Semiconductor device manufacturing method and semiconductor device manufactured using the same
By using sputtering process to form a seed crystal film containing manganese in the trench of the semiconductor device, and by forming the etching and filling film, the problems of pad misalignment and reliability are solved, and the pad bonding performance of the semiconductor device is improved. reliability.
Patent Information
- Application Number
- CN202410436991.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-24
- Filing Date
- 2024-04-11
- Publication Date
- 2024-11-26
AI Technical Summary
As the size of the semiconductor device pads decreases, the misalignment problem of the pads during the bonding process increases, resulting in limited pad reliability and a need to improve semiconductor device manufacturing technology.
The first and second seed films are formed in the lower groove and the upper groove using a sputtering process and a second seed film is formed thereon, including manganese (Mn) to form an improved lower pad pattern and upper soldering The disk pattern is used and the bonding performance of the pad is improved by etching and forming of the fill film.
The pad bonding performance and reliability of semiconductor devices are improved, the pad bonding performance and reliability are ensured, and the bonding force between the lower pad and the upper pad is enhanced.
Smart Images

Figure CN119028996A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the priority of Korean Patent Application No. 10-2023-0066816 filed in the Korean Intellectual Property Office on May 24, 2023, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0003] The present disclosure relates generally to semiconductor devices, and more particularly, to a semiconductor device manufacturing method and a semiconductor device manufactured using the semiconductor device manufacturing method. Background Art
[0004] As electronic products can be reduced in size and / or can be miniaturized, the use of semiconductor devices that bond and electrically connect an upper pad of an upper chip and a lower pad of a lower chip can increase. However, as the size of the lower pad of the lower chip and / or the upper pad of the upper chip can be gradually reduced, misalignment of the pads during the bonding process may increase.
[0005] Because the demand for smaller pad sizes may be limited by pad misalignment and / or reliability of related semiconductor device manufacturing methods, there exists a need for further improvements in semiconductor device manufacturing techniques. Improvements are presented herein. Summary of the invention
[0006] Aspects of the present disclosure provide a method for manufacturing a semiconductor device having improved performance and reliability compared to related semiconductor device manufacturing methods.
[0007] Aspects of the present disclosure provide a semiconductor device having improved performance and reliability compared to related semiconductor devices.
[0008] According to one aspect of the present disclosure, a method for manufacturing a semiconductor device is provided. The method for manufacturing a semiconductor device includes: forming a lower chip and an upper chip; and bonding the lower chip and the upper chip to each other. Forming the lower chip includes: providing a lower substrate; sequentially forming a lower interlayer insulating film and a pre-lower adhesive film on the lower substrate; etching a first portion of the pre-lower adhesive film and a second portion of the lower interlayer insulating film to form a lower groove; forming a first lower seed film in the lower groove using a sputtering process; and forming a second lower seed film on the first lower seed film using a sputtering process. Forming the upper chip includes: providing an upper substrate; sequentially forming an upper interlayer insulating film and a pre-upper adhesive film on the upper substrate; etching a third portion of the pre-upper adhesive film and a fourth portion of the upper interlayer insulating film to form an upper groove; forming a first upper seed film in the upper groove using a sputtering process; and forming a second upper seed film on the first upper seed film using a sputtering process. The second lower seed film and the second upper seed film include manganese (Mn).
[0009] According to one aspect of the present disclosure, a semiconductor device manufacturing method is provided. The semiconductor device manufacturing method includes: forming a lower pad pattern and an upper pad pattern; and joining the lower pad pattern and the upper pad pattern to each other. Forming the lower pad pattern includes: providing a lower interlayer insulating film; etching a first portion of the lower interlayer insulating film to form a lower groove; forming a first lower seed film in the lower groove using a sputtering process; and forming a second lower seed film on the first lower seed film using a sputtering process. Forming the upper pad pattern includes: providing an upper interlayer insulating film; etching a second portion of the upper interlayer insulating film to form an upper groove; forming a pre-upper barrier film along the bottom surface and one or more sidewalls of the upper groove in the upper groove; forming a first upper seed film on the pre-upper barrier film using a sputtering process; forming a pre-upper fill film on the first upper seed film; etching a third portion of the pre-upper fill film to form a groove; and forming a second upper seed film in the groove using a sputtering process. The second lower seed film and the second upper seed film include manganese (Mn).
[0010] According to one aspect of the present disclosure, a semiconductor device is provided. The semiconductor device includes: a substrate including a first side and a second side opposite to each other; a plurality of unit pixels in the substrate and including a photoelectric conversion layer; a pixel isolation pattern in the substrate and configured to separate the plurality of unit pixels; a first inter-wiring insulating film on the first side of the substrate; a first pad pattern in the first inter-wiring insulating film; a first adhesive film extending along the lower surface of the first inter-wiring insulating film; a second inter-wiring insulating film disposed on the lower surface of the first inter-wiring insulating film; a second pad pattern disposed in the second inter-wiring insulating film and in contact with the first pad pattern; a second adhesive film disposed along the upper surface of the second inter-wiring insulating film and in contact with the first adhesive film; and a microlens on the second side of the substrate. The first pad pattern includes a first portion in contact with the second pad pattern and a second portion on the first portion. The second pad pattern includes a third portion in contact with the first pad pattern and a fourth portion below the third portion. The first concentration of manganese (Mn) of the first portion of the first pad pattern is greater than the second concentration of manganese (Mn) of the second portion of the first pad pattern. A third concentration of manganese (Mn) of the third portion of the second pad pattern is greater than a fourth concentration of manganese (Mn) of the fourth portion of the second pad pattern.
[0011] Additional aspects may be set forth in part in the description which follows and, in part, may be obvious from the description which follows, and / or may be learned by practice of the presented embodiments.
[0012] According to one aspect of the present disclosure, a method for manufacturing a semiconductor device is provided. The method for manufacturing a semiconductor device includes: forming a lower chip and an upper chip; and bonding the lower chip and the upper chip to each other. Forming the lower chip includes: providing a lower substrate; sequentially forming a lower interlayer insulating film and a pre-lower adhesive film on the lower substrate; etching a first portion of the pre-lower adhesive film and a second portion of the lower interlayer insulating film to form a lower groove; forming a first lower seed film in the lower groove using a sputtering process; and forming a second lower seed film on the first lower seed film using a sputtering process. Forming the upper chip includes: providing an upper substrate; sequentially forming an upper interlayer insulating film and a pre-upper adhesive film on the upper substrate; etching a third portion of the pre-upper adhesive film and a fourth portion of the upper interlayer insulating film to form an upper groove; forming a first upper seed film in the upper groove using a sputtering process; and forming a second upper seed film on the first upper seed film using a sputtering process. The second lower seed film and the second upper seed film include manganese (Mn).
[0013] According to one aspect of the present disclosure, a semiconductor device manufacturing method is provided. The semiconductor device manufacturing method includes: forming a lower pad pattern and an upper pad pattern; and joining the lower pad pattern and the upper pad pattern to each other. Forming the lower pad pattern includes: providing a lower interlayer insulating film; etching a first portion of the lower interlayer insulating film to form a lower groove; forming a first lower seed film in the lower groove using a sputtering process; and forming a second lower seed film on the first lower seed film using a sputtering process. Forming the upper pad pattern includes: providing an upper interlayer insulating film; etching a second portion of the upper interlayer insulating film to form an upper groove; forming a pre-upper barrier film along the bottom surface and one or more sidewalls of the upper groove in the upper groove; forming a first upper seed film on the pre-upper barrier film using a sputtering process; forming a pre-upper fill film on the first upper seed film; etching a third portion of the pre-upper fill film to form a groove; and forming a second upper seed film in the groove using a sputtering process. The second lower seed film and the second upper seed film include manganese (Mn).
[0014] According to one aspect of the present disclosure, a semiconductor device is provided. The semiconductor device includes: a substrate including a first side and a second side opposite to each other; a plurality of unit pixels in the substrate and including a photoelectric conversion layer; a pixel isolation pattern in the substrate and configured to separate the plurality of unit pixels; a first inter-wiring insulating film on the first side of the substrate; a first pad pattern in the first inter-wiring insulating film; a first adhesive film extending along the lower surface of the first inter-wiring insulating film; a second inter-wiring insulating film disposed on the lower surface of the first inter-wiring insulating film; a second pad pattern disposed in the second inter-wiring insulating film and in contact with the first pad pattern; a second adhesive film disposed along the upper surface of the second inter-wiring insulating film and in contact with the first adhesive film; and a microlens on the second side of the substrate. The first pad pattern includes a first portion in contact with the second pad pattern and a second portion on the first portion. The second pad pattern includes a third portion in contact with the first pad pattern and a fourth portion below the third portion. The first concentration of manganese (Mn) of the first portion of the first pad pattern is greater than the second concentration of manganese (Mn) of the second portion of the first pad pattern. A third concentration of manganese (Mn) of the third portion of the second pad pattern is greater than a fourth concentration of manganese (Mn) of the fourth portion of the second pad pattern.
[0015] Additional aspects may be set forth in part in the description which follows and, in part, may be obvious from the description which follows, and / or may be learned by practice of the presented embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The above and other aspects, features and advantages of certain embodiments of the present disclosure may be more apparent from the following description in conjunction with the accompanying drawings, in which:
[0017] Figures 1 to 5 An exemplary method for manufacturing a semiconductor device according to some embodiments is shown;
[0018] Figure 6 and Figure 7 depicts an exemplary semiconductor device according to some embodiments;
[0019] Figures 8 to 13 An exemplary method for manufacturing a semiconductor device according to some embodiments is shown;
[0020] Fig.14 is a diagram depicting a semiconductor device according to some embodiments;
[0021] Figures 15 to 17 An exemplary semiconductor device according to some embodiments is shown; and
[0022] Figures 18 to 20 An example of a semiconductor device according to some embodiments is depicted. DETAILED DESCRIPTION
[0023] The following description with reference to the accompanying drawings is provided to assist in a comprehensive understanding of the embodiments of the present disclosure as defined by the claims and their equivalents. Various specific details are included to assist in understanding, but these details are considered to be exemplary only. Therefore, it will be appreciated by those of ordinary skill in the art that various changes and modifications may be made to the embodiments described herein without departing from the scope and spirit of the present disclosure. In addition, descriptions of well-known functions and structures have been omitted for clarity and brevity.
[0024] In the description of the accompanying drawings, similar reference numerals may be used to refer to similar or related elements. It should be understood that the singular form of the noun corresponding to the project may include one or more things, unless the relevant context clearly indicates otherwise. As used herein, each phrase such as "A or B", "at least one of A and B", "at least one of A or B", "A, B or C", "at least one of A, B and C" and "at least one of A, B or C" may include any one or all possible combinations of the items listed together in a corresponding phrase. As used herein, terms such as "1st" and "2nd" or "first" and "second" may be used to simply distinguish the corresponding component from other components, and do not limit the component in other aspects (e.g., importance or order). It should be understood that if the term "operably" or "communicatively" is used to mention that an element (e.g., a first element) is "coupled", "coupled to" another element, "connected" or "connected to" another element with another element using or without the term "operably" or "communicatively", it means that the element can be directly (e.g., wired), wirelessly or via a third element coupled to the other element.
[0025] It should be understood that when an element or layer is referred to as being "above", "over", "up", "below", "under", "below", "connected to" or "coupled to" another element or layer, it can be directly above, over, over, under, under, under, directly connected to or coupled to the other element or layer, or there may be intervening elements or layers. Conversely, when an element is referred to as being "directly above", "over", "up", "below", "under", "under", "directly connected to" or "directly coupled to" another element or layer, there are no intervening elements or layers.
[0026] The terms "upper", "middle", "lower", etc. may be replaced with terms such as "first", "second", "third", etc. to describe the relative position of an element. The terms "first", "second", "third", etc. may be used to describe various elements, but the elements are not limited by these terms, and the "first element" may be referred to as the "second element". Alternatively or additionally, the terms "first", "second", "third", etc. may be used to distinguish components from each other and do not limit the present disclosure. For example, the terms "first", "second", "third", etc. may not necessarily refer to any form of order or numerical meaning.
[0027] References throughout this disclosure to "one embodiment," "an embodiment," "an example embodiment," or similar language may indicate that a particular feature, structure, or characteristic described in connection with the indicated embodiment is included in at least one embodiment of the present solution. Thus, throughout this disclosure, the phrases "in one embodiment," "in an embodiment," "in an example embodiment," and similar language may, but do not necessarily, all refer to the same embodiment.
[0028] The embodiments herein may be described and illustrated in terms of blocks that perform one or more functions described as shown in the accompanying drawings. These blocks (which may be referred to herein as units or modules, etc., or names such as devices, logic, circuits, counters, comparators, generators, converters, etc.) may be physically implemented by analog and / or digital circuits (including one or more of logic gates, integrated circuits, microprocessors, microcontrollers, memory circuits, passive electronic components, active electronic components, optical components, etc.), and may also be implemented or driven by software and / or firmware (configured to perform the functions or operations described herein).
[0029] As used herein, the term "Al 2 O 3 ”, “CuMn”, “GaAs”, “GaSb”, “HfO 2 ”, “InAs”, “InP”, “InSb”, “MoS 2 ”, “MoSe 2 ”, “NbN”, “NiB”, “PbTe”, “SiCN”, “SiN”, “SiO”, “SiO x N y ”, “TaN”, “TaO”, “TiN”, “TiSiN”, “VN”, “WCN”, “WN”, “WS 2 "WSe 2 ,” “ZrN,” etc., each of which may refer to a material made of elements included in each of these terms, rather than a chemical formula expressing a stoichiometric relationship.
[0030] Hereinafter, various embodiments of the present disclosure are described with reference to the accompanying drawings.
[0031] Figures 1 to 5 An exemplary method for manufacturing a semiconductor device according to some embodiments is shown. According to some embodiments, the method for manufacturing a semiconductor device may include forming a lower chip, forming an upper chip, and bonding the lower chip and the upper chip to each other.
[0032] Figure 1 and Figure 2 An exemplary process for forming the lower chip is shown. Figure 3 and Figure 4 An exemplary process for forming the upper chip is shown. Figure 5 A semiconductor device in which a lower chip and an upper chip are bonded is shown.
[0033] Reference Figure 1 , forming the lower chip may include providing a lower substrate 11 .
[0034] The lower substrate 11 may be and / or may include a silicon substrate and / or silicon on insulator (SOI). Alternatively or additionally, the lower substrate 11 may include but may not be limited to silicon-germanium, silicon-germanium on insulator (SGOI), indium antimonide (InSb), lead telluride (PbTe), indium arsenide (InAs), indium phosphide (InP), gallium arsenide (GaAs) and gallium antimonide (GaSb).
[0035] The lower interlayer insulating film 12 may be formed on the lower substrate 11. The lower interlayer insulating film 12 may include, for example, silicon oxide (SiO), silicon nitride (SiN), silicon oxynitride (SiO x N y ) and at least one of a low dielectric constant material. The low dielectric constant material may include, for example, but may not be limited to, tetraethyl fluoride orthosilicate (FTEOS), hydrogen silsesquioxane (HSQ), bisbenzocyclobutene (BCB), tetramethyl orthosilicate (TMOS), octamethylchlorotetrasiloxane (OMCTS), hexamethyldisiloxane (HMDS), trimethylsilyl borate (TMSB), diacetoxydi-tert-butylsiloxane (DADBS), trimethylsilyl phosphate (TMSP), polytetrafluoroethylene (PTFE), Tonran silazane (TOSZ), fluorosilicate glass (FSG), polyimide nanofoam (such as polypropylene oxide), carbon-doped silicon oxide (CDO), organosilicate glass (OSG), SiLK TM , amorphous fluorinated carbon, silica aerogel, silica xerogel, mesoporous silica and / or combinations thereof.
[0036] The pre-lower adhesive film 13p may be formed on the lower interlayer insulating film 12. The lower interlayer insulating film 12 may be disposed between the pre-lower adhesive film 13p and the lower substrate 11. The pre-lower adhesive film 13p may be formed of an insulating material. For example, the pre-lower adhesive film 13p may include, but may not be limited to, silicon carbon nitride (SiCN).
[0037] In some embodiments, a lower groove 10t may be formed. For example, the lower groove 10t may be formed by partially etching the pre-lower adhesive film 13p and the lower interlayer insulating film 12. As an example, relative to the upper surface of the lower substrate 11, the bottom surface of the lower groove 10t may be placed at a height lower than the bottom surface of the pre-lower adhesive film 13p. That is, the vertical distance from the upper surface of the lower substrate 11 to the bottom surface of the lower groove 10t may be shorter than the vertical distance from the upper surface of the lower substrate 11 to the bottom surface of the pre-lower adhesive film 13p. However, the present disclosure may not be limited thereto.
[0038] In some embodiments, a pre-lower barrier film 14p may be subsequently formed. For example, the pre-lower barrier film 14p may be formed along the upper surface of the pre-lower adhesive film 13p, the sidewall of the lower trench 10t, and the bottom surface of the lower trench 10t. The pre-lower barrier film 14p may include, for example, tantalum (Ta), tantalum nitride (TaN), titanium (Ti), titanium nitride (TiN), titanium silicon nitride (TiSiN), ruthenium (Ru), cobalt (Co), nickel (Ni), nickel boron (NiB), tungsten (W), tungsten nitride (WN), tungsten carbonitride (WCN), zirconium (Zr), zirconium nitride (ZrN), vanadium (V), vanadium nitride (VN), niobium (Nb), niobium nitride (NbN), platinum (Pt), iridium (Ir), rhodium (Rh), and at least one of a two-dimensional (2D) material. In some embodiments, the 2D material may be and / or may include a metal material and / or a semiconductor material. For example, the 2D material may be and / or may include a 2D allotrope and / or a 2D compound. Alternatively or additionally, the 2D material may include but may not be limited to graphene, molybdenum disulfide (MoS 2 ), Molybdenum diselenide (MoSe 2 ), tungsten diselenide (WSe 2 ) and tungsten disulfide (WS 2 That is, the present disclosure may not be limited thereto, and the 2D material may include additional materials not listed above.
[0039] In some embodiments, the first lower seed film 15p may be formed on the pre-lower barrier film 14p. For example, the first lower seed film 15p may be formed using a sputtering process. Therefore, the grain size of the first lower seed film 15p may be smaller than the grain size of a film formed using another process different from the sputtering process. For example, as described below, the grain size of the first lower seed film 15p may be smaller than the grain size of the lower sacrificial film 17.
[0040] The first lower seed crystal film 15p may be formed non-conformally. For example, the thickness of the first lower seed crystal film 15p formed along the sidewall of the lower trench 10t and the thickness of the first lower seed crystal film 15p formed along the bottom surface of the lower trench 10t may be different from each other. However, the present disclosure may not be limited to this. In some embodiments, the first lower seed crystal film 15p may include a conductive material. For example, the first lower seed crystal film 15p may include but may not be limited to copper (Cu).
[0041] In some embodiments, the second lower seed crystal film 16p may be formed on the first lower seed crystal film 15p. The first lower seed crystal film 15p and the second lower seed crystal film 16p may contact each other. The second lower seed crystal film 16p may be formed using a sputtering process. The second lower seed crystal film 16p may be formed non-conformally. For example, the thickness of the second lower seed crystal film 16p formed along the sidewall of the lower trench 10t and the thickness of the second lower seed crystal film 16p formed along the bottom surface of the lower trench 10t may be different from each other. However, the present disclosure may not be limited to this. The second lower seed crystal film 16p may include a conductive material. For example, the second lower seed crystal film 16p may include but may not be limited to manganese (Mn). As another example, the second lower seed crystal film 16p may include but may not be limited to copper manganese (CuMn).
[0042] In some embodiments, the lower sacrificial film 17 may be formed on the second lower seed film 16p. The lower sacrificial film 17 may be formed by an electroplating process. As a result of forming the lower sacrificial film 17 using the electroplating process, the upper surface of the lower sacrificial film 17 may be a convex curved surface. Alternatively or additionally, since the lower sacrificial film 17 may be formed using the electroplating process, the grain size of the lower sacrificial film 17 may be smaller than the grain size of the first lower seed film 15p. According to some embodiments, the lower sacrificial film 17 may include, but may not be limited to, copper (Cu).
[0043] In some embodiments, the lower sacrificial film 17 may be formed, and / or a heat treatment process may be performed. For example, the heat treatment process may be performed at a temperature higher than 100° C. and / or lower than 200° C. As a result of performing the heat treatment process at a temperature lower than 200° C., manganese (Mn) contained in the second lower seed film 16 p may not diffuse into the first lower seed film 15 p and / or the lower sacrificial film 17 .
[0044] Reference Figure 2 , a lower pad pattern PP_L may be formed. The lower pad pattern PP_L may be disposed inside the lower trench 10t. The lower pad pattern PP_L may be formed by etching the lower sacrificial film 17, the second lower seed film 16p, the first lower seed film 15p, the pre-lower barrier film 14p, and the pre-lower adhesive film 13p. The lower pad pattern PP_L may be formed using a chemical / mechanical polishing (CMP) process.
[0045] The lower adhesive film 13 may be formed by etching the pre-lower adhesive film 13p. The thickness of the pre-lower adhesive film 13p in the vertical direction may be greater than the thickness of the lower adhesive film 13 in the vertical direction. That is, the vertical direction may be the thickness direction of the lower substrate 11. Alternatively, the vertical direction may be a direction perpendicular to the upper side of the lower substrate 11. The lower adhesive film 13 may include, for example, but may not be limited to, silicon carbon nitride (SiCN).
[0046] In some embodiments, the lower pad pattern PP_L may include a lower barrier film 14 , a first lower filling film 15 , and a second lower filling film 16 .
[0047] The lower barrier film 14 may be formed by etching the pre-lower barrier film 14p. The lower barrier film 14 may be disposed along the bottom surface and one or more sidewalls of the lower trench 10t. The lower barrier film 14 may include, for example, at least one of tantalum (Ta), tantalum nitride (TaN), titanium (Ti), titanium nitride (TiN), titanium silicon nitride (TiSiN), ruthenium (Ru), cobalt (Co), nickel (Ni), nickel boron (NiB), tungsten (W), tungsten nitride (WN), tungsten carbonitride (WCN), zirconium (Zr), zirconium nitride (ZrN), vanadium (V), vanadium nitride (VN), niobium (Nb), niobium nitride (NbN), platinum (Pt), iridium (Ir), rhodium (Rh), and a two-dimensional (2D) material.
[0048] The first lower filling film 15 may be formed by etching the first lower seed film 15p. The first lower filling film 15 may be placed on the lower barrier film 14. The first lower filling film 15 may partially fill the lower trench 10t. The first lower filling film 15 may include, but may not be limited to, copper (Cu).
[0049] The second lower filling film 16 may be formed by etching the second lower seed film 16p. The second lower filling film 16 may be placed on the first lower filling film 15. The second lower filling film 16 may at least partially fill the lower trench 10t that may remain after filling the lower barrier film 14 and the first lower filling film 15. The second lower filling film 16 may include, but may not be limited to, copper manganese (CuMn).
[0050] That is, the lower pad pattern PP_L may contain manganese (Mn). In some embodiments, the concentration of manganese (Mn) in the lower pad pattern PP_L may gradually decrease from the upper surface to the lower surface of the lower pad pattern PP_L. However, the present disclosure may not be limited thereto.
[0051] In some embodiments, an upper surface of the lower pad pattern PP_L and an upper surface of the lower adhesive film 13 may be coplanar with each other.
[0052] Reference Figure 3, forming the upper chip may include providing an upper substrate 21. In an embodiment, the formation of the lower chip and the formation of the upper chip may be substantially similar and / or identical.
[0053] The upper substrate 21 may be and / or may include a silicon substrate and / or silicon on insulator (SOI). Alternatively or additionally, the upper substrate 21 may include but may not be limited to silicon-germanium (SiGe), silicon germanium on insulator (SGOI), indium antimonide (InSb), lead telluride (PbTe), indium arsenide (InAs), indium phosphide (InP), gallium arsenide (GaAs) and gallium antimonide (GaSb).
[0054] The upper interlayer insulating film 22 may be formed on the upper substrate 21. The upper interlayer insulating film 22 may include, for example, silicon oxide (SiO), silicon nitride (SiN), silicon oxynitride (SiO x N y ) and at least one of a low dielectric constant material. The low dielectric constant material may include, for example, but may not be limited to, tetraethyl fluoride orthosilicate (FTEOS), hydrogen silsesquioxane (HSQ), bisbenzocyclobutene (BCB), tetramethyl orthosilicate (TMOS), octamethylchlorotetrasiloxane (OMCTS), hexamethyldisiloxane (HMDS), trimethylsilyl borate (TMSB), diacetoxydi-tert-butylsiloxane (DADBS), trimethylsilyl phosphate (TMSP), polytetrafluoroethylene (PTFE), Tonran silazane (TOSZ), fluorosilicate glass (FSG), polyimide nanofoam (such as polypropylene oxide), carbon-doped silicon oxide (CDO), organosilicate glass (OSG), SiLK TM , amorphous fluorinated carbon, silica aerogel, silica xerogel, mesoporous silica and / or combinations thereof.
[0055] The pre-upper adhesive film 23p may be formed on the upper interlayer insulating film 22. The upper interlayer insulating film 22 may be disposed between the pre-upper adhesive film 23p and the upper substrate 21. The pre-upper adhesive film 23p may be formed of an insulating material. For example, the pre-upper adhesive film 23p may include, but may not be limited to, silicon carbon nitride (SiCN).
[0056] In an embodiment, an upper groove 20t may be formed. The upper groove 20t may be formed by partially etching the pre-upper adhesive film 23p and the upper interlayer insulating film 22. For example, relative to the upper side of the upper substrate 21, the bottom surface of the upper groove 20t may be placed at a height lower than the bottom surface of the pre-upper adhesive film 23p. That is, the vertical distance from the upper side of the upper substrate 21 to the bottom surface of the upper groove 20t may be shorter than the vertical distance from the upper side of the upper substrate 21 to the bottom surface of the pre-upper adhesive film 23p. However, the present disclosure may not be limited thereto.
[0057] In some embodiments, the pre-upper barrier film 24 p , the first upper seed film 25 p , the second upper seed film 26 p , and the upper sacrificial film 27 may be sequentially formed.
[0058] For example, a pre-upper barrier film 24p may be formed. The pre-upper barrier film 24p may be formed along the upper surface of the pre-upper adhesive film 23p, the sidewalls of the upper trench 20t, and the bottom surface of the upper trench 20t. The pre-upper barrier film 24p may include a material substantially similar and / or the same as the pre-lower barrier film 14p.
[0059] The first upper seed film 25p may be formed on the pre-upper barrier film 24p. The first upper seed film 25p may be formed using a sputtering process. Therefore, the grain size of the first upper seed film 25p may be smaller than the grain size of the material formed using other processes. For example, as described below, the grain size of the first upper seed film 25p may be smaller than the grain size of the upper sacrificial film 27.
[0060] In some embodiments, the first upper seed film 25p may be formed non-conformally. For example, the thickness of the first upper seed film 25p formed along the sidewall of the upper trench 20t and the thickness of the first upper seed film 25p formed along the bottom surface of the upper trench 20t may be different from each other. However, the present disclosure may not be limited thereto. In some embodiments, the first upper seed film 25p may include a conductive material. For example, the first upper seed film 25p may include but may not be limited to copper (Cu).
[0061] The second upper seed crystal film 26p may be formed on the first upper seed crystal film 25p. The first upper seed crystal film 25p and the second upper seed crystal film 26p may contact each other. The second upper seed crystal film 26p may be formed using a sputtering process. In some embodiments, the second upper seed crystal film 26p may be formed non-conformally. For example, the thickness of the second upper seed crystal film 26p formed along the sidewall of the upper groove 20t and the thickness of the second upper seed crystal film 26p formed along the bottom surface of the upper groove 20t may be different from each other. However, the present disclosure may not be limited to this. In some embodiments, the second upper seed crystal film 26p may include a conductive material. For example, the second upper seed crystal film 26p may include but may not be limited to manganese (Mn). As another example, the second upper seed crystal film 26p may include but may not be limited to copper manganese (CuMn).
[0062] The upper sacrificial film 27 may be formed on the second upper seed film 26p. The upper sacrificial film 27 may be formed using an electroplating process. As a result of forming the upper sacrificial film 27 using an electroplating process, the upper surface of the upper sacrificial film 27 may be a convex curved surface. Alternatively or additionally, since the upper sacrificial film 27 may be formed using an electroplating process, the grain size of the upper sacrificial film 27 may be smaller than the grain size of the first upper seed film 25p. In some embodiments, the upper sacrificial film 27 may include, but may not be limited to, copper (Cu).
[0063] In some embodiments, the upper sacrificial film 27 may be formed and / or a heat treatment process may be performed. The heat treatment process may be performed at a temperature higher than 100° C. and / or lower than 200° C. As a result of performing the heat treatment process at a temperature lower than 200° C., manganese (Mn) contained in the second upper seed film 26 p may not diffuse.
[0064] Reference Figure 4 , an upper pad pattern PP_U may be formed. In some embodiments, the upper pad pattern PP_U may be disposed inside the upper trench 20t. The upper pad pattern PP_U may be formed by etching the upper sacrificial film 27, the second upper seed film 26p, the first upper seed film 25p, the pre-upper barrier film 24p, and the pre-upper adhesive film 23p. The upper pad pattern PP_U may be formed using a CMP process.
[0065] The upper adhesive film 23 may be formed by etching the pre-upper adhesive film 23p. The thickness of the pre-upper adhesive film 23p in the vertical direction may be greater than the thickness of the upper adhesive film 23 in the vertical direction. The vertical direction may refer to the thickness direction of the upper substrate 21. Alternatively, the vertical direction may be a direction perpendicular to the upper side of the upper substrate 21. The upper adhesive film 23 may include, for example, but may not be limited to, silicon carbon nitride (SiCN).
[0066] In some embodiments, the upper pad pattern PP_U may include an upper barrier film 24 , a first upper filling film 25 , and a second upper filling film 26 .
[0067] The upper barrier film 24 may be formed by etching the pre-upper barrier film 24p. The upper barrier film 24 may be placed along the sidewalls and bottom surface of the upper trench 20t. The upper barrier film 24 may include, for example, at least one of tantalum (Ta), tantalum nitride (TaN), titanium (Ti), titanium nitride (TiN), titanium silicon nitride (TiSiN), ruthenium (Ru), cobalt (Co), nickel (Ni), nickel boron (NiB), tungsten (W), tungsten nitride (WN), tungsten carbonitride (WCN), zirconium (Zr), zirconium nitride (ZrN), vanadium (V), vanadium nitride (VN), niobium (Nb), niobium nitride (NbN), platinum (Pt), iridium (Ir), rhodium (Rh), and a two-dimensional (2D) material.
[0068] The first upper filling film 25 may be formed by etching the first upper seed film 25p. The first upper filling film 25 may be placed on the upper barrier film 24. The first upper filling film 25 may partially fill the upper trench 20t. The first upper filling film 25 may include, but may not be limited to, copper (Cu).
[0069] The second upper filling film 26 may be formed by etching the second upper seed film 26p. The second upper filling film 26 may be placed on the first upper filling film 25. The second upper filling film 26 may at least partially fill the upper trench 20t that may be retained after filling the upper barrier film 24 and the first upper filling film 25. The second upper filling film 26 may include but may not be limited to copper manganese (CuMn). That is, the upper pad pattern PP_U may include manganese (Mn). In some embodiments, the concentration of manganese (Mn) in the upper pad pattern PP_U may gradually decrease from the upper surface to the lower surface of the upper pad pattern PP_U. However, the present disclosure may not be limited thereto.
[0070] In some embodiments, an upper surface of the upper pad pattern PP_U and an upper surface of the upper adhesive film 23 may be coplanar with each other.
[0071] Reference Figure 5 , the lower chip and the upper chip may be bonded together. For example, the lower adhesive film 13 and the upper adhesive film 23 may be bonded together. As another example, the lower pad pattern PP_L and the upper pad pattern PP_U may be bonded together.
[0072] In some embodiments, the bonding energy of CuMn-CuMn may be greater than the bonding energy of Cu-Cu. According to some embodiments, manganese (Mn) may be placed on a boundary surface where the lower pad pattern PP_L and the upper pad pattern PP_U are bonded to each other. Therefore, the lower pad pattern PP_L and the upper pad pattern PP_U may be bonded relatively more stably when bonded together.
[0073] In some embodiments, the lower pad pattern PP_L may include a first portion PP_La and a second portion PP_Lb. The second portion PP_Lb of the lower pad pattern PP_L may be placed on the first portion PP_La of the lower pad pattern PP_L. The first portion PP_La of the lower pad pattern PP_L may be placed in the lower interlayer insulating film 12. The second portion PP_Lb of the lower pad pattern PP_L may be placed in the lower adhesive film 13. The concentration of manganese (Mn) in the second portion PP_Lb of the lower pad pattern PP_L may be greater than the concentration of manganese (Mn) in the first portion PP_La of the lower pad pattern PP_L.
[0074] The upper pad pattern PP_U may include a first portion PP_Ua and a second portion PP_Ub. The second portion PP_Ub of the upper pad pattern PP_U may be placed below the first portion PP_Ua of the upper pad pattern PP_U. The first portion PP_Ua of the upper pad pattern PP_U may be placed in the upper interlayer insulating film 22. The second portion PP_Ub of the upper pad pattern PP_U may be placed in the upper adhesive film 23. The concentration of manganese (Mn) in the second portion PP_Ub of the upper pad pattern PP_U may be greater than the concentration of manganese (Mn) in the first portion PP_Ua of the upper pad pattern PP_U.
[0075] In some embodiments, a first height H1 of the lower pad pattern PP_L in the vertical direction may be substantially similar and / or identical to a second height H2 of the upper pad pattern PP_U in the vertical direction. However, the present disclosure may not be limited thereto.
[0076] In the following, reference is made to Figure 6 and Figure 7 A semiconductor device according to some embodiments is described. For ease of description, reference may be briefly described and / or omitted. Figures 1 to 5 Duplicate content of the described features. Figure 6 and Figure 7 is a diagram illustrating a semiconductor device according to some embodiments.
[0077] Reference Figure 6 , the lower pad pattern PP_L and the upper pad pattern PP_U may not be aligned.
[0078] A portion of the lower pad pattern PP_L may contact the upper adhesive film 23. A portion of the upper pad pattern PP_U may contact the lower adhesive film 13. According to some embodiments, when the semiconductor device is miniaturized and / or reduced in size, the sizes of the lower pad pattern PP_L and the upper pad pattern PP_U may be reduced. Therefore, the lower pad pattern PP_L and the upper pad pattern PP_U are more likely to be misaligned when they are bonded to each other.
[0079] In some embodiments, the semiconductor device may include a first boundary surface BR1 and a second boundary surface BR2. The first boundary surface BR1 may be and / or may include a boundary surface between the lower pad pattern PP_L and the upper adhesive film 23. The second boundary surface BR2 may be and / or may include a boundary surface between the upper pad pattern PP_U and the lower adhesive film 13.
[0080] The lower pad pattern PP_L and the upper pad pattern PP_U may each contain manganese (Mn). That is, manganese (Mn) may be placed at the boundary between the lower pad pattern PP_L and the upper adhesive film 23. For example, manganese (Mn) may be placed on the first boundary surface BR1. Alternatively or additionally, manganese (Mn) may be placed at the boundary between the upper pad pattern PP_U and the lower adhesive film 13. As another example, manganese (Mn) may be placed on the second boundary surface BR2.
[0081] When manganese (Mn) is placed at the boundary between the lower pad pattern PP_L and the upper adhesive film 23, the bonding force between the lower pad pattern PP_L and the upper adhesive film 23 can be enhanced compared to a case where manganese (Mn) is not placed at the boundary between the lower pad pattern PP_L and the upper adhesive film 23. Similarly, when manganese (Mn) is placed at the boundary between the upper pad pattern PP_U and the lower adhesive film 13, the bonding force between the upper pad pattern PP_U and the lower adhesive film 13 can be enhanced compared to a case where manganese (Mn) is not placed at the boundary between the upper pad pattern PP_U and the lower adhesive film 13. Therefore, when compared to a related semiconductor device, a semiconductor device with improved reliability can be manufactured.
[0082] Reference Figure 7 , a first height H1 of the lower pad pattern PP_L in the vertical direction may be different from a second height H2 of the upper pad pattern PP_U in the vertical direction. For example, the first height H1 may be greater than the second height H2. However, the present disclosure may not be limited thereto.
[0083] In the following, reference is made to Figures 8 to 13 A method for manufacturing a semiconductor device according to some embodiments is described. Figures 8 to 13 An exemplary method for manufacturing a semiconductor device according to some embodiments is shown. For ease of illustration, Figures 8 to 13 The description can focus on possible differences with those already referenced Figures 1 to 5 The characteristics discussed are different characteristics.
[0084] Reference Figures 8 to 13 , a method for manufacturing a semiconductor device may include forming a lower chip, forming an upper chip, and bonding the lower chip and the upper chip to each other. Forming the lower chip may include forming a lower pad pattern, forming the upper chip may include forming an upper pad pattern, and bonding the lower chip and the upper chip to each other may include bonding the lower pad pattern and the upper pad pattern to each other.
[0085] The formation of the lower chip and the formation of the lower pad pattern can be compared with the reference Figure 1 and Figure 2 Described as being substantially similar and / or identical.
[0086] Reference Figure 8Forming the upper chip may include providing an upper substrate 21. An upper interlayer insulating film 22 and a pre-upper adhesive film 23p may be sequentially formed on the substrate 21.
[0087] In some embodiments, an upper trench 20t may be formed. For example, the upper trench 20t may be formed by partially etching the pre-upper adhesive film 23p and the upper interlayer insulating film 22. The upper trench 20t may be formed to be deeper than the lower trench 10t. For example, the depth of the lower trench 10t in the vertical direction may be less than the depth of the upper trench 20t in the vertical direction.
[0088] In some embodiments, a pre-upper barrier film 24p may be formed. For example, the pre-upper barrier film 24p may be formed along an upper surface of the pre-upper adhesive film 23p, a sidewall of the upper trench 20t, and a bottom surface of the upper trench 20t.
[0089] In some embodiments, the first upper seed film 25p may be formed on the pre-upper barrier film 24p. For example, the first upper seed film 25p may be formed using a sputtering process. Therefore, the grain size of the first upper seed film 25p may be smaller than the grain size of the material formed using other processes. For example, as described below, the grain size of the first upper seed film 25p may be smaller than the grain size of the pre-third upper fill film 28p. The first upper seed film 25p may be formed non-conformally. In some embodiments, the first upper seed film 25p may include a conductive material. For example, the first upper seed film 25p may include but may not be limited to copper (Cu).
[0090] In some embodiments, a pre-third upper fill film 28p may be formed. For example, the pre-third upper fill film 28p may be formed on the first upper seed film 25p. The pre-third upper fill film 28p may be formed using an electroplating process. Since the pre-third upper fill film 28p may be formed using an electroplating process, the upper surface of the pre-third upper fill film 28p may be a convex surface. Alternatively or additionally, since the pre-third upper fill film 28p may be formed using an electroplating process, the grain size of the pre-third upper fill film 28p may be smaller than the grain size of the first upper seed film 25p. In some embodiments, the pre-third upper fill film 28p may include a conductive material. For example, the pre-third upper fill film 28p may include but may not be limited to copper (Cu).
[0091] After forming the preliminary third upper filling film 28p, a heat treatment process may be performed. The heat treatment process may be performed at a temperature higher than 100C and / or lower than 200C.
[0092] Reference Fig. 9A portion of the pre-third upper fill film 28p and a portion of the first upper seed film 25p may be etched using a CMP process. A portion of the pre-third upper fill film 28p and a portion of the first upper seed film 25p may be etched to expose the pre-upper barrier film 24p.
[0093] Reference Fig.10 , the groove RC may be formed by selectively etching a portion of the pre-third upper filling film 28p and a portion of the first upper seed film 25p. The pre-third upper filling film 28p may be formed of a material having an etching selectivity relative to the pre-upper barrier film 24p. Similarly, the first upper seed film 25p may be formed of a material having an etching selectivity relative to the pre-upper barrier film 24p. Therefore, the pre-upper barrier film 24p may not be etched, and only the pre-third upper filling film 28p and the first upper seed film 25p may be selectively etched.
[0094] Reference Fig.11 , a second upper seed crystal film 26p may be formed. The second upper seed crystal film 26p may at least partially fill the recess RC and may be formed on the pre-upper barrier film 24p. The second upper seed crystal film 26p may be formed using a sputtering process. The second upper seed crystal film 26p may include a conductive material. The second upper seed crystal film 26p may include but may not be limited to manganese (Mn). For example, the second upper seed crystal film 26p may include copper manganese (CuMn).
[0095] Reference Fig.12 , an upper pad pattern PP_U may be formed. The upper pad pattern PP_U may be disposed in the upper trench 20t. The upper pad pattern PP_U may be formed by etching the second upper seed film 26p, the pre-third upper filling film 28p, the pre-upper barrier film 24p, the first upper seed film 25p, and the pre-upper adhesive film 23p. The upper pad pattern PP_U may be formed using a CMP process.
[0096] The upper pad pattern PP_U may include an upper barrier film 24 , a first upper filling film 25 , a second upper filling film 26 , and a third upper filling film 28 .
[0097] The upper barrier film 24 may be disposed along the bottom surface and one or more sidewalls of the upper trench 20t. The first upper filling film 25 may be disposed on the upper barrier film 24. The third upper filling film 28 may be disposed on the first upper filling film 25. The second upper filling film 26 may be disposed on the third upper filling film 28.
[0098] As described above, the first and second upper fill films 25 and 26 may be formed using a sputtering process, and the third upper fill film 28 may be formed using an electroplating process. Therefore, the grain size of the first and second upper fill films 25 and 26 may be smaller than that of the third upper fill film 28.
[0099] Reference Fig.13 , the lower chip and the upper chip may be bonded together. For example, the lower adhesive film 13 and the upper adhesive film 23 may be bonded together, and the lower pad pattern PP_L and the upper pad pattern PP_U may be bonded together.
[0100] In some embodiments, the bonding energy of CuMn-CuMn may be greater than the bonding energy of Cu-Cu. According to some embodiments, manganese (Mn) may be placed on a boundary surface where the lower pad pattern PP_L and the upper pad pattern PP_U may be bonded to each other. Therefore, the lower pad pattern PP_L and the upper pad pattern PP_U may be bonded relatively more stably when bonded together.
[0101] In some embodiments, the thickness of the second lower filling film 16 of the lower pad pattern PP_L in the vertical direction may be greater than the thickness of the second upper filling film 26 of the upper pad pattern PP_U in the vertical direction.
[0102] In some embodiments, a first height H1 of the lower pad pattern PP_L in the vertical direction may be smaller than a second height H2 of the upper pad pattern PP_U in the vertical direction.
[0103] Fig.14 is a diagram depicting a semiconductor device according to some embodiments.
[0104] Reference Fig.14 , the lower pad pattern PP_L and the upper pad pattern PP_U may not be aligned. That is, a portion of the lower pad pattern PP_L may contact the upper adhesive film 23, and / or a portion of the upper pad pattern PP_U may contact the lower adhesive film 13. When the semiconductor device is miniaturized and / or reduced in size, the size of the lower pad pattern PP_L and the upper pad pattern PP_U may be reduced. Therefore, the lower pad pattern PP_L and the upper pad pattern PP_U may not be aligned when they are bonded to each other. That is, a portion of the third upper filling film 28 of the upper pad pattern PP_U may contact the lower adhesive film 13.
[0105] The lower pad pattern PP_L and the upper pad pattern PP_U may each contain manganese (Mn). That is, manganese (Mn) may be placed at the boundary between the lower pad pattern PP_L and the upper adhesive film 23. Manganese (Mn) may be placed on the first boundary surface BR1. Alternatively or additionally, manganese (Mn) may be placed at the boundary between the upper pad pattern PP_U and the lower adhesive film 13. Manganese (Mn) may be placed on the second boundary surface BR2.
[0106] When manganese (Mn) is placed at the boundary between the lower pad pattern PP_L and the upper adhesive film 23, the bonding force between the lower pad pattern PP_L and the upper adhesive film 23 can be enhanced compared to the case where manganese (Mn) is not placed at the boundary between the lower pad pattern PP_L and the upper adhesive film 23. Alternatively or additionally, when manganese (Mn) is placed at the boundary between the upper pad pattern PP_U and the lower adhesive film 13, the bonding force between the upper pad pattern PP_U and the lower adhesive film 13 can be enhanced compared to the case where manganese (Mn) is not placed at the boundary between the upper pad pattern PP_U and the lower adhesive film 13. That is, a semiconductor device with improved reliability can be manufactured.
[0107] Reference Figures 15 to 17 A semiconductor device according to some embodiments is described. Figures 15 to 17 The semiconductor device shown may be an image sensor. However, the present disclosure may not be limited thereto. In some embodiments, reference may be made to Figures 1 to 14 A semiconductor device manufacturing method is described to manufacture an image sensor.
[0108] Figures 15 to 17 A semiconductor device may be shown. For example, Fig.15 A plan view of a semiconductor device according to some embodiments may be depicted. Fig.16 Can be along Fig.15 A cross-sectional view taken along line AA of Fig.17 Can be Fig.15 Magnified view of area P.
[0109] Reference Fig.15 and Fig.16 , the semiconductor device may include a first semiconductor chip 100 and a second semiconductor chip 200. The first semiconductor chip 100 may be and / or may include a sensor chip, and the second semiconductor chip 200 may be and / or may include a logic chip. The first semiconductor chip 100 and the second semiconductor chip 200 may be bonded together.
[0110] The first semiconductor chip 100 may include a light receiving region APS, a light shielding region OB, and a pad region PAD. A plurality of unit pixel regions PX arranged two-dimensionally (e.g., in the form of a matrix) may be formed in the light receiving region APS and the light shielding region OB. The unit pixel regions PX may be arranged in the form of a matrix inside a plane extending in the first direction D1 and the second direction D2. In some embodiments, the first direction D1 and the second direction D2 may intersect with each other. Alternatively or additionally, the first direction D1 and the second direction D2 may be substantially perpendicular to each other. The third direction D3 may be substantially perpendicular to the first direction D1 and the second direction D2.
[0111] Active pixels that can receive light to generate active signals can be placed in the light receiving area APS. Alternatively or additionally, optical black pixels that can block light to generate optical black signals can be placed in the light shielding area OB. In some embodiments, the light shielding area OB can be formed, for example, along the periphery of the light receiving area APS. However, the present disclosure may not be limited to this. In some embodiments, a dummy unit pixel area DPX can be formed in the light shielding area OB. The dummy unit pixel area DPX can be a pixel that may not generate an active signal.
[0112] The pad area PAD may be formed around the light shielding area OB. In some embodiments, the pad area PAD may be formed adjacent to the edge of the semiconductor device. However, the present disclosure may not be limited thereto. The pad area PAD may be connected to an external device, etc., and may be configured to send and / or receive electrical signals between the semiconductor device and the external device. For example, the second pad structure 455 may be disposed on the first substrate 110 of the pad area PAD. The second pad structure 455 may be connected to an external device, etc.
[0113] The semiconductor device may include a first substrate 110 , a pixel isolation pattern 120 , a surface insulating film 150 , a first color filter 170 , a mesh pattern 160 , a microlens 180 , a second substrate 210 , a first pad structure 365 , and a second pad structure 455 .
[0114] The first substrate 110 may be and / or may include a semiconductor substrate. For example, the first substrate 110 may be bulk silicon and / or silicon on insulator (SOI). The first substrate 110 may be a silicon substrate, and / or may include other materials, for example, silicon germanium (SiGe), indium antimonide (InSb), lead telluride (PbTe), indium arsenide (InAs), indium phosphide (InP), gallium arsenide (GaAs) and / or gallium antimonide (GaSb). Alternatively or additionally, the first substrate 110 may be an epitaxial layer formed on a base substrate.
[0115] The first substrate 110 may include a first side 110a and a second side 110b opposite to each other. In some embodiments, the second side 110b of the first substrate 110 may be and / or may include a light receiving surface on which light is incident. That is, according to some embodiments, the image sensor may be a backside illumination (BSI) image sensor.
[0116] A plurality of unit pixel regions PX may be formed in the first substrate 110 of the light receiving region APS and the light shielding region OB. Each unit pixel region PX may include a photoelectric conversion layer PD. The first substrate 110 of the light shielding region OB may include a dummy unit pixel region DPX, which may not include the photoelectric conversion layer PD. However, the present disclosure may not be limited thereto. The signal generated in the dummy unit pixel region DPX may be used as information for removing process noise thereafter.
[0117] Each unit pixel region PX may include a photoelectric conversion layer PD, a floating diffusion region FD, and a transfer transistor TX. The photoelectric conversion layer PD may be formed in the first substrate 110 of the light receiving region APS and the light shielding region 0B. The photoelectric conversion layer PD may generate charges proportional to the amount of light incident from the outside. The photoelectric conversion layer PD may transfer the generated and accumulated charges to the floating diffusion region FD.
[0118] The floating diffusion region FD may be formed in the first substrate 110 of the light receiving region APS and the light blocking region OB. The floating diffusion region FD may be formed in the first side 110a of the first substrate 110. Charges transferred to the floating diffusion region FD may be applied to a source follower gate.
[0119] The transfer transistor TX may be buried inside the first substrate 110. One end of the transfer transistor TX may be connected to the photoelectric conversion layer PD, and the other end of the transfer transistor TX may be connected to the floating diffusion region FD. For example, the transfer transistor TX may transfer charges generated from the photoelectric conversion layer PD to the floating diffusion region FD.
[0120] The transfer transistor TX may include a transfer gate, a gate insulating film, and a gate spacer. The transfer gate may include a portion buried in the first substrate 110. The gate insulating film may be placed between the transfer gate and the first substrate 110. The gate spacer may be placed on both sidewalls of the transfer gate.
[0121] The pixel isolation pattern 120 may be formed in the first substrate 110. The pixel isolation pattern 120 may be formed by filling a deep trench with an insulating material, which may be formed by patterning the first substrate 110. The pixel isolation pattern 120 may penetrate the first substrate 110 in the third direction D3. For example, the pixel isolation pattern 120 may extend from the first side 110a to the second side 110b. The pixel isolation pattern 120 may be a front deep trench isolation (FDTI).
[0122] Alternatively or additionally, the pixel isolation pattern 120 may be a back deep trench isolation (BDTI). In such an embodiment, the pixel isolation pattern 120 may extend from the second side 110b toward the first side 110a. The width of the pixel isolation pattern 120 in the second direction D2 may gradually decrease from the second side 110b toward the first side 110a.
[0123] In some embodiments, the pixel isolation pattern 120 may include a lower portion and an upper portion. The upper portion of the pixel isolation pattern 120 may be placed on the lower portion of the pixel isolation pattern 120. The upper surface of the upper portion of the pixel isolation pattern 120 may be the second side 110b. The lower surface of the lower portion of the pixel isolation pattern 120 may be the first side 110a. The lower portion of the pixel isolation pattern 120 may be formed from the first side 110a to the lower surface of the upper portion of the pixel isolation pattern 120 using a doping process.
[0124] The pixel isolation pattern 120 may define (eg, delimit) a dummy unit pixel region DPX and a plurality of unit pixel regions PX. From a planar perspective, the pixel isolation pattern 120 may be formed in a grid pattern and may separate a plurality of unit pixel regions PX and the dummy unit pixel region DPX.
[0125] From a plane perspective, the pixel isolation pattern 120 may have a lattice structure. From a plane perspective, the pixel isolation pattern 120 may surround each unit pixel region PX. The pixel isolation pattern 120 may have a lattice structure extending in the first direction D1 and the second direction D2.
[0126] The pixel isolation pattern 120 may include a liner film 121, a conductive film 122, and a capping film 123. The liner film 121 may be placed along the sidewall of the pixel isolation trench. The conductive film 122 may be placed between the liner films 121. The capping film 123 may be placed on the conductive film 122.
[0127] The liner film 121 may include an oxide film having a lower refractive index than the first substrate 110. For example, the liner film 121 may include, but may not be limited to, silicon oxide (SiO), aluminum oxide (Al 2 O 3 ), tantalum oxide (TaO), and / or a combination thereof. The liner film 121 may refract or reflect light obliquely incident on the photoelectric conversion layer PD. Alternatively or additionally, the liner film 121 may prevent photocharges generated in a specific unit pixel region PX by incident light from moving to an adjacent unit pixel region PX due to random drift. That is, the liner film 121 may increase the light receiving rate of the photoelectric conversion layer PD to improve the quality of the image sensor when compared with a related image sensor.
[0128] In some embodiments, the conductive film 122 may include a conductive material. For example, the conductive film 122 may include but may not be limited to polysilicon (poly Si). In some embodiments, a negative voltage may be applied to the conductive film 122 which may include a conductive material. Therefore, electrostatic discharge (ESD) scratch failure of the image sensor may be effectively prevented. As used herein, an ESD scratch defect may refer to a phenomenon in which charges generated by ESD or the like may accumulate on the surface of the substrate (e.g., the second side 110b) and produce a scratch-like defect on the image to be generated.
[0129] In some embodiments, the capping film 123 may include an insulating material. For example, the capping film 123 may include, but may not be limited to, a silicon-based insulating material (e.g., silicon nitride (SiN), silicon oxide (SiO), silicon oxynitride (SiO x N y )) and high dielectric constant materials (e.g., hafnium oxide (HfO 2 ) and aluminum oxide (Al 2 O 3 )).
[0130] In some embodiments, an element isolation pattern 105 may be provided. That is, the element isolation pattern 105 may be placed in the first substrate 110. For example, the element isolation pattern 105 may be placed in a groove formed by partially recessing the first substrate 110. The groove may be recessed from the first side 110a of the first substrate 110. The element isolation pattern 105 may be a shallow element isolation (STI) film. In some embodiments, the element isolation pattern 105 may define (e.g., delimit) an active region.
[0131] The width of the element isolation pattern 105 in the second direction D2 may gradually decrease from the first side 110a of the first substrate 110 toward the second side 110b. The element isolation pattern 105 may overlap the pixel isolation pattern 120 in the second direction D2 or the first direction D1. The pixel isolation pattern 120 may penetrate the element isolation pattern 105 in the third direction D3. The element isolation pattern 105 may include an insulating material. The element isolation pattern 105 may include, for example, silicon nitride (SiN), silicon oxide (SiO), and silicon oxynitride (SiO x N y ) at least one of.
[0132] The semiconductor device according to some embodiments may further include a first inter-wiring insulating film (e.g., a first inter-wiring insulating film 131, a second inter-wiring insulating film 132, a third inter-wiring insulating film 133, and a fourth inter-wiring insulating film 134). The first inter-wiring insulating films 131 to 134 may be formed on the first side 110a of the first substrate 110. For example, the first inter-wiring insulating films 131 to 134 may cover the first side 110a of the first substrate 110. The first substrate 110 and the first inter-wiring insulating films 131 to 134 may constitute the first semiconductor chip 100. Fig.16 , although the first inter-wiring insulating films 131 to 134 are shown as being divided into four layers, the present disclosure may not be limited thereto. That is, Fig.16 The illustrated number of layers of the first inter-wiring insulating films 131 to 134 may be only an example.
[0133] The first inter-wiring insulating films 131 to 134 may include, for example, but may not be limited to, silicon oxide (SiO), silicon nitride (SiN), silicon oxynitride (SiO x N y ) or at least one of a low dielectric constant (low-k) material having a dielectric constant lower than silicon oxide (SiO).
[0134] A plurality of first contacts (e.g., a first first contact 141 and a second first contact 143) and a plurality of first wiring patterns (e.g., a first first wiring pattern 142, a second first wiring pattern 144, and a third first wiring pattern 145) may be disposed inside the first inter-wiring insulating films 131 to 134. The plurality of first contacts 141 and 143 may electrically connect (e.g., couple) the floating diffusion region FD and the plurality of first wiring patterns 142 to 145. Some of the plurality of first wiring patterns 142 to 145 may be connected to the first connection structure 360. However, the present disclosure may not be limited thereto.
[0135] Each of the first contacts 141 and 143 and the first wiring patterns 142 to 145 may include, for example, but may not be limited to, at least one of tungsten (W), copper (Cu), aluminum (Al), gold (Au), silver (Ag), and / or alloys thereof.
[0136] The first adhesive film 190 may be placed along the lower surface of the first inter-wiring insulating films 131 to 134. In some embodiments, the first adhesive film 190 may be formed of an insulating material. For example, the first adhesive film 190 may include, but may not be limited to, silicon carbon nitride (SiCN).
[0137] The first pad pattern 195 may be placed inside the first inter-wiring insulating films 131 to 134. The lower surface of the first pad pattern 195 may be coplanar with the lower surface of the first adhesive film 190. The first pad pattern 195 may be coplanar with the reference Figures 1 to 5 The described upper pad patterns PP_U are substantially similar and / or identical.
[0138] The first via contact 147 may be placed on the first pad pattern 195. The first pad pattern 195 and the first wiring patterns 142 to 145 may be connected by the first via contact 147. In some embodiments, the first via contact 147 may be formed of a conductive material. For example, the first via contact 147 may be made of and / or may include copper (Cu).
[0139] The second substrate 210 may be and / or may include bulk silicon or silicon on insulator (SOI). The second substrate 210 may be a silicon substrate and / or may include other materials, such as but not limited to silicon germanium (SiGe), indium antimonide (InSb), lead telluride (PbTe), indium arsenide (InAs), indium phosphide (InP), gallium arsenide (GaAs) and / or gallium antimonide (GaSb). Alternatively or additionally, the second substrate 210 may be and / or may include an epitaxial layer formed on a base substrate.
[0140] The second substrate 210 may include an upper side and a lower side. The upper side of the second substrate 210 may be a side facing the first semiconductor chip 100. The lower side of the second substrate 210 may be a side opposite to the upper side of the second substrate 210.
[0141] A plurality of transistors TR may be formed on the upper side of the second substrate 210. The transistor TR may be and / or may include, for example, a logic circuit. The transistor TR may control a transfer transistor TX, a reset transistor, a selection transistor, and a source follower transistor.
[0142] The second inter-wiring insulating film (e.g., the first second inter-wiring insulating film 231 and the second second inter-wiring insulating film 232) may be formed on the second substrate 210. For example, the second inter-wiring insulating films 231 and 232 may at least partially cover the upper surface of the second substrate 210. The second substrate 210 and the second inter-wiring insulating films 231 and 232 may constitute the second semiconductor chip 200. The second inter-wiring insulating films 231 and 232 may include, for example, but may not be limited to, silicon oxide (SiO), silicon nitride (SiN), silicon oxynitride (SiO x N y ) and at least one of a low dielectric constant (low-k) material having a dielectric constant lower than that of silicon oxide (SiO).
[0143] A plurality of second wiring patterns (e.g., first and second wiring patterns 241 and 242) may be placed inside the second inter-wiring insulating films 231 and 232. The plurality of second wiring patterns 241 and 242 may each be connected to the transistor TR and / or may be connected to the floating diffusion region FD of the first semiconductor chip 100.
[0144] Each of the second wiring patterns 241 and 242 may include, for example, but may not be limited to, at least one of tungsten (W), copper (Cu), aluminum (Al), gold (Au), silver (Ag), and / or alloys thereof.
[0145] The second adhesive film 290 may be placed along the upper surfaces of the second inter-wiring insulating films 231 and 232. The second adhesive film 290 may be formed of an insulating material. For example, the second adhesive film 290 may include, but may not be limited to, silicon carbon nitride (SiCN).
[0146] The second pad pattern 295 may be placed inside the second inter-wiring insulating films 231 and 232. The upper surface of the second pad pattern 295 may be coplanar with the upper surface of the second adhesive film 290. The second pad pattern 295 may be coplanar with the reference Figures 1 to 5 The lower pad patterns PP_L discussed are substantially similar and / or identical.
[0147] The second via contact 243 may be placed under the second pad pattern 295. The second pad pattern 295 and the second wiring patterns 241 and 242 may be connected through the second via contact 243. The second via contact 243 may be formed of a conductive material. For example, the second via contact 243 may be formed of, but not limited to, copper (Cu).
[0148] The surface insulating film 150 may be formed on the second side 110b of the first substrate 110. The surface insulating film 150 may extend along the second side 110b of the first substrate 110. In some embodiments, at least a portion of the surface insulating film 150 may contact the pixel isolation pattern 120.
[0149] The surface insulating film 150 may include an insulating material. For example, the surface insulating film 150 may include, but is not limited to, silicon oxide (SiO), silicon nitride (SiN), silicon oxynitride (SiO x N y ), aluminum oxide (Al 2 O 3 ), hafnium oxide (HfO 2 ) and / or at least one of their combinations.
[0150] The surface insulating film 150 may be used as an anti-reflection film to prevent reflection of light to be incident on the first substrate 110, thereby potentially improving the light receiving rate of the photoelectric conversion layer PD. Alternatively or additionally, as described below, the surface insulating film 150 may be used as a planarization film, and / or may form the first color filter 170 and the microlens 180 with uniform heights.
[0151] The first color filter 170 may be formed on the surface insulating film 150 of the light receiving area APS. In some embodiments, the first color filter 170 may be arranged to correspond to each unit pixel area PX. For example, a plurality of first color filters 170 may be arranged two-dimensionally (eg, in a matrix).
[0152] The first color filter 170 may have various color filters according to the unit pixel area PX. For example, the first color filter 170 may be arranged in a Bayer pattern, which may include a red filter, a green filter, and a blue filter. However, the present disclosure may not be limited thereto. For example, without departing from the scope of the present disclosure, the first color filter 170 may include a yellow filter, a magenta filter, and a cyan filter, and / or may also include a white filter.
[0153] The mesh pattern 160 may be formed on the surface insulating film 150. The mesh pattern 160 may be formed as a mesh pattern from a plane perspective, and / or may be interposed between the plurality of first color filters 170.
[0154] The mesh pattern 160 may include a low refractive index material having a refractive index lower than that of silicon (Si). For example, the mesh pattern 160 may include, but may not be limited to, silicon oxide (SiO), aluminum oxide (Al 2 O 3 ), tantalum oxide (TaO), and / or combinations thereof. In some embodiments, the grid pattern 160 can potentially improve the quality of the image sensor by refracting or reflecting light obliquely incident on the image sensor when compared to related image sensors.
[0155] In some embodiments, the first protective film 165 may be formed on the surface insulating film 150 and the mesh pattern 160. The first protective film 165 may be interposed between the surface insulating film 150 and the first color filter 170 and between the mesh pattern 160 and the first color filter 170. For example, the first protective film 165 may extend along the upper surface of the surface insulating film 150 and the contours of the side and upper surface of the mesh pattern 160.
[0156] The first protection film 165 may include, for example, but is not limited to, aluminum oxide (Al 2 O 3In some embodiments, the first protection film 165 may prevent damage to the surface insulation film 150 and the mesh pattern 160 .
[0157] The microlens 180 may be formed on the first color filter 170. The microlens 180 may be arranged to correspond to each unit pixel region PX. For example, the microlens 180 may be arranged two-dimensionally (eg, in the form of a matrix) in a plane.
[0158] Microlens 180 may have a convex shape and / or may have a predetermined radius of curvature. Thus, microlens 180 may collect light that may be incident on photoelectric conversion layer PD. Microlens 180 may include, for example, but may not be limited to, a light-transmitting resin.
[0159] In some embodiments, the second protective film 185 may be formed on the microlens 180. The second protective film 185 may extend along the surface of the microlens 180. The second protective film 185 may include, for example, an inorganic oxide film. The second protective film 185 may include, but may not be limited to, silicon oxide (SiO), titanium oxide (TiO), zirconium oxide (ZrO), hafnium oxide (HfO 2 ) and / or at least one of a combination thereof. In some embodiments, the second protection film 185 may include a low temperature oxide (LTO).
[0160] The second protective film 185 may protect the microlens 180 from external influences. For example, the second protective film 185 may protect the microlens 180 including an organic substance by including an inorganic oxide film. Alternatively or additionally, the second protective film 185 may improve the light-gathering ability of the microlens 180. For example, the second protective film 185 may reduce reflection, refraction, scattering, etc. of incident light reaching the space between the microlenses 180 by filling the space between the microlenses 180.
[0161] According to some embodiments, the semiconductor device may further include a first connection structure 360 and a second connection structure 450 .
[0162] The first connection structure 360 may be formed inside the light shielding region OB. The first connection structure 360 may shield light incident on the light shielding region OB. The first connection structure 360 may be formed on the surface insulating film 150 of the light shielding region OB. The first connection structure 360 may contact the pixel isolation pattern 120. The first connection structure 360 may be connected to the conductive film 122 of the pixel isolation pattern 120.
[0163] For example, a first trench t1 that may expose the conductive film 122 may be formed in the first substrate 110 and the surface insulating film 150 of the light shielding region OB. The first connection structure 360 may be formed in the first trench t1 and / or may contact the conductive film 122 in the light shielding region OB. The first connection structure 360 may extend along the contours of the sidewall and bottom surface of the first trench t1.
[0164] The first connection structure 360 may be electrically connected to the conductive film 122. For example, the first connection structure 360 may be electrically connected to the conductive film 122. The first connection structure 360 may include, for example, a titanium (Ti) film, a titanium nitride (TiN) film, and a tungsten (W) film, which may be sequentially stacked.
[0165] In some embodiments, a first pad structure 365 may be formed on the first connection structure 360. The first pad structure 365 may at least partially fill the first trench t1 that may remain after filling the first connection structure 360. A voltage may be applied to the conductive film 122 of the pixel isolation pattern 120 through the first pad structure 365. Therefore, charges generated by ESD or the like may be discharged to the first pad structure 365 through the conductive film 122, and FSD scratch defects may be prevented.
[0166] The first pad structure 365 may include, for example, but may not be limited to, at least one of tungsten (W), copper (Cu), aluminum (Al), gold (Au), silver (Ag), and / or alloys thereof.
[0167] In some embodiments, the second trench t2 may be formed in the first substrate 110 of the light shielding area OB. The second trench t2 may expose a portion of the first wiring pattern 145 of the first semiconductor chip 100. The first connection structure 360 may be formed in the second trench t2 and / or may connect the first wiring pattern 145. The first connection structure 360 may extend along the bottom surface and one or more sidewalls of the first trench t1.
[0168] In some embodiments, a first filling insulating film 370 may be formed on the first connection structure 360. The first filling insulating film 370 may at least partially fill the second trench t2 that may remain after filling the first connection structure 360. The first filling insulating film 370 may include, for example, but may not be limited to, at least one of silicon oxide, aluminum oxide, tantalum oxide, and a combination thereof.
[0169] In some embodiments, the first capping pattern 375 may be formed on the first filling insulating film 370. The first capping pattern 375 may include a silicon-based insulating material (eg, silicon nitride (SiN), silicon oxide (SiO), and silicon oxynitride (SiO x N y )) and / or high dielectric materials (e.g., hafnium oxide (HfO2 ) and aluminum oxide (Al 2 O 3 )). In some embodiments, the first capping pattern 375 may include a material substantially similar to and / or the same as the capping film 123. However, the present disclosure may not be limited thereto.
[0170] In some embodiments, the second color filter 170c may be formed on the first connection structure 360. For example, the second color filter 170c may be formed to partially cover the first protection film 165 in the light blocking area OB. The second color filter 170c may include, for example, but may not be limited to, a blue color filter.
[0171] In some embodiments, the third protective film 380 may be formed on the second color filter 170c. For example, the third protective film 380 may be formed to partially cover the first protective film 165 in the light shielding area OB. In some embodiments, the second protective film 185 may extend along the surface of the third protective film 380. The third protective film 380 may include, for example, but may not be limited to, a light-transmitting resin. In some embodiments, the third protective film 380 may include a material substantially similar and / or the same as the microlens 180.
[0172] The second connection structure 450 may be formed in the pad area PAD. For example, the second connection structure 450 may be formed on the surface insulating film 150 of the pad area PAD.
[0173] In some embodiments, the third trench t3 may be formed in the first substrate 110 of the pad area PAD. The second connection structure 450 may partially fill the third trench t3. The second connection structure 450 may be formed along a bottom surface and one or more sidewalls of the third trench t3.
[0174] A fourth trench t4 that may expose the first wiring pattern 145 may be formed in the first semiconductor chip 100 of the pad area PAD. The second connection structure 450 may partially fill the fourth trench t4. The second connection structure 450 may be formed along the sidewall and bottom surface of the fourth trench t4.
[0175] The second connection structure 450 may be formed in the fourth trench t4 and may contact a portion of the first wiring pattern 145. The second connection structure 450 may electrically connect a portion of the first wiring pattern 145 with the second pad structure 455. The second connection structure 450 may include, for example, a titanium (Ti) film, a titanium nitride (TiN) film, and a tungsten (W) film, which may be sequentially stacked.
[0176] The second pad structure 455 may be formed on the second connection structure 450. The second pad structure 455 may fill the third trench t3 remaining after filling the second connection structure 450. The second pad structure 455 may include, for example, but may not be limited to, at least one of tungsten (W), copper (Cu), aluminum (Al), gold (Au), silver (Ag), and / or alloys thereof.
[0177] In some embodiments, a portion of the second pad structure 455 may be exposed. For example, an exposure opening may be formed to expose the second pad structure 455. Thus, the second pad structure 455 may be connected to an external device, etc., and / or the second pad structure 455 may be configured to send and / or receive electrical signals between the semiconductor device and the external device.
[0178] The second filling insulating film 470 may be formed on the second connection structure 450. The second filling insulating film 470 may at least partially fill the fourth trench t4 that may remain after filling the second connection structure 450. The second filling insulating film 470 may include, for example, but may not be limited to, silicon oxide (SiO), aluminum oxide (Al 2 O 3 ), tantalum oxide (TaO) and at least one of a combination thereof.
[0179] In some embodiments, the second capping pattern 475 may be formed on the second filling insulating film 470. The second capping pattern 475 may include a silicon-based insulating material (eg, silicon nitride (SiN), silicon oxide (SiO), and silicon oxynitride (SiO x N y )) and high dielectric materials (e.g., hafnium oxide (HfO 2 ) and aluminum oxide (Al 2 O 3 )). In some embodiments, the second capping pattern 475 may include a material substantially similar to and / or the same as the capping film 123. However, the present disclosure may not be limited thereto.
[0180] In some embodiments, the fourth protective film 480 may be formed on the second connection structure 450 of the pad region PAD. For example, the fourth protective film 480 may be formed to partially cover the first protective film 165 in the pad region PAD. In some embodiments, the second protective film 185 may extend along the surface of the fourth protective film 480. The fourth protective film 480 may include, for example, but may not be limited to, a light-transmitting resin. In some embodiments, the fourth protective film 480 may include a material substantially similar and / or the same as the microlens 180.
[0181] exist Fig.17In the embodiment of the present invention, the first pad pattern 195 may include a first barrier film 195BL and a first filling film 195FL. Alternatively or additionally, the first pad pattern 195 may include a first portion 195_1 and a second portion 195_2. The first portion 195_1 of the first pad pattern 195 may refer to a portion that may contact the second pad pattern 295. The second portion 195_2 of the first pad pattern 195 may be placed on the first portion 195_1 of the first pad pattern 195. The concentration of manganese (Mn) of the second portion 195_2 of the first pad pattern 195 may be less than the concentration of manganese (Mn) of the first portion 195_1 of the first pad pattern 195.
[0182] The second pad pattern 295 may include a second barrier film 295BL and a second filling film 295FL. Alternatively or additionally, the second pad pattern 295 may include a first portion 295_1 and a second portion 295_2. The first portion 295_1 of the second pad pattern 295 may refer to a portion in contact with the first pad pattern 195. The second portion 295_2 of the second pad pattern 295 may be placed below the first portion 295_1 of the second pad pattern 295. The concentration of manganese (Mn) of the second portion 295_2 of the second pad pattern 295 may be less than the concentration of manganese (Mn) of the first portion 295_1 of the second pad pattern 295.
[0183] In some embodiments, bonding the first semiconductor chip 100 and the second semiconductor chip 200 together may include bonding the first pad pattern 195 and the second pad pattern 295 together. As described above, according to some embodiments, since the bonding energy between the first pad pattern 195 and the second pad pattern 295 may be relatively high, the first semiconductor chip 100 and the second semiconductor chip 200 may be stably bonded.
[0184] Furthermore, according to some embodiments, even if the first pad pattern 195 and the second pad pattern 295 are not aligned with each other, the first pad pattern 195 and the second pad pattern 295 may be more stably bonded. Thus, a semiconductor device having improved reliability may be manufactured when compared to related semiconductor devices.
[0185] Reference Figures 18 to 20 A semiconductor device according to some embodiments is described. Figures 18 to 20 The semiconductor device shown may be and / or may include a flash memory device. Figures 1 to 14 A semiconductor device manufacturing method is described to manufacture a flash memory device.
[0186] Figures 18 to 20 A semiconductor device according to some embodiments is shown. Fig.18 , a circuit diagram of a flash memory device is shown. Fig.19A cross-sectional view of a flash memory device is shown. Fig. 20 yes Fig.19 A magnified view of region Q.
[0187] like Fig.18 As shown, a memory cell array of a semiconductor device may include a common source line CSL, a plurality of bit lines BL, and a plurality of cell strings CSTR.
[0188] The common source line CSL may extend in the x-direction X. In an embodiment, a plurality of common source lines CSL may be arranged two-dimensionally. For example, a plurality of common source lines CSL may extend in the x-direction X while being spaced apart from each other. Substantially similar and / or identical voltages may be electrically applied to the common source lines CSL, and / or the common source lines CSL may be individually controlled by applying different voltages.
[0189] A plurality of bit lines BL may be arranged two-dimensionally. For example, the bit lines BL may extend in a y direction Y intersecting with the x direction X while being spaced apart from each other. A plurality of cell strings CSTR may be connected in parallel to each bit line BL. The cell strings CSTR may be commonly connected to a common source line CSL. That is, a plurality of cell strings CSTR may be placed between the bit lines BL and the common source line CSL.
[0190] Each cell string CSTR may include a ground selection transistor GST connected to a common source line CSL, a string selection transistor SST connected to a bit line BL, and a plurality of memory cell transistors MCT placed between the ground selection transistor GST and the string selection transistor SST. Each memory cell transistor MCT may include a data storage element. The ground selection transistor GST, the string selection transistor SST, and the memory cell transistor MCT may be connected in series in a z-direction Z. As used herein, the x-direction X, the y-direction Y, and the z-direction Z may be substantially perpendicular to each other.
[0191] The common source line CSL may be commonly connected to the source of the ground selection transistor GST. Alternatively or additionally, the ground selection line GSL, a plurality of word lines WL1 to WLn, and a string selection line SSL may be placed between the common source line CSL and the bit line BL. The ground selection line GSL may be used as a gate electrode of the ground selection transistor GST, the word lines WL1 to WLn (where n is a positive integer greater than zero (0)) may be used as a gate electrode of the memory cell transistor MCT, and the string selection line SSL may be used as a gate electrode of the string selection transistor SST.
[0192] In some embodiments, the erase control transistor ECT may be placed between the common source line CSL and the ground selection transistor GST. The common source line CSL may be commonly connected to the source of the erase control transistor ECT. Alternatively or additionally, the erase control line ECL may be placed between the common source line CSL and the ground selection line GSL. The erase control line ECL may be used as a gate electrode of the erase control transistor ECT. The erase control transistor ECT may generate a gate induced drain leakage (GIDL) to perform an erase operation of the memory cell array.
[0193] Reference Fig.19 and Fig. 20 , the semiconductor device may be and / or may include a chip-to-chip (C2C) structure. The C2C structure may refer to a structure in which an upper chip may be manufactured on a first wafer and a lower chip may be manufactured on a second wafer different from the first wafer, and the upper chip and the lower chip may be connected to each other by a bonding process. The bonding process may refer to a manner of electrically connecting a bonding metal formed on the topmost metal layer of the upper chip to a bonding metal formed on the topmost metal layer of the lower chip. For example, when the bonding metal is formed of copper (Cu), the bonding may be referred to as Cu-Cu bonding. As another example, the bonding metal may be formed of other metals such as, but not limited to, aluminum (Al) and / or tungsten (W).
[0194] like Fig.19 As shown, the semiconductor device may include a unit substrate 500 , a mold structure MS, a first interlayer insulating film 520 , a channel structure CH, a word line cutting structure WLC, a bit line BL, a peripheral circuit board 600 , a peripheral circuit element PT, a first bonding pattern 595 , and a second bonding pattern 695 .
[0195] The unit substrate 500 may include, for example, a semiconductor substrate, such as, but not limited to, a silicon (Si) substrate, a germanium (Ge) substrate, or a silicon-germanium (Si-Ge) substrate. Alternatively or additionally, the unit substrate 500 may include a silicon-on-insulator (SOI) substrate, a germanium-on-insulator (GOI) substrate, etc. In some embodiments, the unit substrate 500 may include impurities. For example, the unit substrate 500 may include n-type impurities (e.g., phosphorus (P), arsenic (As), etc.).
[0196] The mold structure MS may be disposed on the front side of the unit substrate 500. The mold structure MS may include a plurality of gate electrodes (e.g., ECL, GSL, WL1 to WLn, and SSL) and a plurality of mold insulating films 510 that may be alternately stacked on the unit substrate 500. Each of the gate electrodes (e.g., ECL, GSL, WL1 to WLn, and SSL) and each mold insulating film 510 may have a layered structure that may extend in parallel with the front side of the unit substrate 500. The gate electrodes (e.g., ECL, GSL, WL1 to WLn, and SSL) may be spaced apart from each other by the mold insulating film 510 and / or may be sequentially stacked on the unit substrate 500.
[0197] In some embodiments, the gate electrodes (eg, ECL, GSL, WL1 to WLn, and SSL) may include an erase control line ECL, a ground selection line GSL, and a plurality of word lines WL1 to WLn that may be sequentially stacked on the unit substrate 500. In some other embodiments, the erase control line ECL may be omitted.
[0198] The gate electrodes (e.g., ECL, GSL, WL1 to WLn, and SSL) may include but may not be limited to conductive materials, for example, metals (such as tungsten (W), cobalt (Co), and nickel (Ni)) and / or semiconductor materials (such as silicon (Si)). For example, the gate electrodes (e.g., ECL, GSL, WL1 to WLn, and SSL) may include tungsten (W). The gate electrodes (e.g., ECL, GSL, WL1 to WLn, and SSL) may be and / or may include a multilayer film. For example, when the gate electrodes (e.g., ECL, GSL, WL1 to WLn, and SSL) are multilayer films, the gate electrodes (e.g., ECL, GSL, WL1 to WLn, and SSL) may include a gate electrode barrier film and a gate electrode filling film. The gate electrode barrier film may include, for example, titanium nitride (TiN), and / or the gate electrode filling film may include tungsten (W). However, the present disclosure may not be limited thereto.
[0199] The mold insulating film 510 may include an insulating material such as, but not limited to, silicon oxide (SiO), silicon nitride (SiN), and silicon oxynitride (SiO x N y As an example, the mold insulation layer 510 may include silicon oxide (SiO).
[0200] The channel structure CH may be disposed in the mold structure MS. The channel structure CH may penetrate the mold structure MS. For example, the channel structure CH may have a columnar shape (e.g., a cylindrical shape) extending in the z-direction Z. Thus, the channel structure CH may intersect each of the gate electrodes (e.g., ECL, GSL, WL1 to WLn, and SSL). The channel structure CH may be placed in a channel hole passing through the mold structure MS.
[0201] In some embodiments, the channel structure CH may include a semiconductor pattern 530 and an information storage film 532 .
[0202] The semiconductor pattern 530 may extend in the z-direction Z and penetrate the mold structure MS. Although the semiconductor pattern 530 is shown as having a cup shape, this is only an example. For example, the semiconductor pattern 530 may have various shapes, such as but not limited to a cylindrical shape, a rectangular barrel shape, a solid filler shape, etc. The semiconductor pattern 530 may include, for example, but not limited to, a semiconductor material, such as but not limited to single crystal silicon, polycrystalline silicon, an organic semiconductor substance, and a carbon nanostructure.
[0203] The information storage film 532 may be interposed between the semiconductor pattern 530 and each of the gate electrodes (e.g., ECL, GSL, WL1 to WLn, and SSL). For example, the information storage film 532 may extend along the outer side of the semiconductor pattern 530. As another example, the information storage film 532 may extend along the sidewall and bottom surface of the semiconductor pattern 530. The information storage film 532 may include, for example, silicon oxide (SiO), silicon nitride (SiN), silicon oxynitride (SiO x N y ) and / or at least one of a high dielectric constant material having a dielectric constant higher than silicon oxide (SiO). The high dielectric constant material may include, for example, aluminum oxide (Al 2 O 3 ), hafnium oxide (HfO 2 ), lanthanum oxide (LaO), tantalum oxide (TaO), titanium oxide (TiO), lanthanum hafnium oxide (LaHfO), lanthanum aluminum oxide (LaAlO), dysprosium scandium oxide (DyOSc) and / or at least one of their combinations.
[0204] In some embodiments, the information storage film 532 may be formed of a multi-layer film. Fig. 20 As shown, the information storage film 532 may include a tunnel insulating film 532 a , a charge storage film 532 b , and a blocking insulating film 532 c , which may be sequentially stacked on the outer side of the semiconductor pattern 530 .
[0205] The tunnel insulating film 532a may include, for example, silicon oxide (SiO) or a high dielectric constant material having a higher dielectric constant than silicon oxide (for example, aluminum oxide (Al2 O 3 )) and hafnium oxide (HfO 2 )). The charge storage film 532b may include, for example, silicon nitride (SiN). The blocking insulating film 532c may include, for example, silicon oxide (SiO) and / or a high dielectric constant material having a higher dielectric constant than silicon oxide (for example, aluminum oxide (Al 2 O 3 ) and hafnium oxide (HfO 2 )).
[0206] In some embodiments, the channel structure CH may further include a filling pattern 534. The filling pattern 534 may be formed to at least partially fill the inside of the cup-shaped semiconductor pattern 530. The filling pattern 534 may include, but may not be limited to, an insulating material, for example, silicon oxide (SiO).
[0207] In some embodiments, the channel structure CH may further include a channel pad 536. The channel pad 536 may be formed to be connected to the semiconductor pattern 530. For example, the channel pad 536 may be formed in the first interlayer insulating film 520 and connected to an upper portion of the semiconductor pattern 530. The channel pad 536 may include, for example, but may not be limited to, doped polysilicon.
[0208] In some embodiments, the source layer 502 and the source support layer 504 may be placed on the unit substrate 500. The source layer 502 and the source support layer 504 may be interposed between the unit substrate 500 and the mold structure MS.
[0209] In some embodiments, the source layer 502 may be formed to be connected to the semiconductor pattern 530 of the channel structure CH. Fig. 20 As shown, the source layer 502 may penetrate the information storage film 532 and may contact the semiconductor pattern 530. As another example, the source layer 502 may penetrate the sidewall of the information storage film 532 and may be connected to the semiconductor pattern 530.
[0210] In some embodiments, the source layer 502 may be provided as a common source line (eg, Fig.18 The source layer 502 may be formed of, for example but not limited to, a doped polysilicon film and / or a conductive film.
[0211] The word line cutting structure WLC may cut the mold structure MS. The word line cutting structure WLC may cut the gate electrodes (e.g., ECL, GSL, WL1 to WLn, and SSL). The mold structure MS may be cut by the word line cutting structure WLC to form a plurality of memory cell blocks. For example, two adjacent word line cutting structures WLC may define (e.g., define) a memory cell block therebetween. A plurality of channel structures CH may be placed inside each memory cell block defined by the word line cutting structure WLC.
[0212] In some embodiments, the word line cutting structure WLC may include an insulating material. For example, the insulating material may fill the word line cutting structure WLC. The insulating material may include, for example, but may not be limited to, silicon oxide (SiO), silicon nitride (SiN), and silicon oxynitride (SiO x N y ) at least one of.
[0213] The first interlayer insulating film 520 may be placed on the mold structure MS. The first interlayer insulating film 520 may at least partially cover the mold structure MS and the plurality of channel structures CH. The first interlayer insulating film 520 may include an oxide-based insulating material. The first interlayer insulating film 520 may include, for example but not limited to, silicon oxide (SiO), silicon oxynitride (SiO x N y ) and / or at least one of a low dielectric constant (low-k) material having a dielectric constant lower than silicon oxide (SiO).
[0214] In some embodiments, the bit line BL may be placed on the mold structure MS. The bit line BL may be a bit line of the semiconductor device ( Fig.18 The bit line BL may extend in the y direction Y. The bit line BL may be connected to a plurality of channel structures CH. A bit line contact plug BLPG that may be connected to each channel structure CH may be formed in the first interlayer insulating film 520. The bit line contact plug BLPG may be connected to the channel pad 536. The bit line BL may include a conductive material. For example, the bit line BL may include, but may not be limited to, tungsten (W) and / or copper (Cu).
[0215] The second interlayer insulating film 585 may be disposed on the bit line BL. The second interlayer insulating film 585 may be formed of silicon oxide (SiO). The first bonding layer 590 may be disposed on the second interlayer insulating film 585. The first bonding layer 590 may be formed of, for example, silicon carbonitride (SiCN).
[0216] The first bonding pattern 595 may be placed in the second interlayer insulating film 585. The first bonding pattern 595 may include a first bonding barrier film 595BL and a first bonding filling film 595FL. The first bonding pattern 595 may contain manganese (Mn). The concentration of manganese (Mn) in the first bonding pattern 595 may gradually increase with respect to the distance away from the bit line BL.
[0217] In some embodiments, the first bonding pattern 595 may be aligned with the reference Figures 1 to 12 The upper pad patterns PP_U described are substantially similar and / or identical. The cell bonding contact 580 may be disposed between the first bonding pattern 595 and the bit line BL.
[0218] The peripheral circuit board 600 may be placed on the bit line BL. The peripheral circuit board 600 may include, for example, a semiconductor substrate such as a silicon (Si) substrate, a germanium (Ge) substrate, and / or a silicon-germanium (Si-Ge) substrate. Alternatively or additionally, the peripheral circuit board 600 may include a silicon-on-insulator (SOI) substrate, a germanium-on-insulator (GOI) substrate, etc.
[0219] The peripheral circuit element PT may be formed on the peripheral circuit board 600. The peripheral circuit element PT may constitute a peripheral circuit that may control the operation of the semiconductor device. For example, the peripheral circuit element PT may include control logic, a row decoder, a page buffer, etc. As used herein, the surface of the peripheral circuit board 600 on which the peripheral circuit element PT may be placed may be referred to as the front side of the peripheral circuit board 600. Alternatively or additionally, the surface of the peripheral circuit board 600 that may be opposite to the front side of the peripheral circuit board 600 may be referred to as the rear side of the peripheral circuit board 600. In some embodiments, the front side of the peripheral circuit board 600 may face the front side of the unit substrate 500.
[0220] The peripheral circuit element PT may include, for example, a transistor, but may not be limited to a transistor. For example, the peripheral circuit element PT may include various active elements (eg, transistors, etc.) and / or various passive elements (eg, capacitors, resistors, inductors, etc.).
[0221] The peripheral circuit element PT may be separated by a peripheral element isolation film 605. For example, the peripheral element isolation film 605 may be disposed inside the peripheral circuit board 600. The peripheral element isolation film 605 may be a shallow trench isolation (STI) film. The peripheral element isolation film 605 may define (e.g., delimit) an active area of the peripheral circuit element PT. The peripheral element isolation film 605 may include an insulating material. The peripheral element isolation film 605 may include, for example, silicon nitride (SiN), silicon oxide (SiO), and silicon oxynitride (SiO x N y ) at least one of.
[0222] The semiconductor device may further include a plurality of peripheral wiring patterns (e.g., a first wiring pattern 632 and a second wiring pattern 633), a third interlayer insulating film 620, and a plurality of peripheral wiring contacts 631. The plurality of peripheral wiring patterns 632 and 633 and the plurality of peripheral wiring contacts 631 may be electrically connected to each other. Each of the plurality of peripheral wiring patterns 632 and 633 and the plurality of peripheral wiring contacts 631 may include a conductive material. For example, each of the plurality of peripheral wiring patterns 632 and 633 and the plurality of peripheral wiring contacts 631 may include, but may not be limited to, tungsten (W) or copper (Cu).
[0223] The second bonding film 690 may be placed on the second interlayer insulating film 585. The second bonding film 690 may be formed of, for example, silicon carbon nitride (SiCN).
[0224] The second bonding pattern 695 may be placed in the third interlayer insulating film 620. The second bonding pattern 695 may include a second bonding barrier film 695BL and a second bonding filling film 695FL. The second bonding pattern 695 may contain manganese (Mn). As the distance from the peripheral circuit element PT increases, the concentration of manganese (Mn) in the second bonding pattern 695 may gradually increase.
[0225] In some embodiments, the second bonding pattern 695 may be aligned with the reference Figures 1 to 12 The lower pad patterns PP_L discussed are substantially similar and / or identical. The peripheral bonding contact 680 may be disposed between the second bonding pattern 695 and the wiring pattern 633 .
[0226] In some embodiments, the first bonding pattern 595 and the second bonding pattern 695 may be bonded together to manufacture a semiconductor device. As described above, according to some embodiments, since the bonding energy between the first bonding pattern 595 and the second bonding pattern 695 is relatively high, the upper chip and the lower chip may be stably bonded.
[0227] In addition, according to some embodiments of the present disclosure, even when the first bonding pattern 595 and the second bonding pattern 695 are not aligned with each other, the first bonding pattern 595 and the second bonding pattern 695 can be bonded to each other relatively more stably. Therefore, when compared with related semiconductor devices, a semiconductor device with improved reliability can be manufactured.
[0228] Although the present invention has been described with reference to illustrative embodiments, this description is not intended to be interpreted as limiting. Various modifications and combinations of the illustrative embodiments and other embodiments of the present invention will be apparent to those skilled in the art after reference to this description. Therefore, it is intended that the appended claims cover any such modifications or embodiments.
Claims
1. A method for manufacturing a semiconductor device, include: forming a lower chip and an upper chip; as well as bonding the lower chip and the upper chip to each other; Wherein, forming the lower chip comprises: providing a lower substrate; sequentially forming a lower interlayer insulating film and a pre-lower adhesive film on the lower substrate; etching a first portion of the pre-lower adhesive film and a second portion of the lower interlayer insulating film to form a lower trench; forming a first lower seed film in the lower trench using a sputtering process; and forming a second lower seed film on the first lower seed film using the sputtering process, Wherein, forming the upper chip comprises: providing an upper substrate; sequentially forming an upper interlayer insulating film and a pre-adhesive film on the upper substrate; etching a third portion of the pre-upper adhesive film and a fourth portion of the upper interlayer insulating film to form an upper trench; forming a first upper seed film in the upper trench using the sputtering process; and forming a second upper seed film on the first upper seed film using the sputtering process, and The second lower seed film and the second upper seed film include manganese (Mn).
2. The method for manufacturing a semiconductor device according to claim 1, in, forming the lower chip further comprises etching the first lower seed film and the second lower seed film to form a lower pad pattern, and Wherein, forming the upper chip further comprises etching the first upper seed film and the second upper seed film to form an upper pad pattern.
3. The method for manufacturing a semiconductor device according to claim 2, in, Bonding the lower chip and the upper chip includes bonding the lower pad pattern and the upper pad pattern to each other.
4. The method for manufacturing a semiconductor device according to claim 2, in, forming the lower pad pattern includes forming the lower pad pattern to include a fifth portion and a sixth portion on the fifth portion, the sixth portion contacting the upper pad pattern, and The first concentration of manganese (Mn) in the fifth portion is lower than the second concentration of manganese (Mn) in the sixth portion.
5. The method for manufacturing a semiconductor device according to claim 2, in, Forming the lower pad pattern includes etching the pre-lower adhesive film to form a lower adhesive film having a first upper surface coplanar with a second upper surface of the lower pad pattern and at least a portion of the lower adhesive film in contact with the upper pad pattern. 6 . The method for manufacturing a semiconductor device according to claim 5 , further comprising providing manganese (Mn) at a boundary between the lower adhesive film and the upper pad pattern.
7. The method for manufacturing a semiconductor device according to claim 1, in, Forming the lower chip includes forming a preliminary lower barrier film along a bottom surface and one or more sidewalls of the lower trench before forming the first lower seed film.
8. The method for manufacturing a semiconductor device according to claim 1, in, forming the lower chip comprises: performing a heat treatment process after forming the second lower seed film, and Wherein, performing the heat treatment process includes performing the heat treatment process at a first temperature lower than 200°C.
9. The method for manufacturing a semiconductor device according to claim 8, in, Performing the heat treatment process includes performing the heat treatment process at a second temperature higher than 100°C.
10. A method for manufacturing a semiconductor device, include: forming a lower pad pattern and an upper pad pattern; as well as bonding the lower land pattern and the upper land pattern to each other, Wherein, forming the lower pad pattern comprises: providing a lower interlayer insulating film; etching a first portion of the lower interlayer insulating film to form a lower trench; forming a first lower seed film in the lower trench using a sputtering process; and forming a second lower seed film on the first lower seed film using the sputtering process, Wherein, forming the upper pad pattern comprises: providing an upper interlayer insulating film; etching a second portion of the upper interlayer insulating film to form an upper trench; forming a pre-upper barrier film in the upper trench along a bottom surface and one or more sidewalls of the upper trench; forming a first upper seed film on the pre-upper barrier film using the sputtering process; forming a pre-upper filling film on the first upper seed film; etching a third portion of the pre-fill film to form a recess; and A second upper seed film is formed in the groove using the sputtering process, and wherein the second lower seed film and the second upper seed film include manganese (Mn).
11. The method for manufacturing a semiconductor device according to claim 10, in, A first thickness of the lower pad pattern in a vertical direction is smaller than a second thickness of the upper pad pattern in the vertical direction.
12. The method for manufacturing a semiconductor device according to claim 11, in, The forming of the lower pad pattern further includes: performing a heat treatment process after forming the second lower seed film, and Wherein, performing the heat treatment process includes performing the heat treatment process at a temperature lower than 200°C.
13. The method for manufacturing a semiconductor device according to claim 10, in, forming the lower pad pattern further includes forming the lower pad pattern to include a fourth portion and a fifth portion on the first portion, the fifth portion contacting the upper pad pattern, and The first concentration of manganese (Mn) in the fourth portion is less than the second concentration of manganese (Mn) in the fifth portion.
14. The method for manufacturing a semiconductor device according to claim 10, in, forming the lower pad pattern further comprises forming a lower adhesive film on the lower interlayer insulating film, Wherein, forming the upper pad pattern further comprises forming an upper adhesive film on the upper interlayer insulating film, wherein bonding the lower pad pattern and the upper pad pattern comprises bonding the lower adhesive film and the upper adhesive film, and Wherein, a first upper surface of the lower adhesive film is coplanar with a second upper surface of the lower pad pattern.
15. The method for manufacturing a semiconductor device according to claim 14, in, At least a portion of the lower adhesive film is in contact with the upper pad pattern, and The semiconductor device manufacturing method further includes providing manganese (Mn) at a boundary between the lower adhesive film and the upper pad pattern.
16. The method for manufacturing a semiconductor device according to claim 14, in, At least a portion of the upper adhesive film contacts the lower pad pattern, and The semiconductor device manufacturing method further includes providing manganese (Mn) at a boundary between the upper adhesive film and the lower pad pattern.
17. The method for manufacturing a semiconductor device according to claim 10, in, Forming the pre-over-fill film includes forming the pre-over-fill film using an electroplating process.
18. A semiconductor device, include: a substrate including a first side and a second side opposite to each other; a plurality of unit pixels, in the substrate and including a photoelectric conversion layer; a pixel isolation pattern in the substrate and configured to separate the plurality of unit pixels; a first inter-wiring insulating film on the first side of the substrate; a first pad pattern in the first inter-wiring insulating film; a first adhesive film extending along a lower surface of the first inter-wiring insulating film; a second inter-wiring insulating film provided on the lower surface of the first inter-wiring insulating film; a second pad pattern provided in the second inter-wiring insulating film and in contact with the first pad pattern; a second adhesive film disposed along an upper surface of the second inter-wiring insulating film and in contact with the first adhesive film; as well as a microlens on the second side of the substrate, wherein the first pad pattern includes a first portion contacting the second pad pattern and a second portion on the first portion, The second pad pattern includes a third portion contacting the first pad pattern and a fourth portion below the third portion. wherein a first concentration of manganese (Mn) in the first portion of the first pad pattern is greater than a second concentration of manganese (Mn) in the second portion of the first pad pattern, and The third concentration of manganese (Mn) in the third portion of the second pad pattern is greater than the fourth concentration of manganese (Mn) in the fourth portion of the second pad pattern.
19. The semiconductor device according to claim 18, in, A first thickness of the first pad pattern in a vertical direction is greater than a second thickness of the second pad pattern in the vertical direction.
20. The semiconductor device according to claim 18, in, At least a portion of the first adhesive film is in contact with the second land pattern, and Here, manganese Mn is disposed at a boundary between the first adhesive film and the second pad pattern.