Bonding type steel belt reinforced plastic pipe and production process thereof

By wrapping the steel belt reinforcement layer outside the core tube of the plastic pipe and forming a void, combining the rubber layer and the core tube to form an overall structure, the problem of poor stability of the existing plastic pipe structure is solved, and the pressure resistance and ring stiffness are improved, so as to avoid The core tube collapsed.

CN119022140APending Publication Date: 2024-11-26SICHUAN GOLDSTONE ORIENT NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411191577.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The core tube structure of existing reinforced thermoplastic pipes has poor integrity and structural stability, and is prone to water hammer/vacuum phenomenon, especially under negative pressure conditions, which may cause core tube collapse.

Method used

Designed with bonded steel belt reinforced plastic pipe, by wrapping the steel belt reinforced layer on the outside of the plastic core pipe and forming multiple voids. The adhesive layer passes through the void and combines with the core pipe to form a "rivet-type" overall structure, and the plastic is coated on the outside. Protective layer to improve pressure resistance and ring stiffness.

Benefits of technology

The pressure resistance, ring stiffness and structural stability of the plastic pipe are significantly improved, the core pipe collapse is avoided, and the outer peripheral surface of the pipe after production is relatively flush.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119022140A_ABST
    Figure CN119022140A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of composite pipelines, and discloses a bonding type steel belt reinforced plastic pipe and a production process thereof. The steel belt winding reinforcing layer is spirally wound on the outer peripheral surface of the plastic core pipe, and a plurality of gaps are formed in the steel belt winding reinforcing layer; the rubber layer is coated on the peripheral surface of the steel belt winding enhancement layer, and at least part of the rubber layer penetrates through the gap and is combined with the plastic core pipe into a whole; and the protective layer is coated on the peripheral surface of the adhesive layer and is combined with the adhesive layer into a whole. According to the technical scheme, the steel belt winding reinforcing layer with the gaps is arranged on the outer side of the plastic core pipe, so that at least part of the adhesive layer arranged on the outer side of the reinforcing layer can penetrate through the gaps, and the plastic core pipe, the steel belt winding reinforcing layer, the adhesive layer and the protective layer are combined into a whole; therefore, the integral structure is formed, and the pressure resistance, the ring stiffness and the structural integrity of the plastic pipe are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of composite pipes, and in particular to a bonding type steel strip reinforced plastic pipe. Based on this, the present invention also relates to a production process of a bonding type steel strip reinforced plastic pipe. Background Art

[0002] With the development of plastic pipe technology, reinforced thermoplastic pipe (RTP) has been widely used in mining and mineral processing, oil and gas transmission and distribution, municipal water supply and other fields in recent years. Reinforced thermoplastic pipe generally includes an inner pipe, a reinforcing layer coated on the inner pipe and a protective layer coated on the reinforcing layer. The reinforcing layer plays a role in reinforcing the pipe, and the protective layer plays a role in protecting the pipe.

[0003] At present, reinforced thermoplastic plastic pipes are usually made by first extruding a pure plastic core pipe, and after the core pipe is cooled and formed, a reinforcing material is wrapped around the core pipe to form a reinforcing layer to reinforce the pipe, and finally a composite plastic layer is added outside the reinforcing layer as a protective layer to protect the pipe. However, the existing plastic pipes are stacked layer by layer, and the integrity and structural stability are poor. At the same time, the core pipe is prone to water hammer / vacuum phenomenon when conveying liquids. In particular, when negative pressure is formed in the core pipe, the core pipe may collapse. Summary of the invention

[0004] The purpose of the present invention is to overcome the technical problem of poor core tube structure integrity of plastic pipes in the prior art, and to provide a bonded steel belt reinforced plastic pipe and its production process, wherein the plastic pipe has strong structural stability, high ring stiffness and high pressure resistance.

[0005] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a bonded steel-reinforced plastic pipe, comprising: a plastic core pipe; a steel-wrap reinforcement layer, the steel-wrap reinforcement layer is spirally wound on the outer circumference of the plastic core pipe and has a plurality of gaps; an adhesive layer, the adhesive layer is coated on the outer circumference of the steel-wrap reinforcement layer, the adhesive layer at least partially passes through the gaps and is integrated with the plastic core pipe; and a plastic protective layer, the plastic protective layer is coated on the outer circumference of the adhesive layer and is integrated with the adhesive layer.

[0006] Through the above technical solution, a steel belt winding reinforcement layer with multiple gaps is arranged on the outside of the plastic core tube, so that the rubber layer arranged on the outside of the steel belt winding reinforcement layer can at least partially pass through the gap and be combined with the plastic core tube as a whole, thereby forming a "rivet-type" overall structure, so that the plastic core tube, the steel belt winding reinforcement layer, the rubber layer and the protective layer are combined into one, thereby forming an overall structure, thereby improving the pressure resistance, ring stiffness and structural stability of the plastic tube.

[0007] Optionally, the steel strip winding reinforcement layer includes a first steel strip wound at intervals along a first spiral direction on the outer circumferential surface of the core tube.

[0008] Optionally, the steel strip winding reinforcement layer further includes a second steel strip wound at intervals on the outer circumferential surface of the first steel strip along a second spiral direction opposite to the first spiral direction to form a plurality of the gaps.

[0009] Optionally, the thickness of the first steel strip and the second steel strip is 0.15 mm-2.5 mm.

[0010] Optionally, the bonded steel-strip reinforced plastic pipe provided by the present invention further includes a plurality of holes formed on the first steel strip and the second steel strip.

[0011] Optionally, the bonded steel-strip reinforced plastic pipe provided by the present invention further includes a plurality of notches formed on both sides of the first steel strip and the second steel strip extending along the length direction.

[0012] Optionally, the inner and outer surfaces of the first steel strip and the second steel strip of the bonded steel strip reinforced plastic pipe provided by the present invention are coated with glue.

[0013] Optionally, the gap is in the shape of a parallelogram.

[0014] Optionally, the gap has an axial width of 1.5 mm to 30 mm along the plastic core tube.

[0015] Optionally, there are multiple steel belt winding reinforcement layers and rubber layers, which are alternately stacked with each other, so that the rubber layer on the radially outer side of the steel belt winding reinforcement layer passes through the gap and is combined with the plastic core tube or the rubber layer on the radially inner side of the steel belt winding reinforcement layer.

[0016] Optionally, the plastic core tube, the adhesive layer and the plastic protective layer are made of the same material.

[0017] A second aspect of the present invention provides a production process for a bonded steel strip reinforced plastic pipe, comprising the following steps:

[0018] S1, preparing a plastic core tube;

[0019] S2, winding a steel belt around the outer circumference of the plastic core tube to form a plurality of gaps;

[0020] S3, coating the outer peripheral surface of the steel strip winding reinforcement layer with a rubber layer, so that the rubber layer passes through the gap and is integrated with the plastic core tube;

[0021] S4, coating the outer peripheral surface of the adhesive layer with a plastic protective layer.

[0022] Optionally, the steel strip winding reinforcement layer includes a first steel strip and a second steel strip, and the following steps are performed before performing step S2:

[0023] Glue is applied on the inner surface and the outer surface of the first steel strip and the second steel strip.

[0024] Optionally, step S2 includes the following sub-steps:

[0025] S21, heating the outer circumferential surface of the plastic core tube and the inner circumferential surface of the first steel strip;

[0026] S22, winding the first steel belt at intervals on the outer peripheral surface of the plastic core tube along a first spiral direction;

[0027] S23, heating the outer circumferential surface of the first steel strip and the inner circumferential surface of the second steel strip;

[0028] S24, winding the second steel belt at intervals on the outer circumferential surface of the first steel belt along a second spiral direction opposite to the first spiral direction to form a plurality of gaps.

[0029] Optionally, step S3 includes the following sub-steps:

[0030] S31, heating the outer peripheral surface of the steel strip winding reinforcement layer;

[0031] S32, coating the adhesive layer on the outer peripheral surface of the steel strip winding reinforcement layer by using an adhesive film device;

[0032] S33, after at least a portion of the adhesive layer passes through the gap and is integrated with the plastic core tube, the adhesive layer is cooled. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is an isometric view of the bonded steel strip reinforced plastic pipe disclosed in the present invention;

[0034] Figure 2 yes Figure 1 The main view;

[0035] Figure 3 It is a bonded steel-reinforced plastic pipe with a steel-wound reinforcement layer and an adhesive layer. Figure 2 Sectional view in the AA direction;

[0036] Figure 4 It is a bonded steel-reinforced plastic pipe with multiple steel-wound reinforcement layers and adhesive layers. Figure 2 Sectional view in the AA direction;

[0037] Figure 5-Figure 8 is a schematic diagram of the first steel strip and the second steel strip having holes formed with different shapes and distributions;

[0038] Fig. 9 is a schematic diagram of a structure in which the first steel strip and the second steel strip have only notches;

[0039] Fig.10 It is a schematic diagram of the structure in which the first steel belt and the second steel belt have holes and notches.

[0040] Description of Reference Numerals

[0041] 1- plastic core tube; 201- first steel belt; 202- second steel belt; 203- gap; 3- adhesive layer; 4- plastic protective layer; 5- hole; 6- notch. DETAILED DESCRIPTION

[0042] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0043] In the present invention, unless otherwise specified, the directions or positional relationships indicated by terms such as "up, down, left, right, inside, outside, top, bottom" etc. are based on the directions or positional relationships shown in the accompanying drawings and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore should not be understood as a limitation on the present invention.

[0044] In addition, the terms "first", "second", etc. are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0045] In the present invention, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0046] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection, an electrical connection, or communication with each other; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0047] Aiming at the technical problem that the existing reinforced thermoplastic plastic pipe has poor structural stability and integrity, the present invention provides a bonded steel strip reinforced plastic pipe and a production process thereof.

[0048] The first aspect of the present invention provides a bonded steel-reinforced plastic pipe, referring to Figure 1-Figure 4 As shown, the bonded steel-reinforced plastic pipe comprises: a plastic core pipe 1, a steel-reinforced layer 2 spirally wound on the outer circumference of the plastic core pipe 1, a rubber layer 3 coated on the outer circumference of the steel-reinforced layer 2, and a plastic protective layer coated on the outer circumference of the rubber layer 3, wherein the plastic core pipe 1 is provided with a steel-reinforced plastic pipe having a plurality of steel strips and a plurality of steel strips. Figure 3 and Figure 4 As shown, a plurality of gaps 203 are formed on the steel strip winding reinforcement layer 2, so that the adhesive layer 3 at least partially passes through the gaps 203 and is integrated with the plastic core tube 1 located inside the steel strip winding reinforcement layer 2, for example, the adhesive layer 3 at least partially passes through the gaps 203 and is bonded or welded to the plastic core tube 1 as a whole. The outer peripheral surface of the adhesive layer 3 is coated with a plastic protective layer 4, which is arranged on the outermost layer of the pipe material to protect the internal structure of the pipe material, and the plastic protective layer 4 is integrated with the adhesive layer 3, for example, the plastic protective layer 4 is bonded or welded to the adhesive layer 3 as a whole.

[0049] In the prior art, a reinforced thermoplastic plastic pipe generally includes a core pipe, a reinforcement layer and a protective layer. The core pipe and the protective layer are generally composite plastics, and the reinforcement layer is generally a steel fiber tape, steel wire, glass fiber tape, etc. During production, the core pipe, the reinforcement layer and the protective layer are directly stacked and coated in sequence, so that the core pipe, the reinforcement layer and the protective layer are arranged in layers, and the reinforcement layer is directly in contact with the outer peripheral surface of the core pipe and the inner peripheral surface of the protective layer, so that the bonding strength is limited; at the same time, the reinforcement layer, the core pipe and the protective layer are made of different materials, which further reduces the bonding strength between the reinforcement layer and the core pipe and the protective layer, thereby making the integrity and structural stability of the plastic pipe poor. In particular, when the plastic pipe produces water hammer phenomenon when conveying fluid, negative pressure is generated in the plastic pipe. Since the core pipe and the reinforcement layer are arranged in layers and the bonding strength between the two is limited, the reinforcement layer cannot provide the core pipe with negative pressure resistance, causing the core pipe to collapse easily. However, with the bonded steel-strip reinforced plastic pipe provided by the present invention, a steel-strip winding reinforcement layer 2 having a plurality of gaps 203 is arranged on the outside of the plastic core pipe 1, so that the rubber layer 3 arranged on the outside of the steel-strip winding reinforcement layer 2 can at least partially pass through the gaps 203 and be integrated with the plastic core pipe 1 to form a "rivet-type" overall structure. At the same time, the rubber layer 3 is integrated with the plastic protective layer 4 on its outside, so that the plastic core pipe 1, the steel-strip winding reinforcement layer 2, the rubber layer 3 and the plastic protective layer 4 are integrated to form an overall structure, thereby improving the pressure resistance, ring stiffness and structural stability of the plastic pipe. In addition, the rubber layer 3 is also a kind of plastic, so that the bonding strength between the rubber layer 3 and the plastic core pipe 1 and the plastic protective layer 4 is higher, thereby further improving the pressure resistance, ring stiffness and structural stability of the plastic pipe. Moreover, the gaps formed by the steel-strip winding reinforcement layer 2 can be filled by the rubber layer 3, so that the outer peripheral surface of the produced bonded steel-strip reinforced plastic pipe is relatively flat.

[0050] According to one embodiment of the bonded steel belt reinforced plastic pipe of the present invention, the steel belt winding reinforcement layer 2 includes a first steel belt 201 wound at intervals along a first spiral direction on the outer peripheral surface of the plastic core tube 1, so that the first steel belt 201 forms a gap when it is wound on the outer peripheral surface of the plastic core tube 1, so that the adhesive layer 3 can at least partially pass through the gap and be combined with the plastic core tube 1 on the inner side of the first steel belt 201, thereby improving the structural integrity of the plastic pipe.

[0051] Further, according to another embodiment of the bonded steel strip reinforced plastic pipe of the present invention, referring to Figure 1-Figure 4 As shown, the steel belt winding reinforcement layer 2 includes a first steel belt 201 wound at intervals on the outer circumference of the plastic core tube 1 along a first spiral direction and a second steel belt 202 wound at intervals on the outer circumference of the first steel belt 201 along a second spiral direction opposite to the first spiral direction to form a plurality of gaps 203. Figure 1 and Figure 2As shown, the first steel belt 201 is wound on the outer circumference of the plastic core tube 1 at intervals along a first spiral direction to form a plurality of gaps, and the second steel belt 202 is wound on the outer circumference of the first steel belt 201 at intervals along a second spiral direction opposite to the first spiral direction to cover part of the gaps, and the remaining part of the gaps forms a void 203.

[0052] Optionally, the thickness of the first steel strip 201 and the second steel strip 202 is 0.15-2.5 mm, so as to ensure the structural stability and integrity of the formed plastic tube. Specifically, the first steel strip 201 and the second steel strip 202 are rectangular strips, the thickness of the steel strip is 0.15-2.5 mm, and the width of the steel strip is less than the spiral lead of the spirally wound steel strip, so that when the steel strip is wound, a plurality of gaps 203 can be formed on the outer peripheral surface of the inner layer, so that at least part of the rubber layer 3 can pass through the gaps and be combined with the plastic core tube 1 as a whole.

[0053] Optionally, refer to Figure 5-Figure 9 As shown, the bonded steel-strip reinforced plastic pipe provided by the present invention further includes a plurality of holes 5 formed on the first steel strip 201 and the second steel strip 202. As mentioned above, the first steel strip 201 forms a plurality of gaps on the outer peripheral surface of the plastic core tube 1, and the second steel strip 202 covers part of the gaps, and the remaining part of the gaps forms a plurality of gaps 203, and the plurality of holes 5 of the first steel strip 201 and the second steel strip 202 can form a plurality of additional gaps 203 outside the above-mentioned gaps, that is, on the first steel strip 201 and the second steel strip 202 body, thereby increasing the number and distribution position of the gaps 203, and the adhesive layer 3 can at least partially pass through more gaps to "rivet" the first steel strip 201 and the second steel strip 202 and combine with the plastic core tube 1 as a whole, further improving the structural integrity of the plastic pipe.

[0054] Optionally, the shape of the hole 5 can be any shape, such as a triangle, a circle, etc. Figure 5-Figure 9 As shown, the shape of the hole 5 is a rectangle or a long strip with arcs at both ends. Of course, the arrangement of the holes 5 on the first steel strip 201 and the second steel strip 202 can also be arbitrary, or in one embodiment of the present invention, the holes 5 are arranged in an array on the first steel strip 201 and the second steel strip 202, for example, referring to Figure 5-Figure 9 As shown, along the length direction of the first steel strip 201 and the second steel strip 202 (i.e. Figure 5-Figure 9 The horizontal direction in the middle) and the width direction of the first steel strip 201 and the second steel strip 202 (i.e. Figure 5-Figure 9 A plurality of holes 5 are arranged in the vertical direction of the hole 2 to form a hole array of multiple rows and columns, such as Figure 5 As shown, the hole 5 is rectangular, the length direction of the hole 5 is the same as the length direction of the first steel strip 201 and the second steel strip 202, and the holes 5 in any two adjacent rows and / or any two adjacent columns are aligned; Figure 6As shown, the holes 5 are long strips with arc-shaped ends, and the length direction of the long strips is the same as the length direction of the first steel strip 201 and the second steel strip 202. The holes 5 in any two adjacent rows and / or any two adjacent columns are arranged alternately; Figure 7 As shown, the hole 5 is a long strip with arc-shaped ends, and the length direction of the long strip is inclined to the length direction of the first steel strip 201 and the second steel strip 202, and the holes 5 of any two adjacent rows and / or any two adjacent columns are aligned; Figure 8 As shown, the holes 5 are long strips with arc-shaped ends. The length direction of the long strip is inclined to the length direction of the first steel strip 201 and the second steel strip 202. The holes 5 in any two adjacent rows and / or any two adjacent columns are arranged alternately.

[0055] Optionally, refer to Fig. 9 and Fig.10 As shown, the bonded steel strip reinforced plastic pipe provided by the present invention further includes a plurality of notches 6 formed on both sides of the first steel strip 201 and the second steel strip 202 extending along the length direction. Fig. 9 As shown, a plurality of notches 6 are formed on both sides of the first steel strip 201 and the second steel strip 202 extending in the length direction, so that after the first steel strip 201 and the second steel strip 202 are wound, a plurality of gaps 203 can be formed, thereby increasing the number and distribution of the gaps 203, and further improving the structural integrity of the plastic pipe. In addition, the formation of a plurality of notches 6 on both sides of the first steel strip 201 and the second steel strip 202 extending in the length direction can facilitate the winding of the bonded steel strip reinforced plastic pipe formed in the end, especially for small-diameter plastic pipes, such as plastic pipes with a diameter of 4 inches or less. Further, as Fig.10 As shown, a plurality of notches 6 are formed on both sides of the first steel strip 201 and the second steel strip 202 extending along the length direction. On this basis, the aforementioned holes 5 are also formed on the first steel strip 201 and the second steel strip 202 to further increase the number and distribution position of the gaps 203 and improve the structural integrity of the plastic pipe.

[0056] Optionally, the inner and outer surfaces of the first steel belt 201 and the second steel belt 202 are coated with glue, which can improve the bonding strength between the first steel belt 201 and the second steel belt 202, the first steel belt 201 and the outer peripheral surface of the plastic core tube 1, and the second steel belt 202 and the glue layer 3, thereby improving the integrity and structural stability of the bonded steel belt reinforced plastic tube of the present invention.

[0057] Optionally, the shape of the gap 203 can be any shape, as long as the adhesive layer 3 at least partially passes through the gap 203 and is integrated with the plastic core tube 1. Figure 1 and Figure 2As shown, the shape of the gap 203 is a parallelogram. Further, when the first steel strip 201 is wound on the outer circumference of the plastic core tube 1 at intervals along the first spiral direction to form a gap, the second steel strip 202 is wound on the radial outer side of the first steel strip 201 at the same intervals along the second spiral direction, and the gap 203 is a rhombus.

[0058] Optionally, the axial width of the gap 203 along the plastic core tube 1 is 1.5 mm to 30 mm. Figure 1 and Figure 2 As shown, the diagonal length of the parallelogram formed by the gap 203 along the axial direction of the plastic core tube 1 is 1.5 mm-30 mm, so as to ensure that the gap 203 has enough space so that the glue layer 3 can pass through the gap 203 and be integrated with the plastic core tube 1.

[0059] Optionally, the adhesive layer 3 can substantially fill the gap created by the second steel belt and the void 203 created by the steel belt wrapped around the reinforcing layer 2, so that the outer peripheral surface of the bonded steel belt reinforced plastic pipe of the present invention can be kept flush.

[0060] Alternatively, if Figure 3 As shown, the bonded steel-reinforced plastic pipe of the present invention comprises a steel-wound reinforcement layer 2 and a glue layer 3. The steel-wound reinforcement layer 2 has a plurality of gaps 203. The glue layer 3 passes through the gaps 203 and is integrated with the plastic core pipe 1. Alternatively, in one embodiment of the present invention, referring to Figure 4 As shown, the number of steel strip winding reinforcement layers 2 and adhesive layers 3 is multiple, and the multiple steel strip winding reinforcement layers 2 and adhesive layers 3 are alternately stacked with each other, so that steel strip winding reinforcement layers 2 are respectively arranged at different radial positions between the plastic core tube 1 and the plastic protective layer 4 of the bonded steel strip reinforced plastic pipe of the present invention, and the radial outer side of each steel strip winding reinforcement layer 2 is provided with an adhesive layer 3, so that the adhesive layer 3 on the radial outer side of the steel strip winding reinforcement layer 2 at least partially passes through the gap 203 and is combined with the plastic core tube 1 or the adhesive layer 3 on the radial inner side of the steel strip winding reinforcement layer 2. The gaps 203 at different radial positions of the bonded steel strip reinforced plastic pipe can be completely overlapped, partially overlapped, or staggered.

[0061] Optionally, the plastic core tube 1, the rubber layer 3 and the plastic protective layer 4 are made of the same material, for example, the plastic core tube 1, the rubber layer 3 and the plastic protective layer 4 are all made of high-density polyethylene (HDPE), so that the plastic core tube 1 and the rubber layer 3, as well as the rubber layer 3 and the plastic protective layer 4, are welded after heating, and after cooling, the integrity and structural stability of the adhesive steel belt reinforced plastic tube of the present invention are also improved.

[0062] A second aspect of the present invention provides a production process for a bonded steel strip reinforced plastic pipe, comprising the following steps:

[0063] S1, preparing a plastic core tube 1;

[0064] S2, winding the steel belt winding reinforcement layer 2 on the outer circumference of the plastic core tube 1, and forming a plurality of gaps 203;

[0065] S3, coating the outer peripheral surface of the steel belt winding reinforcement layer 2 with a rubber layer 3, so that the rubber layer 3 passes through the gap 203 and is integrated with the plastic core tube 1;

[0066] S4, coating the outer peripheral surface of the adhesive layer 3 with a plastic protective layer 4.

[0067] Through the above technical solution, a steel strip winding reinforcement layer 2 having a plurality of gaps 203 is spirally wound on the outer side of the plastic core tube 1, so that the rubber layer 3 arranged on the outer side of the steel strip winding reinforcement layer 2 can at least partially pass through the gaps 203 and be integrated with the plastic core tube 1, thereby forming a "rivet-type" overall structure. At the same time, the rubber layer 3 is integrated with the plastic protective layer 4 on its outer side, so that the plastic core tube 1, the steel strip winding reinforcement layer 2, the rubber layer 3 and the plastic protective layer 4 are integrated to form an overall structure, thereby improving the pressure resistance, ring stiffness and structural stability of the plastic pipe. In addition, the gaps formed by the steel strip winding reinforcement layer 2 can be filled by the rubber layer 3, so that the outer peripheral surface of the produced bonded steel strip reinforced plastic pipe is relatively flat.

[0068] Optionally, the steel strip winding reinforcement layer 2 includes a first steel strip 201 and a second steel strip 202. The following steps are performed before performing step S2:

[0069] Glue is coated on the inner and outer surfaces of the first steel strip 201 and the second steel strip 202 .

[0070] According to an embodiment of the production process of the bonded steel strip reinforced plastic pipe of the present invention, step S2 includes the following sub-steps:

[0071] S21, heating the outer circumference of the plastic core tube 1 and the inner circumference of the first steel belt 201;

[0072] S22, winding the first steel belt 201 at intervals on the outer peripheral surface of the plastic core tube 1 along the first spiral direction;

[0073] S23, heating the outer circumference of the first steel strip 201 and the inner circumference of the second steel strip 202;

[0074] S24, winding the second steel belt 202 at intervals on the outer circumference of the first steel belt 201 along a second spiral direction opposite to the first spiral direction to form a plurality of gaps 203.

[0075] In this way, the bonding strength between the first steel strip 201 and the outer circumference of the plastic core tube 1, the first steel strip 201 and the second steel strip 202, and the second steel strip 202 and the adhesive layer 3 can be improved, thereby improving the integrity and structural stability of the adhesive steel strip reinforced plastic tube of the present invention.

[0076] Optionally, step S3 includes the following sub-steps:

[0077] S31, heating the outer peripheral surface of the steel belt wrapped around the reinforcement layer 2;

[0078] S32, using a film device to coat the outer peripheral surface of the steel strip winding reinforcement layer 2 with a rubber layer 3;

[0079] S33, after the glue layer 3 at least partially passes through the gap 203 and is integrated with the plastic core tube 1, the glue layer 3 is cooled.

[0080] The basic production process of the bonded steel strip reinforced plastic pipe provided by the present invention is described in detail below: the plastic core pipe 1 is extruded by an extruder, and after the plastic core pipe 1 is sized and cooled to form, the plastic core pipe 1 is pulled by a traction machine to move the plastic core pipe 1 to the winding machine, and the winding operation of the steel strip winding reinforcement layer 2 is prepared. The outer peripheral surface of the plastic core pipe 1 is first heated, and then the first steel strip 201 coated with glue is heated before winding and contacting the plastic core pipe 1, and then the first steel strip 201 is wound on the outer peripheral surface of the plastic core pipe 1 along the first spiral direction at intervals, and the outer peripheral surface of the wound first steel strip 201 and the second steel strip 202 coated with glue are heated before winding and contacting the wound first steel strip, and then the second steel strip 202 is wound on the radial outer side of the first steel strip 201 along the second spiral direction opposite to the first spiral direction, and a plurality of gaps 203 are formed. The plastic core tube 1 wrapped with the first steel strip 201 and the second steel strip 202 is transported to the adhesive film equipment, and the adhesive is extruded by the extruder and compounded on the radial outer side of the second steel strip 202 to form an adhesive layer 3, so that the adhesive layer 3 at least partially passes through the above-mentioned gap 203 and is combined with the plastic core tube 1 as a whole, and wait for the adhesive layer 3 to cool and set. If it is necessary to arrange multiple steel strip winding reinforcement layers 2 and adhesive layers 3, the steel strip winding reinforcement layer 2 is continued to be wound on the outer peripheral surface of the adhesive layer 3 after cooling and setting, and a new adhesive layer 3 is set. After the steel strip winding reinforcement layer 2 and the adhesive layer 3 are set, the plastic core tube 1 provided with the steel strip winding reinforcement layer 2 and the adhesive layer 3 is transported to the protective layer plastic mold, and the extruder extrude the protective layer plastic and cover it on the outer peripheral surface of the adhesive layer 3 to form a plastic protective layer 4, and wait for the plastic protective layer 4 to cool and form, forming the bonded steel strip reinforced plastic tube of the present invention. Finally, the bonded steel strip reinforced plastic tube is pulled to the cutting machine by a traction machine, cut into a predetermined length and stacked.

[0081] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various specific technical features in any appropriate manner. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations. However, these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A bonded steel-reinforced plastic pipe, characterized in that: include: Plastic core tube (1); A steel belt winding reinforcement layer (2), wherein the steel belt winding reinforcement layer (2) is spirally wound on the outer peripheral surface of the plastic core tube (1) and forms a plurality of gaps (203); an adhesive layer (3), the adhesive layer (3) being coated on the outer peripheral surface of the steel strip winding reinforcement layer (2), the adhesive layer (3) at least partially passing through the gap (203) and being integrated with the plastic core tube (1); and A plastic protective layer (4), wherein the plastic protective layer (4) is coated on the outer peripheral surface of the adhesive layer (3) and is integrated with the adhesive layer (3).

2. The bonded steel-reinforced plastic pipe according to claim 1, characterized in that: The steel belt winding reinforcement layer (2) comprises a first steel belt (201) wound at intervals along a first spiral direction on the outer peripheral surface of the plastic core tube (1).

3. The bonded steel-reinforced plastic pipe according to claim 2, characterized in that: The steel strip winding reinforcement layer (2) further comprises a second steel strip (202) wound at intervals on the outer peripheral surface of the first steel strip (201) along a second spiral direction opposite to the first spiral direction and forming a plurality of gaps (203).

4. The bonded steel-reinforced plastic pipe according to claim 3, characterized in that: The thickness of the first steel strip (201) and the second steel strip (202) is 0.15 mm-2.5 mm.

5. The bonded steel-reinforced plastic pipe according to claim 3, characterized in that: It also includes a plurality of holes (5) formed on the first steel belt (201) and the second steel belt (202).

6. The bonded steel-reinforced plastic pipe according to claim 3, characterized in that: It also includes a plurality of notches (6) formed on both sides of the first steel strip (201) and the second steel strip (202) extending along the length direction.

7. The bonded steel-reinforced plastic pipe according to claim 3, characterized in that: The inner and outer surfaces of the first steel strip (201) and the second steel strip (202) are coated with glue.

8. The bonded steel-reinforced plastic pipe according to claim 3, characterized in that: The shape of the gap (203) is a parallelogram.

9. The bonded steel-reinforced plastic pipe according to claim 7, characterized in that: The axial width of the gap (203) along the plastic core tube (1) is 1.5 mm to 30 mm.

10. The bonded steel-reinforced plastic pipe according to claim 1, characterized in that: The steel strip winding reinforcement layer (2) and the adhesive layer (3) are multiple in number and are alternately stacked on each other, so that the adhesive layer (3) on the radially outer side of the steel strip winding reinforcement layer (2) passes through the gap (203) and is integrated with the plastic core tube (1) or the adhesive layer (3) on the radially inner side of the steel strip winding reinforcement layer (2).

11. The bonded steel-reinforced plastic pipe according to any one of claims 1 to 10, characterized in that: The plastic core tube (1), the adhesive layer (3) and the plastic protective layer (4) are made of the same material.

12. A production process for a bonded steel-reinforced plastic pipe, characterized in that: The following steps are involved: S1, preparing a plastic core tube (1); S2, winding a steel belt winding reinforcement layer (2) on the outer circumference of the plastic core tube (1) to form a plurality of gaps (203); S3, coating the outer peripheral surface of the steel strip winding reinforcement layer (2) with a rubber layer (3), so that the rubber layer (3) passes through the gap (203) and is integrated with the plastic core tube (1); S4, coating the outer peripheral surface of the adhesive layer (3) with a plastic protective layer (4).

13. The production process of the bonded steel-strengthened plastic pipe according to claim 12, characterized in that: The steel strip winding reinforcement layer (2) comprises a first steel strip (201) and a second steel strip (202). Before executing step S2, the following steps are first performed: Glue is coated on the inner surface and the outer surface of the first steel strip (201) and the second steel strip (202).

14. The production process of the bonded steel-strip reinforced plastic pipe according to claim 13, characterized in that: Step S2 includes the following sub-steps: S21, heating the outer circumferential surface of the plastic core tube (1) and the inner circumferential surface of the first steel strip (201); S22, winding the first steel belt (201) at intervals on the outer peripheral surface of the plastic core tube (1) along a first spiral direction; S23, heating the outer circumference of the first steel strip (201) and the inner circumference of the second steel strip (202); S24, winding the second steel belt (202) at intervals on the outer circumference of the first steel belt (201) along a second spiral direction opposite to the first spiral direction to form a plurality of gaps (203).

15. The production process of the bonded steel-reinforced plastic pipe according to claim 12, characterized in that: Step S3 includes the following sub-steps: S31, heating the outer peripheral surface of the steel strip winding reinforcement layer (2); S32, using a film device to coat the adhesive layer (3) on the outer peripheral surface of the steel strip winding reinforcement layer (2); S33, after at least a portion of the adhesive layer (3) passes through the gap (203) and is integrated with the plastic core tube (1), the adhesive layer (3) is cooled.