Solar cell and preparation method thereof

By setting a functional layer between the SAM layer and the light absorbing layer of the solar cell, the carrier recombination loss problem is solved and the battery performance is improved.

CN119031731APending Publication Date: 2024-11-26TRINA SOLAR CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411480419.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In solar cells, the recombination loss of carriers at the interface between the SAM layer and the light absorbing layer results in a decrease in the number of effective carriers, thereby reducing the open circuit voltage and battery performance.

Method used

A functional layer is provided between the SAM layer and the light absorbing layer. The material of the functional layer may be an inorganic material with a thickness ranging from 0.1 nm to 20 nm to reduce the composite loss of carriers.

Benefits of technology

By reducing the composite loss of carriers at the interface of the SAM layer and the absorbing layer, the number of available carriers in the solar cell is improved, and the open circuit voltage and battery performance are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031731A_ABST
    Figure CN119031731A_ABST
Patent Text Reader

Abstract

The embodiment of the invention provides a solar cell and a preparation method thereof, and relates to the technical field of photovoltaic cells, the solar cell comprises a glass substrate, an SAM layer, a functional layer and a light absorption layer which are stacked in sequence, and the functional layer is used for reducing the recombination loss of carriers between the SAM layer and the light absorption layer. According to the embodiment of the invention, the functional layer is arranged between the SAM layer and the light absorption layer, and the functional layer is used for reducing the recombination loss of the carriers between the SAM layer and the light absorption layer, so that the recombination loss of the carriers at the interface of the SAM layer and the light absorption layer is reduced, the condition that the number of available effective carriers in the battery is reduced is relieved, and the service life of the battery is prolonged. And the problems that the open-circuit voltage is reduced and the performance of the battery is reduced are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of photovoltaic cells, and in particular, relates to a solar cell and a method for preparing the same. Background Art

[0002] A solar cell is a device that uses light energy to directly convert into electrical energy. Under light conditions, the photovoltaic material in the solar cell absorbs photons, excites electron-hole pairs, and then generates current.

[0003] Solar cells may include a SAM layer as a hole transport layer and a light absorbing layer. When photons are absorbed by the light absorbing layer, a large number of electron-hole pairs will be generated in the light absorbing layer. Due to the limited range of carrier activity, some carriers may recombine at the interface between the SAM layer and the light absorbing layer instead of being effectively transferred to the electrode, resulting in a reduction in the number of effective carriers available in the battery, which in turn leads to a decrease in the open circuit voltage and a decrease in the performance of the battery. Summary of the invention

[0004] The embodiments of the present application provide a solar cell and a method for manufacturing the same to solve or alleviate one or more technical problems in the prior art.

[0005] As one aspect of an embodiment of the present application, an embodiment of the present application provides a solar cell, comprising: Glass substrate; A SAM layer, located on the glass substrate; A functional layer, located on the SAM layer; A light absorbing layer, located on the functional layer; The functional layer is used to reduce the recombination loss of carriers between the SAM layer and the light absorbing layer.

[0006] Optionally, the material of the functional layer includes inorganic material.

[0007] Optionally, the inorganic material includes , , , , , and One or more of .

[0008] Optionally, the thickness of the functional layer ranges from 0.1 nm to 20 nm.

[0009] Optionally, the functional layer comprises a plurality of inorganic layers stacked in sequence.

[0010] Optionally, the plurality of inorganic layers include a first inorganic layer and a second inorganic layer.

[0011] Optionally, the material of the first inorganic layer includes , , , , , and One of; The material of the second inorganic layer includes , , , , , and One of them.

[0012] As another aspect of the embodiments of the present application, the embodiments of the present application further provide a method for preparing the solar cell described in any one of the above items, comprising: providing a glass substrate; forming a SAM layer on the glass substrate; forming a functional layer on the SAM layer; forming a light absorbing layer on the functional layer; The functional layer is used to reduce the recombination loss of carriers between the SAM layer and the light absorbing layer.

[0013] As another aspect of the embodiment of the present application, the embodiment of the present application further provides a photovoltaic assembly, comprising at least one battery string, wherein the battery string comprises at least the solar cell as described in any one of the above items; or A solar cell manufactured by the method for manufacturing a solar cell as described in any one of the above.

[0014] As another aspect of the embodiment of the present application, the embodiment of the present application further provides a photovoltaic system, including the photovoltaic component described above.

[0015] The embodiment of the present application adopts the above-mentioned technical solution, by setting a functional layer between the SAM layer and the light absorbing layer, the functional layer is used to reduce the recombination loss of carriers between the SAM layer and the light absorbing layer, thereby reducing the recombination loss of carriers at the interface between the SAM layer and the light absorbing layer, alleviating the situation of reducing the number of effective carriers available in the battery, and further alleviating the problem of reducing the open circuit voltage and the degradation of battery performance.

[0016] The above summary is for illustrative purposes only and is not intended to be limiting in any way. In addition to the illustrative aspects, embodiments and features described above, further aspects, embodiments and features of the present application will be readily apparent by reference to the accompanying drawings and the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.

[0018] Figure 1 A schematic diagram of the structure of a solar cell according to an embodiment of the present application; Figure 2 Another schematic diagram of the structure of a solar cell according to an embodiment of the present application; Figure 3 A flow chart schematically shows a method for preparing a solar cell according to an embodiment of the present application.

[0019] Description of reference numerals: 10. Glass substrate; 20. SAM layer; 30. Functional layer; 40. Light absorbing layer; 50. Electron transport layer; 60. Metal electrode; 31. First inorganic layer; 32. Second inorganic layer. DETAILED DESCRIPTION

[0020] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. In the accompanying drawings, for clarity, the sizes of layers, regions, elements and their relative sizes may be exaggerated. The same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.

[0021] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there is no intervening element or layer. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present disclosure, the first element, component, region, layer or part discussed below can be represented as the second element, component, region, layer or part. And when the second element, component, region, layer or part is discussed, it does not mean that the present disclosure necessarily has the first element, component, region, layer or part.

[0022] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0023] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0024] The following provides an explanation of the terms used in this application.

[0025] SAM layer: Self-Assembled Monolayer (SAM).

[0026] See also Figure 1 and Figure 2 The embodiment of the present application provides a solar cell, which may include a glass substrate 10, a SAM layer 20, a functional layer 30, a light absorbing layer 40, etc. The following is a detailed description: The glass substrate 10 may be rolled glass, which can provide good physical strength. In other embodiments, the glass substrate 10 may also be FTO glass.

[0027] The SAM layer 20 is located on the glass substrate 10 and can be used as a hole transport layer. The SAM layer 20 can provide a smooth and orderly interface, which is conducive to the movement of holes and reduces the scattering and recombination of holes, thereby improving the carrier transmission efficiency.

[0028] The functional layer 30 is located on the SAM layer 20 , and is used to reduce the recombination loss of carriers between the SAM layer 20 and the light absorbing layer 40 .

[0029] The light absorbing layer 40 is located on the functional layer 30, and the light absorbing layer 40 can be used to absorb sunlight. When ambient light shines on the solar cell, the material in the light absorbing layer 40 absorbs photons and converts their energy into electrical energy. The light absorbing layer 40 can be a single-junction perovskite, a multi-junction perovskite, or a perovskite-crystalline silicon structure.

[0030] In the embodiment of the present application, a functional layer 30 is provided between the SAM layer 20 and the light absorbing layer 40. The functional layer 30 is used to reduce the recombination loss of carriers between the SAM layer 20 and the light absorbing layer 40, thereby reducing the recombination loss of carriers at the interface between the SAM layer 20 and the light absorbing layer 40, alleviating the reduction in the number of effective carriers available in the battery, and further alleviating the problem of reduced open circuit voltage and reduced battery performance.

[0031] In an optional embodiment, the material of the functional layer 30 includes an inorganic material. The inorganic material functional layer 30 has a high electron affinity, which reduces the possibility of recombination with holes in the SAM layer 20. In other embodiments, the material of the functional layer 30 may also include other types of materials, such as semiconductors and metals.

[0032] Furthermore, in this embodiment, the inorganic material of the functional layer 30 may include , , , , , and In other embodiments, the material of the functional layer 30 may include other inorganic materials, such as zinc oxide, nitride, etc.

[0033] In an optional embodiment, the thickness of the functional layer 30 is in the range of 0.1 nm to 20 nm. The functional layer 30 with a thickness in an appropriate range can block the transmission of carriers and reduce the carrier recombination loss between the SAM layer 20 and the light absorbing layer 40 .

[0034] Preferably, the thickness of the functional layer 30 is 1 nm to 10 nm. Specifically, the thickness of the functional layer 30 may be 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 9 nm, 10 nm, 11 nm, 13 nm, 15 nm, 18 nm. In other embodiments, the thickness of the functional layer 30 may also be in other ranges, such as 0.01 nm to 0.1 nm, or 20 nm to 30 nm. Specifically, it may be adjusted according to the specific structure of the solar cell.

[0035] In an optional embodiment, the functional layer 30 includes a plurality of inorganic layers stacked in sequence.

[0036] By way of example, the functional layer 30 may be a multi-layer stacked structure, and the materials between the layers in the functional layer 30 may be the same or different. For example, the functional layer 30 may include two stacked inorganic layers, wherein the materials of the two inorganic layers are the same; or the functional layer 30 may include two stacked inorganic layers, wherein the materials of the two inorganic layers are different; or a stacked inorganic layer and an organic layer; or two stacked inorganic layers and an organic layer, etc.

[0037] For further information, see Figure 2 In this embodiment, the plurality of inorganic layers include a first inorganic layer 31 and a second inorganic layer 32 .

[0038] Specifically, the material of the first inorganic layer 31 includes , , , , , and One of; The material of the second inorganic layer 32 includes , , , , , and One of them.

[0039] The sum of the thickness of the first inorganic layer 31 and the thickness of the second inorganic layer 32 is 0.1 nm to 20 nm. The total thickness of the functional layer 30 in an appropriate range can block the transmission of carriers and reduce the carrier recombination loss between the SAM layer 20 and the light absorbing layer 40 .

[0040] In the case where the material of the first inorganic layer 31 and the material of the second inorganic layer 32 are different, the first inorganic layer 31 and the second inorganic layer 32 can be formed separately. After forming the first inorganic layer 31, the thickness of the first inorganic layer 31 can be measured, and the thickness of the second inorganic layer 32 to be formed can be confirmed based on the thickness of the first inorganic layer 31. The functional layer 30 is formed by the first inorganic layer 31 and the second inorganic layer 32 together, which alleviates the situation where the thickness of the functional layer 30 formed once does not reach the predetermined range.

[0041] By way of example, after the first inorganic layer 31 is formed, it is measured that the thickness of the first inorganic layer 31 is 10 nm, and the thickness of the second inorganic layer 32 is in the range of 0.1 nm to 10 nm.

[0042] In other embodiments, the plurality of inorganic layers may further include more inorganic layers, such as a third inorganic layer and a fourth inorganic layer. The thickness and material of each inorganic layer may be different, and the total thickness of the plurality of inorganic layers ranges from 0.1 nm to 20 nm.

[0043] In an optional embodiment, the material of the SAM layer 20 includes one or more of [2-(9H-carbazole-9-yl)ethyl]phosphonic acid (2PACz), [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid (MeO-2PACz), [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACz), benzoic acid, and 4-[bis(2,4-dimethoxybiphenyl-4-yl)amino]-biphenyl-4-carboxylic acid [MC-43].

[0044] Selecting a suitable hole transport layer material from the optional materials provided in this embodiment can enhance the stability of the device, improve the ability of the device to operate stably for a long time, and reduce the performance degradation of the device under environmental conditions such as light and humidity.

[0045] In an optional embodiment, the light absorbing layer 40 may be a perovskite material, and specifically, the material of the light absorbing layer 40 is an ABX3 structure; Wherein, A is a monovalent cation; The B is a divalent cation; The X is a monovalent anion.

[0046] Furthermore, in this embodiment, the A includes one or a mixture of several monovalent cations selected from cesium, rubidium, methylamine, and guanidine.

[0047] The B includes one or a mixture of several divalent cations selected from the group consisting of lead, copper, zinc, gallium, tin and calcium.

[0048] The X includes one or a mixture of several monovalent anions selected from iodine, bromine, chlorine, fluorine and thiocyanate ions.

[0049] In an optional embodiment, the light absorbing layer 40 may be prepared using a perovskite precursor solution.

[0050] The perovskite precursor solution may include DMF (dimethylformamide) and / or DMSO (dimethyl sulfoxide), and the concentration range of DMF in the perovskite precursor solution may be 0.1% to 100%; the concentration range of DMSO in the perovskite precursor solution may be 0.1% to 100%.

[0051] Specifically, in this embodiment, the light absorbing layer 40 can be prepared by using a large-area thin film material preparation method such as a doctor blade coating method, a slit coating method, a screen printing method, an inkjet printing method, etc. In other embodiments, other methods can also be used to prepare the light absorbing layer.

[0052] The light absorption layer can be a single layer structure or a multi-layer structure, such as a multi-junction perovskite structure. In addition to perovskite materials, the light absorption layer can also include crystalline silicon, perovskite, cadmium selenide (CdTe), copper indium gallium selenide (CIGS), gallium arsenide (GaAs), etc.

[0053] In an optional embodiment, the thickness of the light absorption layer 40 is in the range of 10 nm to 100 μm, and the band gap of the light absorption layer 40 is in the range of 0.9 eV to 3 eV.

[0054] By adjusting the band gap of the light absorbing layer 40 , energy level matching in the device can be achieved, and the transmission and separation of carriers can be optimized, thereby improving the efficiency and performance of the device.

[0055] In an optional embodiment, the solar cell further comprises: The electron transport layer 50 is located on the light absorbing layer 40. The electron transport layer 50 can be used to receive the photogenerated electrons generated from the light absorbing layer and effectively transport these electrons to the corresponding electrodes. The material of the electron transport layer 50 may include zinc oxide (ZnO) or titanium oxide (TiO2). Such materials can promote the transmission of electrons and reduce the occurrence of electron-hole recombination, thereby improving the efficiency of solar cells. In addition, the electron transport layer 50 can also help adjust the energy level alignment of electrons so as to more efficiently inject electrons into the electrodes.

[0056] The metal electrode 60 is located on the electron transport layer 50. The metal electrode 60 can be used to export the electrons collected from the light absorption layer to the external circuit to form a current output, thereby realizing the power conversion of the solar cell. The material of the metal electrode 60 may include silver, copper, aluminum, etc. In some embodiments, the metal electrode 60 can also be made of a mixture of multiple metal materials.

[0057] The present application also provides a method for preparing a solar cell to reduce the recombination loss of carriers between the SAM layer and the light absorbing layer, thereby alleviating the problem of lower open circuit voltage and lower battery performance. Figure 3 , the method comprising: Step S100: providing a glass substrate.

[0058] The glass substrate can be rolled glass, which can provide better physical strength. In other embodiments, the glass substrate can also be FTO glass.

[0059] Step S102: forming a SAM layer on the glass substrate.

[0060] The SAM layer is located on the glass substrate. The SAM layer can serve as a hole transport layer. The SAM layer can provide a smooth and orderly interface, which is conducive to the movement of holes and reduces the scattering and recombination of holes, thereby improving the carrier transmission efficiency.

[0061] Step S104: forming a functional layer on the SAM layer.

[0062] The functional layer is used to reduce the recombination loss of carriers between the SAM layer and the light absorbing layer.

[0063] Step S106: forming a light absorbing layer on the functional layer.

[0064] The light absorbing layer is located on the functional layer, and the light absorbing layer can be used to absorb sunlight. When ambient light shines on the solar cell, the material in the light absorbing layer absorbs photons and converts their energy into electrical energy. The light absorbing layer can be a single-junction perovskite, a multi-junction perovskite, or a perovskite-crystalline silicon structure.

[0065] The method for preparing a solar cell in an embodiment of the present application forms a functional layer between the SAM layer and the light-absorbing layer, and the functional layer is used to reduce the recombination loss of carriers between the SAM layer and the light-absorbing layer, thereby reducing the recombination loss of carriers at the interface between the SAM layer and the light-absorbing layer, alleviating the reduction in the number of effective carriers available in the battery, and further alleviating the problem of reduced open circuit voltage and reduced battery performance.

[0066] In an optional embodiment, the material of the functional layer includes an inorganic material. The functional layer of inorganic material has a high electron affinity, which reduces the possibility of recombination with holes in the SAM layer. In other embodiments, the material of the functional layer may also include other types of materials, such as semiconductors and metals.

[0067] Furthermore, in this embodiment, the inorganic material of the functional layer may include , , , , , and In other embodiments, the material of the functional layer may include other inorganic materials, such as zinc oxide, nitride, etc.

[0068] In an optional embodiment, the thickness of the functional layer is in the range of 0.1 nm to 20 nm. The functional layer with a thickness in an appropriate range can block the transmission of carriers and reduce the carrier recombination loss between the SAM layer and the light absorbing layer.

[0069] Preferably, the thickness of the functional layer is 1 nm to 10 nm. Specifically, the thickness of the functional layer can be 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, 9 nm, 10 nm, 11 nm, 13 nm, 15 nm, 18 nm. In other embodiments, the thickness of the functional layer can also be in other ranges, such as 0.01 nm to 0.1 nm, or 20 nm to 30 nm. It can be adjusted according to the specific structure of the solar cell.

[0070] In an optional embodiment, forming a functional layer on the SAM layer (step S104) may include: A first inorganic layer is formed on the SAM layer, wherein the material of the first inorganic layer comprises , , , , , and One of; A second inorganic layer is formed on the first inorganic layer, wherein the material of the second inorganic layer comprises , , , , , and One of them.

[0071] The sum of the thickness of the first inorganic layer and the thickness of the second inorganic layer is 0.1 nm to 20 nm. The total thickness of the functional layer in an appropriate range can block the transmission of carriers and reduce the carrier recombination loss between the SAM layer and the light absorbing layer.

[0072] After forming the first inorganic layer, the thickness of the first inorganic layer can be measured, and the thickness of the second inorganic layer to be formed can be confirmed based on the thickness of the first inorganic layer. The first inorganic layer and the second inorganic layer can form a functional layer together, which alleviates the situation where the thickness of the functional layer formed in a single time does not reach the predetermined range.

[0073] By way of example, after the first inorganic layer is formed, it is measured that the thickness of the first inorganic layer is 10 nm, and the thickness of the second inorganic layer is in the range of 0.1 nm to 10 nm.

[0074] In other embodiments, the plurality of inorganic layers may further include more inorganic layers, such as a third inorganic layer and a fourth inorganic layer. The thickness and material of each inorganic layer may be different, and the total thickness of the plurality of inorganic layers ranges from 0.1 nm to 20 nm.

[0075] In an optional embodiment, the method for preparing a solar cell may further include: Step S108: forming an electron transport layer on the light absorbing layer.

[0076] The electron transport layer can be used to receive photogenerated electrons generated from the light absorption layer and efficiently transport these electrons to the corresponding electrode. The material of the electron transport layer may include zinc oxide (ZnO) or titanium oxide (TiO2). Such materials can promote the transport of electrons and reduce the occurrence of electron-hole recombination, thereby improving the efficiency of solar cells. In addition, the electron transport layer can also help adjust the energy level alignment of electrons so that electrons can be injected into the electrode more efficiently.

[0077] Step S110: forming a metal electrode on the electron transport layer.

[0078] The metal electrode can be used to export the electrons collected from the light absorption layer to the external circuit to form a current output, thereby realizing the power conversion of the solar cell. The material of the metal electrode may include silver, copper, aluminum, etc. In some embodiments, the metal electrode may also be made of a mixture of multiple metal materials.

[0079] In an optional embodiment, in order to optimize the performance of the functional layer, the forming of the functional layer on the SAM layer (step S104) may specifically include: (1) Trimethylaluminum (TMA) is deposited on the SAM layer by atomic layer deposition (ALD).

[0080] The specific parameters may include: the chamber temperature is 85° C., and the pulse time is 0.4 s.

[0081] (2) Use nitrogen to purge.

[0082] The nitrogen purge time can be 5 s.

[0083] (3) Sedimentation , and then purge with nitrogen.

[0084] Step (3) is repeated multiple times to form a functional layer.

[0085] The following will conduct performance tests on the structure or preparation method of the solar cell provided in the embodiments of the present application and related comparative examples.

[0086] [Example 1] The specific structure of solar cells includes: The glass substrate, SAM layer, functional layer, light absorbing layer, electron transport layer and electrode layer are stacked in sequence. The material of the functional layer includes , the thickness of the functional layer is 7nm.

[0087] The glass substrate was ultrasonically cleaned using isopropyl alcohol (IPA); Me-4PACz monolayer was prepared on glass substrate by spin coating and annealed at 100 °C for 10 min to form SAM layer; Al2O3 was deposited on the SAM layer by ALD method with a thickness of 7nm; The light absorbing layer is deposited on the SAM layer by a one-step spin coating method using a perovskite precursor solution. The perovskite precursor solution includes , the light absorption layer has a band gap of 1.68 eV and a thickness of 500 nm; The electron transport layer is deposited by thermal evaporation. The materials of the electron transport layer include C 60 (Fullerene), thickness is 30nm; The electrode layer is prepared by thermal evaporation. The electrode material includes silver and has a thickness of 100 nm.

[0088] The specific preparation process of the functional layer is as follows: (1) Depositing trimethylaluminum (TMA) on the SAM layer by atomic layer deposition (ALD); specific parameters may include: chamber temperature of 85° C., and pulse time of 0.4 s.

[0089] (2) Purge with nitrogen for 5 seconds.

[0090] (3) Sedimentation , and then purge with nitrogen for 5 s.

[0091] Step (3) was repeated 50 times to form a 7 nm functional layer.

[0092] [Example 2] The structure is basically the same as that of Example 1, except that the thickness of the functional layer is 3 nm.

[0093] The specific preparation process of the functional layer is as follows: (1) Depositing trimethylaluminum (TMA) on the SAM layer by atomic layer deposition (ALD); specific parameters may include: chamber temperature of 85° C., and pulse time of 0.4 s.

[0094] (2) Purge with nitrogen for 5 seconds.

[0095] (3) Sedimentation , and then purge with nitrogen for 5 s.

[0096] Step (3) was repeated 20 times to form a 3 nm functional layer.

[0097] [Example 3] The structure is basically the same as that of Example 1, except that the thickness of the functional layer is 15 nm.

[0098] The specific preparation process of the functional layer is as follows: (1) Depositing trimethylaluminum (TMA) on the SAM layer by atomic layer deposition (ALD); specific parameters may include: chamber temperature of 85° C., and pulse time of 0.4 s.

[0099] (2) Purge with nitrogen for 5 seconds.

[0100] (3) Sedimentation , and then purge with nitrogen for 5 s.

[0101] Step (3) was repeated 120 times to form a 15 nm functional layer.

[0102] [Example 4] The structure is substantially the same as that of Embodiment 1, except that the material of the functional layer includes SiO2 and the thickness of the functional layer is 7 nm.

[0103] The specific preparation process of the functional layer is as follows: (1) Depositing hexamethylsilane on the SAM layer by atomic layer deposition (ALD); specific parameters may include: chamber temperature of 90° C., and pulse time of 0.3 s.

[0104] (2) Purge with nitrogen for 4 seconds.

[0105] (3) Sedimentation , and then purge with nitrogen for 4 s.

[0106] Step (3) was repeated 55 times to form a 7 nm functional layer.

[0107] [Example 5] The structure is substantially the same as that of Example 1, except that the material of the functional layer includes MoO3 and the thickness of the functional layer is 5 nm.

[0108] The specific preparation process of the functional layer is as follows: (1) Mo(CO)6 is deposited on the SAM layer by atomic layer deposition (ALD); specific parameters may include: chamber temperature of 100°C and pulse time of 0.5 s.

[0109] (2) Purge with nitrogen for 5 seconds.

[0110] (3) Sedimentation , and then purge with nitrogen for 5 s.

[0111] Step (3) was repeated 30 times to form a 5 nm functional layer.

[0112] [Comparative Example 1] The specific structure of solar cells includes: The structure of the glass substrate, SAM layer, light absorbing layer, electron transport layer and electrode layer stacked in sequence is basically the same as that of Example 1, except that no functional layer is arranged between the SAM layer and the light absorbing layer.

[0113] The test data is shown in Table 1: Table 1

[0114] It can be seen from the above table that the opening voltage and fill factor of the solar cell in the embodiment of the present application are significantly improved compared with the comparative example, thereby improving the overall performance of the battery.

[0115] The present application also provides a photovoltaic module (not shown) including at least one battery string, the battery string including at least two solar cells as described above, or including a solar cell manufactured by the method for preparing a solar cell in any of the above embodiments. Adjacent solar cells can be connected together by serial welding.

[0116] Multiple battery strings can be electrically connected in series and / or in parallel to form a more flexible battery organization structure. In order to protect the battery string, the photovoltaic module can also include an encapsulation layer and a cover plate. The encapsulation layer can cover the surface of the battery string, and the cover plate can cover the surface of the encapsulation layer away from the battery string.

[0117] In some embodiments, multiple battery strings can be electrically connected through conductive tapes to achieve a series or parallel arrangement of batteries. The encapsulation layer can be made of an organic encapsulation film, such as an ethylene-vinyl acetate copolymer film, a polyethylene octene co-elastic film, or a polyethylene terephthalate film, to provide protection and isolation functions.

[0118] The advantages possessed by the solar cell in any of the above embodiments, or the advantages possessed by the solar cell manufactured by the method for manufacturing the solar cell in any of the above embodiments, are also possessed by the photovoltaic module and will not be elaborated here.

[0119] The embodiment of the present application can provide a photovoltaic system, including the photovoltaic components in any of the above embodiments. The advantages of the above photovoltaic components are also possessed by the photovoltaic system, which will not be repeated here. The above photovoltaic system has a wide range of applications, not only limited to photovoltaic power stations, such as ground power stations, rooftop power stations and water power stations, but also includes various equipment and devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars and solar buildings. Of course, it can be understood that the application scenarios of the photovoltaic system are not limited to this, that is to say, the photovoltaic system can be used in all fields where solar energy is required for power generation. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple photovoltaic components. For example, multiple photovoltaic components may form multiple photovoltaic arrays. The photovoltaic array is connected to a junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter and is converted into the alternating current required by the mains power grid, and then connected to the mains network to realize solar power supply.

[0120] It should be noted that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. The orientation words "inside" and "outside" refer to the inside and outside relative to the outline of each component itself. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Therefore, the exemplary term "above..." can include both "above..." and "below..." orientations. The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used here are interpreted accordingly.

[0121] It should also be noted that "one embodiment", "another embodiment", "embodiment", etc. mentioned in this application refer to the specific features, structures or characteristics described in conjunction with the embodiment included in at least one embodiment generally described in this application. The same expression appearing in multiple places in the specification does not necessarily refer to the same embodiment. Further, when describing a specific feature, structure or characteristic in conjunction with any embodiment, it is claimed that the realization of such feature, structure or characteristic in conjunction with other embodiments also falls within the scope of this application.

[0122] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.

[0123] It should also be noted that the above are only preferred embodiments of the present application, and the patent protection scope of the present application is not limited thereto. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.

Claims

1. A solar cell, characterized in that: Includes the following stacked: Glass substrate; A SAM layer, located on the glass substrate; A functional layer, located on the SAM layer; A light absorbing layer, located on the functional layer; Wherein, the functional layer is used to reduce the recombination loss of carriers between the SAM layer and the light absorbing layer; Wherein, the material of the functional layer includes inorganic material, and the inorganic material includes , , , , , and One or more of .

2. The solar cell according to claim 1, characterized in that The thickness of the functional layer ranges from 0.1 nm to 20 nm.

3. The solar cell according to any one of claims 1 to 2, characterized in that: The functional layer includes a plurality of inorganic layers stacked in sequence.

4. The solar cell according to claim 3, characterized in that: The plurality of inorganic layers include a first inorganic layer and a second inorganic layer.

5. The solar cell according to claim 4, characterized in that: The material of the first inorganic layer includes , , , , , and One of; The material of the second inorganic layer includes , , , , , and One of them.

6. A method for preparing a solar cell according to any one of claims 1 to 5, characterized in that: include: providing a glass substrate; forming a SAM layer on the glass substrate; forming a functional layer on the SAM layer; forming a light absorbing layer on the functional layer; The functional layer is used to reduce the recombination loss of carriers between the SAM layer and the light absorbing layer.

7. A photovoltaic module, characterized in that: include: At least one battery string, the battery string comprising at least two solar cells according to any one of claims 1 to 5; or A solar cell manufactured by the method for manufacturing a solar cell as claimed in claim 6.

8. A photovoltaic system, characterized in that: Comprising the photovoltaic module as claimed in claim 7.

Citation Information

Patent Citations

  • Solar cell and preparation method thereof

    CN117580382A

  • Silver-tungsten gradient distribution electrode material, preparation method and perovskite solar cell