I-shaped magnetic core, mould for processing I-shaped magnetic core and preparation method of I-shaped magnetic core

By designing I-Core core assembly error and instability inductance values ​​with specific angle connections, the assembly efficiency and product yield of inductive magnetic components are improved, and the burr generation is reduced. , ensuring the stability of the inductance value.

CN119028715APending Publication Date: 2024-11-26HENGDIAN GRP DMEGC MAGNETICS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310607870.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The two matching symmetrical arrangements of the existing I-Core cores lead to assembly errors, reducing the assembly efficiency and product yield of inductive magnetic components, and it is impossible to ensure the consistency of the roughness of the upper and lower end surfaces during grinding, resulting in unstable inductance.

Method used

A type I magnetic core is designed, with the connection between the upper end surface and the side end surface at a right angle, and the connection between the lower end surface and the side end surface is a first rounded corner (R0.5mm~R3.0mm), and a specific mold and preparation method are used. Includes hot pressing, sintering, double-end grinding and cleaning steps to ensure the size and surface quality of the core.

Benefits of technology

By distinguishing the two end faces of the magnetic core, the assembly efficiency is improved, the assembly error is reduced, the stability of the inductance value is ensured, and the product yield is improved, while reducing burrs are generated and safety performance is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028715A_ABST
    Figure CN119028715A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of inductor manufacturing, in particular to an I-shaped magnetic core, a mold for machining the I-shaped magnetic core and a preparation method of the I-shaped magnetic core. The I-type magnetic core comprises a body. Wherein the body comprises an upper end face, a lower end face and a side end face, the upper end face and the lower end face are arranged oppositely, one end of the side end face is connected with the upper end face, and the other end of the side end face is connected with the lower end face; the connecting positions of the upper end face and the side end faces are arranged in a right-angle mode, the connecting positions of the lower end face and the side end faces are arranged in a first round corner mode, and the setting range of the first round corner ranges from R0.5 mm to R3.0 mm. Due to the arrangement of the I-shaped magnetic core, the assembly error of the I-shaped magnetic core can be reduced, the assembly efficiency is improved, and the product yield of the inductance magnetic element is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of inductor manufacturing, and in particular to an I-type magnetic core, a mold for processing the I-type magnetic core, and a method for preparing the I-type magnetic core. Background Art

[0002] Inductor magnetic components refer to components such as magnetic cores, wires, and bases that are based on Faraday's law of electromagnetic induction and realize the mutual conversion of electrical energy and magnetic energy. They are mainly used in power supplies and electrical and electronic equipment, and ultimately in downstream industries such as communications, energy, medical care, and automobiles. They are important basic components to ensure the safe and stable operation of electrical and electronic equipment.

[0003] Generally, the magnetic core in the inductive magnetic element can be provided in multiple types, for example, E-Core, PQ-Core, UF-Core, I-Core, etc. In actual use, it is often necessary to pair the mating surfaces of the two magnetic cores, but the two mating surfaces of the I-Core magnetic core in the prior art are symmetrically arranged about the magnetic core. At the same time, in order to reduce the manual flipping process, a double-end grinder is generally used when grinding the upper and lower end surfaces of the magnetic core (that is, a grinding wheel is designed for grinding on the upper and lower end surfaces of the magnetic core). The grinding wheel for grinding the upper surface can adjust the inclination angle of the grinding wheel, while the grinding wheel for grinding the lower surface cannot adjust the inclination angle. This results in that even if the grinding wheel with the same mesh number is used for grinding, the roughness of the upper and lower end surfaces of the magnetic core cannot be guaranteed to be consistent. This is easy to cause pairing errors when assembling the two magnetic cores, thereby reducing the assembly efficiency of the magnetic core, resulting in different inductance values ​​of the inductive magnetic element causing unstable inductance values, and reducing product yield.

[0004] Therefore, it is urgent to design an I-type magnetic core, a mold for processing the I-type magnetic core, and a method for preparing the I-type magnetic core to solve the above technical problems. Summary of the invention

[0005] The first objective of the present invention is to provide an I-type magnetic core, which can reduce the assembly error of the I-type magnetic core, improve the assembly efficiency, and improve the product yield of the inductive magnetic component.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] The present invention provides an I-type magnetic core, comprising:

[0008] The main body comprises an upper end face, a lower end face and a side end face, the upper end face and the lower end face are arranged opposite to each other, one end of the side end face is connected to the upper end face, and the other end of the side end face is connected to the lower end face; and the connection between the upper end face and the side end face is arranged at a right angle, and the connection between the lower end face and the side end face is arranged at a first rounded corner, and the range of the first rounded corner setting is between R0.5mm and R3.0mm.

[0009] As an optional technical solution for an I-type magnetic core, the number of the side end faces is four, and the verticality of two adjacent side end faces is set between 0.07 and 0.09.

[0010] As an optional technical solution for an I-type magnetic core, the perpendicularity between the upper end surface and the side end surface is set to between 0.07 and 0.09.

[0011] As an optional technical solution for an I-type magnetic core, the length of the upper end surface is set to 10mm~65mm with a tolerance of ±0.30mm; the width of the upper end surface is set to 10mm~65mm with a tolerance of ±0.30mm; the width of the side end surface is set to 3mm~20mm with a tolerance of ±0.10mm.

[0012] As an optional technical solution for an I-type magnetic core, the I-type magnetic core is formed by pressing ferrite powder.

[0013] The second purpose of the present invention is to provide a mold for processing an I-type magnetic core, which can reduce the burr generation of the I-type magnetic core, avoid the problem of corner chipping during assembly, and improve safety performance.

[0014] To achieve this object, the present invention adopts the following technical solutions:

[0015] The present invention provides a mold for processing an I-type magnetic core. The mold for processing the I-type magnetic core is used to process and manufacture the I-type magnetic core described above. The mold for processing the I-type magnetic core comprises an upper mold, a concave mold and a lower mold. The concave mold is provided with a groove, and the I-type magnetic core is accommodated in the groove. At least a portion of the upper mold is inserted into the groove, and at least a portion of the lower mold is inserted into the groove, so that the upper mold, the lower mold and the groove can jointly press and form the I-type magnetic core.

[0016] As an optional technical solution for processing a mold for an I-type magnetic core, the groove includes a bottom wall and a side wall, an arc portion and a straight portion are arranged between the bottom wall and the side wall, the arc portion and the straight portion are connected, an end of the arc portion away from the straight portion is connected to the side wall, and an end of the straight portion away from the arc portion is connected to the bottom wall; and the arc portion is arranged with a second rounded angle, the range of the second rounded angle is set to R0.5mm~R5.0mm, and the width of the straight portion is set to 0.2mm~3.0mm.

[0017] The third object of the present invention is to provide a method for preparing an I-type magnetic core, which has simple steps, high processing efficiency and cost savings.

[0018] To achieve this object, the present invention adopts the following technical solutions:

[0019] The present invention provides a method for preparing an I-type magnetic core, the method comprising the steps of:

[0020] Molding: The mold for processing the I-type magnetic core is used to press the I-type magnetic core blank by hot pressing. The molding density of the I-type magnetic core blank is 3.02±0.04g / cm 3 ;

[0021] Sintering: placing the I-type magnetic core blank in a sintering furnace for sintering;

[0022] Grinding: using a double-end surface grinder to grind the sintered I-type magnetic core blank;

[0023] Cleaning: Two cleaning tanks are used for cleaning. The first cleaning tank uses circulating tap water for cleaning, and the second cleaning tank uses deionized water for cleaning. The deionized water is replaced every 8 hours.

[0024] Packaging: The cleaned I-type magnetic core blanks are packaged using an anti-static tray.

[0025] As an optional technical solution for the preparation method of an I-type magnetic core, the forming step includes: marking the upper end surface or the lower end surface of the I-type magnetic core blank to distinguish the grinding surface during subsequent grinding.

[0026] As an optional technical solution for a method for preparing an I-type magnetic core, the grinding step includes: using a grinding wheel to first grind the upper end surface, then grinding the lower end surface, and finally grinding the upper end surface.

[0027] The beneficial effects of the present invention include at least:

[0028] The present invention provides an I-type magnetic core, which includes a body. The body includes an upper end face, a lower end face and a side end face, the upper end face and the lower end face are arranged opposite to each other, one end of the side end face is connected to the upper end face, and the other end of the side end face is connected to the lower end face; and the connection between the upper end face and the side end face is arranged at a right angle, and the connection between the lower end face and the side end face is arranged at a first fillet, and the range of the first fillet setting is between R0.5mm and R3.0mm. By setting the first fillet at the connection between the lower end face and the side end face, and setting the right angle at the connection between the upper end face and the side end face, the two end faces of the I-type magnetic core are distinguished, so that when the operator assembles the I-type magnetic core, the matching surface of the I-type magnetic core can be intuitively and quickly identified by the appearance, thereby improving the efficiency of assembling the I-type magnetic core with other types of magnetic cores, eliminating assembly errors, improving assembly efficiency, making the inductance value of the inductor magnetic element more stable, and improving the product yield of the inductor magnetic element.

[0029] The present invention also provides a mold for processing an I-type magnetic core. The mold for processing the I-type magnetic core can reduce the generation of burrs on the I-type magnetic core, avoid the problem of corner loss during assembly, and improve safety performance.

[0030] The present invention also provides a method for preparing an I-type magnetic core, which has simple steps, high processing efficiency and cost savings. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments of the present invention. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the contents of the embodiments of the present invention and these drawings without paying any creative work.

[0032] Figure 1 This is a schematic structural diagram of an I-type magnetic core provided in Example 1 of the present invention;

[0033] Figure 2 A front view of an I-type magnetic core provided in Example 1 of the present invention;

[0034] Figure 3 for Figure 2 A partial enlarged view of the middle A;

[0035] Figure 4 for Figure 2 A partial enlarged view of point B in the middle;

[0036] Figure 5 A schematic structural diagram of a mold for processing an I-type magnetic core provided in Example 1 of the present invention;

[0037] Figure 6 A front view of the concave mold provided in Example 1 of the present invention;

[0038] Figure 7 A cross-sectional view of the concave die along the CC direction provided by Example 1 of the present invention;

[0039] Figure 8 for Figure 7 A partial enlarged view of point D in the middle.

[0040] Reference numerals

[0041] 100, body; 110, upper end surface; 120, lower end surface; 130, side end surface; 140, first fillet;

[0042] 200, upper die; 300, concave die; 310, groove; 320, bottom wall; 330, side wall; 340, arc portion; 350, straight portion; 400, lower die. DETAILED DESCRIPTION

[0043] In order to make the technical problem solved by the present invention, the technical solution adopted and the technical effect achieved more clearly, the technical solution of the present invention is further explained below with reference to the accompanying drawings and through specific implementation methods.

[0044] In the description of the present invention, unless otherwise clearly specified and limited, the terms "connected", "connected", and "fixed" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0045] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0046] In the description of this embodiment, the terms "upper", "lower", "left", "right" and other directions or positional relationships are based on the directions or positional relationships shown in the drawings, and are only for the convenience of description and simplification of operation, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operate in a specific direction, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used to distinguish in the description and have no special meaning.

[0047] Embodiment 1:

[0048] like Figure 1-Figure 4 As shown, this embodiment provides an I-type magnetic core, which includes a body 100. The body 100 includes an upper end surface 110, a lower end surface 120 and a side end surface 130, the upper end surface 110 and the lower end surface 120 are arranged opposite to each other, one end of the side end surface 130 is connected to the upper end surface 110, and the other end of the side end surface 130 is connected to the lower end surface 120; and the connection between the upper end surface 110 and the side end surface 130 is arranged at a right angle, and the connection between the lower end surface 120 and the side end surface 130 is arranged at a first fillet 140, and the range of the first fillet 140 is between R0.5mm and R3.0mm.

[0049] Based on the above design, in this embodiment, the I-type magnetic core can be formed by pressing ferrite powder, and the I-type magnetic core is in a rectangular shape. Specifically, the I-type magnetic core has four side end faces 130, and the verticality of two adjacent side end faces 130 is set to between 0.07 and 0.09, and optionally, the verticality of two adjacent side end faces 130 is set to 0.08; the verticality between the upper end face 110 and the side end face 130 is set to between 0.07 and 0.09, and optionally, the verticality between the upper end face 110 and the side end face 130 is set to 0.08. By setting a first fillet 140 at the connection between the lower end face 120 and the side end face 130, and setting a right angle at the connection between the upper end face 110 and the side end face 130, the two end faces of the I-type magnetic core are distinguished, so that when the operator assembles the I-type magnetic core, the matching surface of the I-type magnetic core can be intuitively and quickly identified by appearance, thereby improving the efficiency of assembling the I-type magnetic core with other types of magnetic cores, eliminating assembly errors, improving assembly efficiency, making the inductance value of the inductive magnetic element more stable, and improving the product yield of the inductive magnetic element.

[0050] Optionally, the length of the upper end surface 110 of the I-type magnetic core in this embodiment is set to 10mm-65mm, with a tolerance of ±0.30mm; the width of the upper end surface 110 is set to 10mm-65mm, with a tolerance of ±0.30mm; the width of the side end surface 130 is set to 3mm-20mm, with a tolerance of ±0.10mm. Of course, the operator can also set the I-type magnetic core to other sizes according to actual needs, which will not be repeated here.

[0051] like Figure 5-Figure 8 As shown, this embodiment also provides a mold for processing an I-type magnetic core, and the mold for processing an I-type magnetic core is used to process and manufacture the above I-type magnetic core. The mold for processing an I-type magnetic core includes an upper mold 200, a concave mold 300 and a lower mold 400, and a groove 310 is opened on the concave mold 300. The I-type magnetic core is accommodated in the groove 310, at least part of the upper mold 200 is penetrated in the groove 310, and at least part of the lower mold 400 is penetrated in the groove 310, so that the upper mold 200, the lower mold 400 and the groove 310 are pressed together to form the I-type magnetic core.

[0052] Specifically, if Figure 7-Figure 8As shown, the groove 310 includes a bottom wall 320 and a side wall 330, and an arc portion 340 and a straight portion 350 are arranged between the bottom wall 320 and the side wall 330, the arc portion 340 and the straight portion 350 are connected, and the end of the arc portion 340 away from the straight portion 350 is connected to the side wall 330, and the end of the straight portion 350 away from the arc portion 340 is connected to the bottom wall 320; and the arc portion 340 is set with a second fillet, the range of the second fillet is set to R0.5mm~R5.0mm, and the width of the straight portion 350 is set to 0.2mm~3.0mm. Since the body 100 will shrink and deform during the subsequent sintering process, in this embodiment, the second fillet range of the arc portion 340 is greater than the first fillet 140 range at the connection between the lower end face 120 and the side end face 130, so that the size of the manufactured I-type magnetic core can meet the requirements. Optionally, the shrinkage ratio of the mold for processing the I-type magnetic core is set to 1.175, that is, the volume of the groove 310 in the mold for processing the I-type magnetic core is 1.175 times that of the finished I-type magnetic core, thereby ensuring that the size of the finished I-type magnetic core meets the requirements.

[0053] When the second fillet R of the arc portion 340 is less than 0.5, it will be ground off and the R angle will not exist; when the R angle is greater than 5.0, there will be demoulding problems and it will be difficult to demould. Therefore, in this embodiment, the second fillet range of the arc portion 340 is set to R0.5mm~R5.0mm, for example, it can be set to R0.5mm, R1.0mm, R2.0mm, R3.0mm, R4.0mm, R5.0mm and other values. When the width of the straight portion 350 is less than 0.2mm, it will leak and get stuck in the mold; when the width of the straight portion 350 is greater than 3.0mm, there will be demoulding problems and it will be difficult to demould. Therefore, in this embodiment, the width of the straight portion 350 is set to 0.2mm~3.0mm, for example, it can be set to 0.2mm, 1.0mm, 2.0mm, 2.5mm, 3.0mm and other values.

[0054] Optionally, in this embodiment, the grinding amount of the molding surface of the lower mold 400 is set to 0.3 mm to 1.0 mm. A grinding amount less than 0.3 mm will result in missed grinding, and a grinding amount greater than 1.0 mm will result in waste.

[0055] Optionally, in this embodiment, a mark is set on the molding surface of the upper mold 200, which may be a mark such as "△", "*", "text", "number", etc., which is mainly used to distinguish the grinding surface during grinding. In this way, the upper end surface 110 can be marked during the pressing process, which is beneficial to improve the assembly efficiency during the subsequent assembly of the I-type magnetic core.

[0056] In this embodiment, the first fillet 140 is set inside the groove 310 on the die 300 (without a mold joint seam) to achieve the effect of having a product with a first fillet 140 and no burrs, thereby achieving the effect of reducing the product collision and corner chipping; one side of the product has the first fillet 140, and the other side does not have the first fillet 140, and the 3D features are used to distinguish which is the mating surface, thereby avoiding the inductance difference when different surfaces are paired with E-Core or U-Core. The mold for processing the I-type magnetic core in this embodiment can reduce the burrs of the I-type magnetic core, avoid the problem of corner chipping during assembly, and improve safety performance.

[0057] This embodiment also provides a method for preparing an I-type magnetic core, which has simple steps, high processing efficiency, and cost savings. The method for preparing an I-type magnetic core includes the following steps:

[0058] Molding: Use the mold for processing I-type magnetic core to press into I-type magnetic core blank by hot pressing. The molding density of I-type magnetic core blank is 3.02±0.04g / cm 3 According to 4.85±0.04g / cm 3 Sintering density, molding density <2.98g / cm 3 The size of the I-type magnetic core blank will exceed the lower limit, and the molding density will be greater than 3.06g / cm 3 The problem of the size of the I-type magnetic core blank exceeding the upper limit may occur, resulting in the size of the I-type magnetic core blank not meeting the requirements. At the same time, the upper end surface 110 or the lower end surface 120 of the I-type magnetic core blank is marked to distinguish the grinding surface during subsequent grinding. For example, the upper end surface 110 of the I-type magnetic core blank can be marked by the upper mold 200.

[0059] Sintering: Place the I-type magnetic core blank in a sintering furnace for sintering. Specifically, place the I-type magnetic core blank in an environment with a certain temperature and a certain oxygen concentration for sintering. The operator can set the corresponding sintering curve according to the specific magnetic properties. The marked surface contacts the setter plate to ensure the perpendicularity of the ground surface to the other surfaces.

[0060] Grinding: A double-end grinder is used to grind the sintered I-type magnetic core blank. Specifically, a grinding wheel is used to grind the upper end face 110 first, then the lower end face 120, and finally the upper end face 110. Grinding is performed through three process stages to ensure the verticality of the upper end face 110 and the side end face 130, as well as the verticality of the lower end face 120 and the side end face 130. During the third grinding, the operator can select a grinding wheel with a corresponding mesh size according to the inductance requirements.

[0061] Cleaning: Two cleaning tanks are used for cleaning. The first cleaning tank uses circulating tap water for cleaning, and the second cleaning tank uses deionized water for cleaning. The deionized water is replaced every 8 hours.

[0062] Packaging: Use anti-static trays to package the cleaned I-type magnetic core blanks. The cleanliness of the trays must be free of metal particles larger than 200μm, non-metal particles larger than 600μm, and fibers larger than 1200μm.

[0063]

[0064] For this embodiment 1: when designing the mold, the second fillet of the arc portion 340 in the concave mold 300 is set to R1.0mm, and the connecting portion is 0.5mm; the grinding amount is designed to be 0.6mm; the upper mold 200 is marked with "△". During molding, the total height of the I-type magnetic core blank is 5.52±0.10mm, and the molding density is measured to be 3.05g / cm 3 . Place the surface without the "△" mark upwards in a sintering furnace at a certain temperature and oxygen for sintering. After sintering, grind in the order of "△", no mark, and "△". The ground product is cleaned in a two-stage cleaning machine, where the first stage is tap water that is continuously injected and discharged; the second stage is circulating deionized water, and the deionized water is replaced every 8 hours. Finally, use a tray that meets the tray cleanliness requirements for packaging.

[0065] When the product of Example 1 was tested for size, the length, width and height all met the requirements, the verticality of the two adjacent side end faces 130 was 0.06, the verticality between the upper end face 110 and the side end face 130 was 0.04, and the cleanliness was Pass, with no burrs or missing grinding. One side of the I-Core had a first fillet 140 of R0.5mm, and when used with the E-Core, the side without the first fillet 140R could be identified by naked eyes for pairing.

[0066] Other examples and comparative examples are shown in Table 1 and Table 2 below:

[0067] Table 1

[0068]

[0069]

[0070] Table 2

[0071]

[0072]

[0073] Obviously, the above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments herein, and that various obvious changes, readjustments and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention has been described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other equivalent embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.

[0074] Note that in the description of this specification, the description with reference to the terms "some embodiments", "other embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

Claims

1. I-type magnetic core, characterized in that, include: The main body (100) comprises an upper end surface (110), a lower end surface (120) and a side end surface (130); the upper end surface (110) and the lower end surface (120) are arranged opposite to each other; one end of the side end surface (130) is connected to the upper end surface (110), and the other end of the side end surface (130) is connected to the lower end surface (120); and the connection between the upper end surface (110) and the side end surface (130) is arranged at a right angle, and the connection between the lower end surface (120) and the side end surface (130) is arranged at a first rounded corner (140), and the setting range of the first rounded corner (140) is between R0.5mm and R3.0mm.

2. The I-type magnetic core according to claim 1, characterized in that: The number of the side end surfaces (130) is four, and the verticality of two adjacent side end surfaces (130) is set between 0.07 and 0.

09.

3. The I-type magnetic core according to claim 1, characterized in that: The verticality between the upper end surface (110) and the side end surface (130) is set to be between 0.07 and 0.

09.

4. The I-type magnetic core according to claim 1, characterized in that: The length of the upper end surface (110) is set to 10 mm to 65 mm, with a tolerance of ±0.30 mm; the width of the upper end surface (110) is set to 10 mm to 65 mm, with a tolerance of ±0.30 mm; and the width of the side end surface (130) is set to 3 mm to 20 mm, with a tolerance of ±0.10 mm.

5. The I-type magnetic core according to any one of claims 1 to 4, characterized in that: The I-type magnetic core is formed by pressing ferrite powder.

6. A mold for processing an I-type magnetic core, characterized in that: The mold for processing the I-type magnetic core is used for processing and manufacturing the I-type magnetic core described in any one of claims 1 to 5, and the mold for processing the I-type magnetic core comprises an upper mold (200), a concave mold (300) and a lower mold (400), the concave mold (300) is provided with a groove (310), the I-type magnetic core is accommodated in the groove (310), at least a portion of the upper mold (200) is inserted into the groove (310), and at least a portion of the lower mold (400) is inserted into the groove (310), so that the upper mold (200), the lower mold (400) and the groove (310) jointly press and form the I-type magnetic core.

7. The mold for processing an I-type magnetic core according to claim 6, characterized in that: The groove (310) comprises a bottom wall (320) and a side wall (330), an arc portion (340) and a straight portion (350) are arranged between the bottom wall (320) and the side wall (330), the arc portion (340) and the straight portion (350) are connected, one end of the arc portion (340) away from the straight portion (350) is connected to the side wall (330), and one end of the straight portion (350) away from the arc portion (340) is connected to the bottom wall (320); and the arc portion (340) is arranged to have a second rounded angle, the range of the second rounded angle is set to R0.5mm~R5.0mm, and the width of the straight portion (350) is set to 0.2mm~3.0mm.

8. A method for preparing a type I magnetic core, characterized in that: The I-type magnetic core preparation method comprises the steps of: Molding: The mold for processing the I-type magnetic core is used to press the I-type magnetic core blank by hot pressing. The molding density of the I-type magnetic core blank is 3.02±0.04g / cm 3 ; Sintering: placing the I-type magnetic core blank in a sintering furnace for sintering; Grinding: using a double-end surface grinder to grind the sintered I-type magnetic core blank; Cleaning: Two cleaning tanks are used for cleaning. The first cleaning tank uses circulating tap water for cleaning, and the second cleaning tank uses deionized water for cleaning. The deionized water is replaced every 8 hours. Packaging: The cleaned I-type magnetic core blanks are packaged using an anti-static tray.

9. The method for preparing an I-type magnetic core according to claim 8, characterized in that: The forming step comprises: marking the upper end surface (110) or the lower end surface (120) of the I-type magnetic core blank to distinguish the grinding surface during subsequent grinding.

10. The method for preparing an I-type magnetic core according to claim 8, characterized in that: The grinding step comprises: using a grinding wheel to first grind the upper end surface (110), then grinding the lower end surface (120), and finally grinding the upper end surface (110) again.