Cotton stalk biochemical mechanical pulp treated by compound enzyme as well as preparation method and application of cotton stalk biochemical mechanical pulp

Through the composite enzyme treatment method, the problems of high energy consumption and poor fiber binding force during cotton pulping and papermaking process were solved, and excellent performance of cotton stalk biochemical mechanical pulp was prepared, achieving efficient utilization of cotton stalks and shortage of paper raw materials. ease.

CN119021026APending Publication Date: 2024-11-26QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES)

Patent Information

Application Number
CN202411160069.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art has problems such as high energy consumption, high chemical dosage and poor fiber binding force in the cotton stalk pulping and papermaking process, and it is difficult to effectively use cotton stalks as papermaking raw materials.

Method used

Using the composite enzyme treatment method, cotton stalks are pretreated using a complex enzyme composed of cellulase, xylanase and lipase. The cotton stalks are pre-treated by pre-steaming, spiral extrusion, wire rubbing, composite enzyme treatment, hot alkali impregnation and high concentration. By refining and other steps, a cotton stalk biochemical mechanical slurry with excellent performance was prepared.

Benefits of technology

It improves the utilization rate of cotton stalks, reduces energy consumption and chemical consumption, improves the mechanical properties of pulp, enhances tensile strength, tear strength and ring pressure strength, and solves the problem of poor fiber bonding force.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a compound enzyme treated cotton stalk biochemical mechanical pulp and a preparation method and application thereof, the preparation method comprises the following steps: cotton stalks are pretreated, and the pretreatment method comprises the following steps: removing branches of the cotton stalks, washing, cutting into sections and air-drying; the pretreated cotton stalks are sequentially subjected to pre-steaming and spiral extrusion thread rolling; soaking the cotton stalks subjected to thread rolling in a buffer solution of a compound enzyme for compound enzyme treatment, wherein the compound enzyme comprises xylanase, pectinase and lipase; soaking the cotton stalks treated by the compound enzyme in a hot alkali solution for a set time, and then sequentially performing high-concentration pulping, latency, pulp screening and PFI pulping to obtain the cotton stalk biochemical mechanical pulp. The compound enzyme composed of cellulase, xylanase and lipase is used for treating cotton stalks, the treatment effect of chemicals is promoted through the action of the enzyme, the pulping effect is improved, and the paper pulp performance is improved. The method can improve the utilization rate of cotton stalks and effectively relieve the problem of shortage of papermaking raw materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pulping and papermaking, and in particular relates to a biochemical mechanical pulp of cotton stalks treated with a composite enzyme, and a preparation method and application thereof. Background Art

[0002] The statements herein merely provide background information related to the present invention and do not necessarily constitute prior art.

[0003] In order to alleviate the pressure of domestic papermaking raw material shortage, non-wood raw materials have attracted extensive research in pulping and papermaking. For non-wood papermaking raw materials, choosing appropriate pulping and papermaking methods to match the raw materials can regenerate paper and paperboard suitable for different purposes. Cotton is an important economic crop worldwide. If a large amount of by-products (cotton stalks or leaves) left by large-scale cotton planting are left in the fields, it may cause solid waste disposal problems and bring the risk of pests and diseases to subsequent cotton crops. Cotton stalks are an excellent biomass raw material and urgently need attention to fully utilize them. Using cotton stalks for pulping can not only alleviate the shortage of domestic papermaking raw materials, but also increase the high-value utilization of cotton stalks.

[0004] In recent years, high-yield pulping technology has attracted much attention due to its wide adaptability of raw materials, clean production process, and low production investment. Among them, chemical mechanical pulp is developed based on traditional high-yield pulp. Adding chemical additives in the mechanical pulping process is beneficial to improving energy efficiency and improving pulp properties. In addition to chemical methods, biotechnology has attracted much attention because of its environmental friendliness. There are two ways to apply biotechnology to the pulping process. One is to use fungi to pretreat the raw materials, and the other is to directly add biological enzymes during the pulping process. Fungal treatment in the pulping process has the disadvantages of long processing time and low efficiency, while biological enzymes are more suitable for pulping and papermaking processes due to their strong specificity, high efficiency and mild action conditions.

[0005] Cotton stalks can be divided into three parts: cotton stalk bark, xylem and pith. Cotton stalk bark is composed of wood cells, thin-walled cells and bast fibers. The bast fibers are the longest and are excellent raw materials for papermaking. The main fiber source of the xylem is wood fiber. The pith is composed of thin-walled cells, which accounts for a very small proportion. The fiber cell content of cotton stalks is higher than that of most grass raw materials, making it suitable as a raw material for pulping and papermaking. However, the components and morphologies of each part of the cotton stalk are different, and the pulping properties are also quite different. Therefore, the preparation of mechanical pulp from cotton stalks requires strong pretreatment and chemical treatment, which increases energy consumption and the use of chemicals. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a biochemical mechanical pulp of cotton stalks treated with a composite enzyme and a preparation method and application thereof. The composite enzyme composed of cellulase, xylanase and lipase is used to treat cotton stalks, and the effect of the enzyme is used to promote the treatment effect of chemicals, improve the pulping effect, and improve the pulp performance. This method can improve the utilization rate of cotton stalks and effectively alleviate the problem of shortage of papermaking raw materials.

[0007] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0008] In a first aspect, the present invention provides a method for preparing biochemical mechanical pulp of cotton stalks treated with a composite enzyme, comprising the following steps: pretreating the cotton stalks, wherein the pretreatment method comprises debranching, washing, cutting and air-drying the cotton stalks;

[0009] The pretreated cotton stalks are sequentially subjected to pre-steaming and spiral extrusion and thread rolling;

[0010] The cotton stalks after spinning are immersed in a buffer solution of a composite enzyme for composite enzyme treatment, wherein the composite enzyme includes xylanase, pectinase and lipase;

[0011] The cotton stalks treated with the compound enzyme are immersed in a hot alkaline solution for a set time, and then high-concentration pulping, latent removal, pulp screening and PFI pulping are carried out in sequence to obtain the cotton stalk biochemical mechanical pulp.

[0012] In some embodiments, in the complex enzyme, the mass ratio of xylanase, pectinase and lipase is 1-2:1-2:1-2.

[0013] Preferably, the total enzyme dosage of the complex enzyme is 30-50 U / g.

[0014] Preferably, in the buffer solution of the complex enzyme, the buffer solution is a citric acid-sodium citrate solution with a pH value of 4.5-6.5.

[0015] Preferably, the solid-liquid ratio during the complex enzyme treatment is 1:3-10, g / mL; preferably 1:3-8, g / mL; further preferably 1:3-6, g / mL; specifically 1:4, g / mL.

[0016] Preferably, the temperature of the complex enzyme treatment is 45-65°C and the treatment time is 30-90 min.

[0017] Biological enzymes have the advantages of high efficiency, substrate specificity, mild action conditions, etc., and can be used in the preparation process of mechanical pulp to improve the performance of mechanical pulp, reduce energy consumption, and save the consumption of chemicals. In the present invention, xylanase can improve the performance of pulp, pectinase can degrade dissolved substances and colloidal substances, and lipase can degrade lipid substances in cotton stalk skin, thereby improving the bonding of pulp fibers, and a non-wood raw material high-yield pulp with excellent performance is obtained, which can be used to improve the mechanical properties of waste paper pulp, and the finished paper shows good tensile strength, tear strength and ring crush strength.

[0018] In some embodiments, the length of the cut cotton stalk is 4-6 cm. When the length of the cut cotton stalk is 4-6 cm, the subsequent pre-steaming and spiral extrusion have better effects.

[0019] In some embodiments, the solid-to-liquid ratio during pre-steaming is 1:4-8, g / mL; preferably 1:4-6, g / mL; further preferably 1:5, g / mL.

[0020] Preferably, the pre-steaming temperature is 90-100°C and the time is 30-50min; preferably 95°C and 40min. Adding chemicals during the pre-steaming process can promote the thread rolling effect of the raw materials. In this process, without using chemicals, the time and temperature are appropriately extended, and extrusion is performed immediately after steaming without cooling, which promotes the extrusion and thread rolling effect of the cotton stalks.

[0021] In some embodiments, the compression ratio of the spiral extrusion and thread rolling is 1:3-5, preferably 1:4. The use of spiral extrusion for stripping and thread rolling can fully separate and divide the cotton stalks, which is an important step in the preparation process of chemical mechanical pulp.

[0022] In some embodiments, the hot alkali solution is a sodium hydroxide solution, the temperature of the hot alkali solution is 90-100° C., and the mass percentage of the solute in the hot alkali solution is 3-5%. Hot alkali impregnation can effectively improve pulp performance, reduce pulping energy consumption, and improve pulp drainage performance.

[0023] Preferably, the cotton stalks treated with the complex enzyme are immersed in the hot alkaline solution for 30-50 minutes.

[0024] In some embodiments, the rotation speed of high-concentration refining is 3000-3500 rpm, and the gaps between the two stages of refining are 0.3 mm and 0.15 mm.

[0025] In some embodiments, the PFI pulping has a beating degree of 40±2°SR.

[0026] In a second aspect, the present invention provides a biochemical mechanical pulp of cotton stalks treated with a composite enzyme, which is prepared by the preparation method.

[0027] In a third aspect, the present invention provides the use of the biochemical mechanical pulp of cotton stalks treated with the composite enzyme in the paper making of waste paper pulp.

[0028] In some embodiments, the proportion of the cotton stalk biochemical mechanical pulp in the paper sheet is 5%-50%, where % is the mass percentage.

[0029] Preferably, the basis weight of the paper is 80-120 g / m 2 , preferably 100g / m 2 .

[0030] The beneficial effects achieved by one or more embodiments of the present invention are as follows:

[0031] (1) The present invention uses cotton stalks as raw materials and invents a method for preparing a biochemical mechanical pulp of cotton stalks treated with a composite enzyme. Cotton stalks are an excellent biomass raw material and urgently need to be paid attention to in order to fully utilize them. Using cotton stalks for pulping and papermaking can not only alleviate the shortage of domestic papermaking raw materials, but also increase the utilization of cotton stalks.

[0032] (2) The present invention treats cotton stalk chemical mechanical pulp by compounding biological enzymes based on the raw material characteristics of cotton stalks. The biological enzymes have high efficiency, specificity and mild action. Appropriate biological enzymes can be selected to improve the performance of pulp and solve problems in the production process. It can reduce energy loss in the production process and reduce the processing load of pollutants in the production process. Applying biological enzymes in the preparation process of chemical mechanical pulp can not only improve the pulp performance of cotton stalk chemical mechanical pulp, but also reduce environmental pollution and energy consumption.

[0033] (3) The complex enzyme proposed in the present invention is composed of xylanase, pectinase and lipase. These three enzymes are selected according to the characteristics of cotton stalk raw materials. Xylanase can promote the hydrolysis of hemicellulose, thereby promoting the removal of part of lignin and improving the effect of alkali impregnation. Pectinase can degrade pectin in cotton stalk skin to prevent it from becoming dissolved substances and colloidal substances, which affect the binding force between pulp fibers. Lipase can enzymatically hydrolyze lipid substances contained in cotton stalk skin to prevent it from hindering the binding of fine components with long fibers. These three enzymes have a synergistic effect when acting together, which can improve the efficiency of biological enzymes in improving pulp properties. DETAILED DESCRIPTION

[0034] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0035] The specific implementation of the present invention is further described below in conjunction with examples, but the implementation of the present invention is not limited to the scope represented by the examples.

[0036] The present invention will be further described below in conjunction with the embodiments.

[0037] The materials involved in the examples can be purchased from the market. All biological enzymes are from Shandong Longkote Enzyme Preparation Co., Ltd. The enzyme activity of xylanase is 50000 U / mL, the enzyme activity of pectinase is 90000 U / mL, and the enzyme activity of lipase is 50000 U / mL.

[0038] The cotton stalks in the embodiment are from Dezhou, Shandong, and have a cellulose content of 42.37%, a hemicellulose content of 17.41%, a lignin content of 21.87%, and an ash content of 2.06%, where % is mass percentage.

[0039] Example 1

[0040] (1) Wash the debranched cotton stalks, cut them into sections of 4 to 6 cm in length, and air-dry them for later use.

[0041] (2) The cotton stalks obtained in step (1) are pre-steamed, the solid-liquid ratio of the pre-steaming is 1:5 g / mL, the steaming temperature is 95° C., and the insulation time is 40 min.

[0042] (3) The cotton stalk obtained in step (2) is immediately subjected to spiral extrusion and thread rolling, and the compression ratio of the spiral extrusion is 1:4.

[0043] (4) The cotton stalks obtained in step (3) are soaked in a buffer solution containing a complex enzyme composed of xylanase, pectinase and lipase for complex enzyme treatment, wherein the ratio of the complex enzyme (enzyme activity) is xylanase: pectinase: lipase = 2:1:1, the amount of the complex enzyme is 40 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH value of 6.0, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 50°C, and the time is 60 min.

[0044] (5) The cotton stalk obtained in step (4) is immersed in a hot alkaline solution, wherein the sodium hydroxide concentration is 4% (% is mass percentage, the same below), the solid-liquid ratio is 1:4 g / mL, the immersion temperature is 95° C., and the immersion time is 40 min.

[0045] (6) The cotton stalks obtained in step (5) are subjected to high-concentration grinding at a rotation speed of 3500 rpm, and the gaps between the two stages of grinding are 0.3 mm and 0.15 mm. After grinding, the latent force is removed and the pulp is screened, and then PFI beating is performed to increase the beating degree to 40±2°SR, and sheeting is performed.

[0046] (7) The biochemical mechanical pulp of cotton stalks in step (6) is mixed with waste paper pulp, the proportion of the biochemical mechanical pulp of cotton stalks is 15%, and the basis weight of the paper sheet is 100 g / m 2 .

[0047] Results: The pulp yield was 78.32% and the tear index of the paper sheet was 6.09 mN·m 2 / g, tensile index is 31.36N·m / g, ring crush index is 10.85N·m / g, and tear index of cotton stalk-waste pulp mixed paper is 5.52mN·m 2 / g, the tensile index is 19.55N·m / g, and the ring compression index is 6.48N·m / g.

[0048] Example 2

[0049] (1) Wash the debranched cotton stalks, cut them into 4-6 cm long segments, and air-dry them for later use.

[0050] (2) The cotton stalks obtained in step (1) are pre-steamed, the solid-liquid ratio of the pre-steaming is 1:5 g / mL, the steaming temperature is 95° C., and the insulation time is 40 min.

[0051] (3) The cotton stalk obtained in step (2) is immediately subjected to spiral extrusion and thread rolling, and the compression ratio of the spiral extrusion is 1:4.

[0052] (4) The cotton stalks obtained in step (3) are soaked in a buffer solution containing a complex enzyme composed of xylanase, pectinase and lipase for complex enzyme treatment, wherein the ratio of the complex enzyme (enzyme activity) is xylanase: pectinase: lipase = 2:1:1, the amount of the complex enzyme is 40 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH value of 6.0, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 50°C, and the time is 60 min.

[0053] (5) The cotton stalk obtained in step (4) is immersed in a hot alkaline solution, wherein the sodium hydroxide concentration is 4%, the solid-liquid ratio is 1:4 g / mL, the immersion temperature is 95° C., and the time is 40 min.

[0054] (6) The cotton stalks obtained in step (5) are subjected to high-consistency grinding at a rotation speed of 3000 rpm, and the gaps between the two stages of grinding are 0.3 mm and 0.15 mm. After grinding, the latent force is removed and the pulp is screened, and then PFI beating is performed to increase the beating degree to 40±2°SR, and sheeting is performed.

[0055] (7) The biochemical mechanical pulp of cotton stalks in step (6) is mixed with waste paper pulp for papermaking, wherein the proportion of the biochemical mechanical pulp of cotton stalks is 25%, and the papermaking basis weight is 100 g / m 2 Cotton stalk-waste pulp mixed paper sheets.

[0056] Results: The tearing index of cotton stalk-waste pulp mixed paper is 5.67 mN·m 2 / g, the tensile index is 20.96N·m / g, and the ring compression index is 6.78N·m / g.

[0057] Example 3

[0058] (1) Wash the debranched cotton stalks, cut them into 4-6 cm long segments, and air-dry them for later use.

[0059] (2) The cotton stalks obtained in step (1) are pre-steamed, the solid-liquid ratio of the pre-steaming is 1:5 g / mL, the steaming temperature is 95° C., and the insulation time is 40 min.

[0060] (3) The cotton stalk obtained in step (2) is immediately subjected to spiral extrusion and thread rolling, and the compression ratio of the spiral extrusion is 1:4.

[0061] (4) The cotton stalks obtained in step (3) are soaked in a buffer solution containing a complex enzyme composed of xylanase, pectinase and lipase for complex enzyme treatment, wherein the ratio of the complex enzyme (enzyme activity) is xylanase: pectinase: lipase = 1:2:1, the amount of the complex enzyme is 40 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH value of 6.0, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 50°C, and the time is 60 min.

[0062] (5) The cotton stalk obtained in step (4) is immersed in a hot alkaline solution, wherein the sodium hydroxide concentration is 4%, the solid-liquid ratio is 1:4 g / mL, the immersion temperature is 95° C., and the time is 40 min.

[0063] (6) The cotton stalks obtained in step (5) are subjected to high-consistency grinding at a rotation speed of 3200 rpm, and the gaps between the two stages of grinding are 0.3 mm and 0.15 mm. After grinding, the latent force is removed and the pulp is screened, and then PFI beating is performed to increase the beating degree to 40±2°SR, and sheeting is performed.

[0064] (7) The biochemical mechanical pulp of cotton stalks prepared in step (6) is mixed with waste paper pulp, wherein the proportion of the biochemical mechanical pulp of cotton stalks is 15%, and the papermaking basis weight is 100 g / m 2 Cotton stalk-waste pulp mixed paper sheets.

[0065] Results: The pulp yield was 80.07% and the tear index of the paper sheet was 5.77 mN·m 2 / g, tensile index is 30.82N·m / g, ring crush index is 10.46N·m / g, and tear index of cotton stalk-waste pulp mixed paper is 5.48mN·m 2 / g, the tensile index is 19.35N·m / g, and the ring compression index is 6.19N·m / g.

[0066] Example 4

[0067] (1) Wash the debranched cotton stalks, cut them into sections of 4 to 6 cm in length, and air-dry them for later use.

[0068] (2) The cotton stalks obtained in step (1) are pre-steamed, the solid-liquid ratio of the pre-steaming is 1:5 g / mL, the steaming temperature is 95° C., and the insulation time is 40 min.

[0069] (3) The cotton stalk obtained in step (2) is immediately subjected to spiral extrusion and thread rolling, and the compression ratio of the spiral extrusion is 1:4.

[0070] (4) The cotton stalks obtained in step (3) are soaked in a buffer solution containing a complex enzyme composed of xylanase, pectinase and lipase for complex enzyme treatment, wherein the ratio of the complex enzyme (enzyme activity) is xylanase: pectinase: lipase = 1:2:1, the amount of the complex enzyme is 40 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH value of 6.0, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 50°C, and the time is 60 min.

[0071] (5) The cotton stalk obtained in step (4) is immersed in a hot alkaline solution, wherein the sodium hydroxide concentration is 4%, the solid-liquid ratio is 1:4, the immersion temperature is 95° C., and the time is 40 minutes.

[0072] (6) The cotton stalks obtained in step (5) are subjected to high-concentration grinding at a rotation speed of 3500 rpm, and the gaps between the two stages of grinding are 0.3 mm and 0.15 mm. After grinding, the latent force is removed and the pulp is screened, and then PFI beating is performed to increase the beating degree to 40±2°SR, and sheeting is performed.

[0073] (7) The biochemical mechanical pulp of cotton stalks prepared in step (6) is mixed with waste paper pulp, wherein the proportion of the biochemical mechanical pulp of cotton stalks is 15%, and the papermaking basis weight is 100 g / m 2 Cotton stalk-waste pulp mixed paper sheets.

[0074] Results: The tearing index of cotton stalk-waste pulp mixed paper is 5.55 mN·m 2 / g, the tensile index is 20.33N·m / g, and the ring compression index is 6.53N·m / g.

[0075] Example 5

[0076] (1) Wash the debranched cotton stalks, cut them into sections of 4 to 6 cm in length, and air-dry them for later use.

[0077] (2) The cotton stalks obtained in step (1) are pre-steamed, the solid-liquid ratio of the pre-steaming is 1:5 g / mL, the steaming temperature is 95° C., and the insulation time is 40 min.

[0078] (3) The cotton stalk obtained in step (2) is immediately subjected to spiral extrusion and thread rolling, and the compression ratio of the spiral extrusion is 1:4.

[0079] (4) The cotton stalks obtained in step (3) are soaked in a buffer solution containing a complex enzyme composed of xylanase, pectinase and lipase for complex enzyme treatment, wherein the ratio of the complex enzyme (enzyme activity) is xylanase: pectinase: lipase = 1:1:2, the amount of the complex enzyme is 40 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH of 6.0, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 50°C, and the time is 60 min.

[0080] (5) The cotton stalk obtained in step (4) is immersed in a hot alkaline solution, wherein the sodium hydroxide concentration is 4%, the solid-liquid ratio is 1:4 g / mL, the immersion temperature is 95° C., and the time is 40 min.

[0081] (6) The cotton stalks obtained in step (5) are subjected to high-concentration grinding at a rotation speed of 3500 rpm, and the gaps between the two stages of grinding are 0.3 mm and 0.15 mm. After grinding, the latent force is removed and the pulp is screened, and then PFI beating is performed to increase the beating degree to 40±2°SR, and sheeting is performed.

[0082] (7) The biochemical mechanical pulp of cotton stalks in step (6) is mixed with waste paper pulp for papermaking, wherein the proportion of the biochemical mechanical pulp of cotton stalks is 25%, and the papermaking basis weight is 100 g / m 2 Cotton stalk-waste pulp mixed paper sheets.

[0083] Results: The pulp yield was 80.75% and the tear index of the paper sheet was 5.72 mN·m 2 / g, tensile index is 30.77N·m / g, ring crush index is 10.53N·m / g, and tear index of cotton stalk-waste pulp mixed paper is 5.45mN·m 2 / g, the tensile index is 19.23N·m / g, and the ring compression index is 6.23N·m / g.

[0084] Example 6

[0085] (1) Wash the debranched cotton stalks, cut them into sections of 4 to 6 cm in length, and air-dry them for later use.

[0086] (2) The cotton stalks obtained in step (1) are pre-steamed, the solid-liquid ratio of the pre-steaming is 1:5 g / mL, the steaming temperature is 95° C., and the insulation time is 40 min.

[0087] (3) The cotton stalk obtained in step (2) is immediately subjected to spiral extrusion and thread rolling, and the compression ratio of the spiral extrusion is 1:4.

[0088] (4) The cotton stalks obtained in step (3) are soaked in a buffer solution containing a complex enzyme composed of xylanase, pectinase and lipase for complex enzyme treatment, wherein the ratio of the complex enzyme (enzyme activity) is xylanase: pectinase: lipase = 1:1:2, the amount of the complex enzyme is 40 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH of 6.0, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 50°C, and the time is 60 min.

[0089] (5) The cotton stalk obtained in step (4) is immersed in a hot alkaline solution, wherein the sodium hydroxide concentration is 4%, the solid-liquid ratio is 1:4 g / mL, the immersion temperature is 95° C., and the time is 40 min.

[0090] (6) The cotton stalks obtained in step (5) are subjected to high-concentration grinding at a rotation speed of 3500 rpm, and the gaps between the two stages of grinding are 0.3 mm and 0.15 mm. After grinding, the latent force is removed and the pulp is screened, and then PFI beating is performed to increase the beating degree to 40±2°SR, and sheeting is performed.

[0091] (7) The biochemical mechanical pulp of cotton stalks in step (6) is mixed with waste paper pulp for papermaking, wherein the proportion of the biochemical mechanical pulp of cotton stalks is 25%, and the papermaking basis weight is 100 g / m 2 Cotton stalk-waste pulp mixed paper sheets.

[0092] Results: The tearing index of cotton stalk-waste pulp mixed paper is 5.48 mN·m 2 / g, the tensile index is 20.27N·m / g, and the ring compression index is 6.61N·m / g.

[0093] Comparative Example 1

[0094] (1) Wash the debranched cotton stalks, cut them into sections of 4 to 6 cm in length, and air-dry them for later use.

[0095] (2) The cotton stalks obtained in step (1) are pre-steamed, the solid-liquid ratio of the pre-steaming is 1:5 g / mL, the steaming temperature is 95° C., and the insulation time is 40 min.

[0096] (3) The cotton stalk obtained in step (2) is immediately subjected to spiral extrusion and thread rolling, and the compression ratio of the spiral extrusion is 1:4.

[0097] (4) The cotton stalks obtained in step (3) are soaked in a buffer solution containing xylanase for xylanase treatment, wherein the xylanase dosage is 40 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH of 6.0, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 50° C., and the treatment time is 60 min.

[0098] (5) The cotton stalk obtained in step (4) is immersed in a hot alkaline solution, wherein the sodium hydroxide concentration is 4%, the solid-liquid ratio is 1:4, the immersion temperature is 95° C., and the time is 40 minutes.

[0099] (6) The cotton stalks obtained in step (5) are subjected to high-concentration grinding at a rotation speed of 3500 rpm, and the gaps between the two stages of grinding are 0.3 mm and 0.15 mm. After grinding, the latent force is removed and the pulp is screened, and then PFI beating is performed to increase the beating degree to 40±2°SR, and sheeting is performed.

[0100] Results: The pulp yield was 78.97% and the tear index of the paper sheet was 5.96 mN·m 2 / g, the tensile index is 30.56N·m / g, and the ring compression index is 10.28N·m / g.

[0101] Comparative Example 2

[0102] (1) Wash the debranched cotton stalks, cut them into 4-6 cm long segments, and air-dry them for later use.

[0103] (2) The cotton stalks obtained in step (1) are pre-steamed, the solid-liquid ratio of the pre-steaming is 1:5 g / mL, the steaming temperature is 95° C., and the insulation time is 40 min.

[0104] (3) The cotton stalk obtained in step (2) is immediately subjected to spiral extrusion and thread rolling, and the compression ratio of the spiral extrusion is 1:4.

[0105] (4) The cotton stalks obtained in step (3) are soaked in a buffer solution containing pectinase for pectinase treatment, wherein the pectinase dosage is 40 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH of 6.0, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 50°C, and the treatment time is 60 min.

[0106] (5) The cotton stalk obtained in step (4) is immersed in a hot alkaline solution, wherein the sodium hydroxide concentration is 4%, the solid-liquid ratio is 1:4 g / mL, the immersion temperature is 95° C., and the time is 40 min.

[0107] (6) The cotton stalks obtained in step (5) are subjected to high-concentration grinding at a rotation speed of 3500 rpm, and the gaps between the two stages of grinding are 0.3 mm and 0.15 mm. After grinding, the latent force is removed and the pulp is screened, and then PFI beating is performed to increase the beating degree to 40±2°SR, and sheeting is performed.

[0108] Results: The pulp yield was 80.45%, and the tear index of the paper sheet was 5.69 mN·m 2 / g, the tensile index is 29.91N·m / g, and the ring compression index is 9.82N·m / g.

[0109] Comparative Example 3

[0110] (1) Wash the debranched cotton stalks, cut them into 4-6 cm long segments, and air-dry them for later use.

[0111] (2) The cotton stalks obtained in step (1) are pre-steamed, the solid-liquid ratio of the pre-steaming is 1:5 g / mL, the steaming temperature is 95° C., and the insulation time is 40 min.

[0112] (3) The cotton stalk obtained in step (2) is immediately subjected to spiral extrusion and thread rolling, and the compression ratio of the spiral extrusion is 1:4.

[0113] (4) The rolled cotton stalk obtained in step (3) is immersed in a buffer solution containing lipase for lipase treatment, wherein the lipase dosage is 40 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH of 6.0, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 50°C, and the treatment time is 60 min.

[0114] (5) The cotton stalk obtained in step (4) is immersed in a hot alkaline solution, wherein the sodium hydroxide concentration is 4%, the solid-liquid ratio is 1:4 g / mL, the immersion temperature is 95° C., and the time is 40 min.

[0115] (6) The cotton stalks obtained in step (5) are subjected to high-concentration grinding at a rotation speed of 3500 rpm, and the gaps between the two stages of grinding are 0.3 mm and 0.15 mm. After grinding, the latent force is removed and the pulp is screened, and then PFI beating is performed to increase the beating degree to 40±2°SR, and sheeting is performed.

[0116] Results: The pulp yield was 80.81% and the tear index of the paper sheet was 5.62 mN·m 2 / g, the tensile index is 29.81N·m / g, and the ring compression index is 9.90N·m / g.

[0117] Comparative Example 4

[0118] (1) Wash the debranched cotton stalks, cut them into 4-6 cm long segments, and air-dry them for later use.

[0119] (2) The cotton stalks obtained in step (1) are pre-steamed, the solid-liquid ratio of the pre-steaming is 1:5 g / mL, the steaming temperature is 95° C., and the insulation time is 40 min.

[0120] (3) The cotton stalk obtained in step (2) is immediately subjected to spiral extrusion and thread rolling, and the compression ratio of the spiral extrusion is 1:4.

[0121] (4) The cotton stalks obtained in step (3) are soaked in a buffer solution, wherein the buffer solution is a citric acid-sodium citrate solution with a pH of 6.0, a solid-liquid ratio of 1:4 g / mL, a treatment temperature of 50° C., and a treatment time of 60 min.

[0122] (5) The cotton stalk obtained in step (4) is immersed in a hot alkaline solution, wherein the sodium hydroxide concentration is 4%, the solid-liquid ratio is 1:4 g / mL, the immersion temperature is 95° C., and the time is 40 min.

[0123] (6) The cotton stalks obtained in step (5) are subjected to high-concentration grinding at a rotation speed of 3000-3500 rpm, and the gaps between the two stages of grinding are 0.3 mm and 0.15 mm. After grinding, the latent force is removed and the pulp is screened, and then PFI beating is performed to increase the beating degree to 40±2°SR, and sheeting is performed.

[0124] Results: The pulp yield was 81.23% and the tear index of the paper sheet was 5.43 mN·m 2 / g, the tensile index is 26.85N·m / g, and the ring compression index is 9.67N·m / g.

[0125] Comparative Example 5

[0126] (1) Wash the debranched cotton stalks, cut them into sections of 4 to 6 cm in length, and air-dry them for later use.

[0127] (2) The cotton stalks obtained in step (1) are pre-steamed, the solid-liquid ratio of the pre-steaming is 1:5 g / mL, the steaming temperature is 95° C., and the insulation time is 40 min.

[0128] (3) The cotton stalk obtained in step (2) is immediately subjected to spiral extrusion and thread rolling, and the compression ratio of the spiral extrusion is 1:4.

[0129] (4) The cotton stalks obtained in step (3) are soaked in a buffer solution containing a complex enzyme composed of xylanase, pectinase and lipase for complex enzyme treatment, wherein the ratio of the complex enzyme (enzyme activity) is xylanase: pectinase: lipase = 2:1:1, the amount of the complex enzyme is 40 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH of 6.0, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 50°C, and the treatment time is 60 min.

[0130] (5) The cotton stalk obtained in step (4) is immersed in a hot alkaline solution, wherein the sodium hydroxide concentration is 4%, the solid-liquid ratio is 1:4 g / mL, the immersion temperature is 95° C., and the time is 40 min.

[0131] (6) The cotton stalks obtained in step (5) are subjected to high-concentration grinding at a rotation speed of 3500 rpm, and the gaps between the two stages of grinding are 0.3 mm and 0.15 mm. After grinding, the latent force is removed and the pulp is screened, and then PFI beating is performed to increase the beating degree to 40±2°SR, and sheeting is performed.

[0132] (7) The biochemical mechanical pulp of cotton stalks in step (6) is mixed with waste paper pulp, the proportion of the biochemical mechanical pulp of cotton stalks is 5%, and the basis weight of the paper sheet is 100 g / m 2 .

[0133] Results: The tear index of the cotton stalk-waste pulp mixed paper sheet was 5.39 mN·m 2 / g, the tensile index is 18.94N·m / g, and the ring compression index is 6.22N·m / g.

[0134] Comparative Example 6

[0135] (1) Wash the debranched cotton stalks, cut them into 4-6 cm long segments, and air-dry them for later use.

[0136] (2) The cotton stalks obtained in step (1) are pre-steamed, the solid-liquid ratio of the pre-steaming is 1:5 g / mL, the steaming temperature is 95° C., and the insulation time is 40 min.

[0137] (3) The cotton stalk obtained in step (2) is immediately subjected to spiral extrusion and thread rolling, and the compression ratio of the spiral extrusion is 1:4.

[0138] (4) The cotton stalks obtained in step (3) are soaked in a buffer solution containing a complex enzyme composed of xylanase, pectinase and lipase for complex enzyme treatment, wherein the ratio of the complex enzyme (enzyme activity) is xylanase: pectinase: lipase = 1:2:1, the amount of the complex enzyme is 40 U / g, the buffer solution is a citric acid-sodium citrate solution with a pH of 6.0, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 50°C, and the treatment time is 60 min.

[0139] (5) The cotton stalk obtained in step (4) is immersed in a hot alkaline solution, wherein the amount of sodium hydroxide is 4%, the solid-liquid ratio is 1:4 g / mL, the immersion temperature is 95° C., and the time is 40 min.

[0140] (6) The cotton stalks obtained in step (5) are subjected to high-consistency grinding at a rotation speed of 3200 rpm, and the gaps between the two stages of grinding are 0.3 mm and 0.15 mm. After grinding, the latent force is removed and the pulp is screened, and then PFI beating is performed to increase the beating degree to 40±2°SR, and sheeting is performed.

[0141] (7) The biochemical mechanical pulp of cotton stalks in step (6) is mixed with waste paper pulp and prepared into paper, wherein the proportion of the biochemical mechanical pulp of cotton stalks is 5%, and the papermaking basis weight is 100 g / m 2 Cotton stalk-waste pulp mixed paper sheets.

[0142] Results: The tear index of the cotton stalk-waste pulp mixed paper sheet was 5.29 mN·m 2 / g, the tensile index is 18.47N·m / g, and the ring compression index is 6.08N·m / g.

[0143] Comparative Example 7

[0144] (1) Wash the debranched cotton stalks, cut them into sections of 4 to 6 cm in length, and air-dry them for later use.

[0145] (2) The cotton stalks obtained in step (1) are pre-steamed, the solid-liquid ratio of the pre-steaming is 1:5 g / mL, the steaming temperature is 95° C., and the insulation time is 40 min.

[0146] (3) The cotton stalk obtained in step (2) is immediately subjected to spiral extrusion and thread rolling, and the compression ratio of the spiral extrusion is 1:4.

[0147] (4) The rolled cotton stalk obtained in step (3) is immersed in a buffer solution containing a complex enzyme composed of xylanase, pectinase and lipase for complex enzyme treatment, wherein the ratio of the complex enzyme (enzyme activity) is xylanase: pectinase: lipase = 1:1:2, the buffer solution is a citric acid-sodium citrate solution with a pH of 6.0, the solid-liquid ratio is 1:4 g / mL, the treatment temperature is 50°C, and the treatment time is 60 min.

[0148] (5) The cotton stalk obtained in step (4) is immersed in a hot alkaline solution, wherein the amount of sodium hydroxide is 4%, the solid-liquid ratio is 1:4 g / mL, the immersion temperature is 95° C., and the time is 40 min.

[0149] (6) The cotton stalks obtained in step (5) are subjected to high-concentration grinding at a rotation speed of 3500 rpm, and the gaps between the two stages of grinding are 0.3 mm and 0.15 mm. After grinding, the latent force is removed and the pulp is screened, and then PFI beating is performed to increase the beating degree to 40±2°SR, and sheeting is performed.

[0150] (7) The biochemical mechanical pulp of cotton stalks in step (6) is mixed with waste paper pulp and prepared into paper, wherein the proportion of the biochemical mechanical pulp of cotton stalks is 5%, and the papermaking basis weight is 100 g / m 2 Cotton stalk-waste pulp mixed paper sheets.

[0151] Results: The tear index of the cotton stalk-waste pulp mixed paper sheet was 5.27 mN·m 2 / g, the tensile index is 18.40N·m / g, and the ring compression index is 6.11N·m / g.

[0152] Comparative Example 8

[0153] The difference from Example 1 is that the ratio (enzyme activity) of the complex enzyme is xylanase: pectinase=2:1, and the rest is the same as Example 1.

[0154] Results: The pulp yield was 79.61%, and the tear index of the paper sheet was 6.03 mN·m 2 / g, the tensile index is 30.48N·m / g, and the ring compression index is 10.21N·m / g.

[0155] Comparative Example 9

[0156] The difference from Example 1 is that the ratio (enzyme activity) of the complex enzyme is xylanase:lipase=2:1, and the rest is the same as Example 1.

[0157] Results: The pulp yield was 79.53% and the tear index of the paper sheet was 5.98 mN·m 2 / g, the tensile index is 30.43N·m / g, and the ring compression index is 10.21N·m / g.

[0158] Comparative Example 10

[0159] The difference from Example 1 is that the ratio of the complex enzyme (enzyme activity) is pectinase:lipase=1:1, and the rest is the same as Example 1.

[0160] Results: The pulp yield was 80.76% and the tear index of the paper sheet was 5.66 mN·m 2 / g, the tensile index is 29.87N·m / g, and the ring compression index is 9.86N·m / g.

[0161] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing biochemical mechanical pulp of cotton stalks treated with a composite enzyme, characterized in that: The method comprises the following steps: pre-treating the cotton stalks, wherein the pre-treating method comprises removing branches, washing, cutting into sections and air-drying the cotton stalks; The pretreated cotton stalks are sequentially subjected to pre-steaming and spiral extrusion and thread rolling; soaking the rolled cotton stalks in a buffer solution of a composite enzyme for composite enzyme treatment, wherein the composite enzyme comprises xylanase, pectinase and lipase; The cotton stalks treated with the compound enzyme are immersed in a hot alkaline solution for a set time, and then high-concentration pulping, latent removal, pulp screening and PFI pulping are carried out in sequence to obtain the cotton stalk biochemical mechanical pulp.

2. The method for preparing biochemical mechanical pulp of cotton stalk treated with complex enzyme according to claim 1, characterized in that: In the complex enzyme, the mass ratio of xylanase, pectinase and lipase is 1-2:1-2:1-2; Preferably, the total enzyme dosage of the complex enzyme is 30-50 U / g; Preferably, in the buffer solution of the complex enzyme, the buffer solution is a citric acid-sodium citrate solution with a pH value of 4.5-6.5; Preferably, the solid-liquid ratio during the composite enzyme treatment is 1:3-10, g / mL; preferably 1:3-8, g / mL; more preferably 1:3-6, g / mL; specifically 1:4, g / mL; Preferably, the temperature of the complex enzyme treatment is 45-65°C and the treatment time is 30-90 min.

3. The method for preparing biochemical mechanical pulp of cotton stalk treated with complex enzyme according to claim 1, characterized in that: The length of the cut cotton stalks is 4-6 cm.

4. The method for preparing biochemical mechanical pulp of cotton stalk treated with complex enzyme according to claim 1, characterized in that: The solid-liquid ratio during pre-steaming is 1:4-8, g / mL; preferably 1:4-6, g / mL; more preferably 1:5, g / mL; Preferably, the pre-steaming temperature is 90-100°C, and the time is 30-50 min; preferably 95°C, 40 min.

5. The method for preparing biochemical mechanical pulp of cotton stalk treated with complex enzyme according to claim 1, characterized in that: The compression ratio of spiral extrusion thread rolling is 1:3-5, preferably 1:

4.

6. The method for preparing biochemical mechanical pulp of cotton stalk treated with complex enzyme according to claim 1, characterized in that: The hot alkali solution is a sodium hydroxide solution, the temperature of the hot alkali solution is 90-100° C., and the mass percentage of the solute in the hot alkali solution is 3-5%; Preferably, the cotton stalks treated with the complex enzyme are immersed in the hot alkaline solution for 30-50 minutes; Preferably, the rotation speed of high-concentration refining is 3000-3500 rpm, and the gaps between the two stages of refining are 0.3 mm and 0.15 mm.

7. The method for preparing biochemical mechanical pulp of cotton stalk treated with complex enzyme according to claim 1, characterized in that: The beating degree of the PFI beating is 40±2°SR.

8. A biochemical mechanical pulp of cotton stalks treated with a composite enzyme, characterized in that: Prepared by the preparation method described in any one of claims 1 to 7.

9. Use of the biochemical mechanical pulp of cotton stalk treated with the composite enzyme according to claim 8 in paper making of waste paper pulp.

10. The use according to claim 9, characterized in that: The proportion of the cotton stalk biochemical mechanical pulp in the paper making process is 5%-50%, where % is the mass percentage; Preferably, the basis weight of the paper is 80-120 g / m 2 , preferably 100g / m 2 .

Citation Information

Patent Citations

  • Crop straw biological pulping method

    CN109667181A

  • Method for improving drainability of cotton stalk chemi-mechanical pulp

    CN118147937A

Cited By

  • Compound enzyme-treated cotton stalk biochemical mechanical pulp, and preparation method therefor and use thereof