Novel passivation contact structure and photovoltaic cell

By adopting the passivation contact structure of the tunneled oxide layer and the single crystal silicon layer in the photovoltaic cell, the problems of parasitic absorption and carrier recombination loss in the metallized region in the prior art are solved, and electron mobility and photovoltaic cell are improved. Conversion efficiency.

CN222088618UActive Publication Date: 2024-11-29JOLYWOOD (TAIZHOU) SOLAR TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202323614237.2
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-27
Publication Date
2024-11-29
Estimated Expiration
2033-12-27

AI Technical Summary

Technical Problem

The existing passivation contact structures have problems in the metallized area, low electron mobility and carrier recombination losses, which affect the conversion efficiency of photovoltaic cells.

Method used

The tunneling oxide layer and a single crystal silicon layer bonded to its surface are used to replace the polysilicon layer or amorphous silicon layer, and the passivation contact structure is optimized to reduce parasitic absorption and carrier recombination losses and improve electron mobility.

Benefits of technology

It effectively improves the short-circuit current, open-circuit voltage and filling factor of photovoltaic cells, and improves the conversion efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222088618U_ABST
    Figure CN222088618U_ABST
Patent Text Reader

Abstract

The utility model relates to the technical field of photovoltaic cells, and particularly discloses a novel passivation contact structure and a photovoltaic cell with the novel passivation contact structure. The novel passivation contact structure comprises a tunneling oxide layer arranged on the surface of a substrate silicon wafer and a monocrystalline silicon layer bonded on the surface of the tunneling oxide layer, wherein the thickness of the tunneling oxide layer is less than or equal to 2nm; the thickness of the monocrystalline silicon layer ranges from 100 nm to 150 nm. The monocrystalline silicon layer in the novel passivation contact structure replaces a polycrystalline silicon layer of an existing passivation contact structure, so that parasitic absorption is reduced, the current density loss at the long wave of 900-1100 nm is made up, the electron mobility is improved, the carrier recombination loss is reduced, and the service life of the device is prolonged. Therefore, the short-circuit current, the open-circuit voltage and the fill factor of the photovoltaic cell with the novel passivation contact structure are all effectively improved, and the conversion efficiency of the photovoltaic cell is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of photovoltaic cells, in particular to a novel passivation contact structure and a photovoltaic cell. Background Art

[0002] In recent years, with the continuous improvement of passivation technology of solar photovoltaic cells (referred to as PV cells), the recombination problem in non-metallized areas has been basically solved and is no longer a bottleneck for improving the conversion efficiency of PV cells; however, the recombination problem in metallized areas has become increasingly prominent and has become one of the main bottlenecks for improving the conversion efficiency of PV cells.

[0003] At present, the passivation contact structure that can reduce metal recombination has attracted much attention and favor in the photovoltaic market. The existing passivation contact structure (such as CN218957740U and CN207381411U) is mostly composed of a tunneling oxide layer superimposed with a silicon film layer doped with phosphorus or boron atoms (the silicon film layer is an amorphous silicon layer, an amorphous silicon oxide layer, a microcrystalline silicon layer, a microcrystalline silicon oxide layer or a polycrystalline silicon layer, and most of them are polycrystalline silicon layers), and the back metal electrode is in contact with the doped polycrystalline silicon layer to avoid direct contact between the back metal electrode and the substrate silicon wafer to reduce metal recombination.

[0004] However, as one of the important components of the passivation contact structure, the silicon film layer, whether it is an amorphous silicon layer, an amorphous silicon oxide layer, a microcrystalline silicon layer, a microcrystalline silicon oxide layer or a polycrystalline silicon layer (especially a polycrystalline silicon layer), will bring the following problems to varying degrees:

[0005] There are parasitic absorption problems, photovoltaic cells have current density loss at long wavelengths of sunlight, low electron mobility, and carrier recombination losses; further improvements are needed to improve the conversion efficiency of photovoltaic cells. Utility Model Content

[0006] The purpose of the utility model is to overcome the deficiencies of the prior art and provide a novel passivation contact structure and a photovoltaic cell.

[0007] Based on this, the utility model discloses a novel passivation contact structure, comprising: a tunneling oxide layer disposed on the surface of a substrate silicon wafer, and a single crystal silicon layer bonded to the surface of the tunneling oxide layer;

[0008] Wherein, the thickness of the tunnel oxide layer is less than or equal to 2 nm; the thickness of the single crystal silicon layer is 100-150 nm.

[0009] Preferably, the single crystal silicon layer is an intrinsic single crystal silicon layer and / or a doped single crystal silicon layer; the doping type of the doped single crystal silicon layer is P-type and / or n-type.

[0010] Preferably, the substrate silicon wafer is an N-type or P-type crystalline silicon wafer; the thickness of the substrate silicon wafer is 130-160 μm, the resistivity is 0.5-1.5 Ω·cm, and the size is 182 mm×182 mm.

[0011] The utility model also discloses a photovoltaic cell, comprising: a substrate silicon wafer, a passivation contact structure arranged on the front and / or back side of the substrate silicon wafer, a front passivation anti-reflection film and a back passivation anti-reflection film respectively arranged on the front and back side of the substrate silicon wafer, and a metal electrode arranged on the front and / or back side of the substrate silicon wafer;

[0012] The passivation contact structure is a novel passivation contact structure described above in the present utility model.

[0013] Preferably, the passivation contact structure is provided on the back side of the substrate silicon wafer, and the single crystal silicon layer in the passivation contact structure is a doped single crystal silicon layer; the back side passivation anti-reflection film is provided on the back side of the doped single crystal silicon layer;

[0014] The metal electrode comprises a back metal electrode, the upper end of the back metal electrode contacts the local area of ​​the doped single crystal silicon layer, and the lower end of the back metal electrode extends to below the back passivation anti-reflection film.

[0015] Further preferably, the doped single crystal silicon layer is an n+ doped single crystal silicon layer, and the surface doping concentration of the n+ doped single crystal silicon layer is 1×10 20 ~1×10 21 cm -3 , the junction depth is 0.1~0.3μm.

[0016] Preferably, the photovoltaic cell further comprises a selective emitter disposed on the front side of the substrate silicon wafer, and the front passivation anti-reflection film is disposed on the front side of the selective emitter;

[0017] The metal electrode further comprises a front metal electrode, the lower end of the front metal electrode is in contact with the local area of ​​the selective emitter, and the upper end of the front metal electrode extends to the top of the front passivation anti-reflection film.

[0018] Further preferably, the selective emitter comprises a p+ doped emitter disposed on the front side of the substrate silicon wafer, and a p++ heavily doped region extending from a local area of ​​the selective emitter to a local area of ​​the front side of the substrate silicon wafer;

[0019] The square resistance of the p+ doped emitter is 110±25Ω / sq, and the doping concentration is 1×10 20 ~1×10 21 cm -3 , the junction depth is 0.8~1.2μm;

[0020] The square resistance of the P++ heavily doped region is 80±15Ω / sq, and the doping concentration is 1×10 19 ~1×10 20 cm -3 , the junction depth is 1.4~2.2μm.

[0021] Preferably, the back passivation anti-reflection film is a back silicon nitride film with a thickness of 60 to 80 nm;

[0022] The front passivation anti-reflection film comprises an aluminum oxide film and a front silicon nitride film arranged on the front of the aluminum oxide film; the thickness of the aluminum oxide film is 2 to 10 nm, and the thickness of the front silicon nitride film is 60 to 80 nm.

[0023] Preferably, the front side of the substrate silicon wafer is a pyramid velvet surface, and the back side of the substrate silicon wafer is a smooth, flat polished surface.

[0024] Compared with the prior art, the utility model has at least the following beneficial effects:

[0025] The novel passivation contact structure of the utility model comprises: a tunneling oxide layer and a single crystal silicon layer bonded to the surface of the tunneling oxide layer; the single crystal silicon layer in the novel passivation contact structure reduces parasitic absorption by replacing the polycrystalline silicon layer, amorphous silicon layer or microcrystalline silicon layer in the existing passivation contact structure, compensates for the current density loss at the long wave of 900 to 1100 nm, improves the electron mobility, and reduces the carrier recombination loss, so that the short-circuit current, open-circuit voltage and fill factor of the photovoltaic cell with the novel passivation contact structure of the utility model are effectively improved, thereby achieving a further improvement in the conversion efficiency of the photovoltaic cell. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S1.

[0027] Figure 2 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S21.

[0028] Figure 3 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S22.

[0029] Figure 4 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S23.

[0030] Figure 5 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S31.

[0031] Figure 6 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S32.

[0032] Figure 7 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S4.

[0033] Figure 8 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S5.

[0034] Fig. 9 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S6.

[0035] Fig.10 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S71.

[0036] Fig.11 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S72.

[0037] Fig.12 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S73.

[0038] Fig.13 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S8.

[0039] Fig.14 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S9.

[0040] Fig.15 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S10.

[0041] Fig.16 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S11.

[0042] Fig.17 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S12.

[0043] Fig.18 Schematic diagram of the cross-sectional structure of a Topcon battery manufacturing method in Example 1 after step S13.

[0044] Explanation of the accompanying drawings: p+ doped emitter 1; P++ heavily doped region 2; BSG layer 3; tunneling oxide layer 4; injection protection layer 5; hydrogen rich layer 6; single crystal silicon layer 7; n+ doped single crystal silicon layer 8; PSG layer 9; aluminum oxide film 10; front silicon nitride film 11; back silicon nitride film 12; front metal electrode 13; back metal electrode 14. DETAILED DESCRIPTION

[0045] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.

[0046] Example 1

[0047] A method for preparing a novel passivation contact structure of this embodiment includes the following preparation steps:

[0048] Step 1, preparing a tunneling oxide layer 4 on the surface of a target silicon wafer A. The target silicon wafer A is an N-type crystalline silicon wafer or a P-type crystalline silicon wafer; the crystalline silicon wafer can be a single crystal silicon wafer or a multi-crystalline silicon wafer. The target silicon wafer A is a substrate silicon wafer.

[0049] Step 2, injecting hydrogen ions from the surface of the donor silicon wafer B into the interior of the donor silicon wafer B to form a hydrogen-rich layer 6 inside the donor silicon wafer B, and obtaining a single crystal silicon layer 7 located between the hydrogen ion implantation surface of the donor silicon wafer B and the hydrogen-rich layer 6. The donor silicon wafer B is an N-type single crystal silicon wafer or a P-type single crystal silicon wafer.

[0050] Step 3, laminating the surface of the tunnel oxide layer 4 of the target silicon wafer A with the surface of the single crystal silicon layer 7 of the donor silicon wafer B, and then performing Si-to-SiO2 (silicon to silicon oxide) low temperature bonding.

[0051] Step 4, the hydrogen ions in the hydrogen-rich layer 6 are converted into H2 (hydrogen gas) through a thermal reaction. As the amount of H2 increases rapidly, the pressure of the hydrogen-rich layer 6 rises, causing the H2 in the hydrogen-rich layer 6 to escape and peel off the top single crystal silicon layer 7 from the donor silicon wafer B. High-temperature annealing is used to strengthen the bonding so as to firmly bond the single crystal silicon layer 7 to the surface of the tunneling oxide layer 4. The single crystal silicon layer 7 is then post-processed to form a new passivation contact structure of the tunneling oxide layer 4 superimposed on the single crystal silicon layer 7 on the surface of the target silicon wafer A.

[0052] In an example of this embodiment, in step 4, the post-processing is a polishing process, preferably a chemical mechanical polishing process, referred to as a CMP process; at this time, the single crystal silicon layer 7 in the novel passivation contact structure is an intrinsic single crystal silicon layer.

[0053] In another example of this embodiment, in step 4, the post-processing includes polishing and doping treatments performed sequentially on the single crystal silicon layer 7; the doping treatment may be phosphorus doping or boron doping. If the whole layer of the single crystal silicon layer 7 is doped, the whole layer of doped single crystal silicon layer is obtained; or, if the local area of ​​the single crystal silicon layer 7 is doped, the doped single crystal silicon layer is obtained in the local area, and the intrinsic single crystal silicon layer is obtained in the remaining area.

[0054] A novel passivation contact structure of the present embodiment can be prepared by the method for preparing a novel passivation contact structure in steps 1 to 4 above, and comprises a tunneling oxide layer 4 disposed on the surface of a target silicon wafer A, and a single crystal silicon layer 7 bonded to the surface of the tunneling oxide layer 4. The single crystal silicon layer 7 is an intrinsic single crystal silicon layer and / or a doped single crystal silicon layer, and the doping type of the doped single crystal silicon layer is P type and / or n type; the thickness of the single crystal silicon layer 7 is 100 to 150 nm (e.g., 130 nm), and the thickness of the tunneling oxide layer is less than or equal to 2 nm.

[0055] It should be noted that there are three ways to set the novel passivation contact structure in the photovoltaic cell in this embodiment:

[0056] First, the novel passivation contact structure can be arranged on both the front side and the back side of the target silicon wafer A of the photovoltaic cell. In this case, it is a photovoltaic cell with a double-sided novel passivation contact structure.

[0057] Secondly, the novel passivation contact structure can be disposed only on the front side of the target silicon wafer A of the photovoltaic cell. In this case, the photovoltaic cell has the novel passivation contact structure on the front side.

[0058] Thirdly, the novel passivation contact structure can be disposed only on the back side of the target silicon wafer A of the photovoltaic cell, and in this case, it is a photovoltaic cell with a novel passivation contact structure on the back side.

[0059] The following takes the third arrangement of the novel passivation contact structure in the photovoltaic cell as an example to describe in detail a method for manufacturing a photovoltaic cell (Topcon cell) having a novel back passivation contact structure according to this embodiment, including the following manufacturing steps:

[0060] S1, cleaning and texturing the surface of the target silicon wafer A to remove the damaged layer on the surface of the target silicon wafer A caused by cutting, and forming pyramid texturing surfaces on the front and back sides of the target silicon wafer A.

[0061] The target silicon wafer A is an N-type crystalline silicon wafer or a P-type crystalline silicon wafer; an alkaline solution is used for cleaning and texturing, and the alkaline solution is preferably a KOH solution or a NaOH solution.

[0062] In one example of this embodiment, the target silicon wafer A is an N-type single crystal silicon wafer, and the surface of the target silicon wafer A is treated with a heated NaOH solution to remove the damage layer and to form a pyramid velvet surface on the front and back of the target silicon wafer A; the thickness of the target silicon wafer A is 130 to 160 μm (such as 135 μm), the resistivity is 0.5 to 1.5 Ω·cm (such as 1 Ω·cm), and the size is preferably 182 mm×182 mm. After completing step S1, the following is obtained: Figure 1 The structure shown.

[0063] S2, preparing a selective emitter on the pyramid velvet surface on the front side of the target silicon wafer A.

[0064] The selective emitter is preferably a boron-doped selective emitter. Step S2 includes the following specific steps performed in sequence:

[0065] S21, performing boron diffusion doping on the front side of the target silicon wafer A after texturing.

[0066] In one example of the present embodiment, boron diffusion doping is performed on the front side of the target silicon wafer A after texturing to form a p+ doped emitter 1 on the front side of the target silicon wafer A. Specifically, the boron source is preferably boron trichloride, the diffusion temperature is 800-950°C (preferably 850-900°C, such as 880°C), the advancement temperature is 900-1000°C (preferably 900-950°C, such as 930°C), and the square resistance of the p+ doped emitter 1 after the boron diffusion doping process is 110±25Ω / sq, and the doping concentration is 1×10 20 ~1×10 21 cm -3 (e.g. 5.6×10 20 cm -3 ), the junction depth is 0.25-0.5 μm (such as 0.35 μm). After completing step S21, the following is obtained: Figure 2 The structure shown.

[0067] S22, selectively doping the local region of boron diffusion doping to form a heavily doped region.

[0068] Among them, the selective doping is preferably selective laser doping.

[0069] In one example of this embodiment, the target silicon wafer A doped with boron diffusion is selectively doped with SE laser to form a localized P++ heavily doped region 2, which extends from the local area of ​​the selective emitter to the local area on the front side of the target silicon wafer A. The square resistance of the P++ heavily doped region 2 is 80±15Ω / sq, and the doping concentration is 1×10 19 ~1×10 20 cm -3 (e.g. 3.1×10 19 cm-3 ), the junction depth is 0.8-1.5 μm (e.g., 1.2 μm). After completing step S22, the following is obtained: Figure 3 The structure shown.

[0070] In other examples of this embodiment, other existing selective doping methods may be used to form a heavily doped region in the local area of ​​boron diffusion doping.

[0071] S23, performing post-oxidation treatment on the target silicon wafer A to repair the heavily doped area, and forming a BSG layer 3 (borosilicate glass layer) on the outer surface of the target silicon wafer A to prevent the heavily doped area from being damaged during the subsequent cleaning process.

[0072] In one example of the present embodiment, tubular high-temperature oxidation is performed on the selectively doped target silicon wafer A to promote the redistribution of the doped atoms of the p+ doped emitter 1 and the P++ heavily doped region 2 to form a deep junction, thereby obtaining a selective emitter. Specifically, the temperature of the tubular high-temperature oxidation is 800-1200°C (preferably 950-1100°C, such as 1000°C) and the time is 60-200min (preferably 100-150min, such as 120min); after the tubular high-temperature oxidation, the junction depth of the p+ doped emitter 1 is 0.8-1.2μm (such as 0.9μm), the junction depth of the P++ heavily doped region 2 is 1.4-2.2μm (such as 1.86μm), and a borosilicate glass layer is formed on the outer surface of the target silicon wafer A. After completing step S23, the following is obtained. Figure 4 The structure shown.

[0073] In other examples of this embodiment, other existing post-oxidation treatment methods may also be used to complete step S23.

[0074] S3 specifically includes:

[0075] S31, removing the impurity layer (such as borosilicate glass layer) on the side and back of the target silicon wafer A.

[0076] In one example of this embodiment, the target silicon wafer A is preferably subjected to single-sided pickling to remove the borosilicate glass layer on the side and back of the target silicon wafer A, while retaining the borosilicate glass layer on the front of the target silicon wafer A as a front protective layer. Specifically, the pickling solution used for single-sided pickling is preferably an HF solution, and the mass fraction of HF is 3 to 20% (preferably 5 to 10%, such as 8%). After completing step S31, the following is obtained: Figure 5 The structure shown.

[0077] S32, polishing the back side of the target silicon wafer A so that the back side of the target silicon wafer A forms a smooth and flat polished surface.

[0078] In one example of this embodiment, the back side of the target silicon wafer A is preferably subjected to alkali polishing treatment to obtain a smooth and flat polished surface on the back side of the target silicon wafer A. Specifically, the alkali solution used for alkali polishing is preferably a NaOH solution, the volume concentration of NaOH is 5 to 8% (such as 6%), and the reaction temperature is 55 to 65° C. (such as 63° C.). After completing step S32, the following is obtained: Figure 6 The structure shown.

[0079] S4, preparing an ultra-thin tunneling oxide layer 4 on the back side of the target silicon wafer A.

[0080] In one example of this embodiment, it is preferred to use PECVD to deposit an ultra-thin tunneling oxide layer 4 with a thickness less than or equal to 2nm (such as 1nm) on the polished surface of the target silicon wafer A. Specifically, the volume ratio of SiH4:O2 is 1:2-5 (preferably 1:3), the reaction pressure is 8-12pa (preferably 10pa), the deposition temperature is 290-320℃ (preferably 300℃), and the deposition time is 1-3min (preferably 2min). After completing step S4, the following is obtained: Figure 7 The structure shown.

[0081] S5, performing pretreatment on the surface of the donor silicon wafer B as described in step S1.

[0082] The donor silicon wafer B is an N-type single crystal silicon wafer or a P-type single crystal silicon wafer.

[0083] In one example of this embodiment, another N-type single crystal silicon wafer is selected as the donor silicon wafer B, and the surface of the donor silicon wafer B is treated with a heated NaOH solution to remove the damage layer and to form a pyramid velvet surface on the front and back of the donor silicon wafer B; the thickness of the donor silicon wafer B is 140 to 170 μm (such as 160 μm), the resistivity is 0.5 to 1.5 Ω·cm (such as 1.3 Ω·cm), and the size is preferably 182 mm×182 mm. After completing step S5, the following is obtained: Figure 8 The structure shown.

[0084] S6, performing single-side polishing on the donor silicon wafer B processed in S5.

[0085] In one example of this embodiment, the donor silicon wafer B is preferably subjected to single-sided alkaline polishing treatment to obtain a smooth and flat polished surface on one side (such as the front or back side) of the donor silicon wafer B. The alkaline polishing solution is preferably a NaOH solution, the volume concentration of NaOH is 5 to 8% (such as 7%), and the reaction temperature is 55 to 65° C. (such as 60° C.). After completing step S6, the following is obtained: Fig. 9 The structure shown.

[0086] S7, injecting hydrogen ions from the polished surface of the donor silicon wafer B into the interior of the donor silicon wafer B to form a hydrogen-rich layer 6 inside the donor silicon wafer B, and obtaining a single crystal silicon layer 7 located between the polished surface of the donor silicon wafer B and the hydrogen-rich layer 6.

[0087] Wherein, step S7 includes the following specific steps performed in sequence:

[0088] S71, forming an implant protection layer 5 with a thickness of 10 to 50 nm on the polished surface of the donor silicon wafer B.

[0089] In one example of this embodiment, it is preferred that a 10-50 nm (e.g., 26 nm) thick implantation protection layer 5 is formed on the polished surface of the donor silicon wafer B by PECVD. The implantation protection layer 5 is a silicon dioxide layer (the silicon dioxide layer can enhance the randomness of the direction of ion entry and suppress the channeling effect of ion implantation). After completing step S71, the following is obtained: Fig.10 The structure shown.

[0090] S72, injecting hydrogen ions into the interior of the donor silicon wafer B through the surface of the injection protection layer 5 to form a hydrogen-rich layer 6 inside the donor silicon wafer B close to the polishing surface, and obtaining a single crystal silicon layer 7 located between the polishing surface of the donor silicon wafer B and the hydrogen-rich layer 6, the single crystal silicon layer 7 being between the injection protection layer 5 and the hydrogen-rich layer 6.

[0091] In one example of this embodiment, hydrogen ions are implanted into the donor silicon wafer B through the surface of the implant protection layer 5 to form a hydrogen-rich layer 6, and a single crystal silicon layer 7 is obtained between the implant protection layer 5 and the hydrogen-rich layer 6. Specifically, the dose of hydrogen ion implantation is 1×10 15 ~1×10 18 atoms / cm 2 (e.g. 2×10 17 atoms / cm 2 ), the energy range of hydrogen ion implantation is 10-100 keV (such as 55 keV), the temperature of hydrogen ion implantation is room temperature to 200°C (such as 125°C), and the accuracy of hydrogen ion implantation depth is 0.1-0.2 μm (such as 0.13 μm). After completing step S72, the following is obtained: Fig.11 The structure shown.

[0092] S73, removing the implant protection layer 5 to expose the top surface of the single crystal silicon layer 7.

[0093] In one example of this embodiment, after the hydrogen ion implantation is completed, the implantation protection layer 5 is preferably etched and removed by a diluted HF solution or a buffered oxide reagent; more preferably, an HF solution with a mass fraction of HF of 3 to 10% (such as 3.5%). After completing step S73, the following is obtained: Fig.12 The structure shown.

[0094] S8, laminating the back side of the tunnel oxide layer 4 of the target silicon wafer A to the surface of the single crystal silicon layer 7 of the donor silicon wafer B, and then performing Si-to-SiO2 (silicon to silicon oxide) low temperature bonding.

[0095] In one example of this embodiment, it is preferred to perform low-temperature bonding of Si-to-SiO2 by heat treatment or plasma treatment. When low-temperature bonding of Si-to-SiO2 is performed by heat treatment, the temperature of the heat treatment is 80 to 200°C (such as 150°C), the atmosphere of the heat treatment is one of N2, O2 or Ar (such as N2), and the time of the heat treatment is 1 to 2 hours (such as 1.8 hours). When low-temperature bonding of Si-to-SiO2 is performed by plasma treatment, the plasma is generated by one or more of Ar, N2, O2, Ne or H2O (such as Ar and N2). After completing step S8, the following is obtained. Fig.13 The structure shown.

[0096] S9, through thermal reaction, the hydrogen ions in the hydrogen-rich layer 6 are converted into H2. As the amount of H2 increases rapidly, the pressure of the hydrogen-rich layer 6 rises, causing the H2 in the hydrogen-rich layer 6 to escape and peel off the top single crystal silicon layer 7 from the donor silicon wafer B. High-temperature annealing is used to strengthen the bonding, and then polishing treatment (preferably CMP treatment) is performed to form a new passivation contact structure with a tunneling oxide layer 4 superimposed on a single crystal silicon layer 7 on the back side of the target silicon wafer A.

[0097] In one example of this embodiment, the single crystal silicon layer 7 is stripped by an energy source pulse, and the energy source can be a heat source, a cold source or a mechanical force source; preferably, it is a heat source, and the temperature of the thermal reaction is 200-400°C (such as 310°C). Specifically, the temperature of the high temperature annealing is 1000-1300°C (such as 1200°C), the annealing atmosphere is N2, and the annealing time is 2-4h (such as 3h). Thereafter, chemical mechanical polishing (CMP) is used to remove the surface damage layer and smooth the surface of the stripping layer (i.e., the single crystal silicon layer 7). After completing step S9, the following is obtained. Fig.14 The structure shown.

[0098] S10, phosphorus-doping is performed on the single crystal silicon layer 7 on the back side of the target silicon wafer A to form a doped single crystal silicon layer (such as an n+ doped single crystal silicon layer 8).

[0099] In one example of this embodiment, the phosphorus source used to form the doped single crystal silicon layer is preferably phosphine, the diffusion temperature is 700-800° C. (e.g., 730° C.), the advancement temperature is 800-900° C. (e.g., 860° C.), and the surface doping concentration of the n+ doped single crystal silicon layer 8 after phosphorus diffusion doping is 1×10 20 ~1×10 21 cm -3 (e.g. 5×10 20cm -3 ), the junction depth is 0.1-0.3 μm (e.g. 0.25 μm). After completing step S10, the following is obtained: Fig.15 The structure shown.

[0100] S11, removing the PSG layer 9 (phosphosilicate glass layer) formed by phosphorus doping on the target silicon wafer A.

[0101] In one example of this embodiment, the target silicon wafer A is pickled to remove the PSG layer 9 on the side and front of the target silicon wafer A. Specifically, the pickling solution is preferably an HF solution, and the mass fraction of HF is 3 to 10% (such as 6%). After completing step S11, the following is obtained: Fig.16 The structure shown.

[0102] S12, depositing a front passivation anti-reflection film and a back passivation anti-reflection film on the front and back of the target silicon wafer A respectively.

[0103] Among them, the front passivation anti-reflection film is preferably an Al2O3 film (aluminum oxide film 10) and a front SiN film located on the front of the aluminum oxide film 10. x film (front silicon nitride film 11); the back passivation anti-reflection film is preferably the back SiN x Film (back side silicon nitride film 12).

[0104] In one example of this embodiment, an aluminum oxide film 10 with a thickness of 2 to 10 nm is deposited on the front surface of the target silicon wafer A by using the ALD method; preferably, a front silicon nitride film 11 with a thickness of 60 to 80 nm (e.g., 70 nm) and a back silicon nitride film 12 with a thickness of 60 to 80 nm (e.g., 70 nm) are deposited by using the PECVD method. After completing step S12, the following is obtained: Fig.17 The structure shown.

[0105] S13, metallizing the front and back sides of the target silicon wafer A to form a front metal electrode 13 and a back metal electrode 14, respectively; the upper end of the back metal electrode 14 contacts the local area of ​​the doped single crystal silicon layer, and the lower end of the front metal electrode 13 contacts the local area of ​​the selective emitter, and the front metal electrode 13, the heavily doped region and the back metal electrode 14 are arranged in correspondence with each other in sequence.

[0106] In one example of this embodiment, the front metal electrode 13 and the back metal electrode 14 are preferably made of silver aluminum paste; specifically, the silver aluminum paste is printed by screen printing and sintered, and the sintering temperature is 850-890°C (such as 880°C), and the width of the front metal electrode 13 and the back metal electrode 14 are both 25-45μm (such as 33μm). After completing step S13, the following is obtained: Fig.18 The structure shown.

[0107] A photovoltaic cell of the present embodiment can be manufactured by the method for manufacturing a photovoltaic cell with a novel back passivation contact structure using the above steps S1 to 13, and is a Topcon cell, comprising a target silicon wafer A; the front side of the target silicon wafer A is provided with a selective emitter, a front passivation anti-reflection film and a front metal electrode 13 in sequence from bottom to top, the lower end of the front metal electrode 13 is in contact with a local portion of the selective emitter, and the upper end of the front metal electrode 13 extends to above the front passivation anti-reflection film; the back side of the target silicon wafer A is provided with a tunneling oxide layer 4, a doped single crystal silicon layer, a back passivation anti-reflection film and a back metal electrode 14 in sequence from top to bottom, the upper end of the back metal electrode 14 is in contact with a local portion of the doped single crystal silicon layer, and the lower end of the back metal electrode 14 extends to below the back passivation anti-reflection film.

[0108] Performance Testing

[0109] The performance of the novel back passivation contact structure including a tunneling oxide layer and a doped single-crystal silicon layer of Example 1 and the existing back passivation contact structure including a tunneling oxide layer and a doped polysilicon layer were tested. The test results are shown in Table 1 below.

[0110] Table 1

[0111]

[0112] In Table 1, Uoc refers to open circuit voltage, Isc refers to short circuit current, FF refers to fill factor, and Eta refers to conversion efficiency.

[0113] The new back passivation contact structure in the Topcon battery of Example 1 has a lower parasitic absorption of the single-crystalline silicon layer than that of the polycrystalline silicon layer, and the electron mobility of the single-crystalline silicon layer is much higher than that of the polycrystalline silicon layer, and the light absorption of the polycrystalline silicon layer at long wavelengths of 900 to 1100 nm is reduced. Therefore, the short-circuit current gain of the Topcon battery with the new back passivation contact structure in Example 1 is 15 mA; moreover, the single-crystalline silicon layer has a lower interface state density, which can reduce carrier recombination losses, so that the open circuit voltage of the Topcon battery with the new back passivation contact structure in Example 1 is increased by 0.3 mV, and the fill factor is increased by 0.05; and thus the conversion efficiency of the Topcon battery in Example 1 is increased by 0.07%.

[0114] In addition, compared with the amorphous silicon layer, amorphous silicon oxide layer, microcrystalline silicon layer or microcrystalline silicon oxide layer in the existing passivation contact structure, the photovoltaic cell of the utility model with a new back-side passivation contact structure (tunneling oxide layer superimposed on a single crystal silicon layer) is more advantageous in reducing parasitic absorption and carrier recombination losses, compensating for current density losses at long waves, and improving electron mobility. Therefore, the short-circuit current, open-circuit voltage, fill factor and conversion efficiency of the photovoltaic cell of the utility model are also improved.

[0115] Although the preferred embodiments of the utility model embodiments have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the utility model embodiments.

[0116] The technical solution provided by the utility model is introduced in detail above. Specific examples are used in this article to illustrate the principle and implementation method of the utility model. The description of the above embodiments is only used to help understand the core idea of ​​the utility model. At the same time, for general technical personnel in this field, according to the idea of ​​the utility model, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the utility model.

Claims

1. A novel passivation contact structure, characterized in that: include: A tunneling oxide layer disposed on the surface of the substrate silicon wafer, and a single crystal silicon layer bonded to the surface of the tunneling oxide layer; Wherein, the thickness of the tunnel oxide layer is less than or equal to 2 nm; the thickness of the single crystal silicon layer is 100-150 nm.

2. A novel passivation contact structure according to claim 1, characterized in that: The single crystal silicon layer is an intrinsic single crystal silicon layer and / or a doped single crystal silicon layer; the doping type of the doped single crystal silicon layer is P type and / or n type.

3. A novel passivation contact structure according to claim 1, characterized in that: The substrate silicon wafer is an N-type or P-type crystalline silicon wafer; the thickness of the substrate silicon wafer is 130-160 μm, the resistivity is 0.5-1.5 Ω·cm, and the size is 182 mm×182 mm.

4. A photovoltaic cell, characterized in that: include: A substrate silicon wafer, a passivation contact structure provided on the front and / or back of the substrate silicon wafer, a front passivation anti-reflection film and a back passivation anti-reflection film provided on the front and back of the substrate silicon wafer respectively, and a metal electrode provided on the front and / or back of the substrate silicon wafer; The passivation contact structure is a novel passivation contact structure as described in any one of claims 1 to 3.

5. A photovoltaic cell according to claim 4, characterized in that: The passivation contact structure is arranged on the back side of the substrate silicon wafer, and the single crystal silicon layer in the passivation contact structure is a doped single crystal silicon layer; the back passivation anti-reflection film is arranged on the back side of the doped single crystal silicon layer; The metal electrode comprises a back metal electrode, the upper end of the back metal electrode contacts the local area of ​​the doped single crystal silicon layer, and the lower end of the back metal electrode extends to below the back passivation anti-reflection film.

6. A photovoltaic cell according to claim 5, characterized in that: The doped single crystal silicon layer is an n+ doped single crystal silicon layer, and the junction depth of the n+ doped single crystal silicon layer is 0.1-0.3 μm.

7. A photovoltaic cell according to claim 4, characterized in that: It also includes a selective emitter disposed on the front side of the substrate silicon wafer, and the front passivation anti-reflection film is disposed on the front side of the selective emitter; The metal electrode further comprises a front metal electrode, the lower end of the front metal electrode is in contact with the local area of ​​the selective emitter, and the upper end of the front metal electrode extends to the top of the front passivation anti-reflection film.

8. A photovoltaic cell according to claim 7, characterized in that: The selective emitter includes a p+ doped emitter disposed on the front side of the substrate silicon wafer, and a p++ heavily doped region extending from the local area of ​​the selective emitter to the local area of ​​the front side of the substrate silicon wafer; The sheet resistance of the p+ doped emitter is 110±25Ω / sq, and the junction depth is 0.8-1.2μm; The square resistance of the P++ heavily doped region is 80±15Ω / sq, and the junction depth is 1.4-2.2μm.

9. A photovoltaic cell according to claim 4, characterized in that: The back passivation anti-reflection film is a back silicon nitride film with a thickness of 60 to 80 nm; The front passivation anti-reflection film comprises an aluminum oxide film and a front silicon nitride film arranged on the front of the aluminum oxide film; the thickness of the aluminum oxide film is 2 to 10 nm, and the thickness of the front silicon nitride film is 60 to 80 nm.

10. A photovoltaic cell according to claim 4, characterized in that: The front side of the substrate silicon wafer is a pyramid velvet surface, and the back side of the substrate silicon wafer is a smooth and flat polished surface.