Visible light excited room temperature acetic acid gas sensor as well as preparation method and application thereof

By coating Bi2WO6 crystal surface heterojunction on the Al2O3 substrate of the precious metal Pt interdigit electrode, the high-efficiency detection of acetic acid gas at room temperature is achieved by using visible light excitation, solving the problems of high-temperature detection safety risks and high cost in the prior art, and improving the Sensitivity and selectivity of sensors.

CN119023627APending Publication Date: 2024-11-26JIANGXI NORMAL UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410962330.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-18
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing resistive gas sensors require high temperatures when detecting acetic acid gas, which poses safety risks and is cost-effective, and ultraviolet excitation limits the performance of the sensor and the efficiency of sunlight utilization.

Method used

Bi2WO6 crystal surface heterojunction is used as the sensitive layer, and the Bi2WO6 crystal surface heterojunction with nanosheet morphology is prepared by solvent-assisted solid phase reaction method, and coated it on the Al2O3 substrate of the noble metal Pt interdigital electrode, using visible light Excite the high selective detection of room temperature.

Benefits of technology

It realizes efficient detection of acetic acid gas at room temperature, reduces equipment power consumption and cost, and improves sensor sensitivity and selectivity, avoiding the safety risks brought by high temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119023627A_ABST
    Figure CN119023627A_ABST
Patent Text Reader

Abstract

The invention discloses a visible-light-excited room-temperature acetic acid gas sensor and a preparation method and application thereof, and relates to the field of preparation and application of gas sensors, the visible-light-excited room-temperature acetic acid gas sensor comprises a substrate and a Bi2WO6 crystal face heterojunction sensitive layer grown on the surface of the substrate, and the Bi2WO6 crystal face heterojunction is in nanosheet morphology. The preparation method comprises the following steps: preparing a Bi2WO6 crystal face heterojunction by adopting a solvent-assisted solid-phase reaction method; then coating the Bi2WO6 crystal face heterojunction serving as a sensitive layer on an Al2O3 substrate with a noble metal Pt interdigital electrode by adopting a thick film process; the sensor can be used for performing room-temperature high-selectivity detection on acetic acid under the excitation of a low-power-consumption visible light LED. The acetic acid gas sensor has the beneficial effects that the Bi2WO6 crystal face heterojunction in the acetic acid gas sensor has rich oxygen adsorption active sites and efficient space photon-generated carrier separation efficiency, and room-temperature high-selectivity detection of acetic acid gas is realized under the excitation of visible light.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation and application of gas sensors, and in particular to a visible light excited room temperature acetic acid gas sensor and a preparation method and application thereof. Background Art

[0002] Recently, the rapid development of the Internet of Things has led to significant advances in gas sensors. They are widely used in emerging fields such as smart homes, wearable devices, and smart mobile terminals. Therefore, the demand for gas sensors has increased dramatically. Resistive gas sensors based on semiconductor materials have the advantages of simple structure, low cost, ease of use, and easy integration, and are currently the most commonly used type of gas sensors. However, due to the inherent properties of metal oxide gas sensing materials, current resistive gas sensors often need to operate at high temperatures (between 200 and 400°C). This makes it challenging to use sensors in flammable and explosive environments, in addition to significantly increasing the complexity and power consumption of the equipment.

[0003] Researchers have found that photoexcitation can significantly enhance the sensing capabilities of resistive gas sensors. This approach is particularly effective in reducing the operating temperature of the device and can even perform gas detection at room temperature. Photoexcitation essentially improves the sensitivity of semiconductor materials by enhancing surface active centers mainly through photogenerated charges. However, the extremely high recombination rate of photogenerated charges limits their effective participation in gas sensing reactions, thus posing a major obstacle to further improving the performance of sensors under photoexcitation. Building gas sensing materials into semiconductor heterojunctions is widely used to solve the problem of high recombination rates of photogenerated charges. However, achieving effective heterojunctions requires careful consideration of factors such as lattice and band alignment. In addition, the complex preparation process of these heterojunctions significantly increases the manufacturing cost of sensors. On the other hand, current representative metal oxide gas-sensitive materials such as ZnO, SnO2, and TiO2 are wide-bandgap semiconductors (>3.0eV). Therefore, ultraviolet light is usually used as an excitation source. Ultraviolet light poses risks to human health and consumes more energy. In addition, ultraviolet excitation severely limits the ability of sensors to effectively utilize sunlight. Therefore, achieving efficient gas detection at room temperature under visible light excitation represents a key advancement in gas sensor technology.

[0004] Among all kinds of environmental gases, volatile organic compounds (VOCs) have very harmful effects on human health and the environment and are a major environmental hazard. Among them, acetic acid, as a colorless, flammable and explosive VOCs, is widely used in food processing, chemical synthesis and other industries. It can cause serious irritation to human eyes, skin and respiratory tract. According to OSHA regulations, the allowable exposure concentration of acetic acid in the workplace is 10ppm. Therefore, effective detection of acetic acid gas is crucial. At present, although researchers have worked hard to develop a variety of metal oxide semiconductor-based resistive gas sensors for detecting acetic acid. However, these sensors usually require higher operating temperatures (usually above 200°C), which may pose significant safety risks in practical applications. Therefore, it is urgent to develop resistive gas sensors that can achieve efficient detection of acetic acid at room temperature. Summary of the invention

[0005] The purpose of the present invention is to solve at least one of the technical problems existing in the prior art and to provide a visible light excited room temperature acetic acid gas sensor and a preparation method and application thereof. The acetic acid gas sensor of the present invention can realize efficient detection of acetic acid at room temperature.

[0006] The technical solution of the present invention is as follows:

[0007] A first aspect of the present invention provides an acetic acid gas sensor, comprising a substrate and a Bi2WO6 crystal plane heterojunction sensitive layer grown on the surface of the substrate, wherein the Bi2WO6 crystal plane heterojunction is in a nanosheet morphology.

[0008] In a specific embodiment of the present invention, the lateral size of the nanosheet is 1 to 20 μm and the thickness is 200 to 800 nm.

[0009] The lateral size of the nanosheet is preferably 1 to 15 μm, more preferably 1 to 10 μm, further preferably 6 to 10 μm, and further preferably 3 to 10 μm.

[0010] The thickness of the nanosheet is preferably 400 to 800 nm, more preferably 500 to 800 nm, even more preferably 600 to 800 nm, and even more preferably 700 to 800 nm.

[0011] In a specific embodiment of the present invention, the substrate is an Al2O3 substrate having precious metal Pt interdigital electrodes.

[0012] A second aspect of the present invention provides a method for preparing an acetic acid gas sensor, comprising:

[0013] Bi2WO6 crystal surface heterojunction was prepared by solvent-assisted solid phase reaction method;

[0014] Then, the Bi2WO6 crystal plane heterojunction is coated as a sensitive layer onto an Al2O3 substrate having a noble metal Pt interdigital electrode by using a thick film process to obtain an acetic acid gas sensor.

[0015] In a specific embodiment of the present invention, the method for preparing the Bi2WO6 crystal surface heterojunction by solvent-assisted solid phase reaction method specifically comprises the following steps:

[0016] (a) mixing Bi2O3 and WO3 with a flux to form a reaction mixture;

[0017] (b) adding the reaction mixture into a solvent and grinding thoroughly;

[0018] (c) after evaporating the solvent, transferring the reaction mixture to a reaction vessel for heating;

[0019] (d) After the reaction is completed, the obtained product is washed and then dried to obtain a yellow powder.

[0020] In a specific embodiment of the present invention, in step (a), the molar ratio of Bi2O3 to WO3 is 1:1, the molar ratio of the flux to the precursor is 5-20:1, the flux is NaCl or KCl or a eutectic mixture of NaCl and KCl, and the molar ratio of NaCl to KCl is 0-1:0-1;

[0021] The molar ratio of the flux to the precursor is preferably 5-15:1, more preferably 5-10:1.

[0022] The molar ratio of NaCl to KCl is preferably 0.2-1:0.2-1, more preferably 0.5-1:0.5-1.

[0023] In a specific embodiment of the present invention, in step (b), the solvent is ethanol, and the grinding time of the reaction mixture is 0.5-2 hours, preferably 0.5-1.5 hours, and more preferably 0.5-1.0 hours.

[0024] In a specific embodiment of the present invention, in step (c), the heating temperature of the reaction mixture is 600°C-800°C, and the heating time is 2-4 hours; the heating temperature is more preferably 600°C-750°C, and the heating time is 2.5-3.5 hours; the heating temperature is more preferably 600°C-700°C, and the heating time is 3 hours.

[0025] In a specific embodiment of the present invention, the method of using a thick film process to coat a Bi2WO6 crystal plane heterojunction as a sensitive layer onto an Al2O3 substrate having a noble metal Pt interdigital electrode specifically comprises the following steps:

[0026] The prepared Bi2WO6 crystal face heterojunction powder is dissolved in a solvent and formed into a uniform slurry by ultrasonic treatment;

[0027] The slurry is coated on an Al2O3 substrate having a noble metal Pt interdigital electrode, and the solvent is evaporated to obtain an acetic acid gas sensor.

[0028] In a specific embodiment of the present invention, the mass of the Bi2WO6 crystal face heterojunction powder is 1-5 mg, the solvent is ethanol, the volume of the solvent is 10-50 μl, and the ultrasonic time is 5-30 minutes.

[0029] In a specific embodiment of the present invention, the coating amount of the slurry is 1-5 μl.

[0030] A third aspect of the present invention is to provide an application of an acetic acid gas sensor, wherein the acetic acid gas sensor can be used to perform highly selective detection of acetic acid at room temperature under the excitation of a low-power visible light LED.

[0031] The present invention has at least one of the following beneficial effects:

[0032] 1. In the acetic acid gas sensor of the present invention, the Bi2WO6 crystal surface heterojunction has abundant oxygen adsorption active sites and efficient spatial photogenerated carrier separation efficiency, and realizes room temperature highly selective detection of acetic acid gas under visible light excitation.

[0033] 2. The preparation process of the acetic acid gas sensor of the present invention is simple and low-cost, and only requires a solvent-assisted solid phase reaction combined with an annealing treatment.

[0034] 3. The acetic acid gas sensor of the present invention is applied to detect acetic acid gas. The Bi2WO6 crystal surface heterojunction can realize highly selective detection of acetic acid gas at room temperature under visible light excitation without requiring a higher operating temperature. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The X-ray diffraction (XRD) patterns, Raman spectra, atomic configurations of different crystal planes and high-resolution XPS spectra of different samples of Bi2WO6 crystal plane heterojunctions in the present invention are shown.

[0036] Figure 2 The present invention provides scanning electron microscope (SEM) photos, transmission electron microscope (TEM) photos, selected area electron diffraction image (SAED) photos, high-resolution transmission electron microscope (HRTEM) photos and element distribution maps of different samples of Bi2WO6 crystal surface heterojunction.

[0037] Figure 3This is a graph showing the gas-sensing performance of the Bi2WO6 crystal plane heterojunction sensor of the present invention and the comparative sensor to acetic acid under visible light excitation at room temperature.

[0038] Figure 4 The UV-visible absorption spectra, UPS curves, photogenerated charge separation mechanism of Bi2WO6 crystal surface heterojunction and three-dimensional charge density difference diagram on different crystal surface interfaces of different samples of Bi2WO6 crystal surface heterojunction in the present invention are shown.

[0039] Figure 5 The present invention shows photoluminescence (PL) spectra of different samples of Bi2WO6 crystal plane heterojunction, transient photocurrent response, scanning electron microscope (SEM) photos of Bi2WO6 microplates after in-situ photodeposition of metal oxides or noble metals, and in-situ Fourier transform infrared spectra in acetic acid atmosphere. DETAILED DESCRIPTION

[0040] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0041] To achieve the above objectives, the present invention is implemented through the following technical solutions.

[0042] The acetic acid gas sensor provided by the present invention comprises a substrate and a Bi2WO6 crystal plane heterojunction sensitive layer coated on the surface of the substrate using a thick film process. The sensor is composed of an Al2O3 substrate with a noble metal Pt interdigital electrode and a Bi2WO6 crystal plane heterojunction sensitive layer prepared on the substrate using a thick film coating process; the Bi2WO6 crystal plane heterojunction is in the form of a nanosheet, the lateral size of the nanosheet is about 1 to 20 μm, and the thickness is about 200 to 800 nm.

[0043] Preferably, the substrate is an Al2O3 substrate having precious metal Pt interdigital electrodes.

[0044] The method for preparing the acetic acid gas sensor provided by the present invention comprises the following steps:

[0045] Step (1), mixing Bi2O3 and WO3 (as precursors) in a molar ratio of 1:1 with a eutectic mixture of NaCl and KCl (as flux) in a molar ratio of 0-1:0-1, wherein the molar ratio of flux to precursor is 5-20:1, to form a reaction mixture; grinding the mixture thoroughly in a mortar for 0.5-2 hours using ethanol as a solvent; after waiting for the ethanol to evaporate, transferring the obtained mixture into an alumina crucible and heating it in a muffle furnace at 600°C-800°C; after reacting for 2-4 hours, the obtained product is thoroughly washed with ethanol and deionized water, and then dried to obtain a yellow powder.

[0046] Step (2), before coating, a commercial flat Al2O3 gas-sensitive substrate (produced by Huachuang Ruike Technology Co., Ltd.) is repeatedly washed in deionized water and anhydrous ethanol and then dried for use;

[0047] Step (3), dissolving 1-5 mg of the powder sample in 10-50 μl of ethanol and forming a uniform slurry by ultrasonic treatment for 5-30 minutes; then using a micropipette to coat 1-5 μl of the slurry on a commercial Al2O3 substrate pre-engraved with two pairs of platinum electrodes, and waiting for the solvent to evaporate; installing the Al2O3 substrate with the sensing layer on a commercial static gas sensing test device, and performing a gas sensing performance test after aging at a temperature of 20°C-100°C for 24 hours.

[0048] The Bi2WO6 crystal plane heterojunction gas sensor provided by the present invention can realize high-selectivity detection of acetic acid gas at room temperature under visible light excitation.

[0049] The present invention is further described in detail below with specific examples, but the present invention is not limited to the following specific examples.

[0050] In the following embodiments, before coating the Bi2WO6 crystal plane heterojunction sensitive layer on the substrate, the required commercial Al2O3 substrate with precious metal Pt interdigital electrodes is processed by the following steps: the substrate is repeatedly washed in deionized water and anhydrous ethanol and then dried for use.

[0051] Preparation Example 1:

[0052] Bi2O3 and WO3 (as precursors) in a molar ratio of 1:1 were mixed with a eutectic mixture of NaCl and KCl (used as flux) in a molar ratio of 1:0, and the molar ratio of flux to precursor was 5:1 to form a reaction mixture; the mixture was thoroughly ground in a mortar with ethanol as a solvent for 0.5 hours; after waiting for the ethanol to evaporate, the resulting mixture was transferred to an alumina crucible and heated in a muffle furnace at 650°C; after reacting for 3 hours, the resulting product was thoroughly washed with ethanol and deionized water, and then dried to obtain a yellow powder. 2 mg of the powder sample was dissolved in 20 μl of ethanol and a uniform slurry was formed by ultrasonic treatment for 10 minutes; then 2 μl of the slurry was coated on a commercial Al2O3 substrate pre-engraved with two pairs of platinum electrodes using a micropipette, and the solvent was evaporated to obtain the gas sensor BWO-1.

[0053] Preparation Example 2:

[0054] Bi2O3 and WO3 (as precursors) in a molar ratio of 1:1 were mixed with a eutectic mixture of NaCl and KCl (used as flux) in a molar ratio of 0:1, and the molar ratio of flux to precursor was 5:1 to form a reaction mixture; the mixture was thoroughly ground in a mortar with ethanol as a solvent for 0.5 hours; after waiting for the ethanol to evaporate, the resulting mixture was transferred to an alumina crucible and heated in a muffle furnace at 650°C; after reacting for 3 hours, the resulting product was thoroughly washed with ethanol and deionized water, and then dried to obtain a yellow powder. 2 mg of the powder sample was dissolved in 20 μl of ethanol and a uniform slurry was formed by ultrasonic treatment for 10 minutes; then 2 μl of the slurry was coated on a commercial Al2O3 substrate pre-engraved with two pairs of platinum electrodes using a micropipette, and the solvent was evaporated to obtain the gas sensor BWO-2.

[0055] Preparation Example 3:

[0056] Bi2O3 and WO3 (as precursors) in a molar ratio of 1:1 were mixed with a eutectic mixture of NaCl and KCl (used as flux) in a molar ratio of 0:1, and the molar ratio of flux to precursor was 10:1 to form a reaction mixture; the mixture was thoroughly ground in a mortar with ethanol as a solvent for 0.5 hours; after waiting for the ethanol to evaporate, the resulting mixture was transferred to an alumina crucible and heated in a muffle furnace at 650°C; after reacting for 3 hours, the resulting product was thoroughly washed with ethanol and deionized water, and then dried to obtain a yellow powder. 2 mg of the powder sample was dissolved in 20 μl of ethanol and a uniform slurry was formed by ultrasonic treatment for 10 minutes; then 2 μl of the slurry was coated on a commercial Al2O3 substrate pre-engraved with two pairs of platinum electrodes using a micropipette, and the solvent was evaporated to obtain the gas sensor BWO-3.

[0057] Preparation Example 4:

[0058] Bi2O3 and WO3 (as precursors) in a molar ratio of 1:1 were mixed with a eutectic mixture of NaCl and KCl (used as flux) in a molar ratio of 1:1, and the molar ratio of flux to precursor was 20:1 to form a reaction mixture; the mixture was thoroughly ground in a mortar with ethanol as a solvent for 0.5 hours; after waiting for the ethanol to evaporate, the resulting mixture was transferred to an alumina crucible and heated in a muffle furnace at 650°C; after reacting for 3 hours, the resulting product was thoroughly washed with ethanol and deionized water, and then dried to obtain a yellow powder. 2 mg of the powder sample was dissolved in 20 μl of ethanol and a uniform slurry was formed by ultrasonic treatment for 10 minutes; then 2 μl of the slurry was coated on a commercial Al2O3 substrate pre-engraved with two pairs of platinum electrodes using a micropipette, and the solvent was evaporated to obtain the gas sensor BWO-4.

[0059] The steps of performing gas sensitivity testing on the gas sensors prepared in Examples 1-4 are as follows:

[0060] The sensor was mounted on a commercial static gas sensing test device and aged at 20°C-100°C for 24 hours before gas sensing performance testing. The gas sensing performance was tested using a commercial static test device (produced by Huachuang Ruike Technology Co., Ltd.). During the test, the target gas was injected into the test chamber, which was then raised to introduce ambient air. The sensor temperature can be adjusted by an external temperature control system connected to a computer. The gas sensing response is defined as the ratio of the resistance in air and the target gas (R a / R g or R g / R a ), the response time and recovery time of the sensor are defined as the time required for its resistance to reach 90% of the equilibrium resistance when exposed to the target gas and removed from the target gas, respectively.

[0061] The specific results of characterization and performance testing of the sensors prepared in Examples 1-4 are as follows:

[0062] Figure 1The X-ray diffraction (XRD) patterns, Raman spectra, atomic configurations of different crystal planes and high-resolution XPS spectra of different samples of Bi2WO6 crystal plane heterojunctions in the present invention are shown. Figure a shows the XRD spectra of different samples. It can be seen that the pure phase Bi2WO6 has an orthorhombic structure. However, there are obvious differences in the relative intensities of these peaks (Figure b). Generally, with the increase of flux concentration and dosage, the peak intensity of the (002) crystal plane gradually increases. This shows that the addition of flux can affect the crystal plane of Bi2WO6 and promote its growth along the c-axis, resulting in an increase in the exposure ratio of the {001} crystal plane and. The four Bi2WO6 samples were further characterized by Raman spectroscopy (Figure c). The results show that all four samples have significant characteristic Raman peaks, indicating that they have excellent crystallinity. It is worth noting that the peak positions of the Raman peaks of the four samples have undergone some shifts (Figure d). Generally, ~836cm -1 The peak at 100° gradually shifts to the low frequency direction from BWO-1 to BWO-4, which corresponds to the decrease of the WO distance bond length. The shift of Raman spectra here further confirms the difference of the exposed crystal faces of the four Bi2WO6 samples. According to previous reports, the orthorhombic structure Bi2WO6 is composed of perovskite [WO4] 2+ and fluorite type [Bi2O2] 2+ The structure consists of alternating layers. In this structure, the {001} crystal plane perpendicular to the c-axis and the {010} crystal plane parallel to the c-axis have significant differences in surface atomic and electronic properties (Figures e and f). The huge differences between these crystal planes make it possible to form the so-called self-constructed "crystal plane junction" or "surface heterojunction" when they coexist. XPS analysis was performed to further determine the elemental composition of different samples. Figure gi shows that all four samples present double peaks of Bi and W, with minimal differences in chemical states. However, there are significant differences in the O1s peaks of the four samples, with the O1s peak of lattice oxygen at ~530eV and the O1s peak of chemically adsorbed oxygen at about ~531.5eV. The peak intensity ratio of chemically adsorbed oxygen to lattice oxygen is the highest in BWO-1. This shows that BWO-1 has more active sites for oxygen adsorption, which can also be attributed to the different surface properties caused by different crystal planes to a certain extent. According to the classical oxygen adsorption model of resistive gas sensors, chemically adsorbed oxygen is considered to be the active species in the gas-sensing reaction, which means that BWO-1 is expected to show the best gas-sensing performance.

[0063] Figure 2The present invention shows scanning electron microscope (SEM) photos, transmission electron microscope (TEM) photos, selected area electron diffraction image (SAED) photos, high resolution transmission electron microscope (HRTEM) photos and element distribution maps of different samples of Bi2WO6 crystal plane heterojunction. The Bi2WO6 sample shows a microplate morphology. The thickness of the Bi2WO6 microplate gradually decreases from about 800nm ​​to 200nm (Figure ah), indicating that the characteristic crystal plane of Bi2WO6 gradually changes. TEM analysis further characterizes the microplate structure of Bi2WO6 (Figure il). Figures i and j show that BWO-1 presents a plate-like structure under low magnification, and the selected area electron diffraction (SAED) along the

[001] axis confirms its single crystal nature (Figure k). In the HRTEM image (Figure l), two groups of vertical lattice fringes corresponding to the (220) and (200) crystal planes are observed. According to the orthorhombic symmetry of Bi2WO6 and previous studies, the bottom and top surfaces of the Bi2WO6 microplate are determined to be {001} crystal planes, and the side surfaces are {010} crystal planes. Increasing the concentration and amount of flux is conducive to the exposure of the {001} crystal plane, while reducing the exposure of the {010} crystal plane. Combined with the size characteristics observed by scanning electron microscopy, the exposure percentages of the {001} crystal plane in the BWO-1, BWO-2, BWO-3 ​​and BWO-4 microplates are calculated to be approximately 65.1%, 75.6%, 88.3% and 94.3%, respectively. The elemental composition of the sample was determined by energy dispersive spectrometer (EDS) (Figure mp), which confirmed the uniform distribution of Bi, W and O elements in the Bi2WO6 microplate, which was consistent with expectations.

[0064] Figure 3The gas-sensing performance of the Bi2WO6 crystal plane heterojunction sensor and the comparative sensor to acetic acid under visible light excitation at room temperature is shown in Figures ed. The response and recovery curves of four Bi2WO6 microplate sensors exposed to 100ppm acetic acid under visible LED light excitation. The results show good repeatability over multiple cycles. It is worth noting that under the same conditions, the response value of BWO-1 is ~15, which is significantly higher than that of other sensors. The response values ​​of BWO-1, BWO-2, BWO-3 ​​and BWO-4 sensors gradually decrease. Given that these gas-sensitive materials have similar microplate morphology and comparable specific surface areas, the key difference lies in the exposed crystal plane. This shows that the exposed crystal plane is the key to determining the sensing performance of the Bi2WO6 microplate. The recovery curves and dynamic responses of the four sensors to different concentrations of acetic acid are shown in Figures eh. As the concentration of acetic acid increases, the response value gradually increases. Compared with the other three sensors, the BWO-1 sensor exhibits significantly better performance. A linear relationship was observed between the logarithmic concentration and the response value (Figure i). According to the formula LOD = Kσ / S (where LOD represents the limit of detection, K is a constant usually set to 3, σ is the standard deviation of the measured value, and S is the slope), the acetic acid LOD of BWO-1 was determined to be 0.289 ppm. This value is significantly lower than the allowable exposure concentration of acetic acid, indicating that BWO-1 is suitable for detecting low concentrations of acetic acid. In addition, the sensing performance of BWO-1 for 10 other typical VOC gases was tested under the same conditions (Figure j). The results show that BWO-1 has almost no response to volatile organic compounds such as methanol, ethanol, and ethyl acetate, and has good selectivity for acetic acid. In order to observe the response and recovery time of acetic acid detection, a real-time response / recovery kinetic curve within one cycle is further given ( Figure 3 k). The results show that the response time and recovery time of BWO-1 are 186s and 297s, respectively. In order to evaluate the effect of ambient humidity on the sensing performance, acetic acid detection was performed under different humidity environments (Figure l). It can be seen that when the ambient humidity increased from 20% to 80%, the baseline resistance and response value changes remained in a relatively stable range, confirming its effective operation ability under different humidity environments. After 4 months of storage, the BWO-1 sensor was tested for acetic acid. The response value showed only a slight decrease, indicating that the acetic acid detection has good long-term stability. In summary, under visible light excitation, the Bi2WO6 crystal face heterojunction is an ideal candidate for efficient room temperature acetic acid detection.

[0065] Table 1 shows the performance comparison of Bi2WO6 gas sensor and various related acetic acid sensors. Under visible light excitation at room temperature, the response value of BWO-1 sensor to 100 ppm acetic acid is ~15, which shows obvious advantages over previously reported acetic acid sensors, especially in terms of operating temperature.

[0066] Table 1 Performance comparison of Bi2WO6 gas sensor and various related acetic acid sensors

[0067]

[0068] Figure 4 The UV-visible absorption spectra, UPS curves, photogenerated charge separation mechanism of Bi2WO6 crystal face heterojunction and three-dimensional charge density difference on different crystal face interfaces of different samples of Bi2WO6 crystal face heterojunction in the present invention are shown. The UV-visible absorption spectra preliminarily show that the optical band gap of the four Bi2WO6 microplates is about 2.7eV (Figures ad), indicating that it is suitable for visible light absorption. The UPS curves show that the work function of these samples is around 6eV (Figure eh), and the work function gradually increases with the increase of the {001} crystal face ratio. The first-principles calculations are further used to accurately determine the work functions of Bi2WO6 {001} and {010} crystal faces (Figures i and j). The results show that the {001} crystal face has a higher work function than the {010} crystal face. According to previous reports, due to the different work functions and band structure changes between crystal faces, a "face junction" or "surface heterojunction" (Figures k and l) is formed inside the semiconductor single crystal. These junction-induced surface band bending and internal fields are essential for the efficient separation of photogenerated carriers between different facets. This separation plays a key role in improving the performance of photoexcited gas sensors. First-principles calculations were used to analyze the three-dimensional electron density difference at the {001} / {010} interface (Figure k), confirming that there is a large charge transfer from the {010} to the {001} facets. Nevertheless, the differences in {001} and {010} in the four Bi2WO6 microplates lead to different photogenerated carrier separation efficiencies within these facet junctions.

[0069] Figure 5 The photoluminescence (PL) spectra, transient photocurrent responses, scanning electron microscope (SEM) images of Bi2WO6 microplates after in-situ photodeposition of metal oxides or precious metals, and in-situ Fourier transform infrared spectra under acetic acid atmosphere of different samples of Bi2WO6 crystal face junctions in the present invention are shown. PL and photocurrent tests show that BWO-1 has better photogenerated carrier separation efficiency compared with the other three nanocrystals, as manifested by lower PL intensity and higher photocurrent (Figures a and b). This emphasizes that the optimal crystal face ratio can maximize the crystal face junction effect. In order to confirm the effective separation of photogenerated carriers in the Bi2WO6 microplate, selective photodeposition experiments of precious metals and metal oxides were carried out (Figures cf). The results show that from Mn 2+ MnO xSelectively deposited on the {010} crystal plane, indicating preferential enrichment of photogenerated holes. In contrast, noble metal (Ag, Au, Pt) nanoparticles are selectively deposited on the {001} crystal plane surface, indicating preferential accumulation of photogenerated electrons. These findings confirm the enhanced spatial photogenerated carrier separation in the Bi2WO6 crystal plane heterojunction, thereby enhancing the gas sensing performance under photoexcitation. In order to study the gas sensing reaction of acetic acid on the Bi2WO6 surface in detail, in situ Fourier transform infrared spectroscopy (FTIR) technology was used (Figure gl). The FTIR spectra collected from the Bi2WO6 surface after different irradiation times clearly show the 2800-3000 cm-1 corresponding to the OH and CH bonds. -1 These vibrations indicate the formation of cyclic dimers or monomers of acetic acid, which are characterized by strong hydrogen bonding interactions between the acid groups. -1 The peak at 1530 cm-1 is the stretching vibration of the C=O group in the carboxyl group of acetate. 1 The peaks near the Bi2WO6 surface are antisymmetric OCO stretching vibrations. These vibrations are CH3COOH and CH3COO adsorbed on the Bi2WO6 surface. - In addition, 2349 and 2376cm -1 The appearance and increase in intensity of the characteristic CO2 peak at indicated that an oxidation reaction occurred during the process, resulting in the gradual accumulation of CO2 and H2O, indicating that photocatalytic oxidation of acetic acid occurred in the gas-sensitive reaction.

[0070] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A visible light excited room temperature acetic acid gas sensor, characterized in that: It comprises a substrate and a Bi2WO6 crystal plane heterojunction sensitive layer grown on the surface of the substrate, wherein the Bi2WO6 crystal plane heterojunction is in the shape of a nanosheet.

2. A visible light excited room temperature acetic acid gas sensor according to claim 1, characterized in that: The lateral size of the nanosheets is 1 to 20 μm and the thickness is 200 to 800 nm.

3. A visible light excited room temperature acetic acid gas sensor according to claim 1, characterized in that: The substrate is an Al2O3 substrate with precious metal Pt interdigital electrodes.

4. A method for preparing a visible light excited room temperature acetic acid gas sensor, characterized in that: Bi2WO6 crystal surface heterojunction was prepared by solvent-assisted solid phase reaction method; Then, the Bi2WO6 crystal plane heterojunction is coated as a sensitive layer onto an Al2O3 substrate having a noble metal Pt interdigital electrode by using a thick film process to obtain an acetic acid gas sensor.

5. The method for preparing a visible light excited room temperature acetic acid gas sensor according to claim 4, characterized in that: The method for preparing the Bi2WO6 crystal surface heterojunction by solvent-assisted solid phase reaction method specifically comprises the following steps: (a) mixing Bi2O3 and WO3 with a flux to form a reaction mixture; (b) adding the reaction mixture into a solvent and grinding thoroughly; (c) after evaporating the solvent, transferring the reaction mixture to a reaction vessel for heating; (d) After the reaction is completed, the obtained product is washed and then dried to obtain a yellow powder.

6. The method for preparing a visible light excited room temperature acetic acid gas sensor according to claim 5, characterized in that: In step (a), the molar ratio of Bi2O3 to WO3 is 1:1, the molar ratio of the flux to the precursor is 5-20:1, the flux is NaCl or KCl or a eutectic mixture of NaCl and KCl, and the molar ratio of NaCl to KCl is 0-1:0-1; In step (b), the solvent is ethanol and the grinding time of the reaction mixture is 0.5-2 hours; In step (c), the heating temperature of the reaction mixture is 600° C.-800° C., and the heating time is 2-4 hours.

7. The method for preparing a visible light excited room temperature acetic acid gas sensor according to claim 4, characterized in that: The method of using a thick film process to coat a Bi2WO6 crystal plane heterojunction as a sensitive layer onto an Al2O3 substrate having a noble metal Pt interdigital electrode specifically comprises the following steps: The prepared Bi2WO6 crystal face heterojunction powder is dissolved in a solvent and formed into a uniform slurry by ultrasonic treatment; The slurry is coated on an Al2O3 substrate having a noble metal Pt interdigital electrode, and the solvent is evaporated to obtain an acetic acid gas sensor.

8. The method for preparing a visible light excited room temperature acetic acid gas sensor according to claim 7, characterized in that: The mass of the Bi2WO6 crystal face heterojunction powder is 1-5 mg, the volume of the solvent is 10-50 μl, and the ultrasonic time is 5-30 minutes.

9. The method for preparing a visible light excited room temperature acetic acid gas sensor according to claim 7, characterized in that: The coating amount of the slurry is 1-5 μl.

10. Use of the visible light excited room temperature acetic acid gas sensor according to any one of claims 1 to 3, characterized in that: The acetic acid gas sensor can be used to detect acetic acid at room temperature with high selectivity under the excitation of a low-power visible light LED.

Citation Information

Cited By

  • Bi2WO6 / ZnIn2S4 / Ag ternary hierarchical heterojunction as well as preparation method and application thereof

    CN121990609A