Method for recovering polypropylene film

By using a metallocene-catalyzed single-layer polypropylene film for mechanical recycling, the problem of difficult improvement in the optical properties of the polypropylene film is solved, the mechanical properties and gel index of the polypropylene film are improved, and the energy recovery needs are reduced.

CN119032124APending Publication Date: 2024-11-26北欧化工公司
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202380033766.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-26
Filing Date
2023-04-25
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to improve optical performance during the recovery process of polypropylene films, especially in film applications, and the energy demand is high during the recovery process.

Method used

Mechanical recovery using a monolayer polypropylene film containing metallocene catalysis by providing specific properties random propylene copolymers (R-PP), including high melt flow rates, melting temperatures and comonomer content, and by quantitative 13C -NMR spectral analysis determines the defect content of 2,1-region to form a regenerated polypropylene composition to prepare a regenerated polypropylene film.

Benefits of technology

It is achieved to improve the mechanical properties of the polypropylene film without significantly reducing the optical properties, and to reduce the energy demand of the recovery process, and to significantly improve the gel index of the regenerated polypropylene film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005079905390000061
    Figure BDA0005079905390000061
  • Figure BDA0005079905390000071
    Figure BDA0005079905390000071
  • Figure BDA0005079905390000072
    Figure BDA0005079905390000072
Patent Text Reader

Abstract

The present invention relates to a process for forming a regenerated polypropylene film wherein a specific single-layer polypropylene film is recovered, a regenerated polypropylene film obtainable thereby, the use of a single-layer polypropylene film in a recovery process, and the use of a regenerated polypropylene composition in a film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a process for forming a recycled polypropylene film, wherein a specific monolayer polypropylene film is recycled, a recycled polypropylene film obtainable thereby, the use of a monolayer polypropylene film in a recycling process and the use of a recycled polypropylene composition in a film. Background Art

[0002] Polyolefins, particularly polyethylene and polypropylene, are consumed in increasingly large quantities in a wide range of applications including packaging for food and other goods, fibers, automotive parts, and a wide variety of articles.

[0003] Polypropylene based materials have great potential for mechanical recycling as these materials are widely used in packaging. Considering the huge amount of waste collected relative to the amount of waste recycled into the stream, there is still great potential for smart reuse of plastic waste streams and mechanical recycling of plastic waste.

[0004] If sufficient care is taken during the recycling process, it is possible to obtain recycled polyolefins with satisfactory mechanical properties that are not much different from the original material. Alternatively, any reduction in mechanical properties can be corrected by adding various modifiers to the polyolefin.

[0005] While mechanical properties can be modified in this way, it is difficult to improve the optical properties of recycled polyolefins, especially for film applications.

[0006] Therefore, the development of polyolefin films that can be easily recycled without significant degradation of optical properties would represent a significant advance. Summary of the invention

[0007] Accordingly, the present inventors have discovered that certain monolayer polypropylene films comprising metallocene-catalyzed polypropylene are much easier to recycle than similar films comprising Ziegler-Natta-catalyzed polypropylene, both in terms of the final optical properties of the regenerated film and the energy requirements during the recycling process.

[0008] Therefore, the present invention relates to a method for forming a recycled polypropylene film, said method comprising the following steps:

[0009] (a) providing a single-layer polypropylene film, wherein the single-layer polypropylene film comprises at least 90 wt% of a random propylene copolymer (R-PP), based on the total weight of the single-layer polypropylene film, wherein the random propylene copolymer has the following properties:

[0010] i) a melt flow rate (MFR2) of 2.0 to 20.0 g / 10 min measured at 230°C and 2.16 kg according to ISO 1133;

[0011] ii) Melting temperature (T) measured by differential scanning calorimetry (DSC) m ) is 120 to 150° C.;

[0012] iii) By quantitative 13 The total comonomer content determined by C-NMR spectroscopy is 1.0 to 10.0 mol%, wherein the comonomer is selected from ethylene and C4 to C8 α-olefins and combinations thereof;

[0013] iv) By quantitative 13 The content of 2,1-regio defects determined by C-NMR spectroscopy analysis ranged from 0.05 to 1.4 mol %;

[0014] (b) mechanically recovering the film of step (a) to obtain a recycled polypropylene composition; and

[0015] (c) extruding the recycled polypropylene composition of step (b) to form a recycled polypropylene film, preferably a recycled polypropylene cast film.

[0016] In another embodiment, the present invention is directed to a recycled polypropylene film comprising a recycled polypropylene composition having:

[0017] i) a melt flow rate (MFR2) of 2.0 to 20.0 g / 10 min measured at 230°C and 2.16 kg according to ISO 1333;

[0018] ii) Melting temperature (T) measured by differential scanning calorimetry (DSC) m ) is 120 to 150° C.;

[0019] iii) By quantitative 13 The total comonomer content determined by C-NMR spectroscopy is 1.0 to 10.0 mol%, wherein the comonomer is selected from ethylene and C4 to C8 α-olefins and combinations thereof; and

[0020] iv) By quantitative 13 The content of 2,1-regio defects determined by C-NMR spectroscopy analysis ranged from 0.05 to 1.4 mol %;

[0021] The gel index of the recycled polypropylene film measured on a 70 μm film sample is 16.0 to 50.0.

[0022] In another embodiment, the present invention relates to the use of a monolayer polypropylene film for obtaining a recycled polypropylene film, the monolayer polypropylene film comprising at least 90 wt.% of a random propylene copolymer (R-PP) having the following properties:

[0023] i) a melt flow rate (MFR2) of 2.0 to 20.0 g / 10 min measured at 230°C and 2.16 kg according to ISO 1133;

[0024] ii) Melting temperature (T) measured by differential scanning calorimetry (DSC) m ) is 120 to 150° C.;

[0025] iii) By quantitative 13 The total comonomer content determined by C-NMR spectroscopy is 1.0 to 10.0 mol%, wherein the comonomer is selected from ethylene and C4 to C8 α-olefins and combinations thereof;

[0026] iv) By quantitative 13 The content of 2,1-regio defects determined by C-NMR spectroscopy analysis ranged from 0.05 to 1.4 mol %;

[0027] The regenerated polypropylene film has a gel index of 16.0 to 50.0 measured on a 70 μm film sample;

[0028] The recycled polypropylene film is obtained by mechanically recycling the single-layer polypropylene film.

[0029] In a final embodiment, the present invention also relates to the use of a recycled polypropylene composition in a film, preferably a cast film, wherein the recycled polypropylene composition has the following properties:

[0030] i) a melt flow rate (MFR2) of 2.0 to 20.0 g / 10 measured at 230°C and 2.16 kg according to ISO 1133

[0031] ii) Melting temperature (T) measured by differential scanning calorimetry (DSC) m ) is 120 to 150° C.;

[0032] iii) By quantitative 13 The total comonomer content is 1.0 to 10.0 mol% as determined by C-NMR spectroscopy, wherein the comonomer is selected from ethylene and C4 to C8 alpha-olefins; and

[0033] iv) By quantitative 13 The content of 2,1-regio defects determined by C-NMR spectral analysis was 0.05 to 1.4 mol%.

[0034] definition

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the invention belongs. Although preferred materials and methods are described herein, any methods and materials similar or equivalent to those described herein may be used in practice to test the present invention. In describing and claiming the present invention, the following terms will be used according to the definitions listed below.

[0036] Unless expressly stated otherwise, the terms "a", "an", etc., are used to refer to more than one.

[0037] Propylene homopolymers are polymers consisting essentially of propylene monomer units. Due to impurities, especially impurities during commercial polymerization processes, propylene homopolymers may contain up to 0.1 mol% comonomer units, preferably up to 0.05 mol% comonomer units, most preferably up to 0.01 mol% comonomer units.

[0038] The random copolymer of propylene is a copolymer of propylene monomer units and comonomer units, wherein the comonomer units are preferably selected from ethylene and C4-C8 alpha-olefins, wherein the comonomer units are randomly distributed on the polymer chain. The random copolymer of propylene may contain comonomer units from more than one comonomer having different numbers of carbon atoms.

[0039] Unless stated otherwise, the amounts hereinafter are given as weight % (wt.-%).

[0040] Propylene homopolymers and propylene random copolymers usually have only one glass transition temperature. DETAILED DESCRIPTION

[0041] method

[0042] The method of the present invention is a method for forming a recycled polypropylene film, and the method comprises the following steps:

[0043] (a) providing a single-layer polypropylene film, the single-layer polypropylene film comprising at least 90 wt% of a random propylene copolymer (R-PP), the random propylene copolymer having the following properties:

[0044] i) a melt flow rate (MFR2) of 2.0 to 20.0 g / 10 min measured at 230°C and 2.16 kg according to ISO 1333;

[0045] ii) Melting temperature (T) measured by differential scanning calorimetry (DSC) m ) is 120 to 150° C.;

[0046] iii) By quantitative 13The total comonomer content determined by C-NMR spectroscopy is 1.0 to 10.0 mol%, wherein the comonomer is selected from ethylene and C4 to C8 α-olefins and combinations thereof;

[0047] iv) By quantitative 13 The content of 2,1-regio defects determined by C-NMR spectroscopy analysis ranged from 0.05 to 1.4 mol %;

[0048] (b) mechanically recovering the film of step (a) to obtain a recycled polypropylene composition; and

[0049] (c) extruding the recycled polypropylene composition of step (b) to form a recycled polypropylene film, preferably a recycled polypropylene cast film.

[0050] The mechanical recovery of step (b) can be any mechanical recovery method known in the art; however, preferably, the mechanical recovery of step (b) is carried out in a continuous melt mixing device, preferably at a temperature of 170 to 270°C, more preferably at a temperature of 180 to 260°C, and most preferably at a temperature of 185 to 230°C.

[0051] The extrusion of step (c) can be any extrusion method known to those skilled in the art to be suitable for making recycled polypropylene film (preferably recycled polypropylene cast film). Machines designed for implementing such extrusion methods (i.e., extruders) are well known in the art. During the extrusion of such films, the temperature of the melt can be 200 to 290° C.

[0052] Single layer polypropylene film

[0053] The selection of the single layer polypropylene film is a critical factor in the present invention.

[0054] The monolayer polypropylene film according to this invention comprises at least 90 wt%, more preferably at least 95 wt%, further preferably at least 98 wt% of the random propylene copolymer (R-PP).

[0055] In one embodiment the monolayer polypropylene film consists essentially of the random propylene copolymer (R-PP).

[0056] The monolayer polypropylene film of the present invention may contain other components. However, preferably, the monolayer polypropylene film of the present invention only contains the random propylene copolymer (R-PP) defined below as a polymer component. Therefore, based on the total weight of the monolayer polypropylene film, the amount of the random propylene copolymer (R-PP1) may not be 100.0 wt%. Therefore, the remainder of the 100.0 wt% total weight of the monolayer polypropylene film can be achieved by other additives known in the art. However, the remainder should not exceed 10.0 wt%, preferably not more than 5.0 wt%, more preferably not more than 3.0 wt% in the monolayer polypropylene film. For example, the monolayer polypropylene film may also contain a small amount of additives selected from antioxidants, stabilizers, fillers, colorants, nucleating agents and antistatic agents. In general, they are added during the granulation process of the powdery product obtained in the polymerization.

[0057] In case the monolayer polypropylene film comprises an α-nucleating agent, it is preferably free of a β-nucleating agent. The α-nucleating agent is preferably selected from:

[0058] (i) salts of mono- and polycarboxylic acids, for example sodium benzoate or aluminium tert-butylbenzoate,

[0059] (ii) dibenzylidene sorbitol (e.g. 1,3:2,4-dibenzylidene sorbitol) and C1-C8 alkyl-substituted dibenzylidene sorbitol derivatives, for example methyldibenzylidene sorbitol, ethyldibenzylidene sorbitol or dimethyldibenzylidene sorbitol (e.g. 1,3:2,4-di(methylbenzylidene) sorbitol), or substituted nonanol derivatives, for example 1,2,3-trideoxy-4,6:5,7-bis-O-[(4-propylphenyl)methylene]-nonanol,

[0060] (iii) salts of phosphoric acid diesters, for example sodium 2,2'-methylene-bis(4,6-di-tert-butylphenyl)phosphate or bis[2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate]hydroxyaluminum,

[0061] (iv) vinylcycloalkane polymers and vinylalkane polymers (discussed in more detail below), and

[0062] (v) mixtures thereof.

[0063] Such additives are generally commercially available and are described, for example, in "Plastic Additives Handbook" by Hans Zweifel, (pp. 871 to 873, 5th edition, 2001).

[0064] The gel index of the single-layer polypropylene film is preferably in the range of 0.0 to less than 16.0, more preferably in the range of 2.0 to less than 16.0, further preferably in the range of 6.0 to less than 16.0, most preferably in the range of 10.0 to less than 16.0.

[0065] Furthermore, the thickness of the single-layer polypropylene film is preferably 1 to 200 μm, more preferably 5 to 180 μm, further preferably 10 to 160 μm, and most preferably 20 to 130 μm.

[0066] Random propylene copolymer (R-PP)

[0067] The main component present in the monolayer polypropylene film is the random propylene copolymer (R-PP) which is present in an amount of at least 90 wt%.

[0068] The random propylene copolymer (R-PP) has a melt flow rate (MFR2), measured according to ISO 1333 at 230°C and 2.16 kg, of 2.0 to 20.0 g / 10 min, more preferably 2.5 to 10.0 g / 10 min, most preferably 3.0 to 7.0 g / 10 min.

[0069] The random propylene copolymer (R-PP) preferably has a xylene cold soluble content (XCS), determined according to ISO 16152, of 5 to 25 wt.-%, more preferably of 10 to 20 wt.-%, most preferably of 12 to 18 wt.-%.

[0070] The random propylene copolymer (R-PP) preferably has a molecular weight distribution (Mz / Mw) determined by gel permeation chromatography (GPC) of 1.10 to 2.10, more preferably 1.30 to 2.00, most preferably 1.50 to 1.90.

[0071] The random propylene copolymer (R-PP) preferably has a weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) of 200 to 300 kg / mol, more preferably 220 to 280 kg / mol, most preferably 240 to 260 kg / mol.

[0072] The random propylene copolymer (R-PP) preferably has a size average molecular weight (Mz) determined by gel permeation chromatography (GPC) of 400 to 500 kg / mol, more preferably 420 to 480 kg / mol, most preferably 440 to 470 kg / mol.

[0073] Furthermore, the melting temperature (T m) is 120-150°C, more preferably 122-148°C, most preferably 125-145°C.

[0074] In addition, random propylene copolymer (R-PP) is quantitatively 13 The total comonomer content determined by C-NMR spectroscopy is 1.0 to 10.0 mol%, more preferably 3.0 to 9.0 mol%, most preferably 5.0 to 8.0 mol%.

[0075] The comonomers of the random propylene copolymer (R-PP) are selected from ethylene and C4 to C8 α-olefins and combinations thereof.

[0076] Particularly preferably, the random copolymer (R-PP) contains two comonomers, wherein, preferably, the first comonomer is ethylene and the second comonomer is selected from C4 to C8 α-olefins; more preferably, the first comonomer is ethylene and the second comonomer is 1-butene.

[0077] In addition, random propylene copolymer (R-PP) is quantitatively 13 The content of 2,1-regio defects determined by C-NMR spectral analysis is 0.05 to 1.4 mol %, more preferably 0.10 to 1.2 mol %, most preferably 0.20 to 0.90 mol %.

[0078] The presence of 2,1-regio defects in the random propylene copolymer (R-PP) indicates that the random propylene copolymer (R-PP) is polymerized in the presence of a single site catalyst (SSC).

[0079] Accordingly the random propylene copolymer (R-PP) is also preferably polymerized in the presence of a single site catalyst (SSC), more preferably in the presence of a metallocene catalyst.

[0080] The term "2,1 regio defect" used in the present invention is defined as the sum of 2,1-erythro regio defect and 2,1-threo regio defect.

[0081] The random propylene copolymers having the desired high number of regio defects in the propylene composition of the present invention are typically and preferably prepared in the presence of a single site catalyst.

[0082] Preferably, the random propylene copolymer (R-PP) has a gel index in the range of 0.0 to less than 16.0, more preferably in the range of 2.0 to less than 16.0, further preferably in the range of 6.0 to less than 16.0, most preferably in the range of 10.0 to less than 16.0, measured on a 70 μm film sample.

[0083] The random propylene copolymer (R-PP) is also preferably a multimodal random propylene copolymer, more preferably a bimodal random propylene copolymer.

[0084] Multimodal means that the random propylene copolymer (R-PP) comprises two or more different fractions which differ in at least one property, most typically melt flow rate (MFR2) or comonomer content.

[0085] Accordingly, preferably the random propylene copolymer (R-PP) comprises:

[0086] (a) a first random propylene copolymer fraction (R-PP1) having a melt flow rate (MFR2) measured according to ISO 1333 at 230 °C and 2.16 kg of 1.0 to 10.0 g / 10 min, more preferably of 1.3 to 5.0 g / 10 min, most preferably of 1.5 to 3.5 g / 10 min; and

[0087] (b) a second random propylene copolymer fraction (R-PP2) having a melt flow rate (MFR2) greater than the melt flow rate of the first random propylene copolymer fraction.

[0088] The weight ratio between the first random propylene copolymer fraction (R-PP1) and the second random propylene copolymer fraction (R-PP2) [(R-PP1):(R-PP2)] is preferably from 30:70 to 70:30, more preferably from 33:67 to 60:40, most preferably from 35:65 to 50:50.

[0089] The first random propylene copolymer fraction (R-PP1) and the random propylene copolymer (R-PP) together preferably also satisfy inequality (I):

[0090]

[0091] In the formula,

[0092] MFR(R-PP) is the melt flow rate (MFR2) of the random propylene copolymer (R-PP) measured according to ISO 1333 at 230°C and 2.16 kg, and

[0093] MFR(R-PP1) is the melt flow rate (MFR2) of the first random propylene copolymer fraction (R-PP1) measured according to ISO 1333 at 230°C and 2.16 kg.

[0094] More preferably, the first random propylene copolymer fraction (R-PP1) and the random propylene copolymer (R-PP) together satisfy inequality (Ia):

[0095]

[0096] Most preferably, the first random propylene copolymer fraction (R-PP1) and the random propylene copolymer (R-PP) together satisfy inequality (Ib):

[0097]

[0098] Process for the polymerization of random propylene copolymers (R-PP)

[0099] The process for preparing the random propylene copolymer (R-PP) is described in further detail below.

[0100] The random propylene copolymer (R-PP) is preferably produced in a sequential polymerization process.

[0101] The term "sequential polymerization system" means that the random propylene copolymer (R-PP) is produced in at least two reactors connected in series.

[0102] Preferably, the random propylene copolymer (R-PP) has been produced in a dual reactor sequence, wherein the first reactor is a slurry reactor, more preferably a loop reactor, and the second reactor is a gas phase reactor.

[0103] A preferred multi-stage process is a "loop-gas phase" process, such as the process developed by Borealis A / S of Denmark (known as Technology), for example, is described in patent documents such as EP 0 887 379, WO 92 / 12182, WO 2004 / 000899, WO 2004 / 111095, WO 99 / 24478, WO 99 / 24479 or WO 00 / 68315.

[0104] Other suitable slurry-gas phase processes are Basell's method.

[0105] Accordingly, the random propylene copolymer (R-PP) is preferably produced by a process comprising the steps of:

[0106] (a) in a first polymerization reactor (R1), i.e. in a loop reactor (LR), propylene is polymerized with one or more, preferably one or two, different comonomers selected from ethylene and C4 to C8 α-olefins, more preferably selected from ethylene and / or 1-butene, to obtain a first random propylene copolymer fraction (R-PP1),

[0107] (b) transferring the first random propylene copolymer fraction (R-PP1) to a second polymerization reactor (R2),

[0108] (c) in the second polymerization reactor (R2), propylene is polymerized with one or more (preferably one or two) different comonomers selected from ethylene and C4 to C8 α-olefins, more preferably selected from ethylene and / or 1-butene, in the presence of the first random propylene copolymer fraction (R-PP1) to obtain a second random propylene copolymer fraction (R-PP2), wherein the first random propylene copolymer fraction (R-PP1) and the second random propylene copolymer fraction (R-PP2) form a random propylene copolymer (R-PP).

[0109] The prepolymerization as described above may be carried out prior to step (a).

[0110] As stated above, in the specific process for preparing the random propylene copolymer (R-PP) as described above, a single site catalyst (SSC) shall be used. Accordingly, the single site catalyst (SSC) will now be described in more detail.

[0111] The single site catalyst according to the present invention may be any supported metallocene catalyst suitable for producing highly isotactic polypropylene.

[0112] The single site catalyst (SSC) preferably comprises a metallocene complex, a cocatalyst system comprising a boron-containing cocatalyst and / or an aluminoxane cocatalyst and a silica support.

[0113] Preferred metallocene complex catalysts include:

[0114] Racemic-dimethylsilanediylbis[2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride,

[0115] Racemic-trans-dimethylsilanediyl[2-methyl-4-(4'-tert-butylphenyl)-inden-1-yl][2-methyl-4-(4'-tert-butylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride,

[0116] Racemic-trans-dimethylsilanediyl[2-methyl-4-(4'-tert-butylphenyl)-inden-1-yl][2-methyl-4-phenyl-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride,

[0117] Racemic-trans-dimethylsilanediyl[2-methyl-4-(3',5'-tert-butylphenyl)-1,5,6,7-tetrahydro-s-inden-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride,

[0118] Racemic-trans-dimethylsilanediyl[2-methyl-4,8-bis-(4'-tert-butylphenyl)-1,5,6,7-tetrahydro-s-inden-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride,

[0119] Racemic-trans-dimethylsilanediyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-inden-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride,

[0120] Racemic-trans-dimethylsilanediyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-inden-1-yl][2-methyl-4-(3',5'-5-di-tert-butylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium dichloride.

[0121] Particularly preferred is rac-trans-dimethylsilanediyl[2-methyl-4,8-bis-(3',5'-dimethylphenyl)-1,5,6,7-tetrahydro-s-inden-1-yl][2-methyl-4-(3',5'-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl]zirconium(II) dichloride:

[0122]

[0123] The ligands required for forming the complexes and catalysts of the present invention can be synthesized by any method, and skilled organic chemists can design various synthesis schemes to make the necessary ligand materials. For example, WO2007 / 116034 discloses necessary chemical methods. Synthesis schemes can also be generally found in WO 2002 / 02576, WO 2011 / 135004, WO 2012 / 084961, WO 2012 / 001052, WO 2011 / 076780, WO 2015 / 158790 and WO 2018 / 122134. With particular reference to WO2019 / 179959, the most preferred catalysts of the present invention are described.

[0124] According to the present invention, a cocatalyst system comprising a boron-containing cocatalyst and / or an aluminoxane cocatalyst is used in combination with the above-mentioned metallocene catalyst complex.

[0125] Preferred cocatalysts are aluminoxanes (more preferably methylaluminoxane), combinations of aluminoxanes with aluminum alkyls, boron or borate cocatalysts, and combinations of aluminoxanes with boron-based cocatalysts.

[0126] The catalyst can be used in supported or unsupported form, preferably in supported form. The particulate support material used is preferably an organic or inorganic material, such as silicon dioxide, aluminum oxide, zirconium oxide or a mixed oxide (such as silicon dioxide-alumina), in particular silicon dioxide, aluminum oxide or silicon dioxide-alumina. Preferably, a silicon dioxide support is used. Those skilled in the art are aware of the procedures required for supporting metallocene catalysts.

[0127] The use of these vectors is routine in the art.

[0128] Recycled polypropylene compositions and films

[0129] The recycled polypropylene composition obtained in step (b) and the recycled polypropylene film obtained in step (c) may also be defined with respect to the mechanical and optical properties, both with respect to their absolute values ​​and with respect to their values ​​relative to the random propylene copolymer (R-PP) and / or the monolayer polypropylene film.

[0130] In practice, the ratio of MFR2 of the recycled polypropylene composition obtained in step (b) to the MFR2 of the random propylene copolymer (R-PP) of the monolayer polypropylene film provided in step (a) [MFR2(B) / MFR2(A)] is preferably from 1.00 to 1.30, more preferably from 1.00 to 1.20, most preferably from 1.00 to 1.15.

[0131] Further preferably, the ratio of the xylene cold soluble content (XCS) of the recycled polypropylene composition obtained in step (b) measured according to ISO 16152 to the xylene cold soluble content (XCS) of the random propylene copolymer (R-PP) of the monolayer polypropylene film provided in step (a) measured according to ISO 16152 [XCS(B) / XCS(A)] is from 1.00 to 1.30, more preferably from 1.00 to 1.20, most preferably from 1.00 to 1.10.

[0132] It is also preferred that the ratio of the weight average molecular weight (Mw) of the recycled polypropylene composition obtained in step (b) measured by gel permeation chromatography (GPC) to the weight average molecular weight (Mw) of the random propylene copolymer (R-PP) of the single-layer polypropylene film provided in step (a) measured by gel permeation chromatography (GPC) [Mw(B) / Mw(A)] is from 0.90 to 1.00, more preferably from 0.95 to 1.00, most preferably from 0.97 to 1.00.

[0133] Further preferably, the ratio of the size average molecular weight (Mz) of the recycled polypropylene composition obtained in step (b) determined by gel permeation chromatography (GPC) to the size average molecular weight (Mz) of the random propylene copolymer (R-PP) of the single-layer polypropylene film provided in step (a) determined by gel permeation chromatography (GPC) [Mz(B) / Mz(A)] is from 0.90 to 1.00, more preferably from 0.93 to 1.00, most preferably from 0.96 to 1.00.

[0134] It is also preferred that the ratio of the molecular weight distribution (MWD, Mz / Mw) of the recycled polypropylene composition obtained in step (b) determined by gel permeation chromatography (GPC) to the molecular weight distribution (MWD, Mz / Mw) of the random propylene copolymer (R-PP) of the single-layer polypropylene film provided in step (a) determined by gel permeation chromatography (GPC) [MWD(B) / MWD(A)] is from 0.90 to 1.00, more preferably from 0.95 to 1.00, most preferably from 0.98 to 1.00.

[0135] Further preferably, the ratio of the gel index of the regenerated polypropylene film obtained in step (c) to the gel index of the single-layer polypropylene film provided in step (a) [gel index (C) / gel index (A)] is 1.00 to 10.0, more preferably 1.00 to 5.0, most preferably 1.00 to 2.0.

[0136] The ratio of the gel index of the regenerated polypropylene film obtained in step (c) to the gel index of the single-layer polypropylene film provided in step (a) [gel index (C) / gel index (A)] may also be 1.00 to 1.50, more preferably 1.00 to 1.30, most preferably 1.00 to 1.10.

[0137] Alternatively or additionally, the ratio of the gel index of the recycled polypropylene composition obtained in step (b) measured on a 70 μm cast film sample to the gel index of the random propylene copolymer (R-PP) of the single-layer polypropylene film provided in step (a) measured on a 70 μm cast film sample [gel index (B) / gel index (A)] is preferably 1.00 to 10.0, more preferably 1.00 to 5.0, most preferably 1.00 to 2.0.

[0138] The ratio of the gel index of the recycled polypropylene composition obtained in step (b) measured on a 70 μm cast film sample to the gel index of the random propylene copolymer (R-PP) of the single-layer polypropylene film provided in step (a) measured on a 70 μm cast film sample [gel index (B) / gel index (A)] may also be from 1.00 to 1.50, more preferably from 1.00 to 1.30, most preferably from 1.00 to 1.10.

[0139] In a separate embodiment, the present invention is directed to a recycled polypropylene film comprising a recycled polypropylene composition having:

[0140] i) a melt flow rate (MFR2) of 2.0 to 20.0 g / 10 min measured at 230°C and 2.16 kg according to ISO 1333;

[0141] ii) Melting temperature (T) measured by differential scanning calorimetry (DSC) m ) is 120 to 150° C.;

[0142] iii) By quantitative 13 The total comonomer content determined by C-NMR spectroscopy is 1.0 to 10.0 mol%, wherein the comonomer is selected from ethylene and C4 to C8 α-olefins and combinations thereof; and

[0143] iv) By quantitative 13 The content of 2,1-regio defects determined by C-NMR spectroscopy analysis ranged from 0.05 to 1.4 mol %;

[0144] The gel index of the recycled polypropylene film measured on a 70 μm film sample is 16.0 to 50.0.

[0145] The recycled polypropylene composition has a melt flow rate (MFR2) measured according to ISO 1333 at 230°C and 2.16 kg of 2.0 to 20.0 g / 10 min, more preferably 2.5 to 10.0 g / 10 min, most preferably 3.0 to 7.0 g / 10 min.

[0146] The recycled polypropylene composition preferably has a xylene cold soluble content (XCS), determined according to ISO 16152, of 5 to 25 wt.-%, more preferably of 10 to 22 wt.-%, most preferably of 13 to 19 wt.-%.

[0147] The molecular weight distribution (Mz / Mw) of the recycled polypropylene composition as determined by gel permeation chromatography (GPC) is preferably from 1.10 to 2.10, more preferably from 1.30 to 2.00, most preferably from 1.50 to 1.90.

[0148] The weight average molecular weight (Mw) of the recycled polypropylene composition as determined by gel permeation chromatography (GPC) is preferably from 200 to 300 kg / mol, more preferably from 225 to 280 kg / mol, most preferably from 240 to 260 kg / mol.

[0149] The size average molecular weight (Mz) of the recycled polypropylene composition as determined by gel permeation chromatography (GPC) is preferably from 400 to 500 kg / mol, more preferably from 420 to 480 kg / mol, most preferably from 430 to 460 kg / mol.

[0150] In addition, the melting temperature (T m ) is 120 to 150°C, more preferably 122 to 148°C, most preferably 125 to 145°C.

[0151] In addition, the recycled polypropylene composition is quantitatively 13 The total comonomer content determined by C-NMR spectroscopy is 1.0 to 10.0 mol%, more preferably 3.0 to 9.0 mol%, most preferably 5.0 to 8.0 mol%.

[0152] The comonomer of the recycled polypropylene composition is selected from ethylene and C4 to C8 α-olefins and combinations thereof.

[0153] Particularly preferably, the recycled polypropylene composition contains two comonomers, wherein, preferably, the first comonomer is ethylene and the second comonomer is selected from C4 to C8 α-olefins; more preferably, the first comonomer is ethylene and the second comonomer is 1-butene.

[0154] In addition, the recycled polypropylene composition is quantitatively 13 The content of 2,1-regio defects determined by C-NMR spectral analysis is 0.05 to 1.4 mol %, more preferably 0.10 to 1.2 mol %, most preferably 0.20 to 0.9 mol %.

[0155] The presence of 2,1-regio defects in the recycled polypropylene composition indicates that the material recycled into the recycled polypropylene composition was polymerized in the presence of a single site catalyst (SSC).

[0156] The gel index of the recycled polypropylene composition measured on a 70 μm film sample is preferably from 16.0 to 50.0, more preferably from 16.0 to 40.0, further preferably from 16.0 to 30.0, most preferably from 16.0 to 20.0.

[0157] The gel index of the recycled polypropylene film is 16.0 to 50.0, more preferably 16.0 to 40.0, further preferably 16.0 to 30.0, most preferably 16.0 to 20.0.

[0158] The recycled polypropylene film can preferably be obtained by the above method, and more preferably is obtained by the above method.

[0159] All preferred embodiments and alternatives disclosed for the method as described above and the use as described below apply mutatis mutandis to the recycled polypropylene composition and the recycled polypropylene film.

[0160] application

[0161] The invention also relates to the use of the monolayer film according to the invention.

[0162] The present invention also relates to the use of a monolayer polypropylene film for obtaining a recycled polypropylene film, wherein the monolayer polypropylene film comprises at least 90 wt.% of a random propylene copolymer (R-PP), wherein the random propylene copolymer has the following properties:

[0163] i) a melt flow rate (MFR2) of 2.0 to 20.0 g / 10 min measured at 230°C and 2.16 kg according to ISO 1133;

[0164] ii) Melting temperature (T) measured by differential scanning calorimetry (DSC) m ) is 120 to 150° C.;

[0165] iii) By quantitative 13 The total comonomer content determined by C-NMR spectroscopy is 1.0 to 10.0 mol%, wherein the comonomer is selected from ethylene and C4 to C8 α-olefins and combinations thereof;

[0166] iv) By quantitative 13 The content of 2,1-regio defects determined by C-NMR spectroscopy analysis ranged from 0.05 to 1.4 mol %;

[0167] The recycled polypropylene film has a gel index of 16.0 to 50.0 measured on a 70 μm film sample, wherein the recycled polypropylene film is obtained by mechanically recycling the single-layer polypropylene film.

[0168] The use of a recycled polypropylene composition in a film (preferably in a cast film), wherein the recycled polypropylene composition has the following properties:

[0169] i) a melt flow rate (MFR2) of 2.0 to 20.0 g / 10 min measured at 230°C and 2.16 kg according to ISO 1133;

[0170] ii) Melting temperature (T) measured by differential scanning calorimetry (DSC) m ) is 120 to 150° C.;

[0171] iii) By quantitative 13The total comonomer content determined by C-NMR spectroscopy is 1.0 to 10.0 mol%, wherein the comonomer is selected from ethylene and C4 to C8 α-olefins and combinations thereof; and

[0172] iv) By quantitative 13 The content of 2,1-regio defects determined by C-NMR spectral analysis was 0.05 to 1.4 mol%.

[0173] All preferred embodiments and alternatives of the monolayer polypropylene film, random propylene copolymer (R-PP), recycled polypropylene composition, recycled polypropylene film and process of the present invention described above apply mutatis mutandis to the application of the present invention.

[0174] The invention will now be described with reference to the following non-limiting examples.

[0175] Example

[0176] A. Measurement Method

[0177] Unless otherwise defined, the following definitions of terms and determination methods apply to the above general description of the invention, including the claims, as well as to the following examples.

[0178] Melting temperature T m , melting enthalpy H m and crystallization temperature T c

[0179] Parameters 5 to 7 mg samples were measured using a TA Instrument Q2000 Differential Scanning Calorimetry (DSC). DSC was run according to ISO 11357 / Part 3 / Method C2 in a heating / cooling / heating cycle with a scan rate of 10°C / min over a temperature range of -30 to +225°C. The crystallization temperature (Tc) was determined from the cooling step and the melting temperature (T m ) and melting enthalpy (H m ) is determined from the second heating step. The melting temperature and crystallization temperature are taken as the peak values ​​of the endotherm and the exotherm.

[0180] Quantification of microstructure by NMR spectroscopy

[0181] Quantitative nuclear magnetic resonance (NMR) spectroscopy is used to quantify the isotacticity and regioregularity of propylene polymers.

[0182] A Bruker Advance III 400 NMR spectrometer was used to 1 H and 13 C were operated at 400.15 and 100.62 MHz, respectively, and quantitative data were recorded in solution. 13 C{ 1H} NMR spectra. All spectra were obtained using 13 The C-optimized 10 mm extension temperature probe was recorded at 125 °C and nitrogen was used for all pneumatics.

[0183] For propylene homopolymers, about 200 mg of material was dissolved in 1,2-tetrachloroethane-d2 (TCE-d2). To ensure a homogeneous solution, the NMR tube was further heated in a rotary oven for at least 1 hour after initial sample preparation in a heating block. The tube was inserted into the magnet and rotated at 10 Hz. This setting was chosen primarily for the high resolution required for quantification of stereoregularity distribution (Busico, V., Cipullo, R., Prog. Polym. Sci. 26 (2001) 443; Busico, V.; Cipullo, R., Monaco, G., Vacatello, M., Segre, AL, Macromolecules 30 (1997) 6251). Standard single pulse excitation was used, using NOE and a two-stage WALTZ16 decoupling scheme (Zhou, Z., Kuemmerle, R., Qiu, X., Redwine, D., Cong, R., Taha, A., Baugh, D. Winniford, B., J. Mag. Reson. 187 (2007) 225; Busico, V., Carbonniere, P., Cipullo, R., Pellecchia, R., Severn, J., Talarico, G., Macromol. Rapid Commun. 2007, 28, 11289). A total of 8192 (8k) transients were collected for each spectrum.

[0184] A proprietary computer program was used to quantify 13 C{ 1 H} NMR spectra are processed, integrated, and relevant quantitative properties are determined from the integration.

[0185] For propylene homopolymers, all chemical shifts are internally referenced to the methyl isotactic pentad (mmmm) at 21.85 ppm.

[0186] Characteristic signals corresponding to regional defects (Resconi, L., Cavallo, L., Fait, A., Piemontesi, F., Chem. Rev. 2000, 100, 1253; Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157; Cheng, HN, Macromolecules 17 (1984), 1950) or comonomers were observed.

[0187] The stereoregularity distribution is quantified by integrating the methyl region between 23.6-19.7 ppm, correcting for any sites not associated with the stereosequence of interest (Busico, V., Cipullo, R., Prog. Polym. Sci. 26 (2001) 443; Busico, V., Cipullo, R., Monaco, G., Vacatello, M., Segre, AL, Macromolecules 30 (1997) 6251).

[0188] Specifically, the effects of regio defects and comonomers on the quantification of the stereoregularity distribution are corrected by subtracting representative regio defect and comonomer integrals from the specific integrated region of the stereosequence.

[0189] Isotacticity is determined at the pentad level and is reported as the percentage of isotactic pentad (mmmm) sequences over all pentad sequences:

[0190] [mmmm]% = 100*(mmmm / sum of all quintuples)

[0191] The presence of the 2,1 erythro regio defect is indicated by the presence of two methyl sites at 17.7 and 17.2 ppm and confirmed by other characteristic sites. No characteristic signals corresponding to other types of regio defects were observed (Resconi, L., Cavallo, L., Fait, A., Piemontesi, F., Chem. Rev. 2000, 100, 1253).

[0192] The amount of 2,1 erythro regiodefects was quantified using the average integral of two characteristic methyl sites at 17.7 and 17.2 ppm:

[0193] P 21e =(I e6 +I e8 ) / 2

[0194] The amount of 1,2-primarily inserted propene was quantified based on the methyl region, with corrections made for sites not relevant to the primary insertion included in this region and for primary insertion sites excluded from this region:

[0195] P 12 =I CH3 +P 12e

[0196] The total amount of propene is quantified as the sum of the primary inserted propene and all other regio defects present:

[0197] P 总 =P 12+P 21e

[0198] The mole percentage of 2,1 erythro regio defects relative to all propylene was quantified:

[0199] [21e]mol%=100*(P 21e / P 总 )

[0200] Comonomer content

[0201] Quantification of microstructure by NMR spectroscopy

[0202] For ethylene-propylene copolymers

[0203] Quantitative nuclear magnetic resonance (NMR) spectroscopy was also used to quantify the comonomer content and comonomer sequence distribution of the polymers. 1 H and 13 C were operated at 400.15 and 100.62 MHz, respectively, and quantitative data were recorded in solution. 13 C{ 1 H} NMR spectra. All spectra were obtained using 13C optimized 10mm extension temperature probe was recorded at 125℃, and nitrogen was used for all pneumatic devices. About 200mg of material was dissolved in 3ml of 1,2-tetrachloroethane-d2 (TCE-d2) together with chromium (III) acetylacetonate (Cr(acac)3) to obtain a 65mM relaxation agent solution in solvent (Singh, G., Kothari, A., Gupta, V., Polymer Testing 28 5 (2009), 475). To ensure the homogeneity of the solution, the NMR tube was further heated in a rotary oven for at least 1 hour after initial sample preparation in a heating block. After the tube was inserted into the magnet, it was rotated at 10Hz. This setting was chosen mainly for the high resolution required for accurate quantification of ethylene content. Standard single pulse excitation was used, without NOE, using an optimized tip angle, 1 second recycle delay, and a two-stage WALTZ16 decoupling scheme (Zhou, Z., Kuemmerle, R., Qiu, X., Redwine, D., Cong, R., Taha, A., Baugh, D. Winniford, B., J. Mag. Reson. 187 (2007) 225; Busico, V., Carbonniere, P., Cipullo, R., Pellecchia, R., Severn, J., Talarico, G., Macromol. Rapid Commun. 2007, 28, 1128). A total of 6144 (6k) transients were collected for each spectrum.

[0204] A proprietary computer program was used to quantify 13 C{ 1 H} NMR spectra are processed and integrated, and the relevant quantitative properties are determined based on the integration. All chemical shifts are indirectly referenced to the central methylene of the ethylene block (EEE) at 30.00 ppm using the chemical shift of the solvent. This method allows for comparative reference even if this structural unit is not present. Characteristic signals corresponding to ethylene incorporation are observed (Cheng, HN, Macromolecules 17 (1984), 1950).

[0205] When characteristic signals corresponding to 2,1 erythro-type regional defects are observed (as described in "L. Resconi, L. Cavallo, A. Fait, F. Piemontesi, Chem. Rev. 2000, 100 (4), 1253", "Cheng, HN, Macromolecules 1984, 17, 1950" and "WJ. Wang and S. Zhu, Macromolecules 2000, 33 1157"), it is necessary to correct for the influence of regional defects on the determined properties. Characteristic signals corresponding to other types of regional defects are not observed.

[0206] The method of Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157) was used to 13 C{ 1 The comonomer fraction is quantified by integrating multiple signals across the spectral region of the H} spectrum. This method was chosen for its robustness and ability to account for the presence of regio defects when required. Slight adjustments to the integration region were made to improve applicability across the range of comonomer content encountered.

[0207] For systems where only isolated ethylene is observed in the PPEPP sequence, the method of Wang et al. was modified to reduce the effect of non-zero integrals at sites known to be absent. This method reduces the overestimation of ethylene content in such systems and does so by reducing the number of sites used to determine the absolute ethylene content:

[0208] E=0.5(Sββ+Sβγ+Sβδ+0.5(Sαβ+Sαγ))

[0209] By using this set of sites, the corresponding integration formula becomes:

[0210] E=0.5(I H +I G +0.5(I C +I D ))

[0211] The same symbols are used as in the article by Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157). The formula for absolute propylene content is not modified.

[0212] Calculate the mole percentage of comonomer incorporation based on the mole fraction:

[0213] E[mol%]=100*fE

[0214] Calculate the weight percent of comonomer incorporation based on the mole fraction:

[0215] E[weight%]=100*(fE*28.06) / ((fE*28.06)+((1-fE)*42.08))

[0216] The triad-level comonomer sequence distribution was determined using the analytical method of Kakugo et al. (Kakugo, M., Naito, Y., Mizunuma, K., Miyatake, T. Macromolecules 15 (1982) 1150). This method was chosen for its robustness and for its applicability to a wider range of comonomer contents with slight adjustments to the integration region.

[0217] For propylene-ethylene-butene terpolymer

[0218] Quantitative nuclear magnetic resonance (NMR) spectroscopy was used to quantify the comonomer content of the polymers.

[0219] A Bruker Avance III 500 NMR spectrometer was used to 1 H and 13 C were operated at 500.13 and 125.76 MHz, respectively, and quantitative data were recorded in the molten state. 13 C{ 1 H} NMR spectra. All spectra were obtained using 13 A C-optimized 7 mm magic angle spinning (MAS) probe was recorded at 180 °C, with nitrogen used for all pneumatics. Approximately 200 mg of material was loaded into a 7 mm outer diameter zirconium oxide MAS rotor and spun at 4 kHz. This setup was chosen primarily for the high sensitivity required for rapid identification and accurate quantification {klimke06,parkinson07,castignolles09}. Standard single pulse excitation was used, utilizing NOE with a short recycle delay of 3 s {pollard04,klimke06} and an RS-HEPT decoupling scheme {fillip05,griffin07}. A total of 1024 (1k) transients were collected for each spectrum.

[0220] Quantitative 13 C{ 1 H} NMR spectra were processed, integrated, and the relevant quantitative properties were determined from the integration. All chemical shifts were internally referenced to the methyl isotactic pentad (mmmm) at 21.85 ppm.

[0221] A characteristic signal corresponding to 1-butene incorporation {brandolini01} was observed and the comonomer content was quantified.

[0222] The amount of isolated incorporated 1-butene in the PBP sequence was quantified using the integration of the αB2 site at 43.6 ppm indicating the number of reported sites per comonomer:

[0223] B=I αB2 / 2

[0224] The amount of sequentially incorporated 1-butene in the PBBP sequence was quantified using the integration of the ααB2B2 sites at 40.5 ppm, which indicates the number of reporting sites per comonomer:

[0225] BB=2*I ααB2B2

[0226] When BB is present, the value of B must be corrected for the effect of BB on the αB2 site:

[0227] B=(I ααB2 / 2)–BB / 2

[0228] The total 1-butene content was calculated based on the sum of isolated and continuously incorporated 1-butene:

[0229] B 总 =B+BB

[0230] A characteristic signal {brandolini01} corresponding to ethylene incorporation was observed, and the comonomer content was quantified.

[0231] The amount of isolated incorporated ethylene in the PEP sequence was quantified using the integration of the Sββ sites at 24.3 ppm indicating the number of reporting sites per comonomer:

[0232] E=I Sββ

[0233] If a characteristic signal corresponding to continuous incorporation of ethylene in the PEE sequence is observed, the Sβδ site at 27.0 ppm is used for quantification:

[0234] EE=I Sβδ

[0235] Characteristic signals {resconi00} corresponding to regio defects were observed. The presence of isolated 2,1-erythro regio defects was indicated by the presence of two methyl sites at 17.7 and 17.2 ppm, the presence of a methylene site at 42.4 ppm, and confirmed by other characteristic sites. The presence of 2,1-erythro regio defects adjacent to ethylene units was indicated by two inequivalent Sαβ signals at 34.8 ppm and 34.4 ppm, respectively, and Tγγ at 33.7 ppm.

[0236] The integration of the methylene sites at 42.4 ppm was used (I e9 ) for isolated 2,1-erythro regiodefects (P 21e孤立 ) is quantified:

[0237] P 21e孤立 =I e9

[0238] If present, the methine site (I) at 33.7 ppm was used. Tγγ ) to the amount of 2,1 regional defects adjacent to ethylene (P E21 ) for quantification:

[0239] P E21 =I Tγγ

[0240] The total ethylene content was then calculated based on the sum of ethylene from isolated, continuously incorporated, and adjacent 2,1 regio defects:

[0241] E 总 =E+EE+P E21

[0242] Based on S at 46.7 ppm αα The amount of propylene is quantified by the methylene sites (including all αα Additional propylene units covered, for example, factor 3*P 21e孤立 Indicating three missing propylene units from an isolated 2,1-erythro regio defect):

[0243] P 总 =I Sαα +3*P 21e孤立 +B+0.5*BB+E+0.5*EE+2*P E21

[0244] The total mole fraction of 1-butene and ethylene in the polymer is then calculated:

[0245] fB=B 总 / (E 总 +P 总 +B 总 )

[0246] fE=E 总 / (E 总 +P 总 +B 总 )

[0247] Calculate the mole percentage of comonomer incorporation based on the mole fraction:

[0248] B[mol%]=100*fB

[0249] E[mol%]=100*fE

[0250] Calculate the weight percent of comonomer incorporation based on the mole fraction:

[0251] B [weight %] = 100 * (fB * 56.11) / ((fE * 28.05) + (fB * 56.11) + ((1 - (fE + fB)) * 42.08))

[0252] E [weight %] = 100 * (fE * 28.05) / ((fE * 28.05) + (fB * 56.11) + ((1 - (fE + fB)) * 42.08))

[0253] The mole percentage of isolated 2,1-erythro regio defects relative to all propylene is quantified:

[0254] [21e]mol%=100*P 21e孤立 / P 总

[0255] The mole percentage of 2,1 regio defects adjacent to ethylene is quantified relative to all propylene:

[0256] [E21]mol%=100*P E21 / P 总

[0257] The total amount of 2,1 defects is quantified as follows:

[0258]

[21] mol%=[21e]+[E21]

[0259] No characteristic signals {resconi00} corresponding to other types of regional defects (2,1-threo, 3,1 insertion) were observed.

[0260] klimke06: Klimke, K., Parkinson, M., Piel, C., Kaminsky, W., Spiess, HW, Wilhelm, M., Macromol. Chem. Phys. 2006; 207:382.

[0261] parkinson07: Parkinson, M., Klimke, K., Spiess, HW, Wilhelm, M., Macromol. Chem. Phys. 2007; 208:2128.

[0262] pollard04: Pollard, M., Klimke, K., Graf, R., Spiess, HW, Wilhelm, M., Sperber, O., Piel, C., Kaminsky, W., Macromolecules 2004;37:813.

[0263] filip05:Filip,X.,Tripon,C.,Filip,C.,J.Mag.Resn.2005,176,239.

[0264] griffin07: Griffin, JM, Tripon, C., Samoson, A., Filip, C., and Brown, SP, Mag. Res. in Chem. 2007 45, S1, S198.

[0265] castignolles09:Castignolles,P.,Graf,R.,Parkinson,M.,Wilhelm,M.,Gaborieau,M.,Polymer 50(2009)2373.

[0266] resconi00: Resconi, L., Cavallo, L., Fait, A., Piemontesi, F., Chem. Rev. 2000, 100, 1253.

[0267] brandolini01: AJ Brandolini, DDHills, "NMR spectra of polymers and polymer additives", Marcel Deker Inc., 2000.

[0268] Melt flow rate

[0269] The melt flow rate (MFR) is determined according to ISO 1133 - Determination of melt mass-flow rate (MFR) and melt volume-flow rate (MVR) of thermoplastics - Part 1: Standard method and is expressed in g / 10 min. The MFR is an indicator of the fluidity and therefore the processability of the polymer. The higher the melt flow rate, the lower the viscosity of the polymer. The MFR2 of polypropylene is determined at a temperature of 230°C and a load of 2.16 kg.

[0270] Number average molecular weight (M n ), weight average molecular weight (M w ), size average molecular weight and molecular weight distribution (MWD)

[0271] Molecular weight averages (Mz, Mw, Mn) and molecular weight distribution (MWD) (ie, Mz / Mw, where Mz is the size average molecular weight and Mw is the weight average molecular weight) were determined by gel permeation chromatography (GPC) according to ISO 16014-4:2003 and ASTM D 6474-99.

[0272] A PolymerChar GPC instrument equipped with an infrared (IR) detector was used with 3xOlexis and lx Olexis guard columns from Polymer Laboratories, with 1,2,4-trichlorobenzene (TCB, stabilized with 250 mg / L 2,6-di-tert-butyl-4-methyl-phenol) as solvent, at 160°C and a constant flow rate of 1 mL / min. 200 μL of sample solution was injected for each analysis. The column set was calibrated using a universal calibration (according to ISO 16014-2:2003) using at least 15 narrow MWD polystyrene (PS) standards ranging from 0.5 kg / mol to 11 500 kg / mol. The MarkHouwink constants for PS, PE and PP are as described in ASTM D 6474-99. All samples were prepared by dissolving 5.0-9.0 mg of polymer in 8 mL (at 160 °C) stabilized TCB (same as mobile phase) at up to 160 °C with constant gentle shaking in the autosampler of the GPC instrument for 2.5 hours (for PP) and 3 hours (for PE).

[0273] Xylene soluble fraction at room temperature (XS, wt. %): The amount of polymer soluble in xylene is determined at 25°C according to ISO 16152 (fifth edition; 2005-07-01).

[0274] Gel Index

[0275] The optical gel index was measured with an OCS gel counter device consisting of a measuring extruder, connected to which is a cooling roll unit, a heating and cooling unit (Haake C40P, temperature 15-90°C), a line camera (FS-5 / 4096 pixels, for dynamic digital processing of grayscale images) and a take-up unit (automatic stretch control up to 10 N). Details of the film manufacturing are listed below.

[0276] For each material, a line camera is used to detect 5m 2 The average number of gel spots on the membrane surface. The line camera is set to differentiate the gel spot sizes according to the following table:

[0277]

[0278] The number of detected gel spots for each size is multiplied by its respective calculation factor. The sum of all these values ​​gives a final value which is called the Optical Gel Index.

[0279] B. Examples

[0280] The catalyst used in the polymerization process of the random propylene copolymer (R-PP) of the present invention is trans-dimethylsilanediyl [2-methyl-4,8-di(3,5-dimethylphenyl)-1,5,6,7-tetrahydro-s-inden-1-yl] [2-methyl-4-(3,5-dimethylphenyl)-5-methoxy-6-tert-butylinden-1-yl] zirconium dichloride as disclosed as MC-2 in WO 2019 / 179959 A1. The preparation of the supported metallocene catalyst is similar to IE2 in WO 2019 / 179959 A1.

[0281] The catalyst used in the polymerization process of the comparative random propylene copolymer (R-PP2) was prepared as follows:

[0282] Chemicals used:

[0283] 20% butylethylmagnesium (Mg(Bu)(Et), BEM) toluene solution, provided by Chemtura;

[0284] 2-Ethylhexanol, provided by Amphochem;

[0285] 3-Butoxy-2-propanol-(DOWANOL TM PnB), provided by Dow;

[0286] Bis(2-ethylhexyl)citraconate, provided by SynphaBase;

[0287] TiCl4, supplied by Millenium Chemicals;

[0288] Toluene, provided by Aspokem;

[0289] 1-254, provided by Evonik;

[0290] Heptane, supplied by Chevron.

[0291] Preparation of magnesium alkoxides

[0292] The Mg alkoxyl solution was prepared by adding a mixture of 4.7 kg of 2-ethylhexanol and 1.2 kg of butoxypropanol to 11 kg of a 20 wt % butylethylmagnesium (Mg(Bu)(Et)) toluene solution in a 20 L stainless steel reactor under stirring (70 rpm). During the addition, the reactor contents were maintained below 45°C. After the addition was complete, mixing of the reaction mixture was continued at 60°C (70 rpm) for 30 minutes. After cooling to room temperature, 2.3 kg of the donor bis(2-ethylhexyl) citraconate was added to the Mg alkoxyl solution while maintaining the temperature below 25°C. Mixing was continued for 15 minutes under stirring (70 rpm).

[0293] Preparation of solid catalyst components

[0294] 20.3 kg TiCl4 and 1.1 kg toluene were added to a 20 L stainless steel reactor. Under stirring at 350 rpm, the temperature was maintained at 0°C, and 14.5 kg of the Mg alkoxide prepared in Example 1 was added over 1.5 hours. 1.7 L After 1-254 and 7.5 kg of heptane were mixed at 0°C for 1 hour, the temperature of the formed emulsion was raised to 90°C within 1 hour. After 30 minutes, the mixing was stopped and the catalyst droplets solidified, allowing the formed catalyst particles to settle. After settling (1 hour), the supernatant was siphoned off. The catalyst particles were then washed with 45 kg of toluene at 90°C for 20 minutes and then washed twice with heptane (30 kg, 15 minutes). The temperature was lowered to 50°C during the first heptane wash and to room temperature during the second wash.

[0295] The catalyst thus obtained was used together with triethylaluminium (TEAL) as cocatalyst and dicyclopentyldimethoxysilane (D-donor) as donor.

[0296] The ratio of aluminum to donor, the ratio of aluminum to titanium and the polymerization conditions are shown in Table 1.

[0297] Table 1: Preparation of random propylene copolymers CE1 and IE1.

[0298]

[0299] n / a: Not applicable (for metallocene catalysts)

[0300] Polymers CE1 and IE1 were mixed with 400 ppm calcium stearate (CAS No.: 1592-23-0) and 1,000 ppm Irganox B225 (BASF AG, Germany).

[0301] In the second step, CE1 was visbroken by using a co-rotating twin screw extruder at 200-230°C and using an appropriate amount of (tert-butylperoxy)-2,5-dimethylhexane (Trigonox 101, distributed by Akzo Nobel, The Netherlands) to reach the target MFR2. The properties of the pelletized visbroken composition CE1 are given in Table 2.

[0302] The final properties of pelletized IE1 (not visbroken) are also summarized in Table 2.

[0303] Granular IE1 and granular visbroken CE1 were used to prepare monolayer films using a cast film line.

[0304] The monolayer film before recycling was produced on a COEX Barmag 60 cast film line with a production rate of 60 kg / h, a melt temperature of 250°C, and a cooling roll temperature of 25°C. The final film thickness was 70 μm, the width was 115 mm, and the gel index was shown in Table 2.

[0305] Table 2: Properties of random propylene copolymer (R-PP) and monolayer polypropylene films.

[0306]

[0307] The monolayer membranes of CE1 and IE1 were subjected to a recycling process in which the membranes were cut into pieces and recovered as granules in a recycling machine.

[0308] Film recovery was carried out on an Erema small-scale production line model I_605K. It includes a pretreatment unit (PCU) and an extruder for melting and pelletizing. The PCU was operated at 108-110°C, the extruder was operated at a screw speed of 220 U / min, a melt temperature of 176°C and a production rate of about 40 kg / h, and the performance is shown in Table 3.

[0309] The film was made from the pellets of CE1 and IE1 obtained during the recycling process. The film was made on an OCS measuring extruder (ME25 / 5800V3) provided by Optical Control Systems GmbH. The melt temperature was 260°C, the cooling roll temperature was 25°C, and the feed speed was 3m / min. The final film thickness was 70, the width was 1m, and the gel index was shown in Table 3.

[0310] Table 3: Properties of recycled polypropylene compositions and recycled polypropylene films.

[0311]

[0312] As can be seen in Table 3, for CE1 and IE1, MFR2 and XCS increased slightly, while Mz, Mw and Mw / Mw decreased slightly. Most importantly, however, the gel index of the Ziegler-Natta catalyzed comparative example increased from 0.3 to 77.0 after recycling, equivalent to an increase of more than 25,000%, compared to only about 5% for the metallocene catalyzed examples of the present invention.

[0313] It can be clearly seen that the membrane of the present invention has advantages in application in terms of mechanical recovery performance, and the regenerated membrane does not show obvious gel defects; while the gel defects of the comparative membrane may seriously limit its application in such methods.

Claims

1. A method for forming a recycled polypropylene film, the method comprising the following steps: (a) providing a single-layer polypropylene film, wherein the single-layer polypropylene film comprises at least 90 wt% of a random propylene copolymer (R-PP), based on the total weight of the single-layer polypropylene film, wherein the random propylene copolymer has the following properties: i) a melt flow rate (MFR2) of 2.0 to 20.0 g / 10 min measured at 230°C and 2.16 kg according to ISO 1133; ii) Melting temperature (T) measured by differential scanning calorimetry (DSC) m ) is 120 to 150° C.; iii) By quantitative 13 The total comonomer content determined by C-NMR spectroscopy is 1.0 to 10.0 mol%, wherein the comonomer is selected from ethylene and C4 to C8 α-olefins and combinations thereof; iv) By quantitative 13 The content of 2,1-regio defects determined by C-NMR spectroscopy analysis ranged from 0.05 to 1.4 mol %; (b) mechanically recovering the film of step (a) to obtain a recycled polypropylene composition; and (c) extruding the recycled polypropylene composition of step (b) to form a recycled polypropylene film, preferably a recycled polypropylene cast film.

2. The method according to claim 1, wherein: The mechanical recovery of step (b) is carried out in a continuous melt mixing device, preferably at a temperature of 170 to 270°C.

3. The method according to claim 1 or 2, wherein: The random propylene copolymer (R-PP) has a molecular weight distribution (Mz / Mw) determined by gel permeation chromatography (GPC) of 1.10 to 2.10, more preferably of 1.30 to 2.00, most preferably of 1.50 to 1.

90.

4. The method according to any one of claims 1 to 3, wherein: The random propylene copolymer (R-PP) has a xylene cold soluble content (XCS), determined according to ISO 16152, of 5 to 25 wt-%, more preferably of 10 to 20 wt-%, most preferably of 12 to 18 wt-%.

5. The method according to any one of claims 1 to 4, wherein: The random copolymer (R-PP) contains two comonomers, preferably, the first comonomer is ethylene and the second comonomer is selected from C4 to C8 α-olefins; more preferably, the first comonomer is ethylene and the second comonomer is 1-butene.

6. The method according to any one of claims 1 to 5, wherein: The ratio of MFR2 of the recycled polypropylene composition obtained in step (b) to MFR2 of the random propylene copolymer (R-PP) of the single-layer polypropylene film provided in step (a) [MFR2(B) / MFR2(A)] is from 1.00 to 1.30, more preferably from 1.00 to 1.20, most preferably from 1.00 to 1.

15.

7. The method according to any one of claims 1 to 6, wherein: The ratio of the xylene cold soluble content (XCS) of the recycled polypropylene composition obtained in step (b) measured according to ISO 16152 to the xylene cold soluble content (XCS) of the random propylene copolymer (R-PP) of the monolayer polypropylene film provided in step (a) measured according to ISO 16152 [XCS(B) / XCS(A)] is from 1.00 to 1.30, more preferably from 1.00 to 1.20, most preferably from 1.00 to 1.

10.

8. The method according to any one of claims 1 to 7, wherein: The ratio of the weight average molecular weight (Mw) of the recycled polypropylene composition obtained in step (b) measured by gel permeation chromatography (GPC) to the weight average molecular weight (Mw) of the random propylene copolymer (R-PP) of the single-layer polypropylene film provided in step (a) measured by gel permeation chromatography (GPC) [Mw(B) / Mw(A)] is from 0.90 to 1.00, more preferably from 0.95 to 1.00, most preferably from 0.97 to 1.

00.

9. The method according to any one of claims 1 to 8, wherein: The ratio of the gel index of the recycled polypropylene composition obtained in step (b) measured on a 70 μm cast film sample to the gel index of the random propylene copolymer (R-PP) of the single-layer polypropylene film provided in step (a) measured on a 70 μm cast film sample [gel index (B) / gel index (A)] is 1.00 to 1.50, more preferably 1.00 to 1.30, most preferably 1.00 to 1.

10.

10. A recycled polypropylene film, comprising a recycled polypropylene composition having: i) a melt flow rate (MFR2) of 2.0 to 20.0 g / 10 min measured at 230°C and 2.16 kg according to ISO 1333; ii) Melting temperature (T) measured by differential scanning calorimetry (DSC) m ) is 120 to 150° C.; iii) By quantitative 13 The total comonomer content determined by C-NMR spectroscopy is 1.0 to 10.0 mol%, wherein The comonomer is selected from ethylene and C4 to C8 α-olefins and combinations thereof; and iv) By quantitative 13 The content of 2,1-regio defects determined by C-NMR spectroscopy analysis ranged from 0.05 to 1.4 mol %; The gel index of the recycled polypropylene film measured on a 70 μm film sample is 16.0 to 50.

0.

11. The recycled polypropylene film according to claim 10, wherein The recycled polypropylene film can be obtained by the method of claims 1 to 9.

12. Use of a monolayer polypropylene film in obtaining a recycled polypropylene film, the monolayer polypropylene film comprising at least 90 wt.% of a random propylene copolymer (R-PP), the random propylene copolymer having the following properties: i) a melt flow rate (MFR2) of 2.0 to 20.0 g / 10 min measured at 230°C and 2.16 kg according to ISO 1133; ii) Melting temperature (T) measured by differential scanning calorimetry (DSC) m ) is 120 to 150° C.; iii) By quantitative 13 The total comonomer content determined by C-NMR spectroscopy is 1.0 to 10.0 mol%, wherein The comonomer is selected from ethylene and C4 to C8 α-olefins and combinations thereof; iv) By quantitative 13 The content of 2,1-regio defects determined by C-NMR spectroscopy analysis ranged from 0.05 to 1.4 mol %; The regenerated polypropylene film has a gel index of 16.0 to 50.0 measured on a 70 μm film sample; The recycled polypropylene film is obtained by mechanically recycling the single-layer polypropylene film.

13. Use of a recycled polypropylene composition in a film, preferably in a cast film, wherein the recycled polypropylene composition has the following properties: i) a melt flow rate (MFR2) of 2.0 to 20.0 g / 10 min measured at 230°C and 2.16 kg according to ISO 1133; ii) Melting temperature (T) measured by differential scanning calorimetry (DSC) m ) is 120 to 150° C.; iii) By quantitative 13 The total comonomer content determined by C-NMR spectroscopy is 1.0 to 10.0 mol%, wherein The comonomer is selected from ethylene and C4 to C8 α-olefins; as well as iv) By quantitative 13 The content of 2,1-regio defects determined by C-NMR spectral analysis was 0.05 to 1.4 mol%.

Citation Information

Patent Citations

  • Multi-stage process for producing polyethylene

    WO1992012182A1

  • Process for preparing polypropylene

    WO1999024478A1

  • Novel propylene polymers and products thereof

    WO1999024479A1

  • High-stiffness propylene polymers and a process for the preparation thereof

    WO2000068315A1

  • Bridged BIS (indenyl) metallocene compounds

    WO2002002576A1