff layer to enhance its fastness. The viscosity of the yarn fixation agent is 2000mPa.s, and the glue amount is 40g / m 2 , the drying temperature is 140℃. The tufting force of the finished blanket is greater than 10N.
[0092] Step 6: The blanket is subjected to a rolling process to further form fine fluff on the suede surface and enhance its towel-like floor effect. The temperature of the rolling machine is 150°C, the time is 8 minutes, and the rolling volume rate is 10 kg fabric / M3.
[0093] Step 7: Use TPE to make anti-slip treatment on the back, cut and wrap the edges, and package and ship as needed.
[0094] Embodiment 4
[0095] Step 1: First, select polyester DTY 1000D imitation cotton filament, which is made of 600D FDY and 400DPOY raw materials through a texturizing process, and then sanded to simulate the delicate touch of cotton fiber. After pretreatment, heat preservation at 120℃ for 30 minutes, post-treatment, drying and rewinding, the quality and color of the filament are ensured.
[0096] Step 2: Select five 1000D imitation cotton filaments and make them into a strong yarn through a precise doubling process.
[0097] Step 3: Twist and shape the yarn after doubling, set the twist to 500 TPM, and the shaping temperature to 150°C to strengthen the yarn structure and improve the three-dimensional sense and stability of the carpet.
[0098] Step 4: Use a tufting machine for weaving, select a 3 / 8 needle gauge model, hang and thread the yarn according to the weaving process, and combine it with a gray PET needle-punched non-woven fabric base cloth, set the needle gauge to 9.525mm, the stitch to 18 needles / 10cm, and the pile height to 8mm, and finally get a blanket with a gram weight of about 800G / M2.
[0099] Step 5: Place the carpet in water to allow the velvet surface to naturally form fine fluff to reflect the soft texture of the carpet. The water treatment time is 15 minutes.
[0100] Step 6: During the velvet fixation treatment, a velvet fixation agent prepared by EVA glue, stone powder, water and a small amount of additives is used. The viscosity is 1800mPa.s and the glue amount is 45g / m 2 , the drying temperature is controlled at 140℃ to ensure that the tufting force exceeds 10N.
[0101] Step 7: Apply a layer of environmentally friendly hot melt adhesive on the back as an anti-slip layer, then perform precise cutting and edging, and finally package and ship according to customer requirements.
[0102] Embodiment 5
[0103] Step 1: Choose nylon ATY 500D imitation cotton filament. The filament itself has good moisture absorption and simulates the appearance of cotton. After conventional skein dyeing, choose light colors to simulate the natural whiteness of cotton yarn.
[0104] Step 2: Pair 15 500D imitation cotton filaments and twist them 60 times to form a high-strength yarn.
[0105] Step 3: Twisting and shaping, the twist is set to 250TPM, and the shaping temperature is set to 120℃, in order to achieve both simulation effect and maintain the toughness and gloss of the yarn itself.
[0106] Step 4: Use knitting technology to make the blanket, using an electronic jacquard knitting machine, combined with a blended cotton / polyester base fabric, set the weaving density to obtain an ideal loop pile effect, the pile height is 4mm, and the blanket weight is designed to be 600G / M2.
[0107] Step 5: Use a slight ball rolling treatment, with the rolling machine temperature at 100°C and the treatment time for 15 minutes to moderately improve the fineness of the carpet surface pile.
[0108] Step 6: Solvent-free environmentally friendly glue is used for velvet solidification, with a viscosity of 1600mPa.s and a glue amount of 55g / m 2 , the drying temperature is 130℃, ensuring the carpet has excellent durability and pull-out resistance.
[0109] Step 7: Apply TPE anti-slip coating on the back, cut and sew, and then package and ship according to standard specifications.
[0110] Embodiment 6
[0111] This embodiment is basically the same as the first embodiment, the difference being that shuttle knitting is used in step four, specifically a double needle bed fine knitting machine. Of course, in other embodiments, a single needle bed warp knitting machine, a weft circular knitting machine, a flat knitting machine, and a carpet flat knitting machine may also be used.
[0112] In summary, the method for preparing the imitation cotton carpet of the present application simplifies the production process, reduces the production cost, and improves the production efficiency, which is conducive to large-scale industrial production and has broad market application prospects and economic benefits.
[0113] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0114] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing a cotton-like carpet, characterized in that: The following steps are involved: S1. Providing imitation cotton filaments, wherein the imitation cotton filaments are made of any one or more filament raw materials of DTY, ATY, FDY or POY; S2, performing twisting and shaping treatment on the cotton-like filaments; S3, processing the twisted and shaped cotton-like filaments into a blanket having a blanket surface and a back surface; S4, performing post-finishing treatment on the blank blanket to form a fluff layer on the blanket surface; S5, performing adhesive treatment on the back side to obtain the imitation cotton carpet.
2. The method for preparing the imitation cotton carpet according to claim 1, characterized in that: In step S1, the raw material of the filament is polyester or nylon, and the imitation cotton filament is made of DTY or ATY; Alternatively, the cotton-like filament is made by stretching FDY and POY in parallel.
3. The method for preparing the imitation cotton carpet according to claim 2, characterized in that: Before the twisting and shaping process is performed, the method further comprises: Performing a sanding treatment on the cotton-like filaments; or, A plurality of the filament raw materials are paralleled and then subjected to a grinding process.
4. The method for preparing the imitation cotton carpet according to claim 1, characterized in that: In step S2, during the twisting and setting process, the twist is 100-900 TPM and the setting temperature is 60-180°C.
5. The method for preparing the imitation cotton carpet according to claim 1, characterized in that: In step S3, processing the twisted and shaped cotton-like filaments into a blanket includes: The texture and pattern of the loops are manufactured by tufting, knitting or weaving to obtain the blank blanket, which is loop pile and / or cut pile.
6. The method for preparing the imitation cotton carpet according to claim 5, characterized in that: In the tufting process, the base fabric layer is selected from any one of needle-punched nonwoven fabrics, PP base fabrics or cationic base fabrics, the needle pitch of the tufting machine is 2.54-9.525 mm, and the pile height is 1.5-20 mm; and / or, In the weaving process and the knitting process, the weight of the obtained blanket is 200-2000 GSM.
7. The method for preparing the imitation cotton carpet according to claim 1, characterized in that: In step S4, the post-processing is water-falling processing or ball-rolling processing; Wherein, during the ball rolling process, the temperature of the rolling machine is 80-150°C, and the processing time is 3-30 minutes.
8. The method for preparing the imitation cotton carpet according to claim 1, characterized in that: In step S4, the carpet surface is further subjected to a pile fixing treatment, the pile fixing treatment being before or after the post-finishing treatment, and the pile fixing treatment comprises: The fluff layer is heated and treated with a fluff fixing agent, wherein the fluff fixing agent has a viscosity of 1500-2000 mPa.s and a glue amount of 40-60 g / m 2 , the heating temperature is 135-145℃.
9. The method for preparing the imitation cotton carpet according to claim 8, characterized in that: The velvet fixing agent is selected from a mixture of any two of EVA glue, stone powder, water, a thickener or a foaming agent; And / or, in the adhesive backing treatment process, the adhesive backing is selected from any one or more of latex, TPE, hot melt adhesive, non-woven point plastic anti-slip layer, EVA, polyurethane reactive adhesive or modified silicone.
10. The cotton-like carpet prepared by the method for preparing the cotton-like carpet according to any one of claims 1 to 9, characterized in that: The specification of the imitation cotton filament is 75-2500D; the imitation cotton carpet comprises a carpet surface and a back surface, the surface of the carpet surface is provided with a fluff layer, and the back surface is provided with a back adhesive.