Lithium ion secondary battery, battery module, battery pack, and electric device
By using technical means such as high-thermal stability salts and low-impedance additives in lithium-ion secondary batteries, the composition of electrolytes was optimized, and the problem of electrolyte decomposition and life of lithium-ion secondary batteries under high energy density was solved, and better Cycle life and storage performance.
Patent Information
- Application Number
- CN202411116525.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-28
- Publication Date
- 2024-11-26
AI Technical Summary
While increasing the energy density of existing lithium-ion secondary batteries, it is difficult to take into account the cycle life and storage life of the battery cell, especially the accelerated decomposition of the electrolyte under high temperature conditions, resulting in the loss of active materials and deterioration of performance.
The electrolyte containing high-thermal stability salt My+x/yR1(SO2N-)xSO2R2 is used, and the content of high-thermal stability salt is adjusted by adjusting the temperature rise coefficient k1 of the positive electrode sheet, combined with low-impedance additives and lithium salts that inhibit corrosion of aluminum foil. , optimize the composition of the electrolyte to meet specific relationships and proportions, to reduce the impact of high temperature on the electrolyte and improve the performance of the cell.
While increasing the energy density of the battery cell, it extends the cycle life and storage life of the battery, reduces the risk of decomposition of the electrolyte, and improves the overall performance of the battery.
Smart Images

Figure CN119029318A_ABST
Abstract
Description
[0001] This application is a divisional application based on the invention with application number 202180006343.7, application date May 28, 2021, applicant is Contemporary Amperex Technology Co., Ltd., and invention name is "Lithium-ion secondary battery, battery module, battery pack, and electrical device". Technical Field
[0002] The present application relates to the field of lithium-ion secondary batteries, and in particular to a lithium-ion secondary battery, a battery module, a battery pack, and an electrical device with high energy density. Background Art
[0003] Lithium-ion batteries have become the most popular energy storage system due to their low cost, long life, and good safety. They are now widely used in pure electric vehicles, hybrid electric vehicles, smart grids, etc. However, the current lithium-ion secondary batteries are difficult to meet people's higher demand for endurance. To break the problem of "range anxiety" of electric vehicles, it is urgent to develop lithium-ion secondary batteries with higher energy density.
[0004] The energy density can be effectively increased by increasing the discharge capacity per unit volume of active materials in lithium-ion secondary batteries. For example, by reducing the carbon content as a conductive agent on the electrode or the amount of carbon coating on the surface of the positive electrode material particles, the weight of the active material per unit volume can be increased, thereby increasing the discharge capacity per unit volume of the active material. In addition, by increasing the coating weight of the active material and reducing the proportion of inactive substrates used, the discharge capacity per unit volume of the active material can be further improved. However, while achieving high energy density, the above strategy will significantly increase the internal resistance of the battery cell. When charging at a high rate, the battery cell will release heat severely and is therefore under high temperature conditions. At this time, lithium salts such as LiPF in the electrolyte 6 It will accelerate the decomposition to produce HF and PF 5 These highly reactive components will accelerate the destruction of the SEI film, causing the active materials to be exposed to the electrolyte, resulting in the loss of active materials. The repair process of the SEI film will continue to consume active lithium and electrolyte, resulting in further deterioration of the battery cell cycle performance and storage life.
[0005] Therefore, there is a need to increase the energy density of lithium-ion secondary batteries while ensuring the cycle and storage life of the cells. Summary of the invention
[0006] The present application is made in view of the above-mentioned problems, and its purpose is to provide a lithium-ion secondary battery to solve the problem that high energy density cells generate a lot of heat during charging, resulting in electrolyte decomposition and poor cell cycle and storage life.
[0007] In order to achieve the above-mentioned object, the present application provides a lithium-ion secondary battery in a first aspect, which comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode material layer comprises a positive electrode active material and carbon, wherein:
[0008] The electrolyte contains lithium salt (M y+ ) x / y R 1 (SO 2 N - ) x SO 2 R 2 , where M y+ is a metal ion, R 1 , R 2 Each independently represents a fluorine atom, an alkyl group having 1 to 20 carbon atoms, a fluoroalkyl group having 1 to 20 carbon atoms, or a fluoroalkoxy group having 1 to 20 carbon atoms, and x is 1, 2 or 3, and y is 1, 2 or 3; the mass percentage of the lithium salt in the electrolyte is set to k2%;
[0009] The temperature rise coefficient k1 of the positive electrode sheet satisfies 2.5≤k1≤32, where k1=Cw / Mc, Cw is the positive electrode material loading per unit area on the surface of either side of the positive electrode current collector loaded with the positive electrode material layer (mg / cm 2 ), Mc is the carbon content of the positive electrode material layer (%);
[0010] Furthermore, the lithium ion secondary battery satisfies 0.34≤k2 / k1≤8.
[0011] By using a high thermal stability salt (M y+ ) x / y R 1 (SO 2 N - ) x SO 2 R 2 electrolyte, and make the high thermal stability salt (M y+ ) x / y (R 1 SO 2 N) x SO 2 R 2 The content of carbon satisfies a specific relationship with the positive electrode material loading and carbon content of the positive electrode sheet, which can reduce the impact of high temperature on the electrolyte while increasing the volume energy density of the battery cell, thereby obtaining better battery cell performance and solving the problem of difficulty in balancing high energy density and long life.
[0012] In any embodiment, the lithium ion secondary battery satisfies at least one of the following conditions 1) to 3):
[0013] 1) 3.3 ≤ k1 ≤ 14.5;
[0014] 2) 0.48 ≤ k2 / k1 ≤ 7;
[0015] 3)1≤Mc≤7.
[0016] By satisfying at least one of the above conditions 1) to 3), the energy density and / or charge and discharge performance and / or cycle life of the battery can be further improved.
[0017] In any embodiment, the M y+ Selected from Li + 、Na + , K + , Rb + , Cs + Mg 2+ , Ca 2+ , Ba 2+ 、Al 3+ , Fe 2+ , Fe 3+ 、Ni 2+ , and Ni 3+ At least one of, optionally, M y+ Selected from Li + 、Na + , K + , Rb + and Cs + By selecting the above cations, the power performance of the battery cell can be further improved.
[0018] In any embodiment, the R 1 , R 2 are each independently a fluorine atom, an alkyl group having 1 to 10 carbon atoms, a fluoroalkyl group having 1 to 10 carbon atoms, or a fluoroalkoxy group having 1 to 10 carbon atoms. 1 , R 2 Each independently is CH 3 CF 3 or F. By selecting R 1 , R 2 structure, which helps to improve the cycle performance of the battery.
[0019] In any embodiment, the electrolyte of the lithium ion secondary battery further contains a low impedance additive, and optionally, the low impedance additive is a fluorosulfonate NSO 3 F, difluorooxalate borate NDFOB, difluorophosphate NPO 2F 2 , difluorobisoxalate NDFOP, tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, wherein N is a metal ion of the salt, for example, Li + 、Na + , K + , Rb + , Cs + ; Optionally, the low impedance additive is at least one of lithium fluorosulfonate, lithium difluorooxalatoborate, tris(trimethylsilyl)phosphate and lithium difluorophosphate. These low impedance additives can reduce the impedance of the protective film (SEI film) on the surface of the positive and negative electrode sheets, and reduce the deterioration of battery performance caused by temperature rise.
[0020] In any embodiment, the mass percentage of the low impedance additive in the electrolyte is 0.1% to 10%, and can be 0.2% to 5%. By selecting the mass percentage of the low impedance additive, the battery cycle performance can be further improved.
[0021] In any embodiment, the electrolyte of the lithium ion secondary battery further contains a lithium salt that inhibits corrosion of the aluminum foil. Optionally, the lithium salt that inhibits corrosion of the aluminum foil is selected from LiPF 6 、LiAsF 6 , and LiBF 4 By adding lithium salt that inhibits the corrosion of aluminum foil, the corrosion of aluminum foil can be inhibited and the temperature rise inside the battery cell can be reduced.
[0022] In any embodiment, the mass percentage of the lithium salt that inhibits aluminum foil corrosion in the electrolyte is 0.1% to 10%, optionally 0.2% to 5%, optionally 1% to 3%. By selecting the content of the lithium salt that inhibits aluminum foil corrosion, the cycle performance of the battery can be further improved.
[0023] In any embodiment, the total lithium salt content in the electrolyte of the lithium ion secondary battery is in the range of 5wt%-50wt%, optionally in the range of 5wt%-37wt%, optionally in the range of 5wt%-23wt%, based on the total weight of the electrolyte. By selecting the total lithium salt content in the electrolyte, the cycle life and power performance of the lithium ion secondary battery can be improved.
[0024] In any embodiment, the positive electrode active material in the lithium ion secondary battery is selected from one or more of lithium transition metal oxides, lithium phosphates containing olivine structures and their respective modified compounds. Optionally, the lithium transition metal oxide is selected from lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide satisfying a+b+c=1 and a<0.8. a Cob Mn c O 2 , one or more of lithium nickel cobalt aluminum oxide and their modified compounds.
[0025] A second aspect of the present application provides a battery module, which includes the lithium-ion secondary battery of the first aspect of the present application.
[0026] A third aspect of the present application provides a battery pack, which includes the battery module of the second aspect of the present application.
[0027] The fourth aspect of the present application provides an electrical device comprising one or more selected from the lithium-ion secondary battery of the first aspect of the present application, the battery module of the second aspect of the present application, or the battery pack of the third aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work.
[0029] Figure 1 It is a schematic diagram of a lithium ion secondary battery according to one embodiment of the present application.
[0030] Figure 2 yes Figure 1 An exploded view of a lithium-ion secondary battery according to an embodiment of the present application is shown.
[0031] Figure 3 is a schematic diagram of a battery module according to an embodiment of the present application.
[0032] Figure 4 It is a schematic diagram of a battery pack according to one embodiment of the present application.
[0033] Figure 5 yes Figure 4 An exploded view of a battery pack according to an embodiment of the present application is shown.
[0034] Figure 6 Schematic diagram of a device using a lithium ion secondary battery according to an embodiment of the present application as a power source.
[0035] Description of Reference Numerals
[0036] 1 battery pack
[0037] 2 upper box
[0038] 3 lower cabinets
[0039] 4 battery modules
[0040] 5Lithium-ion secondary battery
[0041] 51 Shell
[0042] 52 electrode assembly
[0043] 53 Cover DETAILED DESCRIPTION
[0044] For simplicity, the present application specifically discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an undefined range; and any lower limit can be combined with other lower limits to form an undefined range, and any upper limit can be combined with any other upper limit to form an undefined range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an undefined range.
[0045] Lithium-ion secondary battery
[0046] Generally, lithium-ion secondary batteries include a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The separator is arranged between the positive electrode sheet and the negative electrode sheet to play a role of isolation. The electrolyte plays a role of conducting ions between the positive electrode sheet and the negative electrode sheet.
[0047] The lithium-ion secondary battery of the first aspect of the present application comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode material layer comprises a positive electrode active material and carbon, wherein:
[0048] The electrolyte contains lithium salt (My + )x / Yj Y 1 (SO 2 N-)xSO 2 R 2 , its structural formula can be written as:
[0049] (My+))x / y
[0050] Among them, My + is a metal ion, R 1 , R 2 Each independently represents a fluorine atom, an alkyl group having 1 to 20 carbon atoms, a fluoroalkyl group having 1 to 20 carbon atoms, or a fluoroalkoxy group having 1 to 20 carbon atoms, and x is 1, 2 or 3, and y is 1, 2 or 3; the mass percentage of the lithium salt in the electrolyte is set to k2%;
[0051] The temperature rise coefficient k1 of the positive electrode sheet satisfies 2.5≤k1≤32, where k1=Cw / Mc, Cw is the positive electrode material loading per unit area on the surface of either side of the positive electrode current collector loaded with the positive electrode material layer (mg / cm 2 ), Mc is the carbon content of the positive electrode material layer (%);
[0052] Furthermore, the lithium ion secondary battery satisfies 0.34≤k2 / k1≤8.
[0053] The carbon contained in the positive electrode material layer includes the carbon coated on the surface of the positive electrode active material and the carbon as a conductive agent optionally contained in the positive electrode slurry used to prepare the positive electrode material layer.
[0054] During the charging process, the temperature rise inside the battery cell mainly comes from the temperature rise of the positive electrode sheet, and the temperature rise of the positive electrode sheet is mainly related to the thickness and conductivity of the positive electrode sheet. The thickness of the positive electrode sheet is related to the positive electrode material loading Cw per unit area on the surface of either side of the positive electrode current collector loaded with the positive electrode material layer, and the conductivity is related to the carbon content Mc of the positive electrode material layer. Therefore, the positive electrode sheet temperature rise coefficient k1 is defined as Cw / Mc. When the charging current is constant, the heat generation inside the battery cell is basically positively correlated with the temperature rise coefficient k1. If k1 is too small, the positive electrode material loading is too low, and the carbon content of the positive electrode material layer is too high, and the proportion of inactive substrates is large, which affects the reduction of battery energy density; if k1 is too large, the heat generation of the battery cell is too high, and the positive electrode material loading is too high and the carbon content of the positive electrode material layer is too low, which will lead to a low solid phase transfer rate of lithium ions and deteriorate the battery charging and discharging performance.
[0055] In addition, by adding high thermal stability (M y+ ) x / y R 1 (SO 2 N) x SO 2 R 2 , which can significantly improve the heat resistance coefficient of the electrolyte and reduce the decomposition of the electrolyte at high temperature, so that the battery has a longer cycle life. However, the inventors found in their research that when the concentration of high thermal stability salt is too high, it will lead to an increase in electrolyte viscosity and deterioration of conductivity, which will in turn lead to an increase in the internal resistance of the battery cell. When the salt concentration is too low, the electrolyte has insufficient thermal stability and may decompose at high temperatures, thereby shortening the life of the battery cell. In addition, the inventors also found that the thermal stability salt (M y+ ) x / y R 1 (SO 2 N) x SO 2 R 2The relationship between the mass percentage k2 and the temperature rise coefficient k1 of the positive electrode has a great influence on the cycle life of the battery. When k2 and k1 satisfy the above relationship, while ensuring that the battery has a high energy density, it can also ensure sufficient electrolyte thermal stability, inhibit the decomposition of the electrolyte, and ensure that the battery has a long cycle life.
[0056] In some embodiments, the lithium-ion secondary battery satisfies: 3.3 ≤ k1 ≤ 14.5. By further selecting the value of k1, the energy density and / or charge-discharge performance of the battery can be further improved.
[0057] In some embodiments, the lithium-ion secondary battery satisfies: 0.48 ≤ k2 / k1 ≤ 7. By further selecting the value of k2 / k1, the cycle life of the battery can be further improved.
[0058] In some embodiments, the lithium-ion secondary battery satisfies: 1% ≤ Mc% ≤ 7%, optionally, the lithium-ion secondary battery satisfies: 1% < Mc% ≤ 5%. If the carbon content is too high, the following situations may occur: the proportion of the positive electrode active material per unit volume is low, thus reducing the battery energy density, and it will also lead to too large a surface area of the positive electrode material, thus being prone to water absorption and agglomeration, resulting in difficulty in processing the electrode sheet; if the carbon content is too low, the following situations may occur: the conductivity of the electrode sheet becomes poor, lithium metal deposition may occur during charging, affecting the cycle life of the battery and bringing safety risks.
[0059] In some embodiments, the lithium-ion secondary battery satisfies: 18 ≤ Cw ≤ 32. If the loading amount Cw of the positive electrode material is too low, the proportion of the non-active substrate (such as the current collector) may be large, thus reducing the energy density, while if Cw is too large, the coating difficulty may become high, and the transmission path of lithium ions in the direction perpendicular to the electrode sheet is greatly increased, resulting in difficulty for lithium ions to quickly escape from and embed into the active material, affecting the power performance of the battery cell.
[0060] In some embodiments, the M y+ is selected from at least one of Li + 、Na + 、K + 、Rb + 、Cs + 、Mg 2+ 、Ca 2+ 、Ba 2+ 、Al 3+ 、Fe 2+ 、Fe 3+ 、Ni 2+ 、and Ni 3+ ; optionally, M y+ is selected from Li + 、Na+ , K + , Rb + and Cs + The migration number of the above cations is larger, so that the power performance of the battery cell is better.
[0061] In some embodiments, the R 1 , R 2 are each independently a fluorine atom, an alkyl group having 1 to 10 carbon atoms, a fluoroalkyl group having 1 to 10 carbon atoms, or a fluoroalkoxy group having 1 to 10 carbon atoms. 1 , R 2 Each independently is CH 3 CF 3 or F. By selecting R 1 , R 2 The structure can increase the number of lithium ion migration and make lithium ions more easily dissociated. At the same time, the electrolyte viscosity is small, which makes the electrolyte conductivity higher, which can help improve the cycle performance of the battery.
[0062] In some embodiments, the electrolyte further contains a low impedance additive, and optionally, the low impedance additive is NSO 3 F (fluorosulfonate), NDFOB (difluorooxalate borate), NPO 2 F 2 At least one of (difluorophosphate), NDFOP (difluorobisoxalate), tris(trimethylsilyl)phosphate, tris(trimethylsilyl)phosphite, wherein N is a metal ion of the salt, for example, Li + 、Na + , K + , Rb + , Cs + Optionally, the low impedance additive is LiSO 3 F (lithium fluorosulfonate), LiDFOB (lithium difluorooxalatoborate), tris(trimethylsilyl)phosphate and LiPO 2 F 2(lithium difluorophosphate). Optionally, the mass percentage of the low-impedance additive in the electrolyte is 0.1% to 10%, and can be optionally 0.2% to 5%. In addition to the temperature rise of the positive electrode plate, the impedance of the protective film (SEI film) on the surface of the positive and negative electrode plates also has a great influence on the temperature rise inside the battery cell. The increase in the impedance value of the SEI film will further lead to the temperature rise of the battery cell during charging. Without wishing to be limited to theory, the low-impedance additive can be reduced on the surface of the negative electrode before the electrolyte solvent during the formation process, forming a layer of extremely low-impedance and dense protective film on the surface of the negative electrode, thereby inhibiting the reduction and decomposition of the solvent and other high-impedance additives in the electrolyte on the surface of the negative electrode, thereby reducing the impedance of the SEI film. In addition, if the content of the low-impedance additive is within the above range, the viscosity of the electrolyte will not increase, and the conductivity of the electrolyte can be maintained.
[0063] In some embodiments, the electrolyte further contains a lithium salt that inhibits aluminum foil corrosion. Optionally, the lithium salt that inhibits aluminum foil corrosion is selected from LiPF 6 、LiAsF 6 , and LiBF 4 At least one of. Optionally, the mass percentage of the lithium salt that inhibits aluminum foil corrosion in the electrolyte is 0.1% to 10%, optionally 0.2% to 5%, optionally 1% to 3%. The lithium salt that inhibits aluminum foil corrosion can inhibit aluminum foil corrosion, thereby inhibiting the increase in impedance of the aluminum current collector, reducing the temperature rise inside the battery cell, and improving the safety performance of the battery cell. When the content of the lithium salt that inhibits aluminum foil corrosion is within the above range, it can inhibit aluminum foil corrosion and will not have an adverse effect on the high temperature resistance of the electrolyte.
[0064] In some embodiments, the total lithium salt content in the electrolyte is in the range of 5wt%-50wt%, optionally in the range of 5wt%-37wt%, optionally in the range of 5wt%-23wt%, based on the total weight of the electrolyte. By selecting the total lithium salt content in the electrolyte, the cycle life and power performance of the lithium ion secondary battery can be improved.
[0065] In some embodiments, the positive electrode active material is selected from one or more of lithium transition metal oxides, olivine-structured lithium-containing phosphates and their respective modified compounds. Examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide LiNi a Co b Mn c O 2(a+b+c=1, a<0.8), one or more of lithium nickel cobalt aluminum oxide and modified compounds thereof. Examples of lithium phosphates containing olivine structure may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, a composite material of lithium iron manganese phosphate and carbon and modified compounds thereof. These materials can be obtained through commercial channels. Carbon may be coated on the surface of the positive active material.
[0066] In the present application, the carbon content Mc of the positive electrode material layer can be measured by equipment and methods known in the art. For example, it can be measured by scraping off the positive electrode material layer on the positive electrode current collector and then using an infrared absorption method, for example, referring to GB / T20123-2006 Determination of total carbon and sulfur content of steel-infrared absorption method after high-frequency induction furnace combustion.
[0067] [Electrolyte]
[0068] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The electrolyte includes electrolyte salt and solvent.
[0069] In the present application, the electrolyte salt may be a common electrolyte salt in lithium ion secondary batteries, such as a lithium salt, including the lithium salts described above as high thermal stability salts, lithium salts as low impedance additives, or lithium salts that inhibit corrosion of aluminum foil. As an example, the electrolyte salt may be selected from LiPF 6 (Lithium hexafluorophosphate), LiBF 4 (lithium tetrafluoroborate), LiAsF 6 (lithium hexafluoroarsenate), LiFSI (lithium bis(fluorosulfonyl imide), LiTFSI (lithium bis(trifluoromethanesulfonyl imide), LiTFS (lithium trifluoromethanesulfonate), LiDFOB (lithium difluorooxalatoborate), LiPO 2 F 2 (lithium difluorophosphate), LiDFOP (lithium difluorobis(oxalate)phosphate), LiSO 3 F (lithium fluorosulfonate), NDFOP (difluorobisoxalate), Li 2 F(SO 2 N) 2 SO 2 F, KFSI, CsFSI, Ba(FSI) 2 and LiFSO 2 NSO 2 CH 2 CH 2 CF 3 One or more of the following.
[0070] The type of the solvent is not particularly limited and can be selected according to actual needs. In some embodiments, the solvent is a non-aqueous solvent. Optionally, the solvent may include one or more of linear carbonates, cyclic carbonates, and carboxylates. In some embodiments, the solvent may be selected from ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), tetrahydrofuran, cyclopentane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE). One or more.
[0071] In some embodiments, the electrolyte may also optionally include other additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high temperature performance, and additives that improve battery low temperature performance. As an example, the additive is selected from at least one of a cyclic carbonate compound containing an unsaturated bond, a halogen-substituted cyclic carbonate compound, a sulfate compound, a sulfite compound, a sultone compound, a disulfonic acid compound, a nitrile compound, an aromatic compound, an isocyanate compound, a phosphazene compound, a cyclic anhydride compound, a phosphite compound, a phosphate compound, a borate compound, and a carboxylate compound.
[0072] [Positive electrode]
[0073] The positive electrode sheet includes a positive electrode current collector and a positive electrode material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode material layer includes a positive electrode active material and carbon.
[0074] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode material layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.
[0075] In the lithium-ion secondary battery of the present application, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (such as aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0076] The positive electrode material layer may optionally include a conductive agent. However, there is no specific limitation on the type of the conductive agent, and those skilled in the art may select the conductive agent according to actual needs. As an example, the conductive agent used for the positive electrode material may be selected from one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0077] The positive electrode material layer may also optionally include a binder. As an example, the binder may be one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB).
[0078] In the present application, the positive electrode sheet can be prepared according to methods known in the art. As an example, the carbon-coated positive electrode active material, the conductive agent and the binder can be dispersed in a solvent (such as N-methylpyrrolidone (NMP)) to form a uniform positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet is obtained.
[0079] [Negative electrode]
[0080] The negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode material layer includes a negative electrode active material.
[0081] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode material layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0082] In the lithium ion secondary battery of the present application, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (e.g., copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (e.g., a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0083] In the lithium-ion secondary battery of the present application, the negative electrode material layer generally comprises a negative electrode active material and an optional binder, an optional conductive agent and other optional auxiliary agents, and is generally formed by coating and drying a negative electrode slurry. The negative electrode slurry coating is generally formed by dispersing the negative electrode active material and the optional conductive agent and binder in a solvent and stirring them uniformly. The solvent may be N-methylpyrrolidone (NMP) or deionized water.
[0084] The specific type of the negative electrode active material is not limited, and active materials known in the art that can be used for the negative electrode of lithium-ion secondary batteries can be used, and those skilled in the art can select according to actual needs. As an example, the negative electrode active material can be selected from one or more of graphite, soft carbon, hard carbon, mesophase carbon microspheres, carbon fibers, carbon nanotubes, elemental silicon, silicon oxides, silicon-carbon composites, and lithium titanate.
[0085] As an example, the conductive agent may be selected from one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0086] As an example, the binder can be selected from one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0087] Other optional auxiliary agents include, for example, thickeners (such as sodium carboxymethyl cellulose (CMC-Na)).
[0088] [Isolation film]
[0089] The lithium-ion secondary battery using an electrolyte also includes a separator. The separator is arranged between the positive electrode plate and the negative electrode plate to play an isolating role. The present application has no particular restrictions on the type of separator, and any known porous structure separator with good chemical stability and mechanical stability can be selected. In some embodiments, the material of the separator can be selected from one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular restrictions. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular restrictions.
[0090] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0091] In some embodiments, the lithium-ion secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.
[0092] In some embodiments, the outer packaging of the lithium ion secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the lithium ion secondary battery can also be a soft package, such as a bag-type soft package. The material of the soft package can be plastic, and as plastic, polypropylene (PP), polybutylene terephthalate (PBT) and polybutylene succinate (PBS) can be listed.
[0093] The present application has no particular limitation on the shape of the lithium-ion secondary battery, which may be cylindrical, square, or any other shape. Figure 1 The lithium ion secondary battery 5 is a square structure as an example.
[0094] In some embodiments, reference Figure 2 , the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the lithium-ion secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0095] In some embodiments, lithium-ion secondary batteries can be assembled into a battery module. The number of lithium-ion secondary batteries contained in the battery module can be one or more, and the specific number can be selected by those skilled in the art according to the application and capacity of the battery module.
[0096] Figure 34 is an example of a battery module. Figure 3 In the battery module 4, the plurality of lithium-ion secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of lithium-ion secondary batteries 5 may be fixed by fasteners.
[0097] Optionally, the battery module 4 may further include a housing having a housing space, and the plurality of lithium-ion secondary batteries 5 are housed in the housing space.
[0098] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be selected by those skilled in the art according to the application and capacity of the battery pack.
[0099] Figure 4 and Figure 5 1 is a battery pack 1 as an example. Figure 4 and Figure 5 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.
[0100] In addition, the present application also provides a device, the device includes one or more of the lithium-ion secondary battery, battery module, or battery pack provided in the present application. The lithium-ion secondary battery, battery module, or battery pack can be used as a power source for the device, and can also be used as an energy storage unit for the device. The device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc.
[0101] As the device, a lithium-ion secondary battery, a battery module or a battery pack may be selected according to its use requirements.
[0102] Figure 6 The device is used as an example. The device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the device's requirements for high power and high energy density of lithium-ion secondary batteries, a battery pack or a battery module can be used.
[0103] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a lithium-ion secondary battery may be used as a power source.
[0104] Example
[0105] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0106] 1. Preparation of lithium-ion secondary batteries
[0107] (1) Preparation of positive electrode sheet
[0108] The carbon-coated lithium iron phosphate (LFP) as the positive electrode active material, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) were dissolved in the solvent N-methylpyrrolidone (NMP) according to the weight ratio shown in Table 1, and the positive electrode slurry was obtained after being fully stirred and mixed. The carbon-coated lithium iron phosphate used had the carbon content shown in Table 1. Then, according to the Cw value to be achieved, the positive electrode slurry was evenly coated on the aluminum positive electrode collector, and then dried, cold pressed, and cut to obtain the positive electrode sheet.
[0109] (2) Preparation of negative electrode
[0110] The negative electrode active material artificial graphite, the conductive agent acetylene black, the binder styrene butadiene rubber (SBR), and the thickener sodium carboxymethyl cellulose (CMC-Na) were dissolved in the solvent deionized water at a weight ratio of 95:2:2:1, and mixed evenly to prepare the negative electrode slurry. Then, the negative electrode loading amount was determined according to the Cw value of the corresponding positive electrode, and the negative electrode slurry was evenly coated on the negative electrode current collector copper foil according to the negative electrode loading amount shown in Table 1, and after drying, the negative electrode sheet was obtained by cold pressing and slitting.
[0111] Table 1 (the embodiments or comparative examples using the same parameter values are listed in the same row)
[0112]
[0113]
[0114] (3) Preparation of electrolyte
[0115] In an argon atmosphere glove box (H 2 O<0.1ppm, O 2 <0.1ppm), the organic solvent EC / EMC is uniformly mixed in a volume ratio of 3 / 7, 3wt% of vinylene carbonate and the high thermal stability salt and optional additives in the weight percentages shown in Table 2 are added, and stirred evenly to obtain the corresponding electrolyte, wherein the weight percentage of the vinylene carbonate and the weight percentages shown in Table 2 are both based on the total weight of the obtained electrolyte.
[0116] (4) Preparation of lithium-ion secondary batteries
[0117] The positive electrode sheet prepared in (1) and the negative electrode sheet prepared in (2) are used, and a polypropylene film is used as a separator. The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is between the positive and negative electrode sheets to play a role of isolation, and then wound to obtain an electrode assembly. The electrode assembly is placed in a battery housing, and after drying, an electrolyte is injected, and then a lithium-ion secondary battery is obtained after formation and standing.
[0118] 2. Testing of lithium-ion secondary batteries
[0119] (1) Carbon content test of positive electrode
[0120] Test instrument: High frequency infrared carbon and sulfur analyzer, model HCS-140, purchased from Shanghai Dekai Instrument Co., Ltd.
[0121] Refer to GB / T20123-2006 Determination of total carbon and sulfur content of steel-infrared absorption method after combustion in a high-frequency induction furnace (conventional method). Test process: Scrape off the positive electrode material layer on the positive electrode current collector, heat and burn it in the above-mentioned high-frequency furnace under oxygen-rich conditions, and oxidize the carbon contained in the material into carbon dioxide. The generated gas is treated and introduced into the corresponding absorption cell to absorb the corresponding infrared radiation and convert it into a corresponding digital signal through a detector. The obtained digital signal is sampled by a computer, linearly corrected, converted into a numerical value proportional to the carbon dioxide concentration, and accumulated to obtain a cumulative value. Divide the obtained cumulative value by the sample weight, multiply it by the correction factor, and subtract the blank to obtain the carbon percentage Mc (%) in the sample.
[0122] (2) 45℃ Cycling Performance Test of Lithium-ion Secondary Batteries
[0123] At 45°C, the lithium-ion secondary battery is charged to 3.65V at 1C constant current, then charged to a current of less than 0.05C at 3.65V constant voltage, and then discharged to 2.5V at 1C constant current. This is a charge and discharge process. The charging and discharging are repeated in this way, and the number of cycles when the capacity retention rate of the lithium-ion battery is 80% is calculated. The number of cycles at 45°C of each embodiment and comparative example is shown in Table 1.
[0124] (3) Volume energy density test
[0125] At 25°C, the lithium-ion battery is charged to 3.65V at a constant current of 0.5C, then charged at a constant voltage of 3.65V until the current is less than 0.05C, and then discharged to 2.5V at 0.33C to obtain the discharge energy Q. The length, width, and height of the battery cell are measured with a vernier caliper to calculate the volume V. Volume energy density = Q / V
[0126] Table 2 shows Mc, Cw, k1, k2, volume energy density and 45° C. cycle performance of the lithium ion batteries of the embodiments and comparative examples.
[0127]
[0128]
[0129] As can be seen from Table 1, the k1 of Comparative Example 1 is too low, and accordingly, the energy density of the battery is low. In Comparative Examples 2 to 3, k1 is increased by increasing the loading amount of the positive electrode material layer and reducing the carbon content, and accordingly, the volume energy density of the battery is significantly improved, but the excessively high k1 causes the cycle life of the battery cell to deteriorate significantly. Even if Comparative Example 3 uses a high thermal stability salt and the value of k2 / k1 falls within the scope of this application, the cycle life is still relatively low. On the other hand, the k1 values of Comparative Examples 4-5 fall within the scope of this application, but k2 / k1 is too high or too low, so the cycle life is low.
[0130] In comparison, Examples 1-25 simultaneously use an electrolyte containing a highly stable lithium salt and a positive electrode plate with a large positive electrode material layer load and a low carbon content, which enables the battery cell to have both high energy density and long cycle life.
[0131] Comparing Example 1 with Example 2, it can be seen that the k2 / k1 value of Example 1 is in the range of 0.48-7, thereby obtaining better cycle performance than Example 2. Comparing Example 1 with Example 4, it can be seen that the k1 value of Example 1 is in the range of 3.3-14.5, thereby obtaining better cycle performance than Example 4.
[0132] It can be seen from Examples 8-24 that by adding a low-impedance additive to the electrolyte, the cycle life of the battery can be further improved while ensuring that the battery has a high energy density.
[0133] It can be seen from Examples 16-21 that adding a lithium salt that inhibits aluminum foil corrosion to the electrolyte can inhibit aluminum foil corrosion and reduce the increase in the impedance value of the aluminum foil, thereby further improving the battery cycle life. In addition, when the mass percentage of the lithium salt that inhibits aluminum foil corrosion is in the range of 0.2%-5% (Examples 16, 19-20), the battery cycle life can be further improved.
[0134] Although the present application has been described with reference to the embodiments, various modifications may be made thereto and parts thereof may be replaced with equivalents without departing from the scope of the present application. In particular, the various technical features mentioned in the various embodiments may be combined in any manner as long as there is no structural conflict. The present application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A lithium ion secondary battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the positive electrode sheet comprises a positive electrode current collector and a positive electrode material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode material layer comprises a positive electrode active material and carbon, and wherein the electrolyte comprises a high thermal stability salt (M y+ ) x / y R1(SO2N-) x SO2R2, low impedance additives and lithium salts for inhibiting corrosion of aluminum foil, wherein The M y+ is a metal ion, R1 and R2 are each independently a fluorine atom, an alkyl group having 1 to 20 carbon atoms, a fluoroalkyl group having 1 to 20 carbon atoms, or a fluoroalkoxy group having 1 to 20 carbon atoms, and x is 1, 2 or 3, and y is 1, 2 or 3; The mass percentage of the high thermal stability salt in the electrolyte is 3.1% to 35.4%; The mass percentage of the low impedance additive in the electrolyte is 0.1% to 10%; The total lithium salt content in the electrolyte is 5wt% to 50wt%.
2. The lithium ion secondary battery according to claim 1, wherein The mass percentage of the high thermal stability salt in the electrolyte is 6.9% to 21.5%.
3. The lithium ion secondary battery according to claim 1, wherein The mass percentage of the high thermal stability salt in the electrolyte is 15.4% to 20%.
4. The lithium ion secondary battery according to any one of claims 1 to 3, wherein The M y+ Selected from Li + 、Na + , K + , Rb + , Cs + Mg 2+ , Ca 2+ , Ba 2+ 、Al 3+ , Fe 2+ , Fe 3+ 、Ni 2+ , and Ni 3+ At least one of .
5. The lithium ion secondary battery according to claim 4, wherein: M y+ Selected from Li + 、Na + , K + , Rb + and Cs + At least one of .
6. The lithium ion secondary battery according to any one of claims 1 to 5, wherein: The R1 and R2 are each independently a fluorine atom, an alkyl group having 1 to 10 carbon atoms, a fluoroalkyl group having 1 to 10 carbon atoms, or a fluoroalkoxy group having 1 to 10 carbon atoms.
7. The lithium ion secondary battery according to claim 6, wherein: The R1 and R2 are each independently CH3, CF3 or F.
8. The lithium ion secondary battery according to any one of claims 1 to 7, wherein: The mass percentage of the low-impedance additive in the electrolyte is 0.2% to 5%.
9. The lithium ion secondary battery according to claim 8, wherein: The mass percentage of the low-impedance additive in the electrolyte is 1.5% to 5%.
10. The lithium ion secondary battery according to any one of claims 1 to 9, wherein: The low impedance additive is at least one of fluorosulfonate NSO3F, difluorooxalatoborate NDFOB, difluorophosphate NPO2F2, difluorobisoxalate NDFOP, tris(trimethylsilyl)phosphate, and tris(trimethylsilyl)phosphite, wherein N is a metal ion of the salt.
11. The lithium ion secondary battery according to claim 10, wherein: N is Li + 、Na + , K + , Rb + , Cs + One or more of .
12. The lithium ion secondary battery according to claim 10 or 11, wherein The low impedance additive is at least one of lithium fluorosulfonate, lithium difluorooxalatoborate, tris(trimethylsilyl)phosphate and lithium difluorophosphate.
13. The lithium ion secondary battery according to any one of claims 1 to 12, wherein: The lithium salt for inhibiting aluminum foil corrosion is at least one selected from LiPF6, LiAsF6, and LiBF4.
14. The lithium ion secondary battery according to any one of claims 1 to 13, wherein: The mass percentage of the lithium salt for inhibiting the corrosion of the aluminum foil in the electrolyte is 0.1% to 10%.
15. The lithium ion secondary battery according to claim 14, wherein: The mass percentage of the lithium salt for inhibiting the corrosion of the aluminum foil in the electrolyte is 0.2% to 5%.
16. The lithium ion secondary battery according to claim 15, wherein: The mass percentage of the lithium salt for inhibiting aluminum foil corrosion in the electrolyte can be selected to be 1% to 3%.
17. The lithium ion secondary battery according to any one of claims 1 to 16, wherein: The total lithium salt content in the electrolyte is in the range of 5 wt % to 37 wt %, based on the total weight of the electrolyte.
18. The lithium ion secondary battery according to claim 17, wherein: The total lithium salt content in the electrolyte is in the range of 5 wt % to 23 wt %, based on the total weight of the electrolyte.
19. The lithium ion secondary battery according to any one of claims 1 to 18, wherein: The electrolyte includes a solvent, and the solvent includes one or more of a chain carbonate, a cyclic carbonate, and a carboxylic acid ester.
20. The lithium ion secondary battery according to any one of claims 1 to 19, wherein: The solvent also includes an additive, and the additive includes at least one of a cyclic carbonate compound containing an unsaturated bond, a halogen-substituted cyclic carbonate compound, a sulfate compound, a sulfite compound, a sultone compound, a disulfonic acid compound, a nitrile compound, an aromatic compound, an isocyanate compound, a phosphazene compound, a cyclic anhydride compound, a phosphite compound, a phosphate compound, a borate compound, and a carboxylate compound.
21. The lithium ion secondary battery according to any one of claims 1 to 20, wherein: The positive electrode material loading of the positive electrode plate is 18 mg / cm 2 Up to 32mg / cm 2 .
22. The lithium ion secondary battery according to claim 21, wherein: The positive electrode material loading of the positive electrode plate is 22 mg / cm 2 Up to 29.22mg / cm 2 .
23. The lithium ion secondary battery according to claim 22, wherein: The positive electrode material loading of the positive electrode plate is 22.3 mg / cm 2 Up to 27.27mg / cm 2 .
24. The lithium ion secondary battery according to any one of claims 1 to 23, wherein: The carbon content of the positive electrode material layer is 1% to 7%.
25. The lithium ion secondary battery according to claim 24, wherein: The carbon content of the positive electrode material layer is 1% to 5%.
26. The lithium ion secondary battery according to any one of claims 1 to 25, wherein: The temperature rise coefficient k1 of the positive electrode sheet satisfies 2.5≤k1≤32, where k1=Cw / Mc, Cw is the positive electrode material loading per unit area on the surface of either side of the positive electrode current collector loaded with the positive electrode material layer (mg / cm 2 ), Mc is the carbon content (%) of the positive electrode material layer.
27. The lithium ion secondary battery according to claim 26, wherein: The temperature rise coefficient k1 of the positive electrode plate satisfies 3.3≤k1≤14.
5.
28. The lithium ion secondary battery according to claim 26 or 27, wherein: The mass percentage of the high thermal stability salt in the electrolyte is set to k2%, and the lithium ion secondary battery satisfies 0.34≤k2 / k1≤8.
29. The lithium ion secondary battery according to claim 28, wherein: The lithium ion secondary battery satisfies 0.48≤k2 / k1≤7.
30. The lithium ion secondary battery according to any one of claims 1 to 29, wherein: The positive electrode active material is selected from one or more of lithium transition metal oxides, lithium-containing phosphates with an olivine structure, and their respective modified compounds.
31. The lithium ion secondary battery according to claim 30, wherein: The lithium transition metal oxide is selected from lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt manganese oxide satisfying a+b+c=1 and a<0.8 a Co b Mn c O2, one or more of lithium nickel cobalt aluminum oxide and their modified compounds.
32. The lithium ion secondary battery according to any one of claims 1 to 31, wherein: The positive electrode active material has a carbon coating layer, and the carbon content of the positive electrode active material is 0.2% to 2.8%.
33. The lithium ion secondary battery according to claim 32, wherein: The carbon content of the positive electrode active material is 1.2% to 2.5%.
34. The lithium ion secondary battery according to any one of claims 1 to 33, wherein: The negative electrode plate comprises a negative electrode current collector and a negative electrode material layer located on at least one surface of the negative electrode current collector. The negative electrode material loading of the negative electrode plate is 9.96 mg / cm 2 Up to 15.33mg / cm 2 .
35. The lithium ion secondary battery according to claim 34, wherein: The negative electrode material loading of the negative electrode plate is 10.10 mg / cm 2 Up to 14.12mg / cm 2 . 36 . A battery module comprising the lithium ion secondary battery according to claim 1 .
37. A battery pack comprising the battery module according to claim 36.
38. An electrical device comprising one or more selected from the lithium-ion secondary battery of any one of claims 1 to 35, the battery module of claim 36, or the battery pack of claim 37.
Citation Information
Cited By
Metal battery cell, battery apparatus, and electric apparatus
WO2026175042A1