Production method of low-basis-weight environment-friendly craft paper

By adding specific chemical agents and steps to enhance the hydration force and binding force between the fibers, the problem of insufficient damage resistance of jammed paper is solved, and low-quantity and high-performance jammed paper production is achieved. Meet market demand and reduce resource consumption.

CN119021025APending Publication Date: 2024-11-26ZHONGSHAN YONG FA PAPER IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411372778.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing knot paper has insufficient resistance to breakage, which leads to easy rupture during heavy packaging or complex logistics transportation, inability to effectively protect internal items, and low quantification leads to increased cost and resource consumption.

Method used

After the wood pulp and waste pulp are beaten, chemical agents such as sodium percarbonate solution, sodium hydroxide solution, calcium chloride solution and caprolactam are added to form an intermediate slurry, and washed by hot water suction filtration, molding and dehydration, and pressing Dehydration and drying steps make low-quantity environmentally friendly paper, which enhances the hydration and binding force between the fibers.

Benefits of technology

It improves the crack resistance and strength of knot paper, makes it have excellent break resistance, meets the market's demand for low-quantitative and high-performance knot paper, and reduces resource consumption and costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a low-basis-weight environment-friendly craft paper production method, and belongs to the technical field of packaging paperboards, the production method comprises the following steps: S1, preparing a paper pulp raw material; s2, mixing a paper pulp raw material, a sodium percarbonate solution, a sodium hydroxide solution, a calcium chloride solution, caprolactam and potassium persulfate to obtain intermediate pulp; and S3, carrying out suction filtration washing, molding dehydration and squeezing dehydration on the intermediate slurry, drying after squeezing, and carrying out pre-drying, sizing, post-drying, press polishing, reeling and rewinding to obtain a finished product of the craft paper. According to the invention, the sodium percarbonate solution and the sodium hydroxide solution are added to enhance the hydration force among fibers in the system and greatly increase the complexing amount of metal ions, and on the basis, the calcium chloride solution is added to introduce calcium ions to form strong hydrogen bond linkage with fiber molecules in the system; caprolactam is added to react with hydroxyl groups on paper pulp raw material fibers, so that the binding force between the fibers is further improved, and the kraft liner board finished product has excellent breakage resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of packaging paperboard, and in particular relates to a method for producing low-quantity environmentally friendly kraft paper. Background Art

[0002] With the rapid development of the packaging industry and the continuous improvement of environmental awareness, the market's requirements for packaging materials are becoming increasingly stringent. As a commonly used packaging paper, kraft paper has a wide range of applications, covering the packaging, transportation and storage of various commodities. The basis weight of traditional kraft paper is often high, which, although it guarantees its strength and durability to a certain extent, also increases costs and resource consumption. In addition, with the enhancement of environmental awareness and the market's demand for cost reduction, the development of low-basis-weight kraft paper has become an important development direction for the industry. However, reducing the basis weight often leads to a decrease in the tear resistance of the paper, which brings many challenges to practical applications. For example, when packaging heavy objects or undergoing complex logistics and transportation, kraft paper with insufficient tear resistance is easy to break, and thus cannot effectively protect the internal items.

[0003] Therefore, in order to meet the market demand for low-weight, high-performance kraft paper, technical personnel of various enterprises have continuously carried out technical innovation and improvement, trying to reduce the weight while improving the tear resistance of kraft paper by optimizing the selection and ratio of papermaking raw materials, improving papermaking processes, and adopting new reinforcing agents and additives. It can be seen that the development of a low-weight, high-tear kraft paper has very important practical significance, and it is also an inevitable trend to adapt to market demand and promote the sustainable development of the industry. Summary of the invention

[0004] The purpose of the present invention is to provide a method for producing low-weight environmentally friendly kraft paper, which solves the problem of poor tear resistance of kraft paper in the prior art.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for producing low-quantity environmentally friendly kraft paper, the production method specifically comprising the following steps:

[0007] S1, removing impurities from wood pulp and waste paper pulp through a pressure screen and a slag remover, and then transferring them to a disc grinder for pulping to obtain paper pulp raw materials for standby use;

[0008] S2, stirring the pulp raw material and the sodium percarbonate solution uniformly, adding the sodium hydroxide solution to maintain the pH value of the solution and then controlling the temperature and stirring, adding the calcium chloride solution and stirring after the stirring is completed, and then adding caprolactam and potassium persulfate and stirring to obtain an intermediate slurry;

[0009] S3. Use hot water to filter and wash the intermediate slurry, then shape and dehydrate it, and then press and dehydrate it. After pressing, it is dried, and then it is pre-dried, sizing, post-dried, calendered, coiled, and rewound to obtain the finished kraft paper.

[0010] As a preferred technical solution of the present invention, the mass ratio of the wood pulp to the waste paper pulp in step S1 is 0.4-0.6:1.

[0011] As a preferred technical solution of the present invention, the wood pulp in step S1 includes coniferous wood pulp, and the coniferous wood pulp is crushed at a concentration of 4.0-5.0%; the waste paper pulp includes domestic waste paper pulp, and the domestic waste paper pulp is crushed at a concentration of 7.5-8.0%.

[0012] As a preferred technical solution of the present invention, the mass ratio of the pulp raw material, sodium percarbonate solution, calcium chloride solution, caprolactam and potassium persulfate in step S2 is 1-1.2:0.5-0.6:0.4-0.5:0.5-0.55:0.1-0.12.

[0013] Furthermore, the mass concentration of the sodium percarbonate solution is 1.0-1.1 g / L; the mass concentration of the sodium hydroxide solution is 20%; and the concentration of the calcium chloride solution is 50 mmol / L.

[0014] As a preferred technical solution of the present invention, the pH value of the solution in step S2 is 8-9.

[0015] As a preferred technical solution of the present invention, the temperature of the temperature-controlled stirring in step S2 is 28-30° C. and the time is 1.5-2 h.

[0016] As a preferred technical solution of the present invention, the stirring time of adding the calcium chloride solution in step S2 is 2-3 hours; the stirring time of adding caprolactam and potassium persulfate is 2.5-3 hours.

[0017] As a preferred technical solution of the present invention, the number of suction filtration and washing in step S3 is 3-5 times.

[0018] As a preferred technical solution of the present invention, the molding dehydration in step S3 is dehydration to a dryness of 15-20%; the pressing dehydration is dehydration to a dryness of 40-45%; and the drying is drying to a dryness of 90-95%.

[0019] As a preferred technical solution of the present invention, the present invention also provides a kraft paper produced by the above production method.

[0020] Beneficial effects of the present invention:

[0021] The invention adds sodium percarbonate solution and sodium hydroxide solution so that hydrogen peroxide ions exist in the system and react with pulp raw material fibers, introduces a large number of carboxyl groups, enhances the hydration force between fibers in the system, and greatly increases the complexing amount of metal ions. On this basis, calcium chloride solution is added to introduce calcium ions to form strong hydrogen bond links with fiber molecules in the system, and caprolactam is added to react with hydroxyl groups on pulp raw material fibers to further improve the bonding force between fibers, thereby improving the strength of finished kraft paper, that is, making the finished kraft paper have excellent burst resistance. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Example 1

[0024] A method for producing low-quantity environmentally friendly kraft paper, the production method specifically comprising the following steps:

[0025] S1, removing impurities from wood pulp and waste paper pulp through a pressure screen and a slag remover, and then transferring them to a disc grinder for pulping to obtain paper pulp raw materials for standby use;

[0026] The mass ratio of the wood pulp to the waste paper pulp is 0.5:1;

[0027] The wood pulp includes coniferous wood pulp with a disintegration concentration of 5.0%; the waste paper pulp includes domestic waste paper pulp with a disintegration concentration of 8.0%;

[0028] S2, the pulp raw material and the sodium percarbonate solution with a mass concentration of 1.0g / L are stirred evenly, and a sodium hydroxide solution with a mass concentration of 20% is added to maintain the solution pH = 9, and then the temperature is controlled at 28°C and stirred for 1.5h. After the stirring is completed, a calcium chloride solution with a concentration of 50mmol / L is added and stirred for 2.5h, and then caprolactam and potassium persulfate are added and stirred for 3h to obtain an intermediate slurry;

[0029] The mass ratio of the pulp raw material, the sodium percarbonate solution, the calcium chloride solution, caprolactam and potassium persulfate is 1.1:0.5:0.4:0.53:0.1.

[0030] S3. The intermediate slurry is filtered and washed three times with hot water, and then formed and dehydrated to a dryness of 15%, and then pressed and dehydrated to a dryness of 40%. After pressing, it is dried to a dryness of 95%, and then pre-dried, sizing, post-dried, calendered, coiled, and rewound to obtain a finished kraft paper.

[0031] Example 2

[0032] A method for producing low-quantity environmentally friendly kraft paper, the production method specifically comprising the following steps:

[0033] S1, removing impurities from wood pulp and waste paper pulp through a pressure screen and a slag remover, and then transferring them to a disc grinder for pulping to obtain paper pulp raw materials for standby use;

[0034] The mass ratio of the wood pulp to the waste paper pulp is 0.4:1;

[0035] The wood pulp includes coniferous wood pulp with a disintegration concentration of 4.5%; the waste paper pulp includes domestic waste paper pulp with a disintegration concentration of 7.5%;

[0036] S2, the pulp raw material and the sodium percarbonate solution with a mass concentration of 1.1g / L are stirred evenly, and a sodium hydroxide solution with a mass concentration of 20% is added to maintain the solution pH = 8, and then the temperature is controlled at 29°C and stirred for 2h. After the stirring is completed, a calcium chloride solution with a concentration of 50mmol / L is added and stirred for 2h, and then caprolactam and potassium persulfate are added and stirred for 2.5h to obtain an intermediate slurry;

[0037] The mass ratio of the pulp raw material, the sodium percarbonate solution, the calcium chloride solution, caprolactam and potassium persulfate is 1:0.6:0.45:0.5:0.12.

[0038] S3. The intermediate slurry is filtered and washed with hot water for 4 times, and then formed and dehydrated to a dryness of 20%, and then pressed and dehydrated to a dryness of 45%. After pressing, it is dried to a dryness of 90%, and then pre-dried, sizing, post-dried, calendered, coiled, and rewound to obtain a finished kraft paper.

[0039] Example 3

[0040] A method for producing low-quantity environmentally friendly kraft paper, the production method specifically comprising the following steps:

[0041] S1, removing impurities from wood pulp and waste paper pulp through a pressure screen and a slag remover, and then transferring them to a disc grinder for pulping to obtain paper pulp raw materials for standby use;

[0042] The mass ratio of the wood pulp to the waste paper pulp is 0.6:1;

[0043] The wood pulp includes coniferous wood pulp with a disintegration concentration of 4.0%; the waste paper pulp includes domestic waste paper pulp with a disintegration concentration of 8.0%;

[0044] S2, the pulp raw material and the sodium percarbonate solution with a mass concentration of 1.0g / L are stirred evenly, and a sodium hydroxide solution with a mass concentration of 20% is added to maintain the solution pH = 8.5, and then the temperature is controlled at 30°C and stirred for 2h. After the stirring is completed, a calcium chloride solution with a concentration of 50mmol / L is added and stirred for 3h, and then caprolactam and potassium persulfate are added and stirred for 2.5h to obtain an intermediate slurry;

[0045] The mass ratio of the pulp raw material, the sodium percarbonate solution, the calcium chloride solution, caprolactam and potassium persulfate is 1.2:0.55:0.5:0.55:0.11.

[0046] S3. The intermediate slurry is filtered and washed with hot water for 5 times, and then formed and dehydrated to a dryness of 15%, and then pressed and dehydrated to a dryness of 45%. After pressing, it is dried to a dryness of 90%, and then pre-dried, sizing, post-dried, calendered, coiled, and rewound to obtain a finished kraft paper.

[0047] Comparative Example 1

[0048] Compared with Example 2, the difference is that no sodium percarbonate solution is added in step S2 of Comparative Example 1, and the remaining operating steps and parameters are the same, namely:

[0049] A method for producing low-quantity environmentally friendly kraft paper, the production method specifically comprising the following steps:

[0050] S1, removing impurities from wood pulp and waste paper pulp through a pressure screen and a slag remover, and then transferring them to a disc grinder for pulping to obtain paper pulp raw materials for standby use;

[0051] The mass ratio of the wood pulp to the waste paper pulp is 0.4:1;

[0052] S2, adding a sodium hydroxide solution with a mass concentration of 20% to the pulp raw material to maintain the solution pH = 8, and then controlling the temperature at 29°C and stirring for 2 hours. After the stirring is completed, adding a calcium chloride solution with a concentration of 50 mmol / L and stirring for 2 hours, and then adding caprolactam and potassium persulfate and stirring for 2.5 hours to obtain an intermediate slurry;

[0053] The mass ratio of the pulp raw material, calcium chloride solution, caprolactam and potassium persulfate is 1:0.45:0.5:0.12;

[0054] S3. The intermediate slurry is filtered and washed with hot water for 4 times, and then formed and dehydrated to a dryness of 20%, and then pressed and dehydrated to a dryness of 45%. After pressing, it is dried to a dryness of 90%, and then pre-dried, sizing, post-dried, calendered, coiled, and rewound to obtain a finished kraft paper.

[0055] Comparative Example 2

[0056] Compared with Example 2, the difference is that in step S2 of Comparative Example 2, no sodium hydroxide solution is added to maintain the pH of the solution, and the remaining operating steps and parameters are the same, namely:

[0057] S1, removing impurities from wood pulp and waste paper pulp through a pressure screen and a slag remover, and then transferring them to a disc grinder for pulping to obtain paper pulp raw materials for standby use;

[0058] The mass ratio of the wood pulp to the waste paper pulp is 0.4:1;

[0059] S2, the pulp raw material and the sodium percarbonate solution with a mass concentration of 1.1g / L are stirred evenly, after the stirring is completed, a calcium chloride solution with a concentration of 50mmol / L is added and stirred for 2h, and then caprolactam and potassium persulfate are added and stirred for 2.5h to obtain an intermediate slurry;

[0060] The mass ratio of the pulp raw material, sodium percarbonate solution, calcium chloride solution, caprolactam and potassium persulfate is 1:0.6:0.45:0.5:0.12;

[0061] S3. The intermediate slurry is filtered and washed with hot water for 4 times, and then formed and dehydrated to a dryness of 20%, and then pressed and dehydrated to a dryness of 45%. After pressing, it is dried to a dryness of 90%, and then pre-dried, sizing, post-dried, calendered, coiled, and rewound to obtain a finished kraft paper.

[0062] Comparative Example 3

[0063] Compared with Example 2, the difference is that no calcium chloride solution is added in step S2 of Comparative Example 3, and the remaining operating steps and parameters are the same, that is:

[0064] S1, removing impurities from wood pulp and waste paper pulp through a pressure screen and a slag remover, and then transferring them to a disc grinder for pulping to obtain paper pulp raw materials for standby use;

[0065] The mass ratio of the wood pulp to the waste paper pulp is 0.4:1;

[0066] S2, the pulp raw material and the sodium percarbonate solution with a mass concentration of 1.1g / L are stirred evenly, and a sodium hydroxide solution with a mass concentration of 20% is added to maintain the solution pH = 8, and then the temperature is controlled at 29°C and stirred for 2h. After the stirring is completed, caprolactam and potassium persulfate are added and stirred for 2.5h to obtain an intermediate slurry;

[0067] The mass ratio of the pulp raw material, the sodium percarbonate solution, the caprolactam and the potassium persulfate is 1:0.6:0.5:0.12;

[0068] S3. The intermediate slurry is filtered and washed with hot water for 4 times, and then formed and dehydrated to a dryness of 20%, and then pressed and dehydrated to a dryness of 45%. After pressing, it is dried to a dryness of 90%, and then pre-dried, sizing, post-dried, calendered, coiled, and rewound to obtain a finished kraft paper.

[0069] Comparative Example 4

[0070] Compared with Example 2, the difference is that caprolactam is not added in step S2 of Comparative Example 4, and the remaining operation steps and parameters are the same, that is:

[0071] S1, removing impurities from wood pulp and waste paper pulp through a pressure screen and a slag remover, and then transferring them to a disc grinder for pulping to obtain paper pulp raw materials for standby use;

[0072] The mass ratio of the wood pulp to the waste paper pulp is 0.4:1;

[0073] S2, the pulp raw material and the sodium percarbonate solution with a mass concentration of 1.1g / L are stirred evenly, and a sodium hydroxide solution with a mass concentration of 20% is added to maintain the solution pH = 8, and then the temperature is controlled at 29°C and stirred for 2h. After the stirring is completed, a calcium chloride solution with a concentration of 50mmol / L is added and stirred for 2h, and then potassium persulfate is added and stirred for 2.5h to obtain an intermediate slurry;

[0074] The mass ratio of the pulp raw material, the sodium percarbonate solution, the calcium chloride solution and the potassium persulfate is 1:0.6:0.45:0.12;

[0075] S3. The intermediate slurry is filtered and washed with hot water for 4 times, and then formed and dehydrated to a dryness of 20%, and then pressed and dehydrated to a dryness of 45%. After pressing, it is dried to a dryness of 90%, and then pre-dried, sizing, post-dried, calendered, coiled, and rewound to obtain a finished kraft paper.

[0076] Performance Testing

[0077] According to GB / T 22865-2008, the finished kraft paperboards prepared in Examples 1-3 and Comparative Examples 1-4 were subjected to quantitative and bursting strength tests, and the results are shown in Table 1.

[0078] Table 1

[0079] <![CDATA[Quantitative (g / m 2 )]]> <![CDATA[Bursting strength index (kPa·m 2 / g)]]> Example 1 70 3.96 Example 2 70 4.01 Example 3 70 3.98 Comparative Example 1 75 2.13 Comparative Example 2 80 2.25 Comparative Example 3 75 2.72 Comparative Example 4 75 2.84

[0080] As can be seen from Table 1, the finished kraft paper prepared by the present invention has a low basis weight and excellent burst resistance. This is because the present invention adds sodium percarbonate solution and sodium hydroxide solution so that hydrogen peroxide ions exist in the system and react with pulp raw material fibers, introduces a large number of carboxyl groups, enhances the hydration between fibers in the system, and greatly increases the complexing amount of metal ions. On this basis, calcium chloride solution is added to introduce calcium ions to form strong hydrogen bonds with fiber molecules in the system, and caprolactam is added to react with hydroxyl groups on pulp raw material fibers to further improve the bonding force between fibers, thereby improving the strength of the finished kraft paper, that is, the finished kraft paper has excellent burst resistance.

[0081] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0082] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A method for producing low-quantity environmentally friendly kraft paper, characterized in that: The production method specifically comprises the following steps: S1, removing impurities from wood pulp and waste paper pulp through a pressure screen and a slag remover, and then transferring them to a disc grinder for pulping to obtain paper pulp raw materials for standby use; S2, stirring the pulp raw material and the sodium percarbonate solution uniformly, adding the sodium hydroxide solution to maintain the pH value of the solution and then controlling the temperature and stirring, adding the calcium chloride solution and stirring after the stirring is completed, and then adding caprolactam and potassium persulfate and stirring to obtain an intermediate slurry; S3. Use hot water to filter and wash the intermediate slurry, then shape and dehydrate it, and then press and dehydrate it. After pressing, it is dried, and then it is pre-dried, sizing, post-dried, calendered, coiled, and rewound to obtain the finished kraft paper.

2. The method for producing low-weight environmentally friendly kraft paper according to claim 1, characterized in that: The mass ratio of the wood pulp to the waste paper pulp in step S1 is 0.4-0.6:

1.

3. The method for producing low-weight environmentally friendly kraft paper according to claim 1, characterized in that: In step S2, the mass ratio of the pulp raw material, the sodium percarbonate solution, the calcium chloride solution, the caprolactam and the potassium persulfate is 1-1.2:0.5-0.6:0.4-0.5:0.5-0.55:0.1-0.

12.

4. The method for producing low-weight environmentally friendly kraft paper according to claim 1, characterized in that: The mass concentration of the sodium percarbonate solution is 1.0-1.1 g / L; the mass concentration of the sodium hydroxide solution is 20%; and the concentration of the calcium chloride solution is 50 mmol / L.

5. The method for producing low-weight environmentally friendly kraft paper according to claim 1, characterized in that: The pH value of the solution in step S2 is 8-9.

6. The method for producing low-weight environmentally friendly kraft paper according to claim 1, characterized in that: The temperature of the temperature-controlled stirring in step S2 is 28-30° C. and the time is 1.5-2 h.

7. The method for producing low-weight environmentally friendly kraft paper according to claim 1, characterized in that: The stirring time of adding calcium chloride solution in step S2 is 2-3 hours; the stirring time of adding caprolactam and potassium persulfate is 2.5-3 hours.

8. The method for producing low-weight environmentally friendly kraft paper according to claim 1, characterized in that: The number of suction filtration and washing in step S3 is 3-5 times.

9. The method for producing low-weight environmentally friendly kraft paper according to claim 1, characterized in that: In step S3, the molding dehydration is to dehydrate to a dryness of 15-20%; the pressing dehydration is to dehydrate to a dryness of 40-45%; and the drying is to dry to a dryness of 90-95%.

10. A kraft paper produced by the method for producing low-weight environmentally friendly kraft paper according to any one of claims 1 to 9.