Metal-containing photoresist developer compositions and methods of forming patterns
By using a composition of sulfonimide compounds and organic solvents in the photoresist, the problems of the reduction of sensitivity of existing photoresist and the increase of line edge roughness under extreme ultraviolet exposure are solved, and high-performance photoresist is realized The development effect improves the patterning capability of the semiconductor industry.
Patent Information
- Application Number
- CN202410573611.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-26
- Filing Date
- 2024-05-10
- Publication Date
- 2024-11-26
AI Technical Summary
The sensitivity of existing chemical amplified photoresist is reduced under extreme ultraviolet exposure, and the increase in line edge roughness caused by the acid catalyst process makes it difficult to meet the semiconductor industry's demand for high-performance photoresist.
A metal-containing photoresist developer composition containing sulfonimide compounds and organic solvents is used to improve cleaning ability, reduce residual films and defects, and improve contrast characteristics by forming chelating bonds.
It significantly improves the sensitivity and line edge roughness characteristics of photoresist, reduces the pattern defect rate, enhances the processing ability of smaller features, and meets the needs of high-performance photoresist.
Smart Images

Figure CN119024655A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to and the benefit of Korean Patent Application No. 10-2023-0068547 filed in the Korean Intellectual Property Office on May 26, 2023, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0003] One or more aspects of various embodiments of the present disclosure are directed to a metal-containing photoresist developer composition and a method of forming a pattern, the method including a developing step using the metal-containing photoresist developer composition. Background Art
[0004] In recent years, the semiconductor industry has witnessed a continuous reduction in critical dimensions, and this reduction in dimensions requires (or requires) new types (or new kinds) of high-performance photoresist materials and patterning methods that can meet the needs (or expectations) of processing and patterning materials with smaller and smaller features.
[0005] Related art Chemically amplified (CA) photoresists are designed to ensure relatively high sensitivity, but because the elemental composition of CA photoresists (e.g., less amount of O, F, S and / or C) may reduce the absorbance at a wavelength of about 13.5 nm, the sensitivity may be reduced and the photoresist may partially encounter more difficulties under EUV (extreme ultraviolet, wavelength of 13.5 nm) exposure. In addition, CA photoresists may have difficulties due to roughness issues (e.g., undesirable or suitable roughness) in small feature sizes, and partly due to the nature of the acid catalyst process, experimentally the line edge roughness (LER) may increase as the speed of light decreases. At least partly due to these shortcomings and problems of CA photoresists, a new type (or new class) of high-performance photoresists is needed (or desired) in the semiconductor industry.
[0006] For example, it is necessary (or desirable) to develop a photoresist that can ensure excellent or appropriate etch resistance and resolution while simultaneously (or synchronously) improving sensitivity and enhancing critical dimension (CD) uniformity and line edge roughness (LER) characteristics in a photolithography process. Summary of the invention
[0007] One or more aspects of various embodiments of the present disclosure provide a metal-containing photoresist developer composition.
[0008] One or more aspects of various embodiments of the present disclosure provide a method of forming a pattern including a developing step using the composition.
[0009] A metal-containing photoresist developer composition according to some embodiments includes an organic solvent and a sulfonimide-based compound.
[0010] The sulfonimide-based compound may be at least one selected from the group consisting of the compounds represented by Chemical Formula 1 and Chemical Formula 2.
[0011]
[0012] In Chemical Formula 1 and Chemical Formula 2,
[0013] R 1 and R 2 are each independently fluorine, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C3 to C20 cycloalkenyl, substituted or unsubstituted C3 to C20 cycloalkynyl, substituted or unsubstituted C6 to C20 aryl, substituted or unsubstituted C1 to C20 heteroaryl, or a combination thereof, and
[0014] L 1 is a substituted or unsubstituted C1 to C10 alkylene group, a substituted or unsubstituted C3 to C20 cycloalkylene group, a substituted or unsubstituted C6 to C20 arylene group, a substituted or unsubstituted C1 to C20 heteroarylene group, or a combination thereof.
[0015] The sulfonimide compound may be at least one selected from the compounds listed in Group I.
[0016] Group I
[0017]
[0018] The acidity coefficient (pKa) of the sulfonimide compound may be less than or equal to about 5.
[0019] The metal-containing photoresist developer composition according to some embodiments may include: about 50 wt % to about 99.99 wt % of an organic solvent; and about 0.01 wt % to about 50 wt % of a sulfonyl imide-based compound.
[0020] The metal compound contained in the metal-containing photoresist may be at least one selected from an organooxy group-containing tin compound and an organocarbonyloxy group-containing tin compound.
[0021] The metal-containing photoresist may include a metal compound represented by Chemical Formula 3:
[0022] Chemical formula 3
[0023]
[0024] In chemical formula 3,
[0025] R 3 The alkyl radical may be selected from substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, substituted or unsubstituted C6 to C30 arylalkyl, and -L a -OR a (where L a is a substituted or unsubstituted C1 to C20 alkylene group, and R a is a substituted or unsubstituted C1 to C20 alkyl),
[0026] R 4 to R 6 The alkyl radicals may be each independently selected from substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, substituted or unsubstituted C6 to C30 arylalkyl, -OR b and -OC(=O)R c Selected from
[0027] R b may be a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof,
[0028] R cmay be hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof, and
[0029] Since R 4 to R 6 At least one of the selected can be independently selected from -OR b and -OC(=O)R c Selected from.
[0030] According to some embodiments, a method for forming a pattern includes: coating a metal-containing resist composition on a substrate; coating a composition for removing edge beads from a metal-containing photoresist along an edge of the substrate; drying and heating the resultant to form a metal-containing photoresist layer on the substrate; exposing the metal-containing photoresist layer; and coating the metal-containing photoresist developer composition of the present embodiment and developing the metal-containing photoresist developer composition.
[0031] The method of forming a pattern according to some embodiments may minimize or reduce residual films, scum, and / or defects present in a metal-containing photoresist layer after an exposure process, and may enable easy or appropriate development, thereby achieving excellent or improved contrast characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] These and / or other aspects will become apparent and more easily understood by reading the following description of the embodiments in conjunction with the accompanying drawings, in which:
[0033] Figures 1 to 3 2 is a cross-sectional view illustrating a process sequence of a method of forming a pattern according to one or more embodiments of the present disclosure.
[0034] [Explanation of Reference Numerals]
[0035] 100: Substrate
[0036] 110: Feature layer
[0037] 110P: Characteristic pattern
[0038] 130P: Photoresist pattern
[0039] OP: Opening DETAILED DESCRIPTION
[0040] Hereinafter, embodiments of the present disclosure will be described in more detail with reference to the accompanying drawings. In the following description of the present disclosure, in order to make the present disclosure clear, well-known functions or structures will not be described in detail.
[0041] In order to clearly illustrate the present disclosure, certain descriptions and relationships that should be understood by a person of ordinary skill in the art are not provided, and throughout the disclosure, the same or similar configuration elements are represented by the same reference numerals. In addition, since the size and thickness of each configuration shown in the drawings are arbitrarily shown for better understanding and ease of description, the present disclosure is not necessarily limited thereto.
[0042] In the drawings, the thickness of each layer, film, panel, region, etc. is exaggerated for clarity. In the drawings, the thickness of a portion of each layer and / or region is exaggerated for clarity. It should be understood that when an element (such as a layer, film, region, or substrate) is referred to as being "on" another element, the element may be directly on the other element (such as without any intermediate elements therebetween), or intermediate elements may also be present.
[0043] It should be understood that although the terms first, second, etc. may be used herein to describe various elements, these elements should not be limited by these terms. These terms are only used to distinguish between various elements. Therefore, without departing from the teachings of the present disclosure, the first element may be referred to as the second element. Similarly, the second element may be referred to as the first element.
[0044] As used herein, the singular forms "a", "an" and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise.
[0045] It will also be understood that the terms “includes / including” and / or “comprises / comprising”, when used in the present specification, specify the presence of stated features, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, steps, operations, elements, components and / or groups thereof.
[0046] As used herein, the terms "use," "using," and "used" may be considered synonymous with the terms "utilize," "utilizing," and "utilized," respectively.
[0047] As used herein, expressions such as "at least one of," "one of," and "selected from," when preceding a list of elements, modify the entire list of elements rather than the individual elements in the list. For example, "at least one selected from a, b, and c," "at least one of a, b, or c," and "at least one of a, b, and / or c" may indicate including only a, only b, only c, including (e.g., simultaneously) both a and b, including (e.g., simultaneously) both a and c, including (e.g., simultaneously) both b and c, including all of a, b, and c, or variations thereof.
[0048] As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items.
[0049] In addition, the use of “may” when describing embodiments of the present disclosure refers to “one or more embodiments of the present disclosure.”
[0050] For ease of description, spatially relative terms such as "beneath," "below," "lower," "above," "upper," "bottom," "top," and the like may be used herein to describe the relationship of one element or feature shown in the figures to another (other) element or feature. It should be understood that the spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation shown in the figures. For example, if the device in the figure is turned over, then the elements described as being "below" or "beneath" other elements or features will now be oriented "above" or "on" the other elements or features. Thus, the term "below" may include both above and below orientations. The device may be oriented in other ways (rotated 90 degrees or other orientations), and the spatially relative descriptors used herein should be interpreted accordingly.
[0051] As used herein, the terms "substantially," "about," and similar terms are used as terms of approximation rather than degree, and are intended to account for the inherent deviations in measured or calculated values that one of ordinary skill in the art would recognize. As used herein, "about" or "approximately" are inclusive of the stated value and mean within an acceptable range of deviation for the particular value as determined by one of ordinary skill in the art, taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" can mean within one or more standard deviations, or within ±30%, 20%, 10%, 5% of the stated value.
[0052] Any numerical range described herein is intended to include all sub-ranges of the same numerical precision that fall within the range. For example, the range of "1.0 to 10.0" is intended to include all sub-ranges between (and including) the minimum value 1.0 and the maximum value 10.0, i.e., having a minimum value equal to or greater than 1.0 and a maximum value equal to or less than 10.0, such as (for example) 2.4 to 7.6. Any maximum numerical limit described herein is intended to include all lower numerical limits that fall within it, and any minimum numerical limit described in this specification is intended to include all higher numerical limits that fall within it. Therefore, the applicant reserves the right to amend this specification (including the claims) to explicitly state any sub-ranges that fall within the range explicitly stated herein.
[0053] In the present disclosure, "substituted" means that a hydrogen atom is replaced by deuterium, halogen, hydroxyl, amino, substituted or unsubstituted C1 to C30 amino, nitro, substituted or unsubstituted C1 to C40 silyl, C1 to C30 alkyl, C1 to C10 haloalkyl, C1 to C10 alkylsilyl, C3 to C30 cycloalkyl, C6 to C30 aryl, C1 to C20 alkoxy, or cyano. "Unsubstituted" means that a hydrogen atom remains a hydrogen atom without being replaced by another substituent.
[0054] In the present disclosure, unless otherwise defined, the term "alkyl" may refer to a linear or branched aliphatic hydrocarbon group. The alkyl group may be a "saturated alkyl group" not including any double bond or triple bond.
[0055] The alkyl group may be a C1 to C20 alkyl group. For example, the alkyl group may be a C1 to C10 alkyl group or a C1 to C6 alkyl group. For example, a C1 to C5 alkyl group means that the alkyl chain contains 1 to 5 carbon atoms and may be selected from methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl.
[0056] Examples of the alkyl group may include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, hexyl, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, and the like.
[0057] In the present disclosure, unless otherwise defined, the term "cycloalkyl group" may refer to a monovalent cyclic aliphatic hydrocarbon group.
[0058] In the present disclosure, unless otherwise defined, the term “alkenyl group” may refer to a linear or branched aliphatic hydrocarbon group, and may refer to an aliphatic unsaturated alkenyl group including one or more carbon-carbon double bonds.
[0059] In the present disclosure, unless otherwise defined, the term "alkynyl group" may refer to a linear or branched aliphatic hydrocarbon group, and may refer to an unsaturated alkynyl group including one or more carbon-carbon triple bonds.
[0060] In the present disclosure, "aryl" may refer to a substituent in which all elements (or atoms) of a cyclic substituent or group have p-orbitals, and these p-orbitals form conjugation. Aryl may include monocyclic or polycyclic fused ring (e.g., rings that share adjacent pairs of carbon atoms) functional groups.
[0061] Hereinafter, a metal-containing photoresist developer composition according to some embodiments is described.
[0062] The metal-containing photoresist developer composition according to some embodiments of the present disclosure includes an organic solvent and a sulfonimide compound.
[0063] If a metal-containing photoresist developer composition comprising a sulfonyl imide compound is applied (e.g., utilized) for development, since the imide group of the sulfonyl imide compound forms a chelate bond with the metal-containing resist (e.g., the metal in the resist), excellent or improved contrast characteristics can be achieved by minimizing or reducing residual film / scum / defects on the metal-containing photoresist layer after the exposure process.
[0064] Suitable developers for metal-containing photoresist layers (e.g., in the related art) may include carboxylic acids, which are relatively weak acids and therefore may lack suitable or desired cleaning capabilities for metal-containing photoresist layers and therefore may not fully or properly meet the requirements for processing and patterning smaller features according to pattern refinement.
[0065] In contrast, the metal-containing photoresist developer composition according to some embodiments of the present disclosure contains a sulfonimide compound, which is a relatively stronger acidic material than a carboxylic acid, and thus can ensure improved cleaning ability to sufficiently or appropriately dissolve the unexposed area, thereby significantly minimizing or reducing residual film, scum and / or defects, and thus reducing pattern defect rate.
[0066] For example, the pKa of the sulfonimide compound may be -20≤pKa≤5, such as -15≤pKa≤5.
[0067] If the pKa of the sulfonyl imide compound is within the above range, the membrane removal ability can be further improved.
[0068] The sulfonimide-based compound may be at least one selected from the group consisting of the compounds represented by Chemical Formula 1 and Chemical Formula 2.
[0069]
[0070] In Chemical Formula 1 and Chemical Formula 2,
[0071] R 1 and R 2 may each independently be fluorine, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C3 to C20 cycloalkenyl, substituted or unsubstituted C3 to C20 cycloalkynyl, substituted or unsubstituted C6 to C20 aryl, substituted or unsubstituted C1 to C20 heteroaryl, or a combination thereof, and
[0072] L 1 The group may be a substituted or unsubstituted C1 to C10 alkylene group, a substituted or unsubstituted C3 to C20 cycloalkylene group, a substituted or unsubstituted C6 to C20 arylene group, a substituted or unsubstituted C1 to C20 heteroarylene group, or a combination thereof.
[0073] For example, R 1 and R 2 each independently may be fluorine, a C1-C20 alkyl group which is unsubstituted or substituted with at least one fluorine, a C2-C20 alkenyl group which is unsubstituted or substituted with at least one fluorine, a C2-C20 alkynyl group which is unsubstituted or substituted with at least one fluorine, a C3-C20 cycloalkyl group which is unsubstituted or substituted with at least one fluorine, a C3-C20 cycloalkenyl group which is unsubstituted or substituted with at least one fluorine, a C3-C20 cycloalkynyl group which is unsubstituted or substituted with at least one fluorine, a C6-C20 aryl group which is unsubstituted or substituted with at least one fluorine, a C1-C20 heteroaryl group which is unsubstituted or substituted with at least one fluorine, or a combination thereof, and
[0074] L 1 It may be a C1 to C10 alkylene group which is unsubstituted or substituted with at least one fluorine group, a C3 to C20 cycloalkylene group which is unsubstituted or substituted with at least one fluorine group, a C6 to C20 arylene group which is unsubstituted or substituted with at least one fluorine group, a C1 to C20 heteroarylene group which is unsubstituted or substituted with at least one fluorine group, or a combination thereof.
[0075] In one or more embodiments, R 1 and R 2 may each independently be fluorine, C1 to C20 alkyl group which is unsubstituted or substituted with at least one fluorine, C3 to C20 cycloalkyl group which is unsubstituted or substituted with at least one fluorine, C1 to C20 cycloalkyl group which is unsubstituted or substituted with at least one fluorine, C6 to C20 aryl group which is unsubstituted or substituted with at least one fluorine, or a combination thereof,
[0076] L 1 The group may be a C1 to C5 alkylene group which is unsubstituted or substituted with at least one fluorine group, a C3 to C10 cycloalkylene group which is unsubstituted or substituted with at least one fluorine group, a C6 to C20 arylene group which is unsubstituted or substituted with at least one fluorine group, or a combination thereof.
[0077] In some embodiments, R 1 and R 2 may each independently be fluorine, a C1 to C10 alkyl group which is unsubstituted or substituted with at least one fluorine, a C6 to C20 aryl group which is unsubstituted or substituted with at least one fluorine, or a combination thereof, and
[0078] L 1 It may be a C1 to C3 alkylene group which is unsubstituted or substituted with at least one fluorine group.
[0079] For example, the sulfonimide compound may be at least one selected from the compounds listed in Group I.
[0080] Group I
[0081]
[0082] In some embodiments, the metal-containing photoresist developer composition may include about 50 wt % to about 99.99 wt % of an organic solvent and about 0.01 wt % to about 50 wt % of a sulfonimide-based compound.
[0083] Within any of the above ranges, the sulfonimide compound may be included in an amount less than or equal to about 40 wt %, for example less than or equal to about 30 wt %, less than or equal to about 20 wt %, or less than or equal to about 10 wt %.
[0084] In some embodiments, the metal-containing photoresist developer composition may include a sulfonimide compound in an amount of about 0.01 wt % to about 40 wt %, for example, about 0.01 wt % to about 30 wt %, for example, about 0.01 wt % to about 20 wt %, for example, about 0.01 wt % to about 10 wt %.
[0085] Examples of the organic solvent included in the developer composition may include at least one selected from ethers, alcohols, glycol ethers, aromatic hydrocarbon compounds, ketones, and esters, but are not limited thereto. For example, the organic solvent may include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl celulose acetate, ethyl celulose acetate, diethylene glycol methyl ether, diethylene glycol ethyl ether, propylene glycol, propylene glycol methyl ether (PGME), propylene glycol methyl ether acetate (PGMEA), propylene glycol ethyl ether, propylene glycol ethyl ether acetate, propylene glycol propyl ether acetate, propylene glycol butyl ether, propylene glycol butyl ether acetate, ethanol, propanol, isopropyl alcohol, isobutyl alcohol, 4-methyl-2-pentanol (or methyl isobutyl alcohol), methyl ether, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, propylene glycol propyl ether acetate, propylene glycol butyl ether acetate, ethanol, propanol, isopropyl alcohol, isobutyl alcohol, 4-methyl-2-pentanol (or methyl isobutyl alcohol), methyl ether, propylene glycol ethyl ether ...methyl ether acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether, propylene glycol propyl ether acetate, propylene glycol butyl ether acetate, ethanol, propanol, isopropyl alcohol, isobutyl alcohol, 4-methyl-2-pentanol (or carbinol, MIBC)), hexanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, ethylene glycol, propylene glycol, heptanone, propylene carbonate, butylene carbonate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-hydroxyethyl propionate, 2-hydroxy-2-methylethyl propionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutyrate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, γ-butyrolactone, methyl 2-hydroxyisobutyrate, methoxybenzene, n-butyl acetate, 1-methoxy-2-propyl acetate, methoxyethoxypropionate, ethoxyethoxypropionate or a combination thereof, but are not limited thereto.
[0086] Developer compositions according to the present disclosure may be particularly effective or suitable for removing metal-containing resists, such as undesirable metal residues, such as tin-based metal residues.
[0087] If additives to be described in more detail below are included, an organic solvent may be included in a balance other than the components.
[0088] The developer composition may further include at least one additive selected from the group consisting of a surfactant, a dispersant, a moisture absorbent, and a coupling agent.
[0089] Surfactant can be used to improve coating uniformity and improve the wettability of photoresist developer composition.In certain embodiments, surfactant can be sulfate, sulfonate, phosphate, soap, amine salt, quaternary ammonium salt, polyethylene glycol, alkylphenol ethylene oxide adduct, polyol, nitrogen-containing vinyl polymer or its combination, but is not limited to this.For example, surfactant can include alkylbenzene sulfonate, alkylpyridinium salt, polyethylene glycol and / or quaternary ammonium salt.If photoresist developer composition includes surfactant, then with the gross weight of photoresist developer composition, surfactant can be included in the amount of about 0.001 weight % to about 3 weight %.
[0090] The dispersant can be used to uniformly (or substantially uniformly) disperse the components constituting the photoresist developer composition in the photoresist developer composition. In some embodiments, the dispersant can be an epoxy resin, polyvinyl alcohol, polyvinyl butyral, polyvinyl pyrrolidone, glucose, sodium lauryl sulfate, sodium citrate, oleic acid, linoleic acid, or a combination thereof, but is not limited thereto. If the photoresist developer composition includes a dispersant, then the dispersant can be included in an amount of about 0.001 wt % to about 5 wt % based on the total weight of the photoresist developer composition.
[0091] The hygroscopic agent can be used to prevent or reduce the adverse effects caused by moisture in the photoresist developer composition. For example, the hygroscopic agent can be used to prevent or reduce the oxidation of the metal contained in the photoresist developer composition by moisture. In some embodiments, the hygroscopic agent can be polyoxyethylene nonylphenol ether, polyethylene glycol, polypropylene glycol, polyacrylamide or a combination thereof, but is not limited thereto. If the photoresist developer composition includes the hygroscopic agent, the hygroscopic agent can be included in an amount of about 0.001 wt % to about 10 wt % based on the total weight of the photoresist developer composition.
[0092] If the photoresist developer composition is coated on the underlying film, a coupling agent can be used to improve the adhesion to the underlying film. In some embodiments, the coupling agent may include a silane coupling agent. The silane coupling agent may be vinyl trimethoxysilane, vinyl triethoxysilane, vinyl trichlorosilane, vinyl tris (β-methoxyethoxy) silane, 3-methacryloxypropyl trimethoxysilane, 3-acryloxypropyl trimethoxysilane, p-phenylyl trimethoxysilane, 3-methacryloxypropyl methyl dimethoxysilane, 3-methacryloxypropyl methyl diethoxy silane and / or trimethoxy [3- (phenylamino) propyl] silane, but is not limited thereto. If the photoresist developer composition includes a coupling agent, the coupling agent may be included in an amount of about 0.001 wt % to about 5 wt % based on the total weight of the photoresist developer composition.
[0093] The metal-containing resist composition may include a tin compound. For example, the tin compound may be at least one selected from a tin compound containing an organic oxygen group and a tin compound containing an organic carbonyl oxygen group.
[0094] For example, the metal compound contained in the metal-containing resist may be represented by Chemical Formula 3:
[0095] Chemical formula 3
[0096]
[0097] In chemical formula 3,
[0098] R 3 The alkyl radical may be selected from substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, substituted or unsubstituted C6 to C30 arylalkyl, and -L a -OR a (Where L a is a substituted or unsubstituted C1 to C20 alkylene group, and R a is a substituted or unsubstituted C1 to C20 alkyl),
[0099] R 4 to R 6 The alkyl radicals may be each independently selected from substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, substituted or unsubstituted C6 to C30 arylalkyl, -OR b and -OC(=O)R cSelected from
[0100] R b may be a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof,
[0101] R c may be hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof, and
[0102] Since R 4 to R 6 At least one of the selected can be independently selected from -OR b and -OC(=O)R c Selected from.
[0103] For example, R b and R c Each independently may be a substituted or unsubstituted C1 to C20 alkyl group.
[0104] According to some embodiments, the method of forming a pattern includes a step (or action) of developing using the metal-containing photoresist developer composition of the present embodiment. For example, the pattern produced may be a negative-type (or negative-type) photoresist pattern.
[0105] Hereinafter, a pattern forming method according to some embodiments will be explained in more detail using the accompanying drawings as examples.
[0106] According to some embodiments, the method for forming a pattern includes: coating a metal-containing resist composition on a substrate; coating a composition for removing edge beads from the metal-containing resist along the edge of the substrate; drying and heating the resultant to form a metal-containing resist layer on the substrate; exposing the metal-containing resist layer; and coating a developer composition according to the present embodiment and developing the developer composition.
[0107] For example, forming a pattern using a metal-containing resist composition may include coating the metal-containing resist composition on a substrate having a thin film formed thereon by spin coating, slit coating, inkjet printing, etc., and drying the coated metal-containing resist composition to form a resist layer.
[0108] The metal-containing resist composition may include a tin-based compound. For example, the tin-based compound may include at least one selected from a tin compound containing an organic oxygen group and a tin compound containing an organic carbonyl oxygen group.
[0109] Subsequently, a composition for removing edge beads from a metal-containing photoresist may be applied along the edge of the substrate.
[0110] For example, the composition for removing edge beads from a metal-containing resist may be applied in an appropriate or suitable amount along the edge of a substrate, and after the composition for removing edge beads from a metal-containing resist is transferred, the substrate is rotated at an appropriate or suitable set speed (e.g., 1,000 rpm or greater) to remove the beads located on the edge of the substrate.
[0111] Next, a first heat treatment process of heating the substrate on which the metal-containing resist layer is formed is performed. The first heat treatment process may be performed at a temperature of about 80° C. to about 120° C. In this process, the solvent is evaporated and the metal-containing resist layer may be more firmly bonded to the substrate.
[0112] The resist layer is then selectively exposed using the patterned mask.
[0113] For example, examples of light that can be used in the exposure process may include not only light with a short wavelength such as i-line (wavelength 365nm), KrF excimer laser (wavelength 248nm) and / or ArF excimer laser (wavelength 193nm), but also light with a high energy wavelength such as EUV (extreme ultraviolet, wavelength 13.5nm), electron beam (electron beam, E-Beam), etc.
[0114] For example, the light used for exposure according to some embodiments may be short wavelength light having a wavelength range of about 5 nm to about 150 nm, and light having a high energy wavelength such as EUV (extreme ultraviolet light, wavelength 13.5 nm), E-Beam (electron beam), etc.
[0115] In the step of forming a photoresist pattern, a negative type (or negative-like) pattern may be formed.
[0116] The exposed region of the photoresist layer has a solubility different from that of the unexposed region of the photoresist layer because a polymer is formed by a cross-linking reaction (eg, condensation between organometallic compounds).
[0117] Then, a second heat treatment process is performed on the substrate. The second heat treatment process may be performed at a temperature of about 90° C. to about 200° C. By performing the second heat treatment process, the exposed area of the photoresist layer becomes difficult to dissolve in the developer solution.
[0118] For example, a photoresist pattern corresponding to a negative tone image may be completed by dissolving and then removing the photoresist layer corresponding to the unexposed area using the photoresist developer composition according to the present embodiment.
[0119] According to one or more embodiments, a photoresist pattern formed by exposure to light having a short wavelength such as i-line (wavelength of 365 nm), KrF excimer laser (wavelength of 248 nm), and / or ArF excimer laser (wavelength of 193 nm), but also to light having high energy such as EUV (extreme ultraviolet; wavelength of 13.5 nm) and / or E-Beam (electron beam) may have a thickness width (e.g., thickness and / or width) of about 5 nm to about 100 nm. For example, the photoresist pattern may be formed to have a thickness width (e.g., thickness and / or width) of about 5 nm to about 90 nm, about 5 nm to about 80 nm, about 5 nm to about 70 nm, about 5 nm to about 60 nm, about 5 nm to about 50 nm, about 5 nm to about 40 nm, about 5 nm to about 30 nm, or about 5 nm to about 20 nm.
[0120] The photoresist pattern may have a half-pitch pitch of less than or equal to about 50 nm, for example, less than or equal to about 40 nm, for example, less than or equal to about 30 nm, for example, less than or equal to about 20 nm, for example, less than or equal to about 15 nm, and a line width roughness (e.g., line edge roughness (LER)) of less than or equal to about 10 nm, less than or equal to about 5 nm, less than or equal to about 3 nm, or less than or equal to about 2 nm.
[0121] Hereinafter, a method of forming a pattern will be explained in more detail with reference to the accompanying drawings.
[0122] Figures 1 to 3 are cross-sectional views showing a process sequence to explain a method of forming a pattern.
[0123] Reference Figure 1 , the exposed photoresist layer is developed to form a photoresist pattern 130P.
[0124] In one or more embodiments, the exposed photoresist layer may be developed to remove unexposed regions of the photoresist layer, and a photoresist pattern 130P including (or corresponding to) the exposed regions of the photoresist layer may be formed. The photoresist pattern 130P may include a plurality of openings OP.
[0125] In one or more embodiments, the development of the photoresist layer may be performed by a negative-tone development (NTD) process. Herein, the metal-containing photoresist developer composition according to some embodiments may be used as a developer composition.
[0126] Reference Figure 2 , using photoresist pattern 130P to Figure 1 The feature layer 110 in the result is shown to be processed.
[0127] For example, the feature layer 110 may be processed by one or more of the following suitable processes: etching the feature layer 110 exposed through the opening OP of the photoresist pattern 130P, implanting impurity ions into the feature layer 110, forming an additional film on the feature layer 110 through the opening OP, deforming a portion of the feature layer 110 through the opening OP, and / or the like. Figure 2 An exemplary process (eg, method) of processing the feature pattern 110P by etching the feature layer 110 exposed through the opening OP is shown.
[0128] Reference Figure 3 ,exist Figure 2 The result shown is that the photoresist pattern 130P remaining on the feature pattern 110P is removed. To remove the photoresist pattern 130P, an ashing and / or stripping process may be used.
[0129] Hereinafter, the present disclosure will be described in more detail through examples related to the preparation of the metal-containing photoresist developer composition according to the present embodiment. However, the technical features of the present disclosure are not limited by the following examples.
[0130] Preparation of metal-containing photoresist developer composition
[0131] The sulfonimide compound was mixed with an organic solvent in a polypropylene (PP) bottle according to each composition shown in Table 1, and then completely dissolved therein by shaking the bottle at room temperature (25° C.). Subsequently, the resulting solution was passed through a polytetrafluoroethylene (PTFE) filter having a pore size of 1 μm to prepare a developer composition.
[0132] Table 1
[0133]
[0134] PGME: Propylene glycol monomethyl ether
[0135] PGMEA: Propylene glycol monomethyl ether acetate
[0136] MIBC: Methyl isobutyl carbinol
[0137] EL: Ethyl lactate
[0138] GBL: gamma-butyrolactone
[0139] Preparation of metal-containing photoresist compositions
[0140] An organometallic compound having a structure of Chemical Formula C was dissolved in 4-methyl-2-pentanol at a concentration of 1 wt %, and then filtered using a 0.1 μm PTFE syringe filter, thereby preparing a metal-containing photoresist composition.
[0141] Chemical formula C
[0142]
[0143] Evaluation 1: Residual Film Thickness
[0144] 1.0 mL of the photoresist composition containing an organic metal compound according to the preparation example was spin-coated on a 4-inch silicon wafer at a speed of 800 rpm for 30 seconds, and then allowed to stand for 20 seconds. Subsequently, after heat treatment at 100° C. for 60 seconds and then heat treatment at 180° C. for 60 seconds, 10 mL of each developer composition according to Examples 1 to 12 and Comparative Examples 1 to 4 was spin-coated for 60 seconds and then dried while rotating at a speed of 1,500 rpm, and heat treated at 200° C. for 60 seconds, and the thickness of each film thus obtained was measured using ellipsometry to evaluate the remaining film thickness after the development process with reference to the following criteria. The results are shown in Table 2.
[0145] Criteria for evaluating residual film thickness
[0146] *If the residual film thickness is less than 1.0nm: ○
[0147] * Residual film thickness is 1.0nm or more and less than 3nm: △
[0148] * Residual film thickness is 3nm or more: X
[0149] Assessment 2: Defect Assessment
[0150] The prepared organometallic-containing photoresist (PR) composition was spin-coated on an 8-inch wafer at a speed of 1,500 rpm for 30 seconds and heat-treated at 100° C. for 60 seconds, thereby manufacturing a coated wafer.
[0151] The coated wafer was exposed to 20 to 100 mJ of light using a KrF scanner (PAS 5500 / 700D, ASML) in a 180 nm 1:1 line / space pattern, heat treated at 180° C. for 60 seconds, developed by applying each developer composition of Examples 1 to 12 and Comparative Examples 1 to 4, respectively, at a rotation speed of 1500 rpm for 30 seconds, and cured at 240° C. for 60 seconds.
[0152] After the curing process, the obtained pattern wafer on which the line / space CD pattern is formed is transferred to a critical dimension-scanning electron microscope (CD-SEM) measuring equipment to obtain a CD-SEM image.
[0153] Among the CD-SEM images, images with 180 nm spatial CD were selected, and the defect (scum, bridge, pattern collapse) area ratio in the spatial portion was evaluated with reference to the following criteria using Macview (MounTech Co., Ltd.) program, and the results are shown in Table 2.
[0154] Defect Assessment Criteria
[0155] -A: No defects
[0156] -B: less than 10% defects
[0157] -C: Defects are 10% or more
[0158] Table 2
[0159] Evaluation of residual film thickness Defect Assessment Example 1 ○ A Example 2 ○ A Example 3 ○ A Example 4 ○ A Example 5 ○ A Example 6 ○ A Example 7 ○ A Example 8 ○ A Example 9 ○ A Example 10 ○ A Example 11 ○ A Example 12 ○ A Comparative Example 1 X C Comparative Example 2 △ B Comparative Example 3 X C Comparative Example 4 △ B
[0160] Referring to Table 2, when each of the metal-containing photoresist developer compositions of Examples 1 to 12 was applied, as compared to when each of the metal-containing photoresist developer compositions of Comparative Examples 1 to 4 was applied, since defects were minimized or reduced, excellent or improved ability to remove the metal-containing photoresist layer and excellent or improved pattern characteristics were obtained.
[0161] In the above, some embodiments of the present disclosure have been described and illustrated. However, it should be obvious to those skilled in the art that the present disclosure is not limited to the described embodiments, but can be modified and transformed in various appropriate ways without departing from the spirit and scope of the present disclosure. Therefore, the modified and / or transformed embodiments themselves may not be understood separately from the technical ideas and aspects of the present disclosure, and the modified embodiments are within the scope of the claims of the present disclosure and their equivalent forms.
Claims
1. A metal-containing photoresist developer composition comprising: organic solvents; and Sulfonyl imide compounds.
2. The metal-containing photoresist developer composition according to claim 1, wherein The sulfonimide compound is at least one selected from the compounds represented by Chemical Formula 1 and Chemical Formula 2: and Wherein in Chemical Formula 1 and Chemical Formula 2, R 1 and R 2 are each independently fluorine, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C3 to C20 cycloalkenyl, substituted or unsubstituted C3 to C20 cycloalkynyl, substituted or unsubstituted C6 to C20 aryl, substituted or unsubstituted C1 to C20 heteroaryl, or a combination thereof, and L 1 is a substituted or unsubstituted C1 to C10 alkylene group, a substituted or unsubstituted C3 to C20 cycloalkylene group, a substituted or unsubstituted C6 to C20 arylene group, a substituted or unsubstituted C1 to C20 heteroarylene group, or a combination thereof.
3. The metal-containing photoresist developer composition according to claim 1, wherein The sulfonimide compound is at least one selected from the compounds listed in Group I: Group I 4. The metal-containing photoresist developer composition according to claim 1, wherein The acidity coefficient of the sulfonimide compound is less than or equal to 5.
5. The metal-containing photoresist developer composition according to claim 1, comprising: 50 wt % to 99.99 wt % of said organic solvent; and 0.01 wt % to 50 wt % of the sulfonimide compound.
6. The metal-containing photoresist developer composition according to claim 1, The metal-containing photoresist developer composition is used to develop the metal-containing photoresist, and The metal compound contained in the metal-containing photoresist is at least one selected from the group consisting of a tin compound containing an organic oxygen group and a tin compound containing an organic carbonyl oxygen group.
7. The metal-containing photoresist developer composition according to claim 1, The metal-containing photoresist developer composition is used to develop the metal-containing photoresist. The metal-containing photoresist comprises a metal compound represented by Chemical Formula 3: Chemical formula 3 and Wherein in chemical formula 3, R 3 selected from substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, substituted or unsubstituted C6 to C30 arylalkyl, and -L a -OR a Select from among them L a is a substituted or unsubstituted C1 to C20 alkylene group, and R a is a substituted or unsubstituted C1 to C20 alkyl group, R 4 to R 6 each independently selected from substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, substituted or unsubstituted C6 to C30 arylalkyl, -OR b and -OC(=O)R c Selected from R b is a substituted or unsubstituted C1 to C20 alkyl group, a substituted or unsubstituted C3 to C20 cycloalkyl group, a substituted or unsubstituted C2 to C20 alkenyl group, a substituted or unsubstituted C2 to C20 alkynyl group, a substituted or unsubstituted C6 to C30 aryl group, or a combination thereof, R c is hydrogen, substituted or unsubstituted C1 to C20 alkyl, substituted or unsubstituted C3 to C20 cycloalkyl, substituted or unsubstituted C2 to C20 alkenyl, substituted or unsubstituted C2 to C20 alkynyl, substituted or unsubstituted C6 to C30 aryl, or a combination thereof, and Since R 4 to R 6 At least one of the selected from -OR b and -OC(=O)R c Selected from.
8. A method for forming a pattern, the method comprising: coating a metal-containing resist composition on a substrate; applying a composition for removing edge beads from a metal-containing resist along an edge of the substrate; drying and heating the resultant to form a metal-containing resist layer on the substrate; exposing the metal-containing resist layer; as well as The metal-containing photoresist developer composition according to claim 1 is applied, and the metal-containing photoresist developer composition is developed.
Citation Information
Patent Citations
Feeder apparatus for fixed quantity supply of powder
KR1020230068547A