Semiconductor device and memory device

By forming a longitudinal OS transistor structure on the Si transistor, the difficulties of Si transistors in miniaturization and high integration are solved, and a low-power and high-functional storage device is realized, which improves electrical characteristics and storage performance.

CN119032637APending Publication Date: 2024-11-26SEMICON ENERGY LAB CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034483.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-19
Filing Date
2023-04-07
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing Si transistor memory devices have difficulties in miniaturization and high integration, and are difficult to achieve low power consumption and high functionality.

Method used

Using a longitudinal OS transistor structure, a high-density configuration and a low-power storage device are realized by forming a metal oxide semiconductor layer on the Si transistor, and the characteristics of the oxide semiconductor are used to reduce the off-state current and improve the frequency characteristics.

Benefits of technology

The transistors that are miniaturized and highly integrated are realized, reducing power consumption, improving the uniformity and reliability of electrical characteristics, and enhancing the retention characteristics and read and write speed of the storage device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032637A_ABST
    Figure CN119032637A_ABST
Patent Text Reader

Abstract

Provided is a semiconductor device capable of achieving miniaturization or high integration. The semiconductor device includes: a first conductor; a first oxide and a second oxide electrically connected to the first conductor and having openings; a second conductor electrically connected to the first oxide; a third conductor disposed inside an opening included in the first oxide; a fourth conductor electrically connected to the third conductor; a fifth conductor electrically connected to the second oxide; a sixth conductor disposed inside an opening included in the second oxide; the seventh electric conductor is electrically connected with the sixth electric conductor; and the eighth conductor is electrically connected with the second conductor and the seventh conductor. The fourth conductor is disposed in the same layer as the seventh conductor, and an extension direction of the fourth conductor is the same as an extension direction of the fifth conductor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a semiconductor device, a storage device, and an electronic device. One embodiment of the present invention relates to a method for manufacturing a semiconductor device. One embodiment of the present invention relates to a semiconductor wafer and a module.

[0002] Note that in this specification, etc., semiconductor devices refer to all devices that can work by utilizing semiconductor characteristics. In addition to semiconductor elements such as transistors, semiconductor circuits, computing devices, or storage devices are also a form of semiconductor devices. Display devices (liquid crystal display devices and light-emitting display devices, etc.), projection devices, lighting devices, electro-optical devices, power storage devices, storage devices, semiconductor circuits, camera devices, and electronic devices, etc. sometimes include semiconductor devices.

[0003] Note that one embodiment of the present invention is not limited to the above-mentioned technical field. One embodiment of the invention disclosed in this specification, etc., relates to an object, method, or manufacturing method. In addition, one embodiment of the present invention relates to a process, machine, product, or composition of matter. Background Art

[0004] As memory devices become more highly integrated, the area occupied by the memory needs to be reduced. However, miniaturization of memory devices using Si transistors is becoming increasingly difficult from a technical and cost perspective.

[0005] In recent years, oxide semiconductors have attracted much attention as semiconductor materials that can form transistors in the BEOL (Back end of line) process of forming the wiring of semiconductor devices. The technology of directly forming an OS transistor (a transistor containing a metal oxide in the channel formation region) above an existing Si transistor (a transistor containing silicon in the channel formation region) (also known as BEOL-Tr technology) can form a 3D functional circuit while keeping the design rules unchanged. Therefore, this technology is expected to be a technology that can realize a high-function storage device with low power consumption and low cost.

[0006] Furthermore, if vertical OS transistors can be realized, the design rules can be reduced from 6F to 2 (F is the minimum processing size) minimized to 4F 2 For example, Patent Document 1 discloses a vertical transistor in which the side surfaces of an oxide semiconductor are covered with a word line via a gate insulating layer. [Prior technical literature] [Patent Document]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 2021-108331 Summary of the invention Technical problem to be solved by the invention

[0008] One of the purposes of one embodiment of the present invention is to provide a transistor that can achieve miniaturization or high integration. One of the purposes of one embodiment of the present invention is to provide a transistor with excellent electrical characteristics. One of the purposes of one embodiment of the present invention is to provide a transistor with less uneven electrical characteristics. One of the purposes of one embodiment of the present invention is to provide a transistor with a large on-state current. One of the purposes of one embodiment of the present invention is to provide a transistor with excellent reliability. One of the purposes of one embodiment of the present invention is to provide a novel transistor. One of the purposes of one embodiment of the present invention is to provide a semiconductor device or a storage device including the transistor. One of the purposes of one embodiment of the present invention is to provide a semiconductor device or a storage device with low power consumption. One of the purposes of one embodiment of the present invention is to provide a semiconductor device or a storage device with a high operating speed.

[0009] Note that the recording of these purposes does not prevent the existence of other purposes. Note that one mode of the present invention does not need to achieve all of the above purposes. Purposes other than the above purposes are obvious from the description of the specification, drawings, claims, etc., and can be extracted from the description. Solutions to technical problems

[0010] One embodiment of the present invention is a semiconductor device, comprising: a first conductor; a first oxide and a second oxide electrically connected to the first conductor and having an opening; a second conductor electrically connected to the first oxide; a first insulator arranged inside the opening included in the first oxide; a third conductor on the first insulator; a fourth conductor electrically connected to the third conductor; a fifth conductor electrically connected to the second oxide; a second insulator arranged inside the opening included in the second oxide; a sixth conductor on the second insulator; a seventh conductor electrically connected to the sixth conductor; and an eighth conductor electrically connected to the second conductor and the seventh conductor. The fourth conductor is provided in the same layer as the seventh conductor, and the extension direction of the fourth conductor is the same as the extension direction of the fifth conductor.

[0011] In the above semiconductor device, preferably, an extending direction of the first electrical conductor is orthogonal to an extending direction of the fourth electrical conductor.

[0012] In addition, preferably, the semiconductor device further includes a ninth conductor and a tenth conductor, the ninth conductor is disposed between the first oxide and the second conductor, and the side surface of the ninth conductor is consistent with the side surface of the first oxide, and the tenth conductor is disposed between the second oxide and the fifth conductor, and the side surface of the tenth conductor is consistent with the side surface of the second oxide. In addition, more preferably, the second conductor has a convex shape portion, and the convex shape portion is in contact with the ninth conductor.

[0013] In the above semiconductor device, preferably, a side surface of the first oxide has a tapered shape when viewed in cross section.

[0014] One embodiment of the present invention is a semiconductor device, comprising: a first conductor and a second conductor; a first oxide electrically connected to the first conductor and having an opening; a third conductor electrically connected to the first oxide; a first insulator arranged inside the opening included in the first oxide; a fourth conductor on the first insulator; a fifth conductor electrically connected to the fourth conductor; a second oxide electrically connected to the second conductor and having an opening; a sixth conductor electrically connected to the second oxide; a second insulator arranged inside the opening included in the second oxide; a seventh conductor on the second insulator; an eighth conductor electrically connected to the seventh conductor; and a ninth conductor electrically connected to the third conductor and the eighth conductor. The fifth conductor is provided in the same layer as the eighth conductor, and the extension direction of the fifth conductor is the same as the extension direction of the sixth conductor.

[0015] In the above semiconductor device, preferably, an extending direction of the first conductor is orthogonal to an extending direction of the fifth conductor, and an extending direction of the second conductor is orthogonal to an extending direction of the sixth conductor.

[0016] In addition, preferably, the above-mentioned semiconductor device also includes a tenth conductor and an eleventh conductor, the tenth conductor is arranged between the first oxide and the third conductor, and the side surface of the tenth conductor is consistent with the side surface of the first oxide, and the eleventh conductor is arranged between the second oxide and the sixth conductor, and the side surface of the eleventh conductor is consistent with the side surface of the second oxide.

[0017] In the above semiconductor device, preferably, a side surface of the first oxide has a tapered shape when viewed in cross section.

[0018] One embodiment of the present invention is a storage device including: the above-mentioned semiconductor device; and a layer including a peripheral circuit, the layer being located below the semiconductor device, the peripheral circuit having a function of writing data to the semiconductor device and reading data from the semiconductor device. Effects of the Invention

[0019] According to one embodiment of the present invention, a transistor capable of miniaturization or high integration can be provided. According to one embodiment of the present invention, a transistor having excellent electrical characteristics can be provided. According to one embodiment of the present invention, a transistor having less uneven electrical characteristics can be provided. According to one embodiment of the present invention, a transistor having a large on-state current can be provided. According to one embodiment of the present invention, a transistor having excellent reliability can be provided. According to one embodiment of the present invention, a novel transistor can be provided. According to one embodiment of the present invention, a semiconductor device or a storage device including the transistor can be provided. According to one embodiment of the present invention, a semiconductor device or a storage device having low power consumption can be provided. A semiconductor device or a storage device having a high operating speed can be provided.

[0020] Note that the description of these effects does not prevent the existence of other effects. In addition, one mode of the present invention does not need to have all of the above effects. In addition, the description of the specification, drawings, and claims, etc. clearly has effects other than the above effects, and effects other than the above effects can be obtained from the description of the specification, drawings, and claims, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1A It is a perspective view showing a structural example of a semiconductor device. Figure 1B is a plan view showing a structural example of a semiconductor device. Figure 2A is a plan view showing a structural example of a semiconductor device. Figure 2B and Figure 2C is a cross-sectional view showing a structural example of a semiconductor device. Figure 2D It is a perspective view showing a structural example of a semiconductor device. Figure 2E is a cross-sectional view showing a structural example of a semiconductor device. FIG. 3A to FIG. 3F is a plan view showing a structural example of a semiconductor device. FIG. 4A to FIG. 4E is a plan view showing a structural example of a semiconductor device. Figure 5A and Figure 5B is a cross-sectional view showing a structural example of a semiconductor device. Figure 5C It is a perspective view showing a structural example of a semiconductor device. Fig. 6A is a plan view showing a structural example of a semiconductor device. Figure 6B is a cross-sectional view showing a structural example of a semiconductor device. Figure 6C It is a perspective view showing a structural example of a semiconductor device. Fig. 7A and Figure 7B is a plan view showing a structural example of a semiconductor device. Fig. 8A is a plan view showing a structural example of a semiconductor device. Figure 8B is a cross-sectional view showing a structural example of a semiconductor device. Figure 8C It is a perspective view showing a structural example of a semiconductor device. Fig. 9A and Fig. 9B is a plan view showing a structural example of a semiconductor device. Fig. 10A and Fig. 10B is a cross-sectional view showing a structural example of a semiconductor device. Fig. 10C It is a perspective view showing a structural example of a semiconductor device. Fig.11A and Fig. 11B is a cross-sectional view showing a structural example of a semiconductor device. FIG. 12A to FIG. 12C is a cross-sectional view showing a structural example of a semiconductor device. Fig.13A and Fig.13D is a plan view showing a structural example of a semiconductor device. Fig. 13B and Fig. 13C is a cross-sectional view showing a structural example of a semiconductor device. Fig.14A and Fig. 14B is a cross-sectional view showing a structural example of a semiconductor device. Fig.15A1 and Fig.15B1 It is a top view showing an example of a method for manufacturing a semiconductor device. Fig.15A2 and Fig.15B2 is a cross-sectional view showing an example of a method for manufacturing a semiconductor device. Fig.16A1 and Fig.16B1 It is a top view showing an example of a method for manufacturing a semiconductor device. Fig.16A2 and Figure 16B2 is a cross-sectional view showing an example of a method for manufacturing a semiconductor device. Fig.17A1 and Fig.17B1 It is a top view showing an example of a method for manufacturing a semiconductor device. Fig.17A2 and Figure 17B2 is a cross-sectional view showing an example of a method for manufacturing a semiconductor device. Fig.18A1 and Figure 18B1 It is a top view showing an example of a method for manufacturing a semiconductor device. Fig.18A2 and Figure 18B2 is a cross-sectional view showing an example of a method for manufacturing a semiconductor device. Fig.19A1 and Figure 19B1It is a top view showing an example of a method for manufacturing a semiconductor device. Fig.19A2 and Figure 19B2 is a cross-sectional view showing an example of a method for manufacturing a semiconductor device. Fig.20A1 and Fig.20B1 It is a top view showing an example of a method for manufacturing a semiconductor device. Fig.20A2 and Figure 20B2 is a cross-sectional view showing an example of a method for manufacturing a semiconductor device. Fig.21A1 and Fig.21B1 It is a top view showing an example of a method for manufacturing a semiconductor device. Fig.21A2 and Fig.21B2 is a cross-sectional view showing an example of a method for manufacturing a semiconductor device. Fig.22A1 and Fig.22B1 It is a top view showing an example of a method for manufacturing a semiconductor device. Fig.22A2 and Fig.22B2 is a cross-sectional view showing an example of a method for manufacturing a semiconductor device. Fig.23A is a block diagram showing a structural example of a storage device. Fig. 23B It is a perspective view showing a structural example of a storage device. Fig.24A and Fig. 24B is a circuit diagram showing a structural example of a memory cell. Fig.24C and Fig.24D It is a perspective view showing a structural example of a storage device. Fig.25 is a cross-sectional view showing a structural example of a storage device. Fig.26 is a cross-sectional view showing a structural example of a storage device. FIG. 27A to FIG. 27E This is a diagram for explaining an example of a storage device. FIG. 28A to FIG. 28G It is a diagram for explaining an example of an electronic device. Modes for Carrying Out the Invention

[0022] The following describes the embodiments with reference to the accompanying drawings. It should be noted that a person skilled in the art can easily understand that the embodiments can be implemented in a variety of different forms, and the methods and details can be transformed into various forms without departing from the purpose and scope of the present invention. Therefore, the present invention should not be interpreted as being limited to the contents described in the embodiments shown below.

[0023] In the drawings, the size, thickness of the layer or the area are sometimes exaggerated for obvious reasons. Therefore, the present invention is not limited to the dimensions in the drawings. In addition, in the drawings, ideal examples are schematically shown, so the present invention is not limited to the shapes or numerical values ​​shown in the drawings. For example, in the actual manufacturing process, layers or resist masks are sometimes unintentionally thinned due to etching and other processes, but this is sometimes not reflected in the drawings for ease of understanding. In addition, in the drawings, the same reference numerals are sometimes used in common between different drawings to represent the same parts or parts with the same function, and their repeated descriptions are omitted. In addition, when representing parts with the same function, the same hatching is sometimes used without adding a special reference numeral.

[0024] In addition, for example, in a stereogram or a top view (also referred to as a "plan view"), in order to facilitate understanding of the invention, the description of some constituent elements is sometimes omitted. In addition, the description of some hidden lines is sometimes omitted. In addition, for example, hatching is sometimes omitted in the drawings. In addition, the hatching in the top view of the same constituent element is sometimes different from the hatching in the cross-sectional view.

[0025] In addition, in this specification, for the sake of convenience, ordinal numbers such as first and second are added, but they do not indicate the order of processes or the order of stacking. Therefore, for example, "first" can be appropriately replaced with "second" or "third" for description. In addition, the ordinal numbers recorded in this specification and the like are sometimes inconsistent with the ordinal numbers used to specify one embodiment of the present invention.

[0026] In this specification, for convenience, words and phrases such as "upper" and "lower" are used to indicate the positional relationship of the components with reference to the drawings. In addition, the positional relationship of the components is appropriately changed according to the direction in which each component is described. Therefore, the words and phrases described in the specification are not limited, and the words and phrases can be appropriately changed according to the situation.

[0027] For example, in this specification, when it is clearly stated that "X is connected to Y", it means the following: X is electrically connected to Y; X is functionally connected to Y; X is directly connected to Y. Therefore, the connection relationship is not limited to the connection relationship shown in the drawings or the text, and the connection relationship other than the connection relationship shown in the drawings or the text is also disclosed in the drawings or the text. Here, X and Y are objects (for example, devices, elements, circuits, wiring, electrodes, terminals, conductive films, layers, etc.).

[0028] In this specification, etc., a transistor refers to an element including at least three terminals: a gate, a drain, and a source. The transistor has a region (hereinafter also referred to as a channel formation region) where a channel is formed between the drain (drain terminal, drain region, or drain electrode) and the source (source terminal, source region, or source electrode), and current can flow between the source and the drain through the channel formation region. Note that in this specification, etc., the channel formation region refers to a region where current mainly flows.

[0029] In addition, when transistors with different polarities are used or when the direction of current changes during circuit operation, the functions of the source and drain may be interchanged. Therefore, in this specification, the source and drain may be interchanged.

[0030] Impurities of a semiconductor refer to, for example, elements other than the main components that constitute the semiconductor. For example, an element with a concentration lower than 0.1 atomic % can be said to be an impurity. When impurities are contained, for example, the defect state density of the semiconductor increases, the crystallinity decreases, etc. sometimes occur. When the semiconductor is an oxide semiconductor, the impurities that change the properties of the semiconductor include, for example, Group 1 elements, Group 2 elements, Group 13 elements, Group 14 elements, Group 15 elements, and transition metals other than the main components of the oxide semiconductor. For example, there are hydrogen, lithium, sodium, silicon, boron, phosphorus, carbon, nitrogen, etc. In addition, sometimes water also acts as an impurity. In addition, for example, sometimes the mixing of impurities leads to oxygen vacancies (also called V O :The formation of oxygen vacancy).

[0031] In this specification, etc., "oxynitride" refers to a material whose oxygen content is higher than the nitrogen content in its composition, and "nitride oxide" refers to a material whose nitrogen content is higher than the oxygen content in its composition. For example, when "silicon oxynitride" is described, it refers to a material whose oxygen content is higher than the nitrogen content in its composition, and when "silicon nitride oxide" is described, it refers to a material whose nitrogen content is higher than the oxygen content in its composition.

[0032] Note that in this specification, etc., “insulator” may be referred to as “insulating film” or “insulating layer”. Also, “conductor” may be referred to as “conductive film” or “conductive layer”. Also, “semiconductor” may be referred to as “semiconductor film” or “semiconductor layer”.

[0033] In this specification, etc., "parallel" refers to a state where the angle formed by two straight lines is greater than -10° and less than 10°. Therefore, a state where the angle is greater than -5° and less than 5° is also included. "Approximately parallel" refers to a state where the angle formed by two straight lines is greater than -30° and less than 30°. In addition, "perpendicular" refers to a state where the angle formed by two straight lines is greater than 80° and less than 100°. Therefore, a state where the angle is greater than 85° and less than 95° is also included. "Approximately perpendicular" refers to a state where the angle formed by two straight lines is greater than 60° and less than 120°.

[0034] In this specification, metal oxide refers to an oxide of a metal in a broad sense. Metal oxides are classified into oxide insulators, oxide conductors (including transparent oxide conductors), and oxide semiconductors (Oxide Semiconductor, also referred to as OS). For example, when a metal oxide is used in a semiconductor layer of a transistor, the metal oxide is sometimes referred to as an oxide semiconductor. In other words, an OS transistor can be referred to as a transistor containing a metal oxide or an oxide semiconductor.

[0035] Note that in this specification and the like, normally off means that when no potential is applied to the gate or a ground potential is applied to the gate, the drain current flowing through the transistor per channel width of 1 μm is 1×10 -20 Below A, 1×10 -18 A or less, or 1×10 -16 A or below.

[0036] In this specification and the like, when the same reference numeral is used for a plurality of elements and it is necessary to distinguish between them, a reference numeral such as “[n]” or “[m, n]” may be added to the reference numeral for identification.

[0037] In this specification, etc., "height consistency" refers to a structure in which the heights from a reference surface (for example, a flat surface such as a substrate surface) are equal when viewed from a cross section. For example, in the manufacturing process of a semiconductor device, a flattening process (typically a CMP (Chemical Mechanical Polishing) process) is sometimes performed to expose the surface of a single layer or multiple layers. At this time, the surface to be processed by the CMP process has a structure in which the heights from the reference surface are equal. However, depending on the processing device, processing method or material of the surface to be processed used in the CMP process, the heights of multiple layers may sometimes be different. In this specification, etc., this situation is also regarded as "height consistency". For example, in the case where there are two layers with heights relative to the reference surface (referred to as the first layer and the second layer here), when the difference between the height of the top surface of the first layer and the height of the top surface of the second layer is less than 20nm, it is also referred to as "height consistency".

[0038] In this specification, etc., "ends coincide" means that at least a portion of the outlines of each layer in the stack overlap when viewed from above. For example, it refers to a case where the upper layer and the lower layer are processed using the same mask pattern or a portion of the same mask pattern. However, strictly speaking, sometimes the outlines do not overlap and the outline of the upper layer is located inside the outline of the lower layer or the outline of the upper layer is located outside the outline of the lower layer, and these cases are also included in the case of "ends coincide".

[0039] Note that, in general, it is difficult to clearly distinguish between “completely consistent” and “substantially consistent.” Therefore, in this specification, “consistent” includes both completely consistent and substantially consistent.

[0040] (Implementation Method 1) In this embodiment, a semiconductor device and a method for manufacturing the semiconductor device which are one embodiment of the present invention are described with reference to the drawings.

[0041] One embodiment of the present invention relates to a semiconductor device having a storage layer disposed on a substrate. The storage layer includes a first transistor and a second transistor, and these transistors can be used to form a storage unit. Since the semiconductor device of one embodiment of the present invention includes a storage unit, it has a function of storing data. Therefore, the semiconductor device of one embodiment of the present invention can be called a storage device.

[0042] When a memory cell is formed using the first and second transistors, one of the first and second transistors is used as a write transistor, and the other is used as a read transistor.

[0043] A semiconductor device of one embodiment of the present invention preferably includes a transistor (OS transistor) containing a metal oxide in a channel formation region. The off-state current of the OS transistor is very small. Therefore, by using the OS transistor in a semiconductor device that can be used as a storage device, the storage content can be maintained for a long period of time. That is, no refresh operation is required or the frequency of the refresh operation is extremely low, thereby substantially reducing the power consumption of the semiconductor device. Therefore, a low-power semiconductor device can be provided. In addition, because the frequency characteristics of the OS transistor are high, the semiconductor device can perform high-speed data reading and writing. Thus, a semiconductor device with a fast operating speed can be provided.

[0044] In the first transistor and the second transistor, one of the source and the drain is located at the bottom and the other is located at the top, so the current flows in the up-down direction. In other words, the channel length direction of the first transistor and the second transistor is the up-down direction. That is, the first transistor and the second transistor are vertical transistors. Compared with the so-called lateral transistors in which the current flows in the lateral direction, the vertical transistor can be miniaturized. Therefore, as the structure of the first transistor and the second transistor adopts a vertical structure, the transistors can be configured with high density to achieve high integration in the semiconductor device. In addition, compared with the lateral transistor, the channel width per unit area of ​​the vertical transistor can be expanded. Therefore, the density of the current flowing through the transistor becomes higher, which can increase the on-state current of the transistor and improve the frequency characteristics.

[0045] In addition, OS transistors have a high ability to resist short channel effects. Therefore, compared with transistors containing silicon in the channel formation region (also called Si transistors), OS transistors are not easily affected by the floating body effect even if they have a vertical structure, and the channel length can be easily shortened even if the gate insulating film is thick. That is, the gate leakage current can be reduced, so the retention characteristics of the storage device can be improved.

[0046] The short channel effect refers to the degradation of electrical characteristics that occurs with the miniaturization of transistors (reduction of channel length). Examples of the short channel effect include drain-induced barrier reduction, electron velocity saturation, hot carrier degradation, etc. In addition, specific examples of the short channel effect include a reduction in threshold voltage, an increase in subthreshold swing value, and an increase in leakage current. Here, the subthreshold swing value refers to the change in gate voltage in the subthreshold region that changes the drain current value by one digit with a fixed drain voltage.

[0047] In addition, the channel length of the vertical transistor included in the semiconductor device of one embodiment of the present invention can be controlled according to the thickness of the oxide semiconductor, so that the processing unevenness of the channel length can be reduced compared with the lateral transistor. That is, the density unevenness of the current flowing through the transistor can be suppressed. Therefore, the frequency characteristics can be improved.

[0048] <Structural Example of Semiconductor Device> Hereinafter, a structural example of a semiconductor device according to one embodiment of the present invention will be described. Note that a component in the semiconductor device according to this embodiment may have a single-layer structure or a stacked-layer structure.

[0049] Figure 1A and Figure 1B 1 is a perspective view and a plan view showing a structural example of a semiconductor device according to one embodiment of the present invention. Figure 1A is a perspective view of the semiconductor device 10. In addition, Figure 1B is a top view of the semiconductor device 10 .

[0050] Note that arrows indicating the X direction, Y direction, and Z direction are sometimes attached in the drawings of the present invention. Note that in this specification, "X direction" refers to the direction along the X axis, and sometimes the forward and reverse directions are not distinguished except for the cases clearly stated. The same is true for "Y direction" and "Z direction". In addition, the X direction, Y direction, and Z direction are directions that intersect each other. More specifically, the X direction, Y direction, and Z direction are directions that are orthogonal to each other. In this specification, the X direction, Y direction, or Z direction is sometimes referred to as the "first direction". In addition, the other one is sometimes referred to as the "second direction". In addition, the remaining one is sometimes referred to as the "third direction".

[0051] The semiconductor device 10 includes a plurality of memory cells 100 . Figure 1A The semiconductor device 10 includes an example in which a plurality of memory cells 100 are arranged in a matrix of m rows and n columns (m and n are each independently an integer greater than 2). By arranging the memory cells 100 in a matrix, a memory cell array can be constructed.

[0052] In addition, the rows and columns extend in directions orthogonal to each other. In this embodiment, the X direction is referred to as a "row" and the Y direction is referred to as a "column". Note that the X direction may also be referred to as a "column" and the Y direction may also be referred to as a "row".

[0053] exist Figure 1A In , the memory cell 100 at the first row and first column is represented as memory cell 100[1,1], the memory cell 100 at the second row and first column is represented as memory cell 100[2,1], and the memory cell 100 at the first row and second column is represented as memory cell 100[1,2]. Note that although Figure 1A Although not shown in the figure, the memory cell 100 at the m-th row and n-th column is represented as the memory cell 100 [m, n].

[0054] In addition, in the present embodiment, etc., an arbitrary row is sometimes represented by "i row". In addition, an arbitrary column is sometimes represented by "j column". Therefore, i is an integer greater than 1 and less than m, and j is an integer greater than 1 and less than n. In addition, in the present embodiment, etc., the i-th row and j-th column storage unit 100 is represented as storage unit 100[i, j]. In the present embodiment, etc., when represented as "i+α" (α is a positive integer or a negative integer), "i+α" is not less than 1 and not greater than m. Similarly, when represented as "j+α", "j+α" is not less than 1 and not greater than n.

[0055] In addition, the semiconductor device 10 includes m conductors 262a extending in the row direction, m conductors 246b extending in the row direction, and n conductors 244 extending in the column direction. In the present embodiment, the conductor 262a arranged in the i-th (i-th row) is represented as conductor 262a[i], and the conductor 246b arranged in the i-th (i-th row) is represented as conductor 246b[i]. Similarly, the conductor 244 arranged in the j-th (j-th column) is represented as conductor 244[j].

[0056] The memory cell 100[i,j] is electrically connected to the conductor 262a[i], the conductor 246b[i], and the conductor 244[j]. In other words, the conductor 262a[i] is electrically connected to n memory cells (memory cells 100[i,1] to 100[i,n]), the conductor 246b[i] is electrically connected to n memory cells (memory cells 100[i,1] to 100[i,n]), and the conductor 244[j] is electrically connected to m memory cells (memory cells 100[1,j] to 100[m,j]).

[0057] The conductor 262a described below refers to any one or more of the conductors 262a[1] to 262a[m], and the conductor 246b described below refers to any one or more of the conductors 246b[1] to 246b[m]. Similarly, the conductor 244 described below refers to any one or more of the conductors 244[1] to 244[n]. Similarly, the memory cell 100 described below refers to any one or more of the memory cells 100[1,1] to 100[m,n].

[0058] The conductor 262a, the conductor 246b, and the conductor 244 are used as wiring.

[0059] [Storage unit 100] FIG. 2A to FIG. 2E A plan view, a cross-sectional view, and a perspective view illustrating a structural example of a memory cell included in a semiconductor device according to one embodiment of the present invention. Figure 2A is a top view of the storage unit 100 . Figure 2B is a cross-sectional view of the memory cell 100, also along Figure 2A A cross-sectional view of the portion taken along the dashed line A1 - A2 in FIG. Figure 2C is a cross-sectional view of the memory cell 100, also along Figure 2A A cross-sectional view of the portion along the dashed line B1 - B2 in FIG. Figure 2D is a perspective view of the storage unit 100 .

[0060] The storage unit 100 [1, 1] to the storage unit 100 [m, n] have the same structure, so in FIG. 2 and the like, they are all referred to as the storage unit 100 without adding any identification symbols.

[0061] The memory cell 100 shown in FIG2 includes a transistor 200a and a transistor 200b. Note that the transistor 200a is provided in the same layer as the transistor 200b. Compared with a structure in which the transistor 200a and the transistor 200b are provided in different layers, by providing the transistor 200a and the transistor 200b in the same layer, the transistor 200a and the transistor 200b can be manufactured at the same time, and the manufacturing process of the semiconductor device can be shortened.

[0062] In the following, when describing common contents between components distinguished by letters, the letters may be omitted. For example, when describing common contents between the transistor 200a and the transistor 200b, the transistor 200 may be described as the transistor 200.

[0063] The transistor 200 includes an oxide 230, a conductor 242a on the oxide 230, an insulator 250, and a conductor 260 on the insulator 250. FIG. 2A to FIG. 2C As shown, the side of the conductor 242a is consistent with the side of the oxide 230. In addition, the oxide 230 and the conductor 242a have a cylindrical shape (also referred to as a columnar shape). Note that the cylindrical shape of the oxide 230 and the conductor 242a extends in the Z direction. In addition, the oxide 230 and the conductor 242a have an opening. Note that the openings of the oxide 230 and the conductor 242a are sometimes referred to as openings, hollows, hollow portions, etc. In addition, the openings of the oxide 230 overlap with the openings of the conductor 242a. In addition, the top surface shape of the oxide 230 and the conductor 242a has a hollow circular shape. In other words, the oxide 230 and the conductor 242a have a cylindrical shape provided with a hollow portion. Note that the cylindrical shape provided with a hollow portion is sometimes referred to as a hollow cylindrical shape.

[0064] Note that in this specification, etc., the top surface shape of a component refers to the outline shape of the component when viewed from a plane. In addition, "when viewed from a plane" refers to the situation when viewed from the normal direction of the surface on which the component is formed or the surface of a support (e.g., a substrate) on which the component is formed.

[0065] Figure 2A The top surface shapes of the oxide 230 and the conductor 242a are shown as hollow circular structures, but the present invention is not limited thereto. For example, the top surface shapes of the oxide 230 and the conductor 242a may be hollow elliptical shapes, hollow polygonal shapes, or hollow polygonal shapes with rounded corners. Here, the polygonal shape refers to a triangle, a quadrangle, a pentagon, a hexagon, and the like.

[0066] The insulator 250 and the conductor 260 are disposed inside the openings of the oxide 230 and the conductor 242 a. The insulator 250 has a region in contact with the side surface of the conductor 260 and a region in contact with the bottom surface of the conductor 260 .

[0067] In addition, the memory cell 100 includes a conductor 244. The oxide 230 is electrically connected to the conductor 244. Figure 2B In the structure shown, oxide 230 has a region that contacts at least a portion of the top surface of conductor 244 .

[0068] The conductor 260 is used as a gate electrode of the transistor 200. The insulator 250 is used as a gate insulator of the transistor 200. Note that the gate insulator is sometimes referred to as a gate insulating layer or a gate insulating film. The conductor 244 has a region used as one of the source electrode and the drain electrode of the transistor 200. The conductor 242a is used as the other of the source electrode and the drain electrode of the transistor 200. At least a portion of the region of the oxide 230 overlapping with the conductor 260 is used as a channel formation region of the transistor 200. Note that the region of the oxide 230 overlapping with the conductor 260 may also be referred to as a region of the oxide 230 facing the conductor 260. Alternatively, the region of the oxide 230 overlapping with the conductor 260 may also be referred to as a region of the oxide 230 facing the conductor 260 via the insulator 250. That is, at least a portion of the region of the oxide 230 facing the conductor 260 is used as a channel formation region of the transistor 200.

[0069] The transistor 200 is a so-called vertical transistor in which one of the source electrode and the drain electrode is located below the channel formation region and the other of the source electrode and the drain electrode is located above the channel formation region, whereby current flows in the vertical direction. In addition, the transistor 200 has a structure in which the channel formation region surrounds the gate electrode. Therefore, the transistor 200 can be called a transistor with a CAA (Channel-All-Around: annular channel) structure.

[0070] Note that the channel length of transistor 200 refers to the length of the region where the semiconductor (or the portion where the current flows in the semiconductor when the transistor is in the on state) and the gate electrode overlap each other when viewed from a cross section, the length of the region where the semiconductor and the gate electrode are opposite to each other, or the distance between the source (source region or source electrode) and the drain (drain region or drain electrode) in the channel formation region. That is, the channel length of transistor 200 is equivalent to the thickness of oxide 230. Therefore, the channel length of transistor 200 can be adjusted by adjusting the thickness of oxide 230, so a transistor 200 with a short channel length can be manufactured by reducing the thickness of oxide 230. By depositing oxide 230 using a deposition method that can form a thin film, for example, the channel length of transistor 200 can be made less than 30nm, less than 20nm, less than 15nm, less than 10nm, less than 8nm, or less than 5nm. That is, for example, it is preferred to form oxide 230 in a manner with a thickness of 3nm or more and less than 30nm. Because the off-state current of the OS transistor is extremely small, the off-state current of transistor 200 can be reduced even with the above-mentioned channel length. Figure 2B The channel length of the transistor 200 is shown by a double-pointed arrow.

[0071] On the other hand, when the transistor is operated in the saturation region, the channel length of the transistor is sometimes lengthened in order to improve the electrical characteristics in the saturation region. The transistor 200 is a vertical transistor, so the occupied area of ​​the transistor 200 when viewed from above is not affected by the thickness of the oxide 230. Therefore, the thickness of the oxide 230 corresponding to the channel length may also be thicker. For example, the thickness of the oxide 230 may also be greater than 30 nm and less than 100 nm.

[0072] Therefore, the thickness of the oxide 230 is greater than or equal to 3 nm and less than or equal to 100 nm, preferably greater than or equal to 3 nm and less than or equal to 30 nm, more preferably greater than or equal to 5 nm and less than or equal to 30 nm, and further preferably greater than or equal to 5 nm and less than or equal to 15 nm.

[0073] In addition, the channel width of transistor 200 refers to the length of the region where the semiconductor (or the portion where the current flows in the semiconductor when the transistor is in the on state) and the gate electrode overlap each other when viewed from above, the length of the region where the semiconductor and the gate electrode are opposite to each other, or the length of the channel formation region in the direction perpendicular to the channel length in the channel formation region. That is, the channel width of transistor 200 is equivalent to the hollow circumference of oxide 230. In addition, in a transistor, the channel width does not necessarily have the same value in all regions. In other words, the channel width of a transistor is sometimes not limited to one value. For example, as described below, sometimes the side of the hollow portion of oxide 230 has a tapered shape when the transistor is viewed from a cross section. Therefore, in this specification, etc., the channel width is any value, maximum value, minimum value or average value in the channel formation region. Figure 2E The double-pointed arrows indicate the channel width of the transistor 200. Figure 2E is a cross-sectional view taken along an XY plane including the oxide 230 .

[0074] Note that the values ​​of the channel length and the channel width can be determined by, for example, cross-sectional TEM image analysis or the like.

[0075] The memory cell 100 includes a conductor 262a, a conductor 262c, a conductor 246b, a conductor 246c, and a conductor 256. The conductor 262a is provided in the same layer as the conductor 262c. The conductor 246b is provided in the same layer as the conductor 246c.

[0076] The conductor 262a is electrically connected to the conductor 260 included in the transistor 200a. Figure 2B In the illustrated structure, the conductor 262a has a region in contact with the top surface of the conductor 260 included in the transistor 200a.

[0077] The conductor 262c is electrically connected to the conductor 260 included in the transistor 200b. Figure 2B In the structure shown, the conductor 262c has a region in contact with the top surface of the conductor 260 included in the transistor 200b.

[0078] The conductor 246b is electrically connected to the conductor 242a included in the transistor 200b. In addition, the conductor 246b is electrically connected to the oxide 230 included in the transistor 200b through the conductor 242a included in the transistor 200b. In other words, the conductor 242a included in the transistor 200b is provided between the oxide 230 included in the transistor 200b and the conductor 246b. Figure 2C In the illustrated structure, the conductor 246b has a region that contacts at least a portion of the top surface of the conductor 242a included in the transistor 200b.

[0079] The conductor 246c is electrically connected to the conductor 242a included in the transistor 200a. In addition, the conductor 246c is electrically connected to the oxide 230 included in the transistor 200a through the conductor 242a included in the transistor 200a. In other words, the conductor 242a included in the transistor 200a is provided between the oxide 230 included in the transistor 200a and the conductor 246c. Figure 2B In the illustrated structure, the conductor 246c has a region that contacts at least a portion of the top surface of the conductor 242a included in the transistor 200a.

[0080] The conductor 256 is electrically connected to the conductor 262 c and the conductor 246 c. In other words, the conductor 246 c is electrically connected to the conductor 262 c through the conductor 256 .

[0081] like Figure 2A As shown in FIG. 1 , the conductor 262a and the conductor 246b are provided to extend in the X direction. That is, the direction in which the conductor 262a extends is the same as the direction in which the conductor 246b extends. In addition, the conductor 244 is provided to extend in the Y direction. That is, the conductor 244 extends in a direction perpendicular to the direction in which the conductor 262a extends. In addition, the conductor 244 extends in a direction perpendicular to the direction in which the conductor 246b extends.

[0082] As described above, transistor 200 is a vertical transistor. The vertical transistor can be formed at the intersection of the minimum pitch wiring. Specifically, transistor 200a is formed between the area where conductor 244 and conductor 262a intersect, and transistor 200b is formed between the area where conductor 244 and conductor 246b intersect. Therefore, miniaturization or high integration of semiconductor devices can be achieved.

[0083] In the transistor 200 , a metal oxide serving as a semiconductor (hereinafter, also referred to as an oxide semiconductor) is preferably used for the oxide 230 including a channel formation region.

[0084] The band gap of the metal oxide used as a semiconductor is preferably 2.0 eV or more, and more preferably 2.5 eV or more. By using a metal oxide with a wide band gap, the off-state current of the transistor can be reduced.

[0085] As the oxide 230, for example, metal oxides such as indium oxide, gallium oxide, and zinc oxide are preferably used. In addition, as the oxide 230, for example, a metal oxide containing two or three selected from indium, element M, and zinc is preferably used. Note that element M is one or more selected from gallium, aluminum, silicon, boron, yttrium, tin, antimony, copper, vanadium, beryllium, titanium, iron, nickel, germanium, zirconium, molybdenum, lanthanum, cerium, neodymium, hafnium, tantalum, tungsten, and magnesium. In particular, element M is preferably one or more selected from aluminum, gallium, yttrium, and tin. Note that a metal oxide containing indium, element M, and zinc is sometimes referred to as In-M-Zn oxide.

[0086] Specifically, a metal oxide having the following composition can be used as the oxide 230: In:M:Zn=4:2:3 [atomic ratio] or a composition close thereto; In:M:Zn=1:1:1 [atomic ratio] or a composition close thereto; In:M:Zn=1:1:1.2 [atomic ratio] or a composition close thereto; or In:M:Zn=1:1:2 [atomic ratio] or a composition close thereto. Note that the nearby composition includes a range of ±30% of the desired atomic ratio.

[0087] In particular, an oxide containing indium (In), gallium (Ga), and zinc (Zn) (also described as IGZO) is preferably used as the oxide 230. Alternatively, an oxide containing indium (In), aluminum (Al), and zinc (Zn) (also described as IAZO) may be used as the oxide 230. Alternatively, an oxide containing indium (In), aluminum (Al), gallium (Ga), and zinc (Zn) (also described as IAGZO, IGAZO, or AGIZO) may be used as the oxide 230.

[0088] In addition, in this specification and the like, a metal oxide containing nitrogen may be referred to as a metal oxide (metal oxide). In addition, a metal oxide containing nitrogen may also be referred to as a metal oxynitride (metal oxynitride).

[0089] In the case of using silicon for the channel formation region of a vertical transistor, the electrical characteristics of the vertical transistor become unstable due to the floating body effect. On the other hand, the effective mass of holes in metal oxides such as IGZO, IAZO and IAGZO is large. Therefore, by using the metal oxide in the channel formation region, the accumulation of holes in the channel formation region can be suppressed, thereby manufacturing a vertical transistor that is little affected by the floating body effect or substantially not affected. That is, by using the above-mentioned metal oxide as oxide 230, the transistor 200 can have stable electrical characteristics. Therefore, a transistor with excellent electrical characteristics and a semiconductor device including the transistor can be provided. In addition, a transistor with less uneven electrical characteristics and a semiconductor device including the transistor can be provided.

[0090] The oxide 230 preferably uses a crystalline oxide semiconductor. Examples of crystalline oxide semiconductors include CAAC-OS (c-axis aligned crystalline oxide semiconductor), nc-OS (nanocrystalline oxide semiconductor), polycrystalline oxide semiconductors, and single crystal oxide semiconductors. CAAC-OS or nc-OS is preferably used as the oxide 230, and CAAC-OS is particularly preferably used.

[0091] CAAC-OS has a dense structure with high crystallinity and is a metal oxide with few impurities and defects (e.g., oxygen vacancies). In particular, by heat treating the metal oxide at a temperature at which the metal oxide is not polycrystallized (e.g., above 400°C and below 600°C) after forming the metal oxide, the CAAC-OS can have a dense structure with higher crystallinity. In this way, by further increasing the density of CAAC-OS, the diffusion of impurities or oxygen in the CAAC-OS can be further reduced.

[0092] In addition, it is not easy to observe clear grain boundaries in CAAC-OS, so it is not easy to cause a decrease in electron mobility due to grain boundaries. Therefore, the physical properties of the metal oxide containing CAAC-OS are stable. Therefore, the metal oxide with CAAC-OS has heat resistance and high reliability.

[0093] In addition, when a crystalline oxide such as CAAC-OS is used as the oxide 230, it is possible to suppress the conductor 244 and the conductor 242a from extracting oxygen from the oxide 230. Therefore, even when heat treatment is performed, it is possible to suppress the extraction of oxygen from the oxide 230, so that the transistor is stable to high temperatures (so-called thermal budget) in the manufacturing process. In addition, it is possible to suppress a decrease in the conductivity of the conductor 244 and the conductor 242a.

[0094] In nc-OS, the atomic arrangement in a tiny region (e.g., a region between 1 nm and 10 nm, and in particular, a region between 1 nm and 3 nm) is periodic. In other words, nc-OS has tiny crystals (also called nanocrystals). In addition, in nc-OS, no regularity of crystal orientation is observed between different nanocrystals, and therefore no orientation is observed in the entire film. That is, when nc-OS is used as oxide 230, the film properties of oxide 230 are fixed regardless of the direction of carrier flow in oxide 230, and therefore the electrical properties of the transistor are very stable.

[0095] Oxide semiconductors have various structures and various characteristics. The oxide 230 may include two or more of CAAC-OS, nc-OS, a-like OS (amorphous-like oxide semiconductor), amorphous oxide semiconductor, polycrystalline oxide semiconductor, and CAC-OS (cloud-aligned composite oxide semiconductor).

[0096] For example, when the CAAC-OS film is structurally analyzed using an XRD device, a peak indicating the c-axis orientation is detected at 2θ = 31° or near it in the Out-of-plane XRD measurement using θ / 2θ scanning. Note that the position (2θ value) of the peak indicating the c-axis orientation sometimes varies depending on the type and composition of the metal elements constituting the CAAC-OS. For example, multiple bright spots (spots) are observed in the electron diffraction pattern of the CAAC-OS film. In addition, when the spot of the incident electron beam passing through the sample (also called a direct spot) is used as the symmetry center, a certain spot and other spots are observed at point-symmetrical positions.

[0097] On the other hand, when the nc-OS film is subjected to electron diffraction using an electron beam whose beam diameter is equal to or smaller than the size of the nanocrystal (for example, greater than 1 nm and less than 30 nm) (also called nanobeam electron diffraction), an electron diffraction pattern is sometimes obtained in which multiple spots are observed in a ring-shaped area centered on the direct spot.

[0098] The oxide 230 may be referred to as a semiconductor layer including a channel formation region of the transistor 200. The material that can be used for the semiconductor layer is not limited to metal oxides (oxide semiconductors) used as semiconductors. For example, semiconductors such as single crystal silicon, polycrystalline silicon, or amorphous silicon may be used as the semiconductor layer, and for example, low temperature polycrystalline silicon (LTPS: Low Temperature Poly Silicon) may also be used.

[0099] Alternatively, as the semiconductor layer, for example, a transition metal chalcogenide used as a semiconductor can be used, for example, molybdenum sulfide (typically MoS2), molybdenum selenide (typically MoSe2), molybdenum telluride (typically MoTe2), tungsten sulfide (typically WS2), tungsten selenide (typically WSe2), tungsten telluride (typically WTe2), hafnium sulfide (typically HfS2), hafnium selenide (typically HfSe2), zirconium sulfide (typically ZrS2), zirconium selenide (typically ZrSe2), etc. can also be used.

[0100] The oxide 230 can be deposited by sputtering, chemical vapor deposition (CVD: Chemical Vapor Deposition) method, molecular beam epitaxy (MBE: Molecular Beam Epitaxy) method, pulsed laser deposition (PLD: Pulsed Laser Deposition) method or ALD (Atomic Layer Deposition: Atomic Layer Deposition) method. In particular, the oxide 230 is preferably deposited by sputtering. By using the sputtering method, a crystalline metal oxide can be formed. In addition, the sputtering method is a deposition method that can form a thin film, so it is suitable for the deposition of the oxide 230.

[0101] Here, in a transistor of a so-called all-around gate structure in which the side of a metal oxide used as a semiconductor is covered by a word line via a gate insulating layer, a metal oxide is provided inside an opening formed in the word line or the gate insulating layer. In order to miniaturize the transistor, it is necessary to make the inner wall of the opening as perpendicular to the substrate surface as possible. At this time, high step coverage is required in the deposition of the metal oxide, so the degree of freedom of the deposition method of the metal oxide is limited.

[0102] On the other hand, the transistor 200 is manufactured by forming an opening in the stacked body of the oxide 230 and the conductor 242a and forming the insulator 250 and the conductor 260 inside the opening. In this case, the oxide 230 only needs to be formed on the conductor 244, and high step coverage is not required in the deposition of the oxide 230. Therefore, the method that can be used for the deposition of the oxide 230 can be made more free. For example, the oxide 230 can be deposited by sputtering, so that a metal oxide with crystallinity can be formed.

[0103] When forming openings or recesses, double imaging techniques such as LELE (Litho-Etch-Litho-Etch) and SADP (Self-Aligned Double Patterning), quadruple imaging techniques such as SAQP (Self-Aligned Quadruple Patterning), and multiple imaging techniques such as octuplet imaging can be used. By using multiple imaging techniques, fine openings or fine recesses can be formed.

[0104] In addition, a shrinking agent can also be used on the resist pattern to shrink the opening of the resist pattern. For example, a shrinking agent is applied to the surface of the resist and then heat treated. As a result, the resist reacts with the shrinking agent to form a reaction layer on the surface of the resist. At this time, the reaction layer is formed on the side of the opening of the resist pattern, so the opening can be shrunk. By using the opening to obtain a shrunk resist pattern, a fine opening or a fine recess can be formed. The above-mentioned shrinking agent is sometimes referred to as a pattern shrinking agent or a hole shrinking agent.

[0105] Alternatively, a fine pattern may be directly formed by exposure using EUV (Extreme Ultraviolet) light or the like.

[0106] Alternatively, the above-mentioned methods may be combined to perform patterning.

[0107] In this way, an oxide semiconductor that is little affected by the floating body effect or substantially not affected by the floating body effect is deposited by sputtering, and then a cylindrical channel with a hollow portion is formed using multiple imaging techniques such as SAQP. By adopting a vertical transistor having a gate electrode disposed in the hollow portion, a transistor capable of miniaturization or high integration can be provided. By using this transistor, a memory cell having a minimum processing size (F) of, for example, less than 15 nm can be realized. Here, the minimum processing size (F) is, for example, the width of the conductor 244 in the X direction, the width of the conductor 262a in the Y direction, or the width of the conductor 246b in the Y direction.

[0108] As the conductor 242a, for example, it is preferred to use a nitride containing tantalum, a nitride containing titanium, a nitride containing molybdenum, a nitride containing tungsten, a nitride containing tantalum and aluminum, or a nitride containing titanium and aluminum. In one embodiment of the present invention, it is particularly preferred to use a nitride containing tantalum. In addition, for example, ruthenium oxide, ruthenium nitride, an oxide containing strontium and ruthenium, or an oxide containing lanthanum and nickel, etc. can also be used. These materials are conductive materials that are not easily oxidized or materials that remain conductive even if they absorb oxygen, so they are preferred.

[0109] Note that hydrogen contained in the oxide 230 or the like may diffuse into the conductor 242a. In particular, when a nitride containing tantalum is used as the conductor 242a, hydrogen contained in the oxide 230 or the like may easily diffuse into the conductor 242a, and the diffused hydrogen may bond with nitrogen contained in the conductor 242a. In other words, hydrogen contained in the oxide 230 or the like may be absorbed by the conductor 242a.

[0110] In addition, since the conductor 242a has a region in contact with the oxide 230, it is preferable to use a conductive material containing oxygen. By using a conductive material containing oxygen as the conductor 242a, the conductivity can be maintained even if the conductor 242a absorbs oxygen. In addition, even when an insulator containing oxygen is used as the insulator 250, the conductor 242a can maintain conductivity, which is preferable.

[0111] As the conductive material containing oxygen, there can be mentioned indium oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide (also referred to as ITO), indium tin oxide containing titanium oxide, indium tin oxide with silicon added (also referred to as ITSO), indium zinc oxide (also referred to as IZO (registered trademark)), and indium zinc oxide containing tungsten oxide. In addition, as the conductive material containing oxygen, there can be mentioned ruthenium oxide, an oxide containing strontium and ruthenium, or an oxide containing lanthanum and nickel. In this specification, etc., a conductive film deposited using a conductive material containing oxygen is sometimes referred to as an oxide conductive film.

[0112] The insulator 250 is preferably formed using an insulator having a function of suppressing the diffusion of oxygen. By adopting this structure, the diffusion of oxygen contained in the oxide 230 to the conductor 260 can be suppressed. That is, the formation of oxygen vacancies in the oxide 230 can be suppressed. In addition, the oxidation of the conductor 260 caused by the oxygen contained in the oxide 230 can be suppressed. Therefore, the electrical characteristics of the transistor 200 can be improved to improve the reliability.

[0113] For example, an insulator containing an oxide of one or both of aluminum and hafnium is preferably used as the insulator 250. As the insulator, aluminum oxide, hafnium oxide, an oxide containing aluminum and hafnium (hafnium aluminate), or an oxide containing hafnium and silicon (hafnium silicate) can be used.

[0114] In addition, a high-k material may be used for the insulator 250. By using a high-k material as the insulator 250, the equivalent oxide thickness (EOT) of the insulator used as the gate insulator can be thinned. Therefore, the insulation withstand voltage of the insulator 250 can be improved.

[0115] Examples of high dielectric constant materials include gallium oxide, hafnium oxide, zirconium oxide, oxides containing aluminum and hafnium, oxynitrides containing aluminum and hafnium, oxides containing silicon and hafnium, oxynitrides containing silicon and hafnium, and nitrides containing silicon and hafnium.

[0116] Alternatively, the insulator 250 may be made of silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, silicon oxide to which fluorine is added, silicon oxide to which carbon is added, silicon oxide to which carbon and nitrogen are added, or silicon oxide having pores.

[0117] In addition, the insulator 250 extends in the Z direction. The top surface of the insulator 250 included in the transistor 200a is preferably located above the top surface of the conductor 246c. Therefore, it is possible to prevent the conductor 246c from contacting the conductor 262a and causing leakage current and short circuit between the conductor 246c and the conductor 262a. Note that when the insulator is provided between the conductor 246c and the conductor 260 included in the transistor 200a and the top surface of the insulator is located above the top surface of the conductor 246c, the top surface of the insulator 250 included in the transistor 200a may also be located below the top surface of the conductor 246c.

[0118] Similarly, the top surface of the insulator 250 included in the transistor 200b is preferably located above the top surface of the conductor 246b. Therefore, it is possible to prevent the conductor 246b from contacting the conductor 262c and causing leakage current and short circuit between the conductor 246b and the conductor 262c. Note that when the insulator is provided between the conductor 246b and the conductor 260 included in the transistor 200b and the top surface of the insulator is located above the top surface of the conductor 246b, the top surface of the insulator 250 included in the transistor 200b may also be located below the top surface of the conductor 246b.

[0119] exist Figure 2B In the figure, the insulator 250 is shown to have a single-layer structure, but the present invention is not limited thereto, and a stacked structure of two or more layers may be used. For example, when the insulator 250 has a two-layer stacked structure, an insulator having a function of inhibiting oxygen diffusion may be used to form an insulator disposed on the oxide 230 side, and an insulator disposed on the conductor 260 side may be formed using a high dielectric constant material.

[0120] As the conductor 260, for example, it is preferable to use a nitride containing tantalum, a nitride containing titanium, a nitride containing molybdenum, a nitride containing tungsten, a nitride containing tantalum and aluminum, a nitride containing titanium and aluminum, or a ruthenium nitride. In addition, for example, ruthenium oxide, an oxide containing strontium and ruthenium, or an oxide containing lanthanum and nickel may also be used. These materials are conductive materials that are not easily oxidized or materials that still maintain conductivity even if oxygen is absorbed, so these materials are suitable when an insulating material containing oxygen is used as the insulator 250 in contact with the conductor 260.

[0121] In addition, a conductive material having a function of suppressing the diffusion of impurities such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules, and copper atoms is preferably used as the conductor 260. Alternatively, a conductive material having a function of suppressing the diffusion of oxygen (for example, at least one of oxygen atoms and oxygen molecules) may be used. Examples of conductive materials having a function of suppressing the diffusion of oxygen include titanium, titanium nitride, tantalum, tantalum nitride, ruthenium, and ruthenium oxide.

[0122] In addition, when the conductor 260 has a function of suppressing the diffusion of oxygen, it is possible to suppress the decrease in conductivity caused by oxidation of the conductor 260 by oxygen contained in the insulator 250. As a conductive material having a function of suppressing the diffusion of oxygen, for example, titanium, titanium nitride, tantalum, tantalum nitride, ruthenium, or ruthenium oxide is preferably used.

[0123] Conductors 246b and 246c are preferably made of a conductive material mainly composed of tungsten, copper, or aluminum. Conductors 246b and 246c may each have a laminated structure, for example, a laminated structure of titanium or titanium nitride and the above conductive materials.

[0124] Conductors 262a and 262c are preferably made of a conductive material mainly composed of tungsten, copper, or aluminum. Conductors 262a and 262c may each have a laminated structure, for example, a laminated structure of titanium or titanium nitride and the above conductive materials.

[0125] Here, Figure 3A Yes Figure 2A 242a, insulator 250, conductor 260, conductor 246b, and conductor 246c in a top view. Note that for ease of understanding, Figure 3A The outlines of the conductor 244 and the conductor 262a are indicated by dashed lines. FIG. 3B to FIG. 3F Show Figure 3A A modified example of the structure shown. FIG. 3A to FIG. 3F It is also a top view for explaining an example of the structure of a semiconductor device. Figure 3D and Figure 3F The outline of the conductor 262c is indicated by a dotted line.

[0126] FIG. 3A to FIG. 3F The region 264b shown is a region where the conductor 246b overlaps with the conductor 242a disposed below the conductor 246b. FIG. 3A to FIG. 3F The illustrated region 264c is a region where the conductor 246c overlaps with the conductor 242a disposed below the conductor 246c.

[0127] like Figure 3A As shown in FIG. 1 , the conductor 246b has an opening. In addition, an insulator 250 and a conductor 260 are provided in the opening. Note that when viewed from above, Figure 3A The width of the conductor 246b in the Y direction is equal to the diameter of the outer circumference of the insulator 250. Figure 3BIn the case where the width of the conductor 246b in the Y direction is smaller than the diameter of the outer circumference of the insulator 250, the conductor 246b is divided by the insulator 250. However, the divided conductors 246b are electrically connected via the conductor 242a provided below the conductor 246b. Therefore, the conductor 246b extends in the X direction via the conductor 242a provided below the conductor 246b, so the conductor 246b can be regarded as extending in the X direction.

[0128] On the other hand, when looking down, Figure 3C As shown, when the width of the conductor 246b in the Y direction is greater than the diameter of the outer circumference of the insulator 250, the conductor 246b extends in the X direction as a continuous conductor.

[0129] Note that although FIG. 3A to FIG. 3C Although the structure in which the insulator 250 and the conductor 260 are provided in the opening included in the conductor 246b is shown, the present invention is not limited thereto. The opening included in the conductor 246b may also be provided with the conductor 260 and an insulator covering the side of the conductor 260. The insulator may be composed of only the insulator 250 or may be composed of the insulator 250 and an insulator provided on the insulator 250.

[0130] In addition, the conductor 246b may be extended in the X direction by the conductor 242a provided below the conductor 246b, and may not have the same contour as the outer periphery of the insulator 250 in a plan view. Figure 3D As shown, the end of the conductor 246b in the region overlapping the conductor 242a provided below the conductor 246b in a plan view may be in a linear shape. Figure 3D The structure in which the conductor 246b and the conductor 262c do not overlap is shown.

[0131] Note that the shape of a region of the conductor 246c that overlaps with the conductor 242a of the transistor 200a may be the same as the shape of the conductor 246b.

[0132] Figure 3A The structure in which the conductor 246c is provided on both the A1 side and the A2 side of the center of the conductor 260 of the transistor 200a is shown, but the present invention is not limited to this. The conductor 246c can be electrically connected to the conductor 242a of the transistor 200a. Figure 3E As shown, the conductor 246c may be provided only on the A2 side of the center of the conductor 260 of the transistor 200a.

[0133] Figure 3D The structure shown in FIG. 1 is similar, and the conductor 246c may be provided only on the A2 side of the center of the conductor 260 of the transistor 200a (see FIG. 10 ). Figure 3F ).

[0134] like Figure 2A As shown in FIG. 1 , in a plan view, the conductor 244 overlaps the center of the hollow cylindrical shape of the oxide 230. Note that the conductor 244 only needs to contact at least a portion of the oxide 230 and does not need to overlap the center of the hollow cylindrical shape of the oxide 230. For example, Figure 4A As shown, the conductor 244 may be arranged at a position away from the center of the hollow cylindrical shape of the oxide 230 in the X direction when viewed from above. Note that Figure 4A is a top view of the storage unit 100 .

[0135] Figure 2A 2 shows a structure in which a straight line that divides the width of the conductor 262a in the Y direction into two halves overlaps with the center of the conductor 260 included in the transistor 200a when viewed from above. Note that the conductor 262a only needs to be in contact with at least a portion of the conductor 260 included in the transistor 200a. For example, Figure 4B As shown, the conductor 262a may be arranged at a position where a straight line (dotted line B3-B4) that divides the width of the conductor 262a in the Y direction in half is away from the center of the conductor 260 in the Y direction when viewed from above. Note that Figure 4B is a top view of the storage unit 100 .

[0136] Figure 2A 2 shows a structure in which a straight line that divides the width of the conductor 246b in the Y direction into two halves overlaps with the center of the conductor 260 included in the transistor 200b when viewed from above. Note that the conductor 246b only needs to be in contact with at least a portion of the conductor 260 included in the transistor 200b. For example, Figure 4C As shown, the conductor 246b may be arranged at a position where a straight line (dash-dotted line B5-B6) that divides the width of the conductor 246b in the Y direction in half is away from the center of the conductor 260 in the Y direction when viewed from above. Figure 4C is a top view of the storage unit 100 .

[0137] Note that when considering Figure 4B In the structure shown in FIG. 1 , it can be said that the center of the conductor 260 included in the transistor 200a can also be located at a position away from the straight line that divides the width of the conductor 262a in the Y direction into two halves. In addition, when considering Figure 4C In the structure shown in FIG. 1 , it can be said that the center of the conductor 260 included in the transistor 200 b may also be located at a position away from the straight line that divides the width of the conductor 246 b in the Y direction into half in the Y direction. Figure 4DAs shown, the following structure may be adopted: the center of the conductor 260 included in the transistor 200b is closer to the A1 side than the straight line (dash-dot line B5-B6) which divides the width of the conductor 246b in the Y direction into two halves, and the center of the conductor 260 adjacent to the conductor 260 in the X direction is closer to the A2 side than the dash-dot line B5-B6. With this structure, the distance between the transistor 200b and the transistor 200b adjacent to the transistor 200b in the X direction can be increased without changing the distance between the conductors 244.

[0138] Note that in Figure 4D When the transistor 200b is arranged as shown in FIG. 1 , the distance between the transistor 200b and the transistor 200a included in the memory cell 100 adjacent to the memory cell 100 including the transistor 200b in the Y direction may be reduced. Therefore, the transistor 200a is preferably arranged in the same manner as the transistor 200b. For example, Figure 4D As shown, the following structure may be adopted: the center of the conductor 260 included in the transistor 200a is closer to the A1 side than the straight line (dash-dotted line B3-B4) which divides the width of the conductor 262a in the Y direction into two halves, and the center of the conductor 260 adjacent to the conductor 260 in the X direction is closer to the A2 side than the dash-dotted line B3-B4. With this structure, it is possible to suppress the distance between the transistor 200a and the transistor 200b from being reduced.

[0139] By adopting Figure 4D The structure shown can reduce the distance between the transistors 200a, the distance between the transistors 200b, and the distance between the wirings, thereby providing a semiconductor device with a high degree of integration of memory cells.

[0140] In addition, by having Figure 4D The structure shown in FIG. 1 can increase the circumference of the hollow space included in the oxide 230 while maintaining the intervals between the conductors 246 b and the intervals between the conductors 262 a. Therefore, the channel width of the transistor is increased, and the on-state current can be increased. For example, Figure 4E As shown in FIG. 1 , the circumference of the hollow area of ​​the oxide 230 of the transistor 200b is made larger than the circumference of the hollow area of ​​the oxide 230 of the transistor 200a. With this structure, the channel width of the transistor 200b is increased. Therefore, the on-state current of the transistor 200b used as a readout transistor can be increased, thereby providing a semiconductor device with a fast readout speed.

[0141] Although Figure 2B and Figure 2CThe conductors 246b and 246c are shown as having flat bottom surfaces, but the present invention is not limited thereto. The conductors 246b and 246c may be in contact with at least a portion of the top surface of the conductor 242a of the transistor 200b and the transistor 200a, respectively, and the conductors 246b and 246c may have either or both convex portions and concave portions.

[0142] For example, Figure 5A As shown, the conductor 246c may also have a convex portion 246c1. The convex portion 246c1 is provided in a region where the conductor 246c overlaps with the conductor 242a of the transistor 200a. In this case, the top surface shape of the convex portion 246c1 is similar to FIG. 3A to FIG. 3F The shape of any of the regions 264c shown in FIG. 24 is the same as that of the region 264c shown in FIG. 24. In addition, the convex shape portion 246c1 is in contact with the conductor 242a of the transistor 200a.

[0143] In addition, for example, Figure 5B As shown in FIG. 1 , the conductor 246b may also have a convex portion 246b1. The convex portion 246b1 is provided in a region where the conductor 246b overlaps with the conductor 242a of the transistor 200b. In this case, the top surface shape of the convex portion 246b1 is similar to that of the conductor 246b1. FIG. 3A to FIG. 3F The shape of any of the regions 264b shown in FIG. 24 is the same as that of the region 264b shown in FIG. 24. The convex shape portion 246b1 is in contact with the conductor 242a of the transistor 200a.

[0144] Note that a method for forming the conductor 246b and the conductor 246c having a convex shape portion will be described below.

[0145] Figure 5C The conductor 246b and the conductor 246c have a convex shape and the top surface shape of the conductor 246b and the conductor 246c is Figure 3D A perspective view of the storage unit 100 in the shape shown.

[0146] [Storage Unit 100A] FIG. 6A to FIG. 6C 100. Note that in the memory cell shown below, the same reference numerals are given to components having the same functions as the components constituting the memory cell 100. In addition, the following mainly describes the parts different from the memory cell 100, and the description of the overlapping parts is omitted.

[0147] Fig. 6A is a top view of the storage unit 100A, Figure 6B is a cross-sectional view of a memory cell 100A, Figure 6C2 is a perspective view of a memory cell 100A. The memory cell 100A is different from the memory cell 100 shown in FIG. 2 in that it includes a conductor 244 a and a conductor 244 b instead of the conductor 244 .

[0148] The conductor 244a is electrically connected to the oxide 230 included in the transistor 200a, and the conductor 244b is electrically connected to the oxide 230 included in the transistor 200b. Note that in FIG6 , the conductor 244a and the conductor 244b are provided so as to extend in the Y direction. That is, the conductor 244a extends in a direction perpendicular to the extending direction of the conductor 262a. In addition, the conductor 244b extends in a direction perpendicular to the extending direction of the conductor 246b.

[0149] The conductor 244a is used as one of a source electrode and a drain electrode of the transistor 200a and a wiring. The conductor 244b is used as one of a source electrode and a drain electrode of the transistor 200b and a wiring.

[0150] By adopting the above structure, the write bit line and the read bit line of the memory cell can exist independently. Note that the structure of the memory cell is described in Embodiment 2.

[0151] Fig. 7A FIG. 6 is a top view of a memory cell array in which the memory cells 100A shown in FIG. 6 are arranged in a matrix. Fig. 7A In FIG. 1 , the conductor 262 a and the conductor 246 b extend in the X direction, the conductor 244 extends in the Y direction, and the line segment connecting the transistor 200 a and the transistor 200 b included in the memory cell 100A is inclined with respect to the X direction.

[0152] like Fig. 7A As shown, one conductor 244 is electrically connected to the first memory cell and the second memory cell adjacent to the first memory cell in the X direction. For example, in the memory cells located in the i-th row, the conductor 244[j] is electrically connected to the memory cell 100A[i, j-1] and the memory cell 100A[i, j]. That is, the conductor 244[j] corresponds to the conductor 244b of the memory cell 100A[i, j-1] and the conductor 244a of the memory cell 100A[i, j].

[0153] Note that the present invention is not limited to the above-mentioned structure. Figure 7B As shown, the conductor 262a and the conductor 246b may extend in the X direction, the conductor 244 may extend obliquely in the X direction, and the line segment connecting the transistor 200a and the transistor 200b included in the memory cell 100A may be parallel to the Y direction. By adopting this structure, the memory density of the semiconductor device can sometimes be further improved.

[0154] [Storage unit 100B] FIG. 8A to FIG. 8C An example of a structure different from the above-mentioned storage unit 100 or storage unit 100A is shown. Note that in the storage unit shown below, components having the same functions as the components constituting the above-mentioned storage unit 100 or storage unit 100A are given the same reference numerals. In addition, the following mainly describes the parts different from the above-mentioned storage unit 100 or storage unit 100A, and the description of the repeated parts is omitted.

[0155] Fig. 8A is a top view of the storage unit 100B, Figure 8B is a cross-sectional view of a memory cell 100B, Figure 8C It is a perspective view of the storage unit 100B.

[0156] The memory cell 100B includes a transistor 200a, a transistor 200b, a conductor 244b, a conductor 244c, a conductor 246a, a conductor 246b, a conductor 256, a conductor 262a, and a conductor 262c.

[0157] The conductor 244 b is electrically connected to the oxide 230 included in the transistor 200 b , and the conductor 244 c is electrically connected to the oxide 230 included in the transistor 200 a .

[0158] The conductor 246 a is electrically connected to the conductor 242 a included in the transistor 200 a , and the conductor 246 b is electrically connected to the conductor 242 a included in the transistor 200 b .

[0159] The conductor 256 is electrically connected to the conductor 244c and the conductor 262c.

[0160] Note that in FIG. 8 , the conductor 262 a and the conductor 244 b are provided to extend in the X direction, the conductor 246 a and the conductor 246 b are provided to extend in the Y direction, and the line segment connecting the transistor 200 a and the transistor 200 b is inclined with respect to the X direction.

[0161] By adopting the above structure, the write bit line and the read bit line of the memory cell can exist independently.

[0162] Fig. 9A FIG. 8 is a top view of a memory cell array in which the memory cells 100B shown in FIG. 8 are arranged in a matrix. Fig. 9A In FIG. 1 , the conductor 262 a and the conductor 244 b extend in the X direction, the conductor 246 extends in the Y direction, and the line segment connecting the transistor 200 a and the transistor 200 b included in the memory cell 100B is inclined with respect to the X direction.

[0163] like Fig. 9AAs shown, one conductor 246 is electrically connected to the first memory cell and the second memory cell adjacent to the first memory cell in the X direction. For example, in the memory cell located in the i-th row, the conductor 246[j] is electrically connected to the memory cell 100B[i, j-1] and the memory cell 100B[i, j]. That is, the conductor 246[j] corresponds to the conductor 246b of the memory cell 100B[i, j-1] and the conductor 246a of the memory cell 100B[i, j].

[0164] Note that the present invention is not limited to the above-mentioned structure. Fig. 9B As shown, the conductor 262a and the conductor 244b may extend in the X direction, the conductor 246 may extend obliquely in the X direction, and the line segment connecting the transistor 200a and the transistor 200b included in the memory cell 100B may be parallel to the Y direction. By adopting this structure, the memory density of the semiconductor device can sometimes be further increased.

[0165] [Storage unit 100C] FIG. 10C to FIG. 10B An example of a structure different from the above-mentioned storage unit 100, storage unit 100A or storage unit 100B is shown. Note that in the storage unit shown below, components having the same functions as the components constituting the above-mentioned storage unit 100, storage unit 100A or storage unit 100B are given the same reference numerals. In addition, the following mainly describes the parts different from the above-mentioned storage unit 100, storage unit 100A or storage unit 100B, and the description of the repeated parts is omitted.

[0166] Fig. 10A and Fig. 10B is a cross-sectional view of a memory cell 100A, Fig. 10C 2 is a perspective view of a memory cell 100C. The main difference between the memory cell 100C and the memory cell 100, the memory cell 100A or the memory cell 100B is the stacking of the transistor 200a and the transistor 200b.

[0167] The memory cell 100C includes a transistor 200a, a transistor 200b, a conductor 244b, a conductor 244c, a conductor 246a, a conductor 246b, and a conductor 262a.

[0168] The conductor 244c is electrically connected to the oxide 230 included in the transistor 200a and the conductor 260 included in the transistor 200b. That is, the oxide 230 included in the transistor 200a is electrically connected to the conductor 260 included in the transistor 200b through the conductor 244c.

[0169] In the memory cell 100B, the oxide 230 included in the transistor 200a and the conductor 260 included in the transistor 200b are electrically connected through the conductor 244c, the conductor 256 and the conductor 262c, and in the memory cell 100C, the oxide 230 included in the transistor 200a and the conductor 260 included in the transistor 200b are electrically connected only through the conductor 244c. By adopting the structure of the memory cell 100C, the number of steps in the manufacturing process of the semiconductor device can be reduced and the productivity can be improved. In addition, it is not necessary to provide an area for arranging the conductor 256, thereby further improving the memory density of the semiconductor device.

[0170] 10 , when the transistor 200a and the transistor 200b are stacked, the thickness of the oxide 230 included in the transistor 200a and the thickness of the oxide 230 included in the transistor 200b can be different. That is, the channel lengths of the transistor 200a and the transistor 200b can be different.

[0171] By increasing the channel length of the transistor, the deviation of the Vth of the transistor can be reduced. Therefore, for example, the thickness of the oxide 230 included in the transistor 200b is made larger than the thickness of the oxide 230 included in the transistor 200a. At this time, the channel length of the transistor 200b used as a read transistor is increased, thereby realizing a memory cell with high read accuracy.

[0172] In addition, the smaller the channel length, the smaller the on-resistance, and the transistor can achieve high-speed operation. Thus, for example, the thickness of the oxide 230 included in the transistor 200a is made smaller than the thickness of the oxide 230 included in the transistor 200b. At this time, the channel length of the transistor 200a used as a write transistor is reduced, thereby realizing a memory cell with a fast write speed. Furthermore, by increasing the thickness of the oxide 230 included in the transistor 200b, the channel length of the transistor 200b used as a read transistor is increased, thereby realizing a memory cell with a fast write speed and high read accuracy.

[0173] Note that in the structure shown in FIG. 10 , since transistor 200a and transistor 200b are not arranged in the same layer, the transistor structure may also be different. For example, one of transistor 200a and transistor 200b may also be a planar transistor, a staggered transistor, or an inversely staggered transistor. In addition, a top-gate or bottom-gate transistor structure may also be adopted. In addition, a gate may also be provided above and below the semiconductor layer forming the channel.

[0174] In the structure shown in FIG. 10 , the semiconductor layer of the transistor 200 a and the semiconductor layer of the transistor 200 b may be formed using the same material or different materials.

[0175] As other semiconductor materials that can be used for the semiconductor layer of one of the transistors 200a and 200b, for example, a semiconductor composed of a single element or a compound semiconductor can be cited. As semiconductors composed of a single element, for example, silicon and germanium can be cited. As compound semiconductors, for example, gallium arsenide and silicon germanium can be cited. In addition, as compound semiconductors, for example, organic semiconductors and nitride semiconductors can be cited. Note that the above-mentioned oxide semiconductor is also a type of compound semiconductor. Note that these semiconductor materials may also contain impurities as dopants.

[0176] Examples of silicon that can be used for the semiconductor layer include single crystal silicon, polycrystalline silicon, microcrystalline silicon, and amorphous silicon. Examples of polycrystalline silicon include low temperature polycrystalline silicon (LTPS: Low Temperature Poly Silicon).

[0177] A transistor using amorphous silicon as a semiconductor layer can be formed on a large glass substrate and can be manufactured at low cost. A transistor using polycrystalline silicon as a semiconductor layer has high field effect mobility and can operate at high speed. In addition, a transistor using microcrystalline silicon as a semiconductor layer has high field effect mobility compared to a transistor using amorphous silicon and can operate at high speed.

[0178] [Modification Example of Transistor 200] Below, refer to FIG. 11A to FIG. 12C A description is given of a structural example different from the above-described transistor 200. Note that in this section, a modified example of the transistor 200 included in the memory cell 100 shown in FIG2 is described, but the structure of the modified example of the transistor 200 described later can also be applied to the memory cells (memory cells 100A to 100C) shown in FIGS. 6 to 10.

[0179] Fig.11A Show Figure 2B A modified example of the transistor 200 is shown. Fig.11A is a cross-sectional view of the memory cell 100 . Fig.11A The transistor 200 is shown with Figure 2B The difference between the transistor 200 shown is the shape of the oxide 230 and the conductor 242a. Specifically, Fig.11A The transistor 200 is shown with Figure 2B The transistor 200 shown is different in that the side surfaces of the oxide 230 and the conductor 242a have a tapered shape.

[0180] In this specification, etc., a tapered shape refers to a shape in which at least a portion of the side surface of a structure is inclined relative to a substrate surface or a formed surface. For example, it refers to a shape having a region where the angle (also referred to as a taper angle) formed by the inclined side surface and the substrate surface or the formed surface is less than 90 degrees. Note that the side surface and the substrate surface of the structure do not necessarily need to be completely flat, and may be a nearly planar shape with a slight curvature or a nearly planar shape with fine concave-convex shapes.

[0181] like Fig.11A As shown, when the transistor 200 is viewed from a cross section, the side surface of the opening side of the oxide 230 (the side of the insulator 250) may also have a cone shape with a cone angle θ. Here, the cone angle θ is the angle formed by the side surface of the opening side of the oxide 230 and the substrate surface. Note that one of the two sides extending from the vertex of the cone angle θ is not limited to the substrate surface, but may also be the top surface of the conductor 244 or the bottom surface of the oxide 230. That is, the cone angle θ may also be the angle formed by the side surface of the oxide 230 and the top surface of the conductor 244 or the bottom surface of the oxide 230. At this time, the side surface on the outside of the oxide 230 also has a cone shape with a cone angle θ.

[0182] By making the side surface of the opening of the oxide 230 tapered, the coverage of the insulator 250 provided in the opening of the oxide 230 is improved, thereby reducing defects such as voids. In addition, by increasing the area of ​​the bottom surface of the oxide 230, the area of ​​the region where the conductor 244 contacts the oxide 230 can be increased.

[0183] The closer the taper angle θ is to 90 degrees, the closer the conductor 260 can be placed below the opening of the oxide 230. Thus, the area of ​​the oxide 230 overlapping the conductor 260 can be increased to stabilize the electrical characteristics of the transistor. In addition, the occupied area of ​​the transistor 200 can be reduced. For example, the taper angle θ is greater than 80 degrees, greater than 85 degrees, or greater than 87 degrees and less than 90 degrees.

[0184] In the above structure, the top surface of the oxide 230 also has a hollow circular shape. That is, in the above structure, the oxide 230 has a hollow truncated cone shape. That is, the area of ​​the upper bottom surface of the truncated cone shape of the oxide 230 (the surface on the side of the conductor 242a) is smaller than the area of ​​the lower bottom surface of the truncated cone shape of the oxide 230 (the surface on the side of the conductor 244).

[0185] Similar to the oxide 230, the side surface of the opening side (insulator 250 side) of the conductor 242a and the side surface of the outer side of the conductor 242a have a tapered shape. The angle formed by the side surface of the opening of the conductor 242a and the substrate surface and the angle formed by the side surface of the outer side of the conductor 242a and the substrate surface are consistent or approximately consistent with the taper angle θ. Note that the angle formed by the side surface of the opening of the conductor 242a and the substrate surface and the angle formed by the side surface of the outer side of the conductor 242a and the substrate surface may not be consistent with the taper angle θ depending on the combination of the material used for the oxide 230 and the material used for the conductor 242a or the processing conditions of the oxide 230 and the conductor 242a.

[0186] In addition, the conductor 242a has a hollow truncated cone shape. That is, the area of ​​the upper bottom surface of the truncated cone shape of the conductor 242a (the surface on the conductor 246b or conductor 246c side) is smaller than the area of ​​the lower bottom surface of the truncated cone shape of the conductor 242a (the surface on the oxide 230 side).

[0187] Fig. 11B Show Figure 2B A modified example of the transistor 200 is shown. Fig. 11B is a cross-sectional view of the memory cell 100 . Fig. 11B The transistor 200 is shown with Figure 2B The transistor 200 is shown to differ in that it includes a conductor 242b.

[0188] The conductor 242b is disposed between the oxide 230 and the conductor 244. Fig. 11B In the embodiment, the conductor 242b is provided so as to be in contact with the bottom surface of the oxide 230. In addition, the conductor 242b is provided so as to be in contact with at least a portion of the top surface of the conductor 244.

[0189] The conductor 242b has a cylindrical shape (also referred to as a cylindrical shape). Note that the cylindrical shape of the conductor 242b extends in the Z direction. In addition, the conductor 242b has an opening. In addition, the top surface of the conductor 242b has a hollow circular shape. In other words, the conductor 242b has a cylindrical shape provided with a hollow portion. The conductor 242b is used as one of the source electrode and the drain electrode of the transistor 200.

[0190] An insulator 250 and a conductor 260 are arranged inside the opening included in the conductor 242b. With this structure, the end of the region where the oxide 230 and the conductor 260 overlap via the insulator 250 can be brought closer to the conductor 244. In other words, the region where the oxide 230 and the conductor 260 do not overlap via the insulator 250, the so-called Loff region, can be reduced or eliminated. Therefore, the frequency characteristics of the transistor 200 can be improved. As a result, the write speed and read speed of the memory cell 100 can be improved, the operating speed of the semiconductor device 10 can be improved, and the like can be improved. As a result, a semiconductor device with a high operating speed can be provided.

[0191] Note that the conductive film to be the conductor 242a and the conductive film to be the conductor 242b are deposited in different steps, and therefore, the conductor 242a and the conductor 242b may be formed using different materials or may be formed using the same material.

[0192] exist Figure 2B In the embodiment, the oxide 230 has a single-layer structure, but the present invention is not limited thereto. For example, the oxide 230 may also have a stacked-layer structure of two or more layers.

[0193] Fig. 12A Show Figure 2B A modified example of the transistor 200 is shown. Fig. 12A is a cross-sectional view of the memory cell 100 . Fig. 12A The transistor 200 is shown with Figure 2B The transistor 200 shown is different in that the oxide 230 has a three-layer stacked structure of an oxide 230_1 , an oxide 230_2 , and an oxide 230_3 .

[0194] The oxide 230_2 is used as a channel formation region of the transistor 200 , the oxide 230_1 is used as one of a source region and a drain region of the transistor 200 , and the oxide 230_3 is used as the other of the source region and the drain region of the transistor 200 .

[0195] As the oxide 230_2, the metal oxides that can be used as the oxide 230 described above may be used.

[0196] The oxide 230_1 and the oxide 230_3 are preferably made of a material having a higher conductivity than the oxide 230_2. In addition, the oxide 230_1 and the oxide 230_3 are preferably made of a degenerate oxide semiconductor.

[0197] For example, as the oxide 230_1 and the oxide 230_3, a material to which nitrogen is added to a metal oxide that can be used as the oxide 230_2 can be used. Specifically, a metal oxide (also referred to as a metal oxynitride) containing indium, the above-mentioned element M, zinc, and nitrogen is preferably used. More specifically, an oxide containing indium (In), gallium (Ga), zinc (Zn), and nitrogen (also referred to as an oxynitride containing In, Ga, and Zn or IGZO to which nitrogen is added), an oxide containing indium (In), aluminum (Al), zinc (Zn), and nitrogen (also referred to as an oxynitride containing In, Al, and Zn or IAZO to which nitrogen is added), or an oxide containing indium (In), aluminum (Al), gallium (Ga), zinc (Zn), and nitrogen (also referred to as an oxynitride containing In, Al, Ga, and Zn, IAGZO to which nitrogen is added, IGAZO to which nitrogen is added, or AGIZO to which nitrogen is added) can be used.

[0198] For example, IGZO to which nitrogen is added tends to have a wurtzite crystal structure. The wurtzite crystal structure has high lattice conformity with the crystal structure of the crystal possessed by the In-M-Zn oxide. Therefore, by using a metal oxynitride having a wurtzite crystal structure as the oxide 230_1, the crystallinity of the oxide 230_2 can be improved. That is, it is easy to form a metal oxide having a CAAC structure as the oxide 230_2.

[0199] In addition, as described above, when CAAC-OS is used as the oxide 230_2, the crystals contained in the oxide 230_2 are oriented in the c-axis relative to the substrate surface. Impurities in the CAAC-OS tend not to diffuse in the c-axis. That is, by using CAAC-OS as the oxide 230_2, impurities can be suppressed from mixing into the oxide 230_2. For example, nitrogen can be suppressed from mixing into the oxide 230_2. Therefore, the conductivity of the oxide 230_2 can be suppressed from increasing.

[0200] Note that, although the above description describes a material in which nitrogen is added to the metal oxide that can be used as the oxide 230_2, the element added to the metal oxide that can be used as the oxide 230_2 may be any element as long as it can improve the conductivity of the metal oxide. As such an element, for example, one or more selected from hydrogen, Group 15 elements (typically nitrogen (N), phosphorus (P), arsenic (As), and antimony (Sb)), boron (B), aluminum (Al), argon (Ar), helium (He), neon (Ne), indium (In), fluorine (F), chlorine (Cl), titanium (Ti), and zinc (Zn) can be used.

[0201] The metal oxide used as oxide 230_1 and oxide 230_3 may have a higher conductivity than oxide 230_2. For example, oxide 230_1 and oxide 230_3 may contain an element common to oxide 230_2 as a main component in addition to oxygen and have a different chemical composition from oxide 230_2.

[0202] In the case where the oxide 230_1 and the oxide 230_3 and the oxide 230_2 contain a common element as a main component in addition to oxygen, the oxide 230 preferably has a stacked structure of a plurality of oxide layers having different chemical compositions. For example, in the case where an In-M-Zn oxide is used as the oxide 230_2, it is preferred that the ratio of the number of atoms of indium in the metal oxide used as the oxide 230_1 or the oxide 230_3 to the sum of the number of atoms of the metal element as the main component is greater than the ratio of the number of atoms of indium in the metal oxide used as the oxide 230_2 to the sum of the number of atoms of the metal element as the main component. In addition, it is preferred that the ratio of the number of atoms of indium in the metal oxide used as the oxide 230_1 or the oxide 230_3 to the element M is greater than the ratio of the number of atoms of indium in the metal oxide used as the oxide 230_2 to the element M.

[0203] By including a common element other than oxygen as a main component, the oxide 230_1, the oxide 230_3, and the oxide 230_2 can reduce the defect state density at the interface between the oxide 230_1, the oxide 230_3, and the oxide 230_2. Since the defect state density at the interface between the oxide 230_1, the oxide 230_3, and the oxide 230_2 can be reduced, the influence of interface scattering on carrier conduction is small, and a high on-state current can be obtained.

[0204] Alternatively, titanium oxide, molybdenum oxide, zinc oxide, indium oxide, tungsten oxide, magnesium oxide, calcium oxide, tin oxide, indium zinc oxide, indium tin oxide, or indium tin oxide containing silicon may be used as the oxide 230_1 and the oxide 230_3 .

[0205] Note that in the case where the oxide 230 has the above-mentioned three-layer stacked structure, as Fig. 12B As shown in FIG. 1 , the conductor 242a is not necessarily provided. In this case, the conductor 246b or the conductor 246c is used as the conductor 242a. That is, the conductor 246b or the conductor 246c is used as the wiring and the other of the source electrode and the drain electrode. By adopting a structure without providing the conductor 242a, the number of steps in the manufacturing process of the semiconductor device can be reduced and the productivity can be improved.

[0206] Fig. 12C Show Figure 2B A modified example of the transistor 200 is shown. Fig. 12C is a cross-sectional view of the memory cell 100 . Fig. 12C The transistor 200 is shown with Figure 2B The difference of the transistor 200 shown is that the oxide 230 has a stacked structure of two layers, namely, an oxide 230_1 and an oxide 230_2 .

[0207] When heat treatment is performed while the conductor 242a is in contact with the oxide 230_2, the sheet resistance of the oxide 230_2 near the conductor 242a may decrease. In addition, the carrier concentration may increase. Therefore, the resistance of the oxide 230_2 near the conductor 242a can be reduced in a self-aligned manner.

[0208] In the above case, for example, Fig. 12C As shown, a region 230_22 is formed in the oxide 230_2. The region 230_22 is a region of the oxide 230_2 that is close to the conductor 242a and has low resistance. The region 230_22 is used as the other of the source region and the drain region. In addition, the region used as the channel formation region in the oxide 230_2 is recorded as a region 230_21. Note that in the oxide 230_2, it is sometimes difficult to clearly observe the boundaries between the regions.

[0209] Note that, depending on the material used for the conductor 242a, the region 230_22 may not be formed. In this case, the oxide 230_2 has the region 230_21. Also, depending on the material used for the conductor 244, a region with low resistance may be formed near the conductor 244 of the oxide 230_1.

[0210] <Detailed Configuration Example of Semiconductor Device> Below, refer to FIG. 13A to FIG. 13D A detailed structural example of a semiconductor device according to one embodiment of the present invention is described. Note that in the semiconductor device described below, components having the same functions as the components constituting the semiconductor device described in the above <Structural example of semiconductor device> are given the same reference numerals. In addition, the following mainly describes the parts different from the semiconductor device described in the above <Structural example of semiconductor device>, and the description of the overlapping parts is omitted.

[0211] FIG. 13A to FIG. 13D 1 and 2 are a top view and a cross-sectional view of a semiconductor device including the memory cell 100 . Fig.13A and Fig.13D is a top view of the semiconductor device. Fig. 13B and Fig. 13C is a cross-sectional view of the semiconductor device. Fig. 13B It is along Fig.13AA cross-sectional view of the portion along the dot-dash line A1-A2 in FIG. Fig. 13C It is along Fig.13A The cross-sectional view of the portion of the dot-dash line B1-B2 in FIG. Fig.13D yes Fig.13A A top view of the area enclosed by the double-dashed line in FIG. Fig. 13B The cross section of the dotted line C1-C2 in FIG. Fig.13A In the top view, some components are omitted for clarity.

[0212] FIG. 13A to FIG. 13D The semiconductor device shown includes a plurality of memory cells 100 arranged in a matrix. Fig.13A Two of the plurality of memory cells 100 included in the semiconductor device are shown.

[0213] FIG. 13A to FIG. 13D The semiconductor device shown includes: an insulator 216 and a conductor 244 on a substrate (not shown); a transistor 200a, a transistor 200b, an insulator 275b, an insulator 250b, and an insulator 274 on the insulator 216 and the conductor 244; a conductor 246b, a conductor 246c, an insulator 276, and an insulator 278 on the transistor 200a, the transistor 200b, the insulator 275b, the insulator 250b, and the insulator 274; an insulator 277b on the conductor 246b; an insulator 277c and a conductor 256 on the conductor 246c; and a conductor 262a, a conductor 262c, and an insulator 285 on the insulator 276, the insulator 277b, the insulator 277c, the insulator 278, and the conductor 256. The insulator 216 , the insulator 274 , the insulator 276 , the insulator 277 b , the insulator 277 c , the insulator 278 , and the insulator 285 serve as interlayer films.

[0214] When looking down, FIG. 13A to FIG. 13D In the semiconductor device shown, the conductor 262a does not overlap with the conductor 246c. In addition, the conductor 262c does not overlap with the conductor 246b.

[0215] FIG. 13A to FIG. 13D The memory cell 100 included in the semiconductor device shown in the figure is composed of a transistor 200a and a transistor 200b. Note that the transistor 200a and the transistor 200b are electrically connected through the conductor 262c, the conductor 256, and the conductor 246c. FIG. 13A to FIG. 13D The memory cell 100 shown is also Figure 3D , Figure 5A , Figure 5B and Figure 5C A detailed structural example of the memory cell 100 is shown.

[0216] [Details of the storage unit 100] like Fig. 13B and Fig. 13C As shown, transistor 200 includes: a conductor 244 (conductor 244_1 and conductor 244_2) configured in a manner embedded in an insulator 216; an oxide 230_1 and an insulator 275a on the insulator 216 and the conductor 244; an oxide 230_2 on the oxide 230_1; an oxide 230_3 on the oxide 230_2; a conductor 242a on the oxide 230_3; an insulator 250a on the insulator 275a; and a conductor 260 on the insulator 250a.

[0217] Hereinafter, the oxide 230_1 , the oxide 230_2 , and the oxide 230_3 may be collectively referred to as an oxide 230 .

[0218] Insulator 275a, insulator 250a, and conductor 260 are disposed inside the openings of oxide 230 and conductor 242a. Insulator 250a has a region in contact with the side surface of conductor 260 and a region in contact with the bottom surface of conductor 260. Insulator 275a has a region in contact with the side surface of insulator 250a, a region in contact with the bottom surface of insulator 250a, a region in contact with the side surface on one side of the opening of oxide 230, a region in contact with the side surface on one side of the opening of conductor 242a, and a region in contact with the top surface of conductor 244. In this structure, it can also be said that insulator 275a and insulator 250a each have a recessed portion. For example, as Figure 4A As shown, when the conductor 244 is arranged at a position offset in the X direction from the center of the hollow cylindrical shape of the oxide 230 in a plan view, the insulator 275 a may have a region in contact with the insulator 216 .

[0219] Fig.13D It corresponds to the XY plane at or near the center of the oxide 230_2. Fig.13D In the case where the top surface of the oxide 230_2 has a hollow circle shape, the insulator 275a is set in a concentric circle shape inside the oxide 230_2, the insulator 250a is set in a concentric circle shape inside the insulator 275a, and the conductor 260 is set in a concentric circle shape inside the insulator 250a.

[0220] Here, the width of the oxide 230_2 in the direction from the center of the hollow portion of the oxide 230_2 to the outer periphery of the cylindrical shape is referred to as the width H1. In other words, the width H1 is half the difference between the outer diameter and the inner diameter of the hollow cylindrical shape.

[0221] In order to prevent adjacent oxides 230_2 from contacting each other, the width H1 needs to be less than half of the minimum processing size (F). On the other hand, in order to form a hollow cylindrical oxide 230_2, the width H1 needs to be a certain size. When the minimum processing size (F) is, for example, 15nm, the width H1 is preferably greater than 1nm and less than 7nm, more preferably greater than 1.5nm and less than 6nm, and further preferably greater than 2nm and less than 5nm. By adopting this structure, adjacent oxides 230_2 can be non-contacting with each other, and at least an insulator 275b can be provided between adjacent oxides 230_2. Note that the range of suitable width H1 is not limited to the above range. The width H1 can be appropriately set according to the minimum processing size and the thickness of the insulator 275b.

[0222] The oxide 230 has a region overlapping with the conductor 244. More specifically, the oxide 230_1 has a region contacting at least a portion of the top surface of the conductor 244. In addition, the oxide 230 has a region overlapping with the conductor 242a. More specifically, the oxide 230_3 has a region contacting at least a portion of the bottom surface of the conductor 242a.

[0223] The height of the uppermost portion of the insulator 250 a coincides with the height of each of the uppermost portion of the insulator 275 a , the uppermost portion of the insulator 275 b , the uppermost portion of the insulator 250 b , and the uppermost portion of the insulator 274 .

[0224] Insulator 276 is provided on insulator 275a and insulator 250a. In addition, conductor 262a or conductor 262c is located on insulator 276. That is, insulator 276 is provided between insulator 275a and insulator 250a and conductor 262a or conductor 262c. Insulator 276 has a region overlapping with insulator 275a and insulator 250a. In addition, insulator 276 has a region in contact with the bottom surface of conductor 262a or conductor 262c. In other words, at least a portion of the bottom surface of conductor 262a or conductor 262c is in contact with the top surface of insulator 276.

[0225] Insulator 276 is used as an interlayer film. Insulator 276 has a cylindrical shape and has an opening. That is, insulator 276 has a cylindrical shape with a hollow portion. In other words, the top surface shape of insulator 276 has a hollow circular shape. Conductor 260 is provided in the hollow portion of insulator 276. In addition, when the cross-sectional shape of conductor 260 is a circular shape, insulator 276 is provided in a concentric circle shape on the outside of conductor 260.

[0226] In a plan view, the diameter of the hollow portion of the insulator 276 is preferably equal to or larger than the diameter of the inner side of the recess of the insulator 250a in which the conductor 260 is disposed. By adopting this structure, the conductor 260 can be more reliably embedded in the recess of the insulator 250a. Fig.14A As shown, sometimes a part of the conductor 246c is arranged on the insulator 275a or on the insulator 275a and the insulator 250a. In this case, by adopting the above structure, the conductor 260 can also be embedded in the recessed portion of the insulator 250a. In addition, the same is true for the case where a part of the conductor 246b is arranged on the insulator 275a or on the insulator 275a and the insulator 250a.

[0227] In addition, the cylindrical profile of the insulator 276 is preferably consistent with the profile of the insulator 275a. By adopting this structure, the area of ​​contact between the conductor 242a and the conductor 246b or the conductor 246c can be further increased compared with a structure in which the cylindrical profile of the insulator 276 is larger than the profile of the insulator 275a. In addition, by adopting this structure, the distance between the conductor 262a and the conductor 246c and the distance between the conductor 262c and the conductor 246b can be further increased compared with a structure in which the cylindrical profile of the insulator 276 is smaller than the profile of the insulator 275a. Therefore, leakage current and short circuit between the conductor 262a and the conductor 246c and between the conductor 262c and the conductor 246b can be prevented.

[0228] In addition, the insulator 276 preferably extends in the Z direction so that the top surface of the conductor 246b or the conductor 246c is located between the bottom surface and the top surface of the insulator 276. In other words, the insulator 276 preferably extends in the Z direction so that the top surface of the conductor 246b or the conductor 246c is located above the bottom surface of the insulator 276 and below the top surface of the insulator 276. By adopting such a structure, the contact between the conductor 262a and the conductor 246c and the contact between the conductor 262c and the conductor 246b can be prevented, thereby preventing leakage current and short circuit between the conductor 262a and the conductor 246c and between the conductor 262c and the conductor 246b.

[0229] An insulator 277b is provided on the conductor 246b, and an insulator 277c is provided on the conductor 246c. Fig. 13B As shown, the insulator 277c and the conductor 246c have a region where the ends coincide with each other. Although not shown, the insulator 277b and the conductor 246b have a region where the ends coincide with each other.

[0230] The conductor 260 is used as a gate electrode of the transistor 200. In addition, the insulator 275a and the insulator 250a are used as gate insulators of the transistor 200. In addition, the conductor 244 is used as one of the source electrode and the drain electrode of the transistor 200, and the conductor 242a is used as the other of the source electrode and the drain electrode of the transistor 200. In addition, at least a portion of the region of the oxide 230 overlapping with the conductor 260 is used as a channel formation region of the transistor 200. For example, the oxide 230_2 is used as a channel formation region of the transistor 200, the oxide 230_1 is used as one of the source region and the drain region of the transistor 200, and the oxide 230_3 is used as the other of the source region and the drain region of the transistor 200.

[0231] A metal oxide (hereinafter also referred to as an oxide semiconductor) used as a semiconductor is preferably used for the oxide 230_2 including the channel formation region in the transistor 200. In some cases, a portion of the region of the oxide 230_1 and the oxide 230_3 overlapping the conductor 260 is used as the channel formation region.

[0232] Note that Fig. 13B In the transistor 200 shown, the oxide 230 has a three-layer stacked structure of oxide 230_1 , oxide 230_2 , and oxide 230_3 , but the present invention is not limited thereto. For example, the oxide 230 may have a single-layer structure or a stacked structure of two or more layers.

[0233] The material, structure, and the like of the oxide 230 (the oxide 230_1 , the oxide 230_2 , and the oxide 230_3 ) can refer to the contents described in the above-mentioned <Structural Example of Semiconductor Device>.

[0234] The relative dielectric constant of insulator 216, insulator 274, insulator 276, insulator 277b, insulator 277c, insulator 278, and insulator 285 is preferably low. By using a material with a low relative dielectric constant for the interlayer film, the parasitic capacitance generated between the wirings can be reduced. For example, as insulator 216, insulator 274, insulator 276, insulator 277b, insulator 277c, insulator 278, and insulator 285, silicon oxide, silicon oxynitride, silicon nitride, silicon oxide added with fluorine, silicon oxide added with carbon, silicon oxide added with carbon and nitrogen, silicon oxide with pores, or resin can be used appropriately. As the resin, for example, polyester, polyolefin, polyamide (nylon, aramid, etc.), polyimide, polycarbonate, or acrylic resin can be cited.

[0235] The conductor 244 has a region overlapping with the oxide 230. More specifically, the conductor 244 is arranged so as to be in contact with at least a portion of the bottom surface of the oxide 230_1. Here, the conductor 244 is preferably provided so as to be embedded in an opening of the insulator 216.

[0236] The conductor 244 includes a two-layer structure of a conductor 244_1 and a conductor 244_2. The conductor 244_1 is provided in a manner of contacting the bottom surface and the side wall of the opening portion of the insulator 216. The conductor 244_2 is provided in a manner of being embedded in the recess formed in the conductor 244_1. Here, the height of the top surface of the conductor 244_2 is consistent with the height of the top surface of the conductor 244_1 and the height of the top surface of the insulator 216.

[0237] Here, as the conductor 244_1, a conductive material having a function of suppressing the diffusion of oxygen (for example, at least one of oxygen atoms and oxygen molecules) is preferably used. Alternatively, as the conductor 244_1, a conductive material having a function of suppressing the diffusion of impurities such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules (N2O, NO, NO2, etc.), copper atoms, etc. is preferably used.

[0238] By using a conductive material having a function of suppressing the diffusion of oxygen as the conductor 244_1, it is possible to suppress oxidation of the conductor 244_2 and reduce the conductivity. As the conductive material having a function of suppressing the diffusion of oxygen, for example, titanium, titanium nitride, tantalum, tantalum nitride, ruthenium, or ruthenium oxide can be used. Therefore, as the conductor 244_1, a single layer or a stack of the above conductive materials can be used. For example, titanium nitride can be used as the conductor 244_1.

[0239] In addition, it is preferable that a conductive material containing tungsten, copper, or aluminum as a main component is used for the conductor 244_2. For example, tungsten can be used for the conductor 244_2.

[0240] In addition, the resistivity of the conductor 244 is designed in consideration of the potential applied to the conductor 244, and the thickness of the conductor 244 is set according to the resistivity. In addition, the thickness of the insulator 216 is substantially the same as that of the conductor 244. Here, it is preferable to reduce the thickness of the conductor 244 and the insulator 216 within the range allowed by the design of the conductor 244. By reducing the thickness of the insulator 216, the absolute amount of impurities such as hydrogen contained in the insulator 216 can be reduced, so the diffusion of the impurities into the oxide 230 can be suppressed.

[0241] Notice, Fig. 13B The conductor 244 is shown to have a two-layer structure of the conductor 244_1 and the conductor 244_2, but the present invention is not limited thereto. For example, the conductor 244 may have a single-layer structure or a stacked-layer structure of three or more layers.

[0242] Note that the material and structure of the conductor 244 can refer to the contents described in the above-mentioned <Structural example of semiconductor device>. In addition, the conductor 244 can also use the conductive material that can be used for the conductor 242a.

[0243] The conductor 242a overlaps with the oxide 230. More specifically, the conductor 242a is provided in contact with the top surface of the oxide 230_3.

[0244] Notice, Fig. 13B The conductor 242a is shown as a single-layer structure, but the present invention is not limited thereto, and the conductor 242a may also have a stacked structure of two or more layers. For example, the conductor 242a may also have a two-layer stacked structure of a first conductor on the oxide 230_3 and a second conductor on the first conductor.

[0245] The first conductor of the conductor 242a is preferably composed of a conductive material having a characteristic that is not easily oxidized. Thus, the first conductor of the conductor 242a can be suppressed from being oxidized and the conductivity of the conductor 242a can be reduced. In addition, the first conductor of the conductor 242a can have a characteristic of easily absorbing (extracting) hydrogen. Thus, the hydrogen in the oxide 230 diffuses into the first conductor of the conductor 242a, and the hydrogen concentration of the oxide 230 can be reduced. Therefore, the transistor 200 can have stable electrical characteristics.

[0246] The second conductor of the conductor 242a is preferably composed of a conductive material having a higher conductivity than the first conductor of the conductor 242a. In this case, the second conductor of the conductor 242a only needs to have a region having a higher conductivity than the first conductor of the conductor 242a at least in a part thereof. In addition, the second conductor of the conductor 242a is preferably composed of a conductive material having a lower resistivity than the first conductor of the conductor 242a. Thus, a semiconductor device with suppressed wiring delay can be manufactured.

[0247] In addition, the second conductor of the conductor 242a can have a property of easily absorbing hydrogen. Therefore, the hydrogen absorbed by the first conductor of the conductor 242a also diffuses into the second conductor of the conductor 242a, and the hydrogen concentration in the oxide 230 can be further reduced. Therefore, the transistor 200 can have stable electrical characteristics.

[0248] Here, as the first conductor and the second conductor of the conductor 242a, it is preferable to use a conductive material having the same constituent elements and different chemical compositions. In this case, the first conductor and the second conductor of the conductor 242a can be continuously deposited without being exposed to the atmospheric environment. By depositing the film without being exposed to the atmospheric environment, impurities or moisture from the atmospheric environment can be prevented from adhering to the surface of the first conductor of the conductor 242a, thereby keeping the first conductor of the conductor 242a and the second conductor clean.

[0249] In addition, it is preferred that a tantalum nitride having a high ratio of nitrogen atoms to tantalum is used as the first conductor of the conductor 242a, and a tantalum nitride having a low ratio of nitrogen atoms to tantalum is used as the second conductor of the conductor 242a. For example, a tantalum nitride having a ratio of nitrogen atoms to tantalum of 1.0 to 2.0 is used as the first conductor of the conductor 242a, preferably 1.1 to 1.8, and more preferably 1.2 to 1.5. In addition, for example, a tantalum nitride having a ratio of nitrogen atoms to tantalum of 0.3 to 1.5 is used as the second conductor of the conductor 242a.

[0250] By increasing the ratio of the number of nitrogen atoms relative to tantalum in the nitride containing tantalum, the oxidation of the nitride containing tantalum can be suppressed. In addition, the oxidation resistance of the nitride containing tantalum can be improved. In addition, the diffusion of oxygen into the nitride containing tantalum can be suppressed. Therefore, it is preferred that a nitride containing tantalum, in which the ratio of the number of nitrogen atoms relative to tantalum is high, is used as the first conductor of the conductor 242a. Thus, it is possible to prevent an oxide layer from being formed between the first conductor of the conductor 242a and the oxide 230, or the thickness of the oxide layer can be reduced.

[0251] In addition, by reducing the ratio of the number of nitrogen atoms to tantalum in the nitride containing tantalum, the resistivity of the nitride can be reduced. Therefore, it is preferable to use a nitride containing tantalum as the second conductor of the conductor 242a, in which the ratio of the number of nitrogen atoms to tantalum is low. In this way, a semiconductor device with suppressed wiring delay can be manufactured.

[0252] Note that in the conductor 242a, it is sometimes difficult to clearly observe the boundary between the first conductor and the second conductor. In the case where a tantalum nitride is used for the conductor 242a, the concentrations of tantalum and nitrogen detected in each layer do not necessarily have to change in stages for each layer, but may also change gradually in the region between the first conductor and the second conductor (also referred to as gradation). That is, in the conductor 242a, the closer the region is to the oxide 230, the higher the ratio of the number of nitrogen atoms relative to tantalum. Therefore, the ratio of the number of nitrogen atoms relative to tantalum in the region below the conductor 242a is preferably higher than the ratio of the number of nitrogen atoms relative to tantalum in the region above the conductor 242a.

[0253] The thickness of the first conductor of the conductor 242a is 0.1 nm or more and 5.0 nm or less, preferably 0.5 nm or more and 3.0 nm or less, and more preferably 1.0 nm or more and 3.0 nm or less. In this case, at least a portion of the first conductor of the conductor 242a has an area with the above thickness. In addition, the thickness of the first conductor of the conductor 242a is preferably smaller than the thickness of the second conductor of the conductor 242a. In this case, at least a portion of the first conductor of the conductor 242a has an area with a thickness smaller than that of the second conductor of the conductor 242a.

[0254] Note that, although an example is shown here in which the first and second conductors of the conductor 242a are formed of conductive materials having the same constituent elements but different chemical compositions, the present invention is not limited thereto, and the first and second conductors of the conductor 242a may be formed of different conductive materials. For example, a nitride containing tantalum may be used as the first conductor of the conductor 242a, and a nitride containing titanium or tungsten may be used as the second conductor of the conductor 242a.

[0255] Note that the material and structure of the conductor 242 a may refer to the contents described in the above-mentioned <Structural example of semiconductor device>.

[0256] In a plan view, the insulator 275a is arranged inside the openings of the oxide 230 and the conductor 242a (the hollow parts of the oxide 230 and the conductor 242a). The insulator 275a is used as a part of the gate insulator. In a plan view, the insulator 275b is arranged outside the cylindrical shape of the oxide 230 and the conductor 242a.

[0257] The details will be described later, but the insulator 275a and the insulator 275b are formed in the same process. Therefore, the insulator 275a includes the same insulating material as the insulator 275b. In addition, the thickness of the insulator 275b is equal to the thickness of the insulator 275a.

[0258] In addition, the insulator 275a is provided in the same layer as the insulator 275b. Fig. 13B In the figure, the insulator 275a and the insulator 275b are arranged on the insulator 216 and the conductor 244.

[0259] An oxygen blocking insulating film is preferably used as the insulator 275a and the insulator 275b. As the insulator 275a and the insulator 275b, for example, an insulator containing an oxide of one or both of aluminum and hafnium is preferably used. As the insulator, aluminum oxide, hafnium oxide, an oxide containing aluminum and hafnium (hafnium aluminate), an oxide containing hafnium and silicon (hafnium silicate), etc. can be used. In this embodiment, aluminum oxide is used as the insulator 275a and the insulator 275b. In this case, the insulator 275a and the insulator 275b are insulators containing at least oxygen and aluminum.

[0260] like Fig. 13B As shown in FIG. 1 , insulator 275a is provided in contact with the side of the opening of oxide 230. In addition, insulator 275b is provided in contact with the outer side of oxide 230. That is, oxide 230 is covered by insulator 275a and insulator 275b. Therefore, insulator 275a and insulator 275b having oxygen barrier properties can be used to prevent oxygen in oxide 230 from being separated during heat treatment or the like. Therefore, the formation of oxygen vacancies in oxide 230 can be suppressed. As a result, oxygen vacancies and V generated in oxide 230 can be reduced. O H. Therefore, the electrical characteristics and reliability of the transistor 200 can be improved.

[0261] Even if the insulator 274 and the insulator 250a contain excessive oxygen, excessive supply of oxygen to the oxide 230 can be suppressed. Therefore, excessive oxidation of the oxide 230_1 and the oxide 230_3 to reduce the on-state current of the transistor 200 or reduce the field effect mobility can be suppressed.

[0262] In addition, if Fig. 13B As shown, the insulator 275a is provided in a manner in contact with the side surface of the opening side of the conductor 242a, and the insulator 275b is provided in a manner in contact with the outer side surface of the conductor 242a. That is, the conductor 242a is covered by the insulator 275a and the insulator 275b. Therefore, it is possible to suppress the side surface of the conductor 242a from being oxidized and the oxide film from being formed on the side surface. Therefore, it is possible to suppress the decrease in the on-state current of the transistor 200 or the decrease in the field effect mobility.

[0263] When aluminum oxide is used as the insulator 275a and the insulator 275b, aluminum is sometimes added to the region of the oxide 230_2 that contacts the insulator 275a and its vicinity, and the region of the oxide 230_2 that contacts the insulator 275b and its vicinity. For example, when IGZO is used as the oxide 230_2, the region of the oxide 230_2 that contacts the insulator 275a and its vicinity, and the region of the oxide 230_2 that contacts the insulator 275b and its vicinity contain indium, gallium, aluminum, and zinc.

[0264] In addition, if Fig. 13B As shown in FIG. 1 , since the insulator 275a formed of aluminum oxide or the like is provided in contact with the side surface of the opening of the oxide 230_2, the indium contained in the oxide 230_2 is sometimes distributed at the interface between the oxide 230_2 and the insulator 275a and its vicinity. Therefore, the surface near the opening side of the oxide 230_2 has an atomic number ratio close to that of indium oxide or close to that of In-Zn oxide. When the number of indium atoms in the oxide 230_2, especially near the surface near the opening side of the oxide 230_2, is relatively large, the field effect mobility of the transistor 200 can be improved.

[0265] The insulator 275a needs to be provided in the opening of the conductor 242a and the oxide 230 together with the insulator 250a and the conductor 260. In order to realize the miniaturization of the transistor 200, the thickness of the insulator 275a is preferably small. The thickness of the insulator 275a is greater than 0.1nm and less than 5.0nm, preferably greater than 0.5nm and less than 3.0nm, and more preferably greater than 1.0nm and less than 3.0nm. At this time, at least a portion of the insulator 275a is a region having the above thickness. In addition, the thickness of the insulator 275a is preferably smaller than the thickness of the insulator 250a. At this time, at least a portion of the insulator 275a is a region having a thickness less than that of the insulator 250a.

[0266] In order to reduce the thickness of the insulator 275a as described above, it is preferred to deposit the insulator 275a using the ALD method. The ALD method includes a thermal ALD method that uses only thermal energy to react a precursor and a reactant, a PEALD method that uses a reactant excited by plasma, and the like. In the PEALD method, deposition can be performed at a lower temperature by using plasma, so it is sometimes preferred.

[0267] The ALD method can deposit atoms for each layer, thereby achieving the effects of being able to deposit extremely thin films, being able to deposit structures with high aspect ratios, being able to deposit with fewer defects such as pinholes, being able to deposit with excellent coverage, and being able to deposit at low temperatures. Therefore, the insulator 275a can be deposited with a small thickness and high coverage on the side surfaces of the openings of the conductor 242a and the oxide 230.

[0268] The precursor used in the ALD method sometimes contains carbon, etc. Therefore, the film formed by the ALD method sometimes contains more impurities such as carbon than the film formed by other deposition methods. In addition, the quantitative analysis of impurities can be performed by secondary ion mass spectrometry (SIMS: Secondary Ion Mass Spectrometry), X-ray photoelectron spectroscopy (XPS: X-ray Photoelectron Spectroscopy) or Auger electron spectroscopy (AES: Auger Electron Spectroscopy).

[0269] The insulator 250a is disposed in the recess of the insulator 275a. The insulator 250a is used as a part of the gate insulator. In addition, the insulator 250b is disposed so as to be in contact with the top surface of the insulator 275b.

[0270] The details will be described later, but the insulator 250a and the insulator 250b are formed in the same process. Therefore, the insulator 250a includes the same insulating material as the insulator 250b. In addition, the thickness of the insulator 250b is equal to the thickness of the insulator 250a.

[0271] In addition, Fig. 13B , the insulator 250a is disposed on the insulator 275a, and the insulator 250b is disposed on the insulator 275b. As described above, since the insulator 275a is disposed in the same layer as the insulator 275b, the insulator 250a can be regarded as being disposed in the same layer as the insulator 250b.

[0272] Note that the materials and structures of the insulators 250a and 250b may refer to the contents of the insulator 250 described in the above-mentioned <Structural example of semiconductor device>.

[0273] In this embodiment, hafnium oxide is used as the insulator 250a and the insulator 250b. In this case, the insulator 250a and the insulator 250b contain at least oxygen and hafnium.

[0274] The conductor 260 is disposed in the recess of the insulator 250a. In the transistor 200, the conductor 260 is formed in a self-aligned manner so as to fill the openings of the oxide 230 and the conductor 242a.

[0275] Fig. 13B Although the conductor 260 is shown as a single-layer structure, the present invention is not limited thereto. For example, the conductor 260 may also have a stacked structure of two or more layers.

[0276] Note that the material and structure of the conductor 260 may refer to the contents described in the above-mentioned <Structural Example of Semiconductor Device>.

[0277] The conductor 246b is arranged on the conductor 242a included in the transistor 200b. In addition, the conductor 246b is arranged in a manner of contacting at least a portion of the top surface of the conductor 242a included in the transistor 200b. In addition, the conductor 246b has a convex shape portion in a region overlapping with the conductor 242a included in the transistor 200b. The conductor 246b is used as wiring.

[0278] The conductor 246c is disposed on the conductor 242a included in the transistor 200a. The conductor 246c is disposed in contact with at least a portion of the top surface of the conductor 242a included in the transistor 200a. The conductor 246c has a convex shape in a region overlapping with the conductor 242a included in the transistor 200a.

[0279] Note that the materials and structures of the conductors 246 b and 246 c can refer to the contents described in the above-mentioned <Structural example of semiconductor device>.

[0280] The conductor 262a is disposed on the conductor 260 included in the transistor 200a. The conductor 262a is disposed so as to be in contact with the top surface of the conductor 260 included in the transistor 200a. The conductor 262a is used as a wiring.

[0281] The conductor 262a preferably has a two-layer structure of a conductor 262a_1 and a conductor 262a_2 on the conductor 262a_1. For example, the conductor 262a_1 is preferably arranged so as to surround the bottom and side surfaces of the conductor 262a_2. Fig. 13B The middle conductor 262a has a two-layer structure of a conductor 262a_1 and a conductor 262a_2, but may also have a single-layer structure or a stacked-layer structure of three or more layers.

[0282] The conductor 262c is disposed on the conductor 260 included in the transistor 200b. The conductor 262c is disposed so as to be in contact with the top surface of the conductor 260 included in the transistor 200b.

[0283] The conductor 262c preferably has a two-layer structure of a conductor 262c_1 and a conductor 262c_2 on the conductor 262c_1. For example, the conductor 262c_1 is preferably arranged so as to surround the bottom and side surfaces of the conductor 262c_2. Fig. 13B The middle conductor 262c has a two-layer structure of a conductor 262c_1 and a conductor 262c_2, but may also have a single-layer structure or a stacked-layer structure of three or more layers.

[0284] like Fig. 13B As shown, the top surface height of the conductor 262a is consistent with the top surface heights of the conductor 262c and the insulator 285.

[0285] As the conductor 262a_1 and the conductor 262c_1, it is preferable to use a conductive material having a function of suppressing the diffusion of impurities such as hydrogen atoms, hydrogen molecules, water molecules, nitrogen atoms, nitrogen molecules, nitrogen oxide molecules, copper atoms, etc. In addition, it is preferable to use a conductive material having a function of suppressing the diffusion of oxygen (for example, at least one of oxygen atoms and oxygen molecules).

[0286] When the conductors 262a_1 and 262c_1 have a function of suppressing the diffusion of oxygen, it is possible to suppress the decrease in conductivity caused by oxidation of the conductors 262a_2 and 262c_2 by oxygen contained in the insulator 285. As a conductive material having a function of suppressing the diffusion of oxygen, for example, titanium, titanium nitride, tantalum, tantalum nitride, ruthenium, or ruthenium oxide can be used.

[0287] In addition, since the conductor 262a is used as wiring, it is preferable to use a conductor with high conductivity. For example, the conductor 262a_2 can use a conductive material with tungsten, copper or aluminum as a main component. In addition, the conductor 262a_2 can have a laminated structure, for example, a laminated structure of titanium or titanium nitride and the above conductive material. In addition, the conductor 262c_2 is the same.

[0288] Note that the materials and structures of the conductors 262a and 262c can refer to the contents described in the above-mentioned <Structural example of semiconductor device>.

[0289] [Materials constituting semiconductor devices] Hereinafter, constituent materials that can be used for semiconductor devices will be described.

[0290] <<Substrate>> As a substrate for forming the transistor 200, for example, an insulator substrate, a semiconductor substrate, or a conductor substrate can be used. As an insulator substrate, for example, a glass substrate, a quartz substrate, a sapphire substrate, a stabilized zirconia substrate (yttria stabilized zirconia substrate, etc.), a resin substrate, etc. can be cited. In addition, as a semiconductor substrate, for example, a semiconductor substrate made of silicon or germanium, etc., or a compound semiconductor substrate composed of silicon carbide, silicon germanium, gallium arsenide, indium phosphide, zinc oxide, or gallium oxide can be cited. In addition, a semiconductor substrate having an insulator region inside the above-mentioned semiconductor substrate can also be cited, such as an SOI (Silicon On Insulator; Silicon on Insulator) substrate, etc. As a conductor substrate, a graphite substrate, a metal substrate, an alloy substrate, a conductive resin substrate, etc. can be cited. Alternatively, a substrate containing a metal nitride, a substrate containing a metal oxide, etc. can be cited. In addition, an insulator substrate provided with a conductor or a semiconductor, a semiconductor substrate provided with a conductor or an insulator, a conductor substrate provided with a semiconductor or an insulator, etc. can also be cited. Alternatively, a substrate having an element provided on these substrates can also be used. Examples of the element provided over the substrate include a capacitor, a resistor, a switching element, a light emitting element, and a memory element.

[0291] <<Insulator>> Examples of the insulator include oxides, nitrides, oxynitrides, oxynitrides, metal oxides, metal oxynitrides, and metal oxynitrides having insulating properties.

[0292] For example, when miniaturization and high integration of transistors are being carried out, problems such as leakage current may occur due to the thin filming of the gate insulator. By using a high-k material as an insulator used as a gate insulator, it is possible to achieve low voltage when the transistor is operating while maintaining the physical thickness. On the other hand, by using a material with a low relative dielectric constant for an insulator used as an interlayer film, it is possible to reduce the parasitic capacitance generated between wirings. Therefore, it is preferable to select a material according to the function of the insulator.

[0293] Examples of insulators having a relatively high dielectric constant include gallium oxide, hafnium oxide, zirconium oxide, oxides containing aluminum and hafnium, oxynitrides containing aluminum and hafnium, oxides containing silicon and hafnium, oxynitrides containing silicon and hafnium, and nitrides containing silicon and hafnium.

[0294] Examples of insulators having a relatively low relative dielectric constant include silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, silicon oxide added with fluorine, silicon oxide added with carbon, silicon oxide added with carbon and nitrogen, and silicon oxide or resin having pores.

[0295] In addition, by surrounding a transistor using a metal oxide with an insulator having the function of inhibiting the permeation of impurities such as hydrogen and oxygen, the electrical characteristics of the transistor can be stabilized. As an insulator having the function of inhibiting the permeation of impurities such as hydrogen and oxygen, for example, a single layer or a stack of insulators containing boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium or tantalum can be used. Specifically, as an insulator having the function of inhibiting the permeation of impurities such as hydrogen and oxygen, metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, tantalum oxide, and metal nitrides such as aluminum nitride, silicon oxynitride, and silicon nitride can be used.

[0296] In addition, the insulator used as the gate insulator is preferably an insulator having a region containing oxygen that is released by heating. For example, by using a structure in which silicon oxide or silicon oxynitride having a region containing oxygen that is released by heating is in contact with the oxide 230, the oxygen vacancies contained in the oxide 230 can be filled.

[0297] <<Conductor>> As the conductor, it is preferred to use a metal element selected from aluminum, chromium, copper, silver, gold, platinum, tantalum, nickel, titanium, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium, ruthenium, iridium, strontium and lanthanum, an alloy with the above metal elements as a component, or an alloy combining the above metal elements, etc. For example, it is preferred to use tantalum nitride, titanium nitride, tungsten, a nitride containing titanium and aluminum, a nitride containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, an oxide containing strontium and ruthenium, an oxide containing lanthanum and nickel, etc. In addition, tantalum nitride, titanium nitride, a nitride containing titanium and aluminum, a nitride containing tantalum and aluminum, ruthenium oxide, ruthenium nitride, an oxide containing strontium and ruthenium, and an oxide containing lanthanum and nickel are conductive materials that are not easily oxidized or materials that absorb oxygen and still maintain conductivity, so they are preferred. Alternatively, a semiconductor having high conductivity, such as polycrystalline silicon containing an impurity element such as phosphorus, or silicide such as nickel silicide may be used.

[0298] In addition, a plurality of conductive layers formed of the above-mentioned materials may be stacked. For example, a laminated structure in which a material containing the above-mentioned metal element and a conductive material containing oxygen are combined may be used. In addition, a laminated structure in which a material containing the above-mentioned metal element and a conductive material containing nitrogen are combined may be used. In addition, a laminated structure in which a material containing the above-mentioned metal element, a conductive material containing oxygen, and a conductive material containing nitrogen are combined may be used.

[0299] In addition, when an oxide is used in the channel formation region of the transistor, a laminated structure combining a material containing the above-mentioned metal element and a conductive material containing oxygen is preferably used as a conductor used as a gate electrode. In this case, the conductive material containing oxygen is preferably arranged on one side of the channel formation region. By arranging the conductive material containing oxygen on one side of the channel formation region, oxygen separated from the conductive material is easily supplied to the channel formation region.

[0300] In particular, as a conductor used as a gate electrode, it is preferable to use a conductive material containing a metal element contained in a metal oxide in which a channel is formed and oxygen. In addition, a conductive material containing the above-mentioned metal element and nitrogen can also be used. For example, a conductive material containing nitrogen such as titanium nitride and tantalum nitride can be used. In addition, indium tin oxide, indium oxide containing tungsten oxide, indium zinc oxide containing tungsten oxide, indium oxide containing titanium oxide, indium tin oxide containing titanium oxide, indium zinc oxide, and indium tin oxide added with silicon can also be used. In addition, indium gallium zinc oxide containing nitrogen can also be used. By using the above-mentioned materials, hydrogen contained in the metal oxide in which a channel is formed can sometimes be captured. Alternatively, hydrogen mixed from an external insulator can sometimes be captured.

[0301] [Modification Example of Memory Cell 100] Below, refer to Fig. 14B A configuration example different from that of the memory cell 100 shown in FIG. 13 will be described.

[0302] Fig. 14B A modified example of the memory cell 100 shown in FIG. 13 is shown. Fig. 14B is a cross-sectional view of a semiconductor device including the memory cell 100 . Fig. 14B The memory cell 100 shown in FIG. 13 differs from the transistor 200 shown in FIG. 13 in that it includes an insulator 254 a , an insulator 254 b , an insulator 212 , and an insulator 247 .

[0303] The insulator 254a is located between the insulator 250a and the conductor 260. Specifically, the insulator 254a is disposed in the recess of the insulator 250a. In addition, the insulator 254a is disposed in a manner in contact with the side surface and the bottom surface of the conductor 260. In this structure, it can also be said that the insulator 254a has a recess. In addition, the height of the uppermost portion of the insulator 254a is consistent with the height of the uppermost portion of the insulator 275a and the uppermost portion of the insulator 250a.

[0304] The insulator 254a is used as a part of the gate insulator. As the insulator 254a, a hydrogen blocking insulating film is preferably used. Thus, it is possible to suppress the diffusion of impurities such as hydrogen contained in the conductor 260 into the oxide 230_2. As the insulator 254a, for example, silicon nitride is preferably used. In addition, for example, as the insulator 254a, silicon nitride deposited by the PEALD method is preferably used. In this case, the insulator 254a contains at least nitrogen and silicon. Alternatively, as the insulator 254a, for example, aluminum oxide, magnesium oxide, hafnium oxide, gallium oxide, indium gallium zinc oxide or silicon oxynitride may be used. The insulator 254a may be, for example, less permeable to hydrogen than the insulator 250a. In addition, as the insulator 254a, for example, a material that is less permeable to hydrogen than the insulator 250a may be used.

[0305] In addition, the insulator 254 a may also have oxygen barrier properties, thereby preventing oxygen contained in the insulator 254 a from diffusing into the conductor 260 .

[0306] In addition, the insulator 254a needs to be provided in the openings provided by the oxide 230 and the conductor 242a together with the insulator 275a, the insulator 250a and the conductor 260. In order to realize the miniaturization of the transistor, the thickness of the insulator 254a is preferably small. The thickness of the insulator 254a is greater than 0.1 nm and less than 5.0 nm, preferably greater than 0.5 nm and less than 3.0 nm, and more preferably greater than 1.0 nm and less than 3.0 nm. At this time, at least a portion of the insulator 254a is a region having the above thickness. In addition, the thickness of the insulator 254a is preferably smaller than the thickness of the insulator 250a. At this time, at least a portion of the insulator 254a is a region having a thickness less than that of the insulator 250a.

[0307] In a plan view, the insulator 254b is arranged outside the oxide 230 and the conductor 242a (on the side of the insulator 275b). In addition, the insulator 254b is located between the insulator 250b and the insulator 274. Specifically, the insulator 254b is arranged in contact with the top surface of the insulator 250b. In addition, the insulator 254b is arranged in contact with the side surface and the bottom surface of the insulator 274.

[0308] The insulator 254a and the insulator 254b are formed in the same process. Therefore, the insulator 254a includes the same insulating material as the insulator 254b. In addition, the thickness of the insulator 254a is equal to the thickness of the insulator 254b.

[0309] The insulator 247 is located between the conductor 262a and the insulator 277c, the insulator 278, and the insulator 285. In addition, the insulator 247 is located between the conductor 262c and the insulator 277b, the insulator 278, and the insulator 285. In addition, the insulator 247 is provided in contact with the side surface of the conductor 262a or the conductor 262c.

[0310] The insulator 247 is preferably used as a blocking insulating film to suppress the diffusion of impurities such as water and hydrogen into the conductor 262a or the conductor 262c. Thus, it is possible to suppress the diffusion of impurities such as hydrogen in the insulator 285 into the oxide 230_2 via the conductor 262a or the conductor 262c. As the insulator 247, an insulator that can be used for the insulator 254a can be used. For example, as the insulator 247, silicon nitride deposited by the PEALD method can be used. In this case, the insulator 247 contains at least nitrogen and silicon.

[0311] In addition, an insulator made of the same material as the insulator 247 may be formed so as to cover the side surface of the region of the conductor 260 exposed from the insulator 276 .

[0312] The insulator 212 is disposed on a substrate (not shown) and is located below the insulator 216 and the conductor 244 .

[0313] The insulator 212 is used as an interlayer film. The insulator 212 is preferably used as a blocking insulating film for suppressing diffusion of impurities such as water and hydrogen from the substrate side to the transistor 200. By providing the insulator 212, diffusion of impurities such as water and hydrogen from the substrate side to the transistor 200 side can be suppressed.

[0314] As the insulator 212, the insulator that can be used as the insulator 254a can be used. For example, as the insulator 212, it is preferable to use a nitride containing silicon such as silicon nitride or silicon nitride oxide. Specifically, as the insulator 212, silicon nitride deposited by sputtering can be used. By depositing the insulator 212 by sputtering, high-density silicon nitride can be formed. In addition, as the insulator 212, silicon nitride deposited by PEALD or CVD can also be stacked on the silicon nitride deposited by sputtering.

[0315] <Method for manufacturing semiconductor device> Next, use FIG. 15A1 to FIG. 22B2 illustrate FIG. 13A to FIG. 13D A method for manufacturing a semiconductor device is shown.

[0316] exist FIG. 15A1 to FIG. 22B2 In the drawings, A1 and B1 are top views. A2 and B2 are cross-sectional views of portions along dashed lines A1-A2 in A1 and B1 in the drawings, respectively. For clarity, some components are omitted in the top views of A1 and B1 in the drawings.

[0317] Hereinafter, an insulating material for forming an insulator, a conductive material for forming a conductor, or a semiconductor material for forming a semiconductor can be appropriately deposited using a plating method, a sputtering method, a CVD method, an MBE method, a PLD method, an ALD method, or the like.

[0318] As the sputtering method, there can be cited an RF sputtering method using a high frequency power supply as a sputtering power supply and a DC sputtering method using a direct current power supply. As the DC sputtering method, there is also a pulsed DC sputtering method in which the voltage applied to the electrode is changed in a pulsed manner. The RF sputtering method is mainly used when depositing an insulating film, and the DC sputtering method is mainly used when depositing a metal conductive film. In addition, the pulsed DC sputtering method is mainly used when depositing compounds such as oxides, nitrides, and carbides using a reactive sputtering method.

[0319] Note that the CVD method can be classified into a plasma enhanced CVD (PECVD) method using plasma, a thermal CVD (TCVD: Thermal CVD) method using heat, or a photo CVD (Photo CVD) method using light, etc. Furthermore, it can be classified into a metal CVD (MCVD: Metal CVD) method or an organic metal CVD (MOCVD: Metal Organic CVD) method according to the source gas used.

[0320] By utilizing the plasma CVD method, a high-quality film can be obtained at a lower temperature. In addition, since plasma is not used in the thermal CVD method, the plasma damage caused to the object to be processed can be reduced. For example, the wiring, electrodes, and components (transistors, capacitors, etc.) included in the semiconductor device sometimes generate charge accumulation (charge up) due to receiving charges from the plasma. At this time, the wiring, electrodes, and components included in the semiconductor device are sometimes damaged due to the accumulated charge. On the other hand, since the above-mentioned plasma damage does not occur in the case of the thermal CVD method without using plasma, the yield of the semiconductor device can be improved. In addition, in the thermal CVD method, plasma damage during deposition is not generated, so a film with fewer defects can be obtained.

[0321] As the ALD method, a thermal ALD method in which a precursor and a reactant are reacted using only thermal energy, a PEALD method using a reactant excited by plasma, or the like is used.

[0322] The CVD method and the ALD method are different from the sputtering method in which particles released from a target material or the like are deposited. Therefore, the CVD method and the ALD method are deposition methods that are not easily affected by the shape of the object to be processed and have good step coverage. In particular, the ALD method has good step coverage and thickness uniformity, so the ALD method is suitable for forming a film covering the surface of an opening with a high aspect ratio. However, the deposition rate of the ALD method is relatively slow, so it is sometimes preferred to use it in combination with other deposition methods such as the CVD method with a fast deposition rate.

[0323] In addition, when the CVD method is used, a film of any composition can be deposited by adjusting the flow ratio of the source gas. For example, when the CVD method is used, a film whose composition continuously changes can be deposited by changing the flow ratio of the source gas while performing deposition. When deposition is performed while changing the flow ratio of the source gas, since the time required for conveying or adjusting the pressure is not required, the deposition time can be shortened compared to the case where formation is performed using a plurality of deposition chambers. Therefore, the productivity of the semiconductor device can sometimes be improved.

[0324] When the ALD method is used, a film of any composition can be deposited by introducing different precursors at the same time. Alternatively, when introducing different precursors, a film of any composition can be deposited by controlling the number of cycles of each precursor.

[0325] First, a substrate (not shown) is prepared, and an insulator 216 (not shown) is deposited on the substrate. The insulator 216 is preferably deposited using a sputtering method. By using a sputtering method that does not require the use of molecules containing hydrogen as a deposition gas, the hydrogen concentration in the insulator 216 can be reduced.

[0326] In this embodiment, silicon oxide is deposited by pulse DC sputtering using a silicon target in an atmosphere containing oxygen as the insulator 216. By using pulse DC sputtering, the thickness can be made more uniform, thereby improving the sputtering rate, deposition speed, and film quality.

[0327] In Settings Fig. 14B In the case of the insulator 212 shown, the insulator 212 and the insulator 216 are preferably deposited continuously without being exposed to the atmosphere. For example, a multi-chamber deposition apparatus can be used. In this way, the insulator 212 and the insulator 216 can be deposited while reducing the hydrogen in the film, and the mixing of hydrogen into the film between each deposition step can be suppressed.

[0328] Next, an opening is formed in the insulator 216. The opening includes, for example, a groove and a slit. Sometimes, the region where the opening is formed is referred to as an opening portion. When forming the opening, a wet etching method can be used, but a dry etching method is preferable for micro-machining.

[0329] As a dry etching device, a capacitively coupled plasma (CCP: Capacitively Coupled Plasma) etching device including parallel plate electrodes can be used. The capacitively coupled plasma etching device including parallel plate electrodes can also adopt a structure in which a high-frequency voltage is applied to one of the parallel plate electrodes. Alternatively, a structure in which multiple different high-frequency voltages are applied to one of the parallel plate electrodes can be adopted. Alternatively, a structure in which a high-frequency voltage with the same frequency is applied to each of the parallel plate electrodes can be adopted. Alternatively, a structure in which a high-frequency voltage with different frequencies is applied to each of the parallel plate electrodes can be adopted. Alternatively, a dry etching device with a high-density plasma source can be used. For example, as a dry etching device with a high-density plasma source, an inductively coupled plasma (ICP: Inductively Coupled Plasma) etching device or the like can be used.

[0330] In addition, an insulator used as an etching stop film when etching the insulator 216 to form an opening is preferably provided in contact with the bottom surface of the insulator 216. For example, when silicon oxide or silicon oxynitride is used as the insulator 216 for forming the opening, the insulator is preferably silicon nitride, aluminum oxide, or hafnium oxide. For example, the insulator may also be provided Fig. 14B Insulator 212 is shown. In other words, insulator 212 preferably has this function.

[0331] After the opening is formed, a conductive film is deposited to become the conductor 244_1. The conductive film preferably includes a conductor having a function of inhibiting oxygen transmission. For example, tantalum nitride, tungsten nitride, or titanium nitride can be used. Alternatively, a laminated film of a conductor having a function of inhibiting oxygen transmission and tantalum, tungsten, titanium, molybdenum, aluminum, copper, or a molybdenum-tungsten alloy can be used.

[0332] In this embodiment, a titanium nitride film is deposited as a conductive film to be the conductor 244_1. By providing the above-mentioned metal nitride below the conductor 244_2, it is possible to suppress the conductor 244_2 from being oxidized by the insulator 216 and the like. In addition, even if a metal that easily diffuses, such as copper, is used as the conductor 244_2, it is possible to prevent the metal from diffusing outward from the conductor 244_1.

[0333] Next, a conductive film to be the conductor 244_2 is deposited. As the conductive film, tantalum, tungsten, titanium, molybdenum, aluminum, copper, or a molybdenum-tungsten alloy can be used. In this embodiment, a tungsten film is deposited as the conductive film.

[0334] Next, the conductive film to be the conductor 244_1 and the conductive film to be the conductor 244_2 are partially removed by CMP treatment to expose the insulator 216. As a result, the conductor 244_1 and the conductor 244_2 remain only in the opening formed in the insulator 216, thereby forming the conductor 244 (the conductor 244_1 and the conductor 244_2). In some cases, a portion of the insulator 216 is removed by this CMP treatment.

[0335] Next, an oxide film 230_1A, an oxide film 230_2A, and an oxide film 230_3A are sequentially deposited on the insulator 216 and the conductor 244 (see Fig.15A1 and Fig.15A2 ). It is preferred that the oxide film 230_1A, the oxide film 230_2A, and the oxide film 230_3A are continuously deposited without being exposed to the atmosphere. By performing the deposition without being exposed to the atmosphere, impurities or moisture from the atmosphere can be prevented from being attached to the oxide film 230_1A and the oxide film 230_2A, so that the interface between the oxide film 230_1A and the oxide film 230_2A and the vicinity thereof, and the interface between the oxide film 230_2A and the oxide film 230_3A and the vicinity thereof can be kept clean.

[0336] For example, when the oxide film 230_1A, the oxide film 230_2A, and the oxide film 230_3A are deposited by sputtering, oxygen or a mixed gas of oxygen and a rare gas is used as the sputtering gas. By increasing the proportion of oxygen contained in the sputtering gas, the excess oxygen in the deposited oxide film can be increased. In addition, when the oxide film is deposited by sputtering, for example, a target such as the above-mentioned In-M-Zn oxide can be used.

[0337] When a metal oxide film to which nitrogen is added is deposited as the oxide film 230_1A and the oxide film 230_3A by sputtering, the metal oxide film to which nitrogen is added can be deposited even if the target does not contain nitrogen by including nitrogen gas in the sputtering gas. When the metal oxide film is deposited by adding nitrogen gas, the greater the nitrogen flow rate ratio, the higher the carrier mobility of the metal oxide film can be.

[0338] The nitrogen flow ratio can be appropriately set within a range of 10% to 100% according to the characteristics required by the oxide 230_1 and the oxide 230_3. At this time, for example, the sputtering gas can be a mixed gas of nitrogen gas and argon gas. In addition, the sputtering gas can be a mixed gas of nitrogen gas and oxygen gas, or a mixed gas of nitrogen gas, oxygen gas and argon gas.

[0339] Note that when a target material containing nitrogen is used as the target material, nitrogen need not be used as the sputtering gas even in the case of depositing a metal oxide film to which nitrogen is added.

[0340] When the sputtering gas of the oxide film 230_1A contains oxygen gas, part of the oxygen contained in the sputtering gas may be supplied to the insulator 216. Therefore, the ratio of oxygen contained in the sputtering gas may be 70% or more, preferably 80% or more, and more preferably 100%.

[0341] The sputtering gas is preferably highly purified. For example, as the sputtering gas, oxygen gas, nitrogen gas or argon gas, a high-purity gas having a dew point of -40°C or less, preferably -80°C or less, more preferably -100°C or less, and further preferably -120°C or less is used, thereby preventing moisture and the like from mixing into the metal oxide film as much as possible.

[0342] In the case of forming the oxide film 230_2A by sputtering, when the deposition is performed under the condition that the ratio of oxygen contained in the sputtering gas is greater than 30% and less than 100%, preferably greater than 70% and less than 100%, an oxygen-excess oxide semiconductor is formed. A transistor using an oxygen-excess oxide semiconductor in a channel formation region can obtain relatively high reliability. Note that one embodiment of the present invention is not limited to this. In the case of forming the oxide film 230_2A by sputtering, when the deposition is performed under the condition that the ratio of oxygen contained in the sputtering gas is set to greater than 1% and less than 30%, preferably greater than 5% and less than 20%, an oxygen-deficient oxide semiconductor is formed. A transistor using an oxygen-deficient oxide semiconductor in a channel formation region can have a higher field effect mobility. In addition, by performing deposition while heating the substrate, the crystallinity of the oxide film can be improved.

[0343] Regarding the deposition method of the oxide film 230_3A, the deposition method of the oxide film 230_1A may be referred to.

[0344] Note that the oxide film 230_1A, the oxide film 230_2A, and the oxide film 230_3A are preferably deposited by sputtering without being exposed to the atmosphere. For example, a multi-chamber deposition apparatus may be used. Thus, hydrogen can be prevented from entering the oxide film 230_1A, the oxide film 230_2A, and the oxide film 230_3A between deposition steps.

[0345] In addition, when a metal oxide film to which nitrogen is added is deposited by sputtering as the oxide film 230_1A and the oxide film 230_3A and a metal oxide film is deposited by sputtering as the oxide film 230_2A, the type of gas introduced into the sputtering device is switched after the oxide film 230_1A is deposited, that is, the introduction of nitrogen is stopped to deposit the oxide film 230_2A. Also, the type of gas introduced into the sputtering device is switched after the oxide film 230_2A is deposited, that is, nitrogen is introduced to deposit the oxide film 230_3A. Thus, the oxide film 230_1A, the oxide film 230_2A, and the oxide film 230_3A can be deposited continuously, which is suitable for mass production.

[0346] In this embodiment, a metal oxide film to which nitrogen is added is deposited by sputtering as the oxide film 230_1A and the oxide film 230_3A. In addition, the oxide film 230_2A is deposited by sputtering using an oxide target with In:Ga:Zn=4:2:4.1 [atomic ratio], an oxide target with In:Ga:Zn=1:1:1 [atomic ratio], an oxide target with In:Ga:Zn=1:1:1.2 [atomic ratio], or an oxide target with In:Ga:Zn=1:1:2 [atomic ratio]. Each oxide film can be formed by appropriately selecting deposition conditions and atomic ratios according to the characteristics required for the oxide 230_1, the oxide 230_2, and the oxide 230_3.

[0347] Next, heat treatment is preferably performed. The heat treatment can be performed within a temperature range where polycrystallization does not occur in the oxide film 230_1A, the oxide film 230_2A, and the oxide film 230_3A, and can be performed at a temperature above 250°C and below 650°C, preferably above 400°C and below 600°C. In addition, the heat treatment is performed in an atmosphere of nitrogen gas or an inert gas or in an atmosphere containing an oxidizing gas of more than 10 ppm, more than 1%, or more than 10%. For example, when heat treatment is performed in a mixed atmosphere of nitrogen gas and oxygen gas, the proportion of oxygen gas can be set to about 20%. In addition, the heat treatment can also be performed under reduced pressure. Alternatively, the heat treatment can also be performed in an atmosphere of nitrogen gas or an inert gas, and then heat treatment is performed in an atmosphere containing an oxidizing gas of more than 10 ppm, more than 1%, or more than 10% to fill the separated oxygen.

[0348] In addition, the gas used in the above heat treatment is preferably highly purified. For example, the amount of water contained in the gas used in the above heat treatment is 1 ppb or less, preferably 0.1 ppb or less, and more preferably 0.05 ppb or less. By using highly purified gas for heat treatment, it is possible to prevent moisture and the like from being absorbed by the oxide film 230_1A, the oxide film 230_2A, and the oxide film 230_3A as much as possible.

[0349] In this embodiment, as a heat treatment, a treatment is performed for 1 hour under the conditions of a flow ratio of nitrogen gas to oxygen gas of 4:1 and a temperature of 400°C. Such a heat treatment including oxygen gas can reduce impurities such as carbon, water, and hydrogen in the oxide film 230_2A. By reducing the impurities in the film in this way, the crystallinity of the oxide film 230_2A is improved, and a denser structure with a higher density can be achieved. Therefore, the crystallized area in the oxide film 230_2A can be increased, and the in-plane unevenness of the crystallized area in the oxide film 230_2A can be reduced. Therefore, the in-plane unevenness of the electrical characteristics of the transistor 200 can be reduced.

[0350] In addition, by performing heat treatment, the hydrogen concentration in the insulator 216 and the oxide film 230_2A can be reduced. In particular, the oxide 230_2 formed of the oxide film 230_2A is used as a channel formation region of the transistor 200. Therefore, the transistor 200 including the oxide 230_2 with reduced hydrogen concentration has excellent reliability and is therefore preferred.

[0351] Next, a conductive film 242A is deposited on the oxide film 230_3A (see Fig.15A1 and Fig.15A2 ). For example, a tantalum nitride film may be deposited as the conductive film 242A by sputtering. In addition, heat treatment may be performed before depositing the conductive film 242A. The heat treatment may also be performed under reduced pressure, wherein the conductive film 242A is continuously deposited without being exposed to the atmosphere. By performing such treatment, moisture and hydrogen attached to the surface of the oxide film 230_3A may be removed, and the moisture concentration and hydrogen concentration in the oxide film 230_1A, the oxide film 230_2A, and the oxide film 230_3A may be reduced. The temperature of the heat treatment is preferably above 100°C and below 400°C. In this embodiment, the temperature of the heat treatment is set to 200°C.

[0352] Next, an insulating film 291A is deposited on the conductive film 242A (see Fig.15A1 and Fig.15A2 As the insulating film 291A, it is preferable to use an insulating film having a function of suppressing the permeation of oxygen. For example, as the insulating film 291A, an aluminum oxide film or a silicon nitride film may be deposited by a sputtering method.

[0353] The conductive film 242A and the insulating film 291A are preferably deposited by sputtering without being exposed to the atmosphere. For example, a multi-chamber deposition apparatus may be used. Thus, the conductive film 242A and the insulating film 291A can be deposited while reducing hydrogen in the film, and hydrogen can be prevented from being mixed into the film between each deposition step. In addition, when a hard mask is formed on the insulating film 291A, the film that becomes the hard mask can also be continuously deposited without being exposed to the atmosphere.

[0354] Next, the oxide film 230_1A, the oxide film 230_2A, the oxide film 230_3A, the conductive film 242A, and the insulating film 291A are processed into a hollow cylindrical shape by photolithography to form the oxide 230 (the oxide 230_1, the oxide 230_2, and the oxide 230_3), the conductor 242a, and the insulator 291. Here, the oxide 230_1, the oxide 230_2, the oxide 230_3, the conductor 242a, and the insulator 291 are formed so that at least a part thereof overlaps with the conductor 244. The above processing can be performed by a dry etching method or a wet etching method.

[0355] Note that in photolithography, first, the resist is exposed through a mask. Then, a developer is used to remove or leave the exposed area to form a resist mask. Then, the conductor, semiconductor or insulator can be processed into a desired shape by etching through the resist mask. For example, a resist can be exposed using a KrF excimer laser, an ArF excimer laser, an EUV light, etc. to form a resist mask. In addition, an immersion technique in which a liquid (e.g., water) is filled between the substrate and the projection lens for exposure can also be used. In addition, an electron beam or an ion beam can also be used instead of the above light. Note that when an electron beam or an ion beam is used, a mask is not required. In addition, the resist mask can be removed by performing a dry etching process such as ashing, performing a wet etching process, performing a wet etching process after a dry etching process, or performing a dry etching process after a wet etching process.

[0356] Furthermore, a hard mask made of an insulator or a conductor may be used under the resist mask. When a hard mask is used, an insulating film or a conductive film serving as a hard mask material may be formed on the conductive film 242A and a resist mask may be formed thereon, and then the hard mask material may be etched to form a hard mask of a desired shape. The etching of the conductive film 242A etc. may be performed after removing the resist mask or without removing the resist mask. In the case of the latter, the resist mask sometimes disappears during etching. The hard mask may be removed by etching after etching the conductive film 242A etc. On the other hand, when the hard mask material does not affect the subsequent process or can be used in the subsequent process, it is not necessarily necessary to remove the hard mask. In this embodiment, the insulator 291 is used as a hard mask.

[0357] Hereinafter, an example of a method of forming the oxide 230 (the oxide 230_1 , the oxide 230_2 , and the oxide 230_3 ), the conductor 242 a , and the insulator 291 having a hollow cylindrical shape by photolithography will be described.

[0358] First, a resist mask 292 (see Fig.15A1 and Fig.15A2 ). At least a portion of the resist mask 292 is provided on a region overlapping with the conductor 244 .

[0359] Note that the top surface of the resist mask 292 is circular, but the present invention is not limited thereto, and for example, the top surface may also have an elliptical shape, a polygonal shape such as a triangle or a quadrangle. In addition, when the top surface has a polygonal shape, the polygonal shape may also have rounded corners.

[0360] For example, the resist is exposed through a mask, and a developer is used to remove or leave the exposed area, thereby forming the resist mask 292. Note that the resist mask 292 can also be shrunk by isotropic etching using oxygen plasma. Shrinking the resist mask is sometimes called resist-slimming or resist-trimming. By shrinking the resist mask 292, the resist mask 292 can be miniaturized.

[0361] Alternatively, for example, the resist mask 292 may be formed by exposing the resist through a mask capable of forming a line pattern, exposing the resist again through the mask rotated 90 degrees about the Z axis, and removing or leaving the exposed area using a developer. Through this processing, the top surface of the resist mask 292 becomes a rounded shape or a circular shape.

[0362] When forming the resist mask 292, it is preferable to use the above-mentioned multiple imaging technique. For example, the resist mask 292 may be formed by forming a resist mask having a line pattern extending in the X direction using the multiple imaging technique, and processing the resist mask having a line pattern extending in the X direction using the multiple imaging technique for forming a resist mask having a line pattern extending in the Y direction. Through this processing, the top surface shape of the resist mask 292 becomes a rounded shape or a circular shape.

[0363] Next, an insulating film 293A is deposited on the resist mask 292 (see Fig.15A1 and Fig.15A2 ). The thickness of the insulating film 293A is equivalent to Fig.13D Therefore, the thickness of the insulating film 293A may be appropriately set according to the design of the transistor 200 .

[0364] Next, the insulating film 293A is anisotropically etched to form the insulator 293 (see Fig.15B1 and Fig.15B2As anisotropic etching of the insulating film 293A, for example, a dry etching method can be used. By anisotropic etching of the insulating film 293A, an insulator 293 is formed on the side of the resist mask 292. That is, the insulator 293 can be called a side wall.

[0365] Next, the resist mask 292 is removed (see Fig.15B1 and Fig.15B2 ). By removing the resist mask 292, the insulator 293 remains on the insulating film 291A. Note that the top surface shape of the opening of the insulator 293 corresponds to the top surface shape of the resist mask 292. For example, when the top surface of the resist mask 292 has a circular shape, as shown in FIG. Fig.15B1 As shown, the top surface of the insulator 293 is a hollow cylindrical shape. In addition, when the top surface shape of the resist mask 292 is the above-mentioned elliptical shape, the top surface of the insulator 293 is a hollow elliptical shape. In addition, when the top surface shape of the resist mask 292 is the above-mentioned polygonal shape with rounded corners, the top surface of the insulator 293 is a hollow polygonal shape with rounded corners.

[0366] Next, using the insulator 293 as a hard mask, a portion of the insulating film 291A, a portion of the conductive film 242A, a portion of the oxide film 230_3A, a portion of the oxide film 230_2A, and a portion of the oxide film 230_1A are processed until the top surfaces of the insulator 216 and the conductive body 244 are exposed (see Fig.16A1 and Fig.16A2 ). As the above-mentioned processing, dry etching or wet etching can be used. Processing using the dry etching method is suitable for micro-processing. In addition, the insulating film 291A, the conductive film 242A, the oxide film 230_3A, the oxide film 230_2A, and the oxide film 230_1A can also be processed under different conditions.

[0367] By performing the above processing, the insulator 291, the conductor 242a, and the oxide 230 (the oxide 230_3, the oxide 230_2, and the oxide 230_1) having the same or substantially the same top surface shape as the top surface shape of the insulator 293 are formed (see Fig.16A1 and Fig.16A2 ). That is, when viewed from above, the ends of the insulator 291, the conductor 242a, and the oxide 230 are aligned. In addition, the oxide 230, the conductor 242a, and the insulator 291 all become hollow cylindrical shapes. Note that, as described above, the top surface shapes of the oxide 230, the conductor 242a, and the insulator 291 correspond to the top surface shape of the resist mask 292. Therefore, the above-mentioned "hollow cylindrical shape" can be appropriately changed to various names according to the top surface shape of the resist mask 292.

[0368] An example of a method of forming the oxide 230 , the conductor 242 a , and the insulator 291 having a hollow cylindrical shape by photolithography has been described above.

[0369] It is also preferable to adopt a structure in which the side surfaces of the oxide 230 and the conductor 242a are perpendicular to the top surface of the insulator 216. With such a structure, when a plurality of transistors 200 are provided, a smaller area and higher density can be achieved.

[0370] Note that this is not limited to the above structure. Fig.11A As described above, the side surfaces of the oxide 230 and the conductor 242a may have a tapered shape. When the side surfaces have a tapered shape, the coverage of the insulating film or the like that becomes the insulator 275a in the subsequent process is improved, and defects such as voids can be reduced.

[0371] Next, the insulator 293 is removed (see Fig.16B1 and Figure 16B2 ).

[0372] In the above-described steps, impurities may sometimes adhere to the side surfaces of the oxide 230, the conductor 242a, and the insulator 291, or diffuse into the inside of them. In this case, a step of removing these impurities may be performed. Examples of such impurities include hafnium, aluminum, silicon, tantalum, fluorine, and chlorine.

[0373] In order to remove impurities attached to the side of the oxide 230 in the above-mentioned etching process, a cleaning process is performed. As a cleaning method, there are wet cleaning using a cleaning liquid or the like (which may also be referred to as a wet etching process), plasma treatment using plasma, cleaning using a heat treatment, etc., and the above cleanings may be appropriately combined. Note that due to this cleaning process, the above-mentioned groove portion may become deeper.

[0374] As wet cleaning, an aqueous solution, pure water or carbonated water, etc., obtained by diluting ammonia, oxalic acid, phosphoric acid or hydrofluoric acid with carbonated water or pure water, can be used. Alternatively, ultrasonic cleaning can be performed using the above-mentioned aqueous solution, pure water or carbonated water. In addition, the above-mentioned cleaning can also be appropriately combined.

[0375] Note that in this specification, etc., an aqueous solution of hydrofluoric acid diluted with pure water is sometimes referred to as dilute hydrofluoric acid, and an aqueous solution of ammonia diluted with pure water is sometimes referred to as dilute ammonia water. In addition, the concentration, temperature, etc. of the aqueous solution can be appropriately adjusted according to the impurities to be removed, the structure of the semiconductor device to be washed, etc. The ammonia concentration of the dilute ammonia water is set to be greater than 0.01% and less than 5%, preferably greater than 0.1% and less than 0.5%. In addition, the hydrogen fluoride concentration of the dilute hydrofluoric acid is set to be greater than 0.01ppm and less than 100ppm, preferably greater than 0.1ppm and less than 10ppm.

[0376] In addition, it is preferable to use a frequency of 200 kHz or more, and more preferably 900 kHz or more for ultrasonic cleaning. By using such a frequency, damage to the oxide 230 and the like can be reduced.

[0377] The above-mentioned washing treatment may be performed multiple times, and the washing liquid may be changed for each washing treatment. For example, the first washing treatment may be a treatment using dilute hydrofluoric acid or dilute ammonia water, and the second washing treatment may be a treatment using pure water or carbonated water.

[0378] In addition, heat treatment may be performed after the above-mentioned etching or the above-mentioned washing. The heat treatment may be performed at a temperature of 100°C or higher and 450°C or lower, preferably 350°C or higher and 400°C or lower. In addition, the heat treatment is performed in an atmosphere of nitrogen gas or an inert gas or an atmosphere containing an oxidizing gas of 10 ppm or higher, 1% or higher, or 10% or higher. For example, the heat treatment is preferably performed in an oxygen atmosphere. Thus, oxygen is supplied to the oxide 230_2, thereby reducing oxygen vacancies. In addition, by performing the above-mentioned heat treatment, the crystallinity of the oxide 230_2 may be improved. In addition, the heat treatment may also be performed under reduced pressure. Alternatively, the heat treatment may be performed in an oxygen atmosphere, and then the heat treatment may be continuously performed in a nitrogen atmosphere without being exposed to the atmosphere.

[0379] Note that the above-mentioned cleaning treatment and heat treatment may be performed before removing the insulator 293 .

[0380] Next, an insulating film 275A is deposited on the insulator 216, the conductor 244, and the insulator 291 (see Fig.16B1 and Figure 16B2 ). In other words, the insulating film 275A is deposited to cover the oxide 230 , the conductor 242 a , and the insulator 291 .

[0381] The insulating film 275A is preferably deposited using the ALD method. As described above, the insulating film 275A is preferably deposited thinly, and the thickness non-uniformity needs to be suppressed to a small value. In this regard, the ALD method is a deposition method that alternately introduces precursors and reactants (for example, oxidants, etc.). Since the thickness of the film can be adjusted by the number of times the cycle is repeated, the thickness can be precisely adjusted. In addition, as Fig.16B1 and Figure 16B2 As shown, the insulating film 275A needs to be deposited with high coverage on the side surfaces of the openings formed in the oxide 230, the conductor 242a, and the insulator 291, and on the top surfaces of the conductor 244 and the insulator 216. In particular, the insulating film 275A is preferably deposited with high coverage on the side surfaces of the oxide 230 and the side surfaces of the conductor 242a. Since the ALD method can deposit each atomic layer on the bottom surface and the side surfaces of the above-mentioned opening, the insulating film 275A can be deposited with high coverage in the opening.

[0382] When the insulating film 275A is deposited by the ALD method, ozone (O3), oxygen (O2), water (H2O), etc. can be used as an oxidant. By using ozone (O3), oxygen (O2), etc. that do not contain hydrogen as an oxidant, diffusion of hydrogen into the oxide 230 can be reduced.

[0383] As the insulating film 275A, it is preferable to use an insulating film having a function of suppressing the penetration of oxygen. For example, as the insulating film 275A, an aluminum oxide film can be deposited by the ALD method. In this way, the oxide 230 and the conductor 242a can be covered by the insulating film 275A having a function of suppressing the diffusion of oxygen. Thus, it is possible to suppress the direct diffusion of oxygen from the insulator 274 and the like to the oxide 230 and the conductor 242a in the subsequent process.

[0384] Then, microwave treatment can also be performed in an oxygen-containing atmosphere. Here, microwave treatment refers to, for example, treatment using a device including a power supply that generates high-density plasma using microwaves. In addition, in this specification, microwave refers to an electromagnetic wave with a frequency of more than 300 MHz and less than 300 GHz.

[0385] Microwave treatment, for example, preferably uses a microwave processing device that includes a power supply that generates high-density plasma using microwaves. Here, the frequency of the microwave processing device is set to be greater than 300 MHz and less than 300 GHz, preferably greater than 2.4 GHz and less than 2.5 GHz, for example, 2.45 GHz. By using high-density plasma, high-density oxygen free radicals can be generated. In addition, the power of the power supply that applies microwaves in the microwave processing device is greater than 1000 W and less than 10000 W, preferably greater than 2000 W and less than 5000 W. In addition, the microwave processing device may also include a power supply that applies RF to one side of the substrate. In addition, by applying RF to one side of the substrate, the oxygen ions generated by the high-density plasma can be efficiently introduced into the oxide 230_2.

[0386] In addition, the microwave treatment is preferably carried out under reduced pressure, and the pressure is 10Pa or more and 1000Pa or less, preferably 300Pa or more and 700Pa or less. In addition, the treatment temperature is 750°C or less, preferably 500°C or less, for example, about 400°C. In addition, it is also possible to continuously perform heat treatment without being exposed to the atmosphere after the oxygen plasma treatment. For example, it is heated to 100°C or more and 750°C or less, preferably 300°C or more and 500°C or less.

[0387] In addition, for example, the above-mentioned microwave treatment can be performed using oxygen gas and argon gas. Here, the oxygen flow ratio (O2 / (O2+Ar)) is greater than 0% and less than 100%, preferably greater than 0% and less than 50%, more preferably greater than 10% and less than 40%, and further preferably greater than 10% and less than 30%. In this way, by performing microwave treatment in an oxygen-containing atmosphere, the carrier concentration in the oxide 230_2 can be reduced. In addition, by preventing excessive oxygen from being introduced into the processing chamber during microwave treatment, the carrier concentration in the oxide 230_2 and the oxide 230_3 can be prevented from being excessively reduced.

[0388] By performing microwave treatment in an oxygen-containing atmosphere, microwaves or high frequencies such as RF can be used to convert oxygen gas into plasma and the oxygen plasma can be applied to oxide 230_2. At this time, microwaves or high frequencies such as RF can also be irradiated to oxide 230_2. In other words, high frequencies such as microwaves or RF or oxygen plasma can be applied to oxide 230_2. Through the action of plasma, microwaves, etc., V of oxide 230_2 can be reduced. O H is separated from the oxide 230_2 to remove hydrogen. In other words, the V contained in the oxide 230_2 can be reduced. O H. Therefore, the oxygen vacancies and V O H and reduce the carrier concentration. In addition, by supplying oxygen radicals generated in the above oxygen plasma or oxygen contained in the insulator 275a to oxygen vacancies formed in the oxide 230_2, oxygen vacancies in the oxide 230_2 can be further reduced, thereby reducing the carrier concentration.

[0389] In addition, an insulating film 275A having oxygen barrier properties is provided so as to be in contact with the side surface of the conductor 242a. Therefore, it is possible to suppress the formation of an oxide film on the side surface of the conductor 242a due to the microwave treatment.

[0390] Since the film quality of the insulating film 275A can be improved, the reliability of the transistor 200 is improved.

[0391] Next, an insulating film 250A is deposited on the insulating film 275A (see Fig.16B1 and Figure 16B2 ). The insulating film 250A preferably uses an insulator having a function of suppressing the diffusion of oxygen. By adopting such a structure, it is possible to suppress oxidation of the conductor 260 by oxygen contained in the oxide 230. For example, as the insulating film 250A, a hafnium oxide film can be deposited by a thermal ALD method.

[0392] When the above-mentioned microwave treatment is not performed after the insulating film 275A is deposited, it is preferable to continuously deposit the insulating film 275A and the insulating film 250A without exposing them to the atmosphere. By performing the deposition without exposing them to the atmosphere, impurities or moisture from the atmosphere can be prevented from adhering to the insulating film 275A, so that the interface between the insulating film 275A and the insulating film 250A and the vicinity thereof can be kept clean.

[0393] Next, an insulating film 274A is deposited on the insulating film 250A (see Fig.16B1 and Figure 16B2 ). For example, a silicon oxide film can be deposited as the insulating film 274A by a sputtering method. By using a sputtering method that does not require the use of molecules containing hydrogen as a deposition gas, the hydrogen concentration in the insulating film 274A can be reduced. In addition, heat treatment can be performed before depositing the insulating film 274A. In this embodiment, a silicon oxide film is deposited as the insulating film 274A by a CVD method.

[0394] Next, the insulating film 274A, the insulating film 250A, and the insulating film 275A are processed by CMP until the insulator 291 is exposed. By this CMP process, the insulating film 274A forms the insulator 274 and the insulator 274c, the insulating film 250A forms the insulator 250a and the insulator 250b, and the insulating film 275A forms the insulator 275a and the insulator 275b (see FIG. Fig.17A1 and Fig.17A2 ).

[0395] As described above, the oxide 230, the conductor 242a, and the insulator 291 all have a hollow cylindrical shape. That is, the laminate of the oxide 230, the conductor 242a, and the insulator 291 has a hollow cylindrical shape. The insulator 275a is provided in a manner in contact with the inner wall of the hollow portion of the laminate, the top surface of the insulator 216, and the top surface of the conductor 244, the insulator 250a is provided in a manner in contact with the inner wall and bottom surface of the recess formed in the insulator 275a, and the insulator 274c is provided in a manner embedded in the recess formed in the insulator 250a.

[0396] Insulator 275b is provided in contact with the outer side surface of the stack, the top surface of insulator 216, and the top surface of conductor 244. Insulator 250b is provided in contact with the top surface of insulator 275b, and insulator 274 is provided in contact with the top surface of insulator 250b.

[0397] Sometimes, a portion of the insulator 291 is removed by the above-mentioned CMP process.

[0398] The height of the top surface of the insulator 274 is consistent with the height of the top surface of each of the insulators 291 and 274c. In addition, the height of the topmost portion of each of the insulators 250a, 250b, 275a, and 275b is consistent.

[0399] Next, the insulator 291 is removed to expose the top surface of the conductor 242a (see Fig.17B1 and Figure 17B2 ) The insulator 291 may be removed by dry etching or wet etching.

[0400] By removing the insulator 291, the top surface of the conductor 242a can be exposed in a self-aligned manner. Therefore, the conductor 246b and the conductor 246c to be formed later can be arranged in a manner that they are in contact with the conductor 242a without alignment. When the insulator 291 is removed by etching, it is preferable to use an etching condition with a high selectivity ratio to prevent the insulator 274c from being removed by the etching. Thus, the insulator 274c can remain after the insulator 291 is removed.

[0401] Next, a conductive film to become the conductor 246b and the conductor 246c and an insulating film to become the insulator 277b and the insulator 277c are sequentially deposited. Next, a portion of the conductive film and a portion of the insulating film are processed by photolithography ( Fig.18A1 and Fig.18A2 ). Through this processing, the conductor 246b, the conductor 246c, the insulator 277b and the insulator 277c can be formed. At this time, the convex shape portion is formed in the area of ​​the conductor 246b overlapping with the conductor 242a and the area of ​​the conductor 246c overlapping with the conductor 242a. When performing this processing, wet etching can be used, but dry etching is preferred for micro-processing.

[0402] Next, an insulating film serving as the insulator 278 is deposited over the insulators 277b, 277c, and the insulator 274. This insulating film may be deposited using the same material as that of the insulating films serving as the insulators 277b and 277c, or may be deposited using a different material.

[0403] Next, the insulating film to be the insulator 278 is processed by CMP until the insulator 277b and the insulator 277c are exposed. The insulator 278 having a flattened top surface is formed by the CMP process. Note that the insulator 277b and the insulator 277c may be partially removed by the CMP process.

[0404] Next, an opening is formed in the region of the insulator 278 that overlaps with the insulator 274c, the insulator 250a, and the insulator 275a (see Figure 18B1 and Figure 18B2). In the case where the resist mask 292 is formed using the above-mentioned multiple imaging technique, the above-mentioned multiple imaging technique is also used when forming the opening in the insulator 278.

[0405] Next, an insulating film 276A is deposited on the insulator 274c, the insulator 250a, the insulator 275a, the insulator 277b, the insulator 277c, and the insulator 278 (see Fig.19A1 and Fig.19A2 ). The insulating film 276A is preferably deposited by the ALD method. The insulating film 276A needs to be deposited with high coverage on the bottom and side surfaces of the opening formed in the insulator 278. Since the ALD method can deposit each atomic layer on the bottom and side surfaces of the above-mentioned opening, the insulating film 276A can be deposited with high coverage in the opening. In this embodiment, a silicon nitride film is deposited as the insulating film 276A by the PEALD method.

[0406] Next, the insulating film 276A is anisotropically etched to form the insulator 276 (see Figure 19B1 and Figure 19B2 ). Due to the formation of the insulator 276, a portion of the top surface of the insulator 250a and the top surface of the insulator 274c are exposed.

[0407] As the anisotropic etching, for example, dry etching may be used. By providing the insulator 276 on the side wall of the opening, the physical distance between the conductor 246b or the conductor 246c and the conductor 260 to be formed later can be maintained. Therefore, the conductor 246b or the conductor 246c can be prevented from being electrically connected to the conductor 260. In other words, the conductor 246b or the conductor 246c can be prevented from being electrically connected to the conductor 260.

[0408] Next, the insulator 274c is removed (see Fig.20A1 and Fig.20A2 ) The insulator 274c may be removed by dry etching or wet etching.

[0409] When the insulator 274c is removed by etching, it is preferable to use etching conditions with a high selectivity ratio to prevent the insulator 250a and the insulator 276 from being removed by the etching. Thus, the insulator 250a and the insulator 276 can remain after the insulator 274c is removed.

[0410] Next, the conductive film 260_1A and the conductive film 260_2A are sequentially deposited (see Fig.20B1 and Figure 20B2 ). In this embodiment, a titanium nitride film is deposited as the conductive film 260_1A by an ALD method, and a tungsten film is deposited as the conductive film 260_2A by a CVD method.

[0411] Next, the conductive film 260_1A and the conductive film 260_2A are processed by CMP until the insulator 277b, the insulator 277c, and the insulator 278 are exposed, thereby forming the conductive body 260 (see Fig.21A1 and Fig.21A2 ). Thus, the conductor 260 is arranged so as to be embedded in the opening of the insulator 276 and the recess of the insulator 250a. That is, the conductor 260 is arranged so as to be embedded in the opening formed in the oxide 230 via the insulator 275a and the insulator 250a.

[0412] Note that Fig.21A2 In the embodiment, a portion of the conductive film 260_1A remains in the opening of the insulator 276 and the recess of the insulator 250a, thereby forming the conductive body 260, but the present invention is not limited to this. Depending on the conditions of the above-mentioned CMP treatment or the opening size or depth of the insulator 276, a portion of the conductive film 260_1A and a portion of the conductive film 260_2A may remain in the opening of the insulator 276 and the recess of the insulator 250a. In this case, the conductive body 260 has a stacked structure of a first conductive body formed by the conductive film 260_1A and a second conductive body formed by the conductive film 260_2A. In addition, as Fig.21A2 As shown, in the case where the conductive film 260_1A is left only in the opening of the insulator 276 and the recess of the insulator 250a, the conductive film 260_2A may not be deposited.

[0413] Through the above-described CMP process, part of the insulator 277 b , part of the insulator 277 c , and part of the insulator 278 may be removed.

[0414] Next, an opening that reaches the conductor 246c is formed in the insulator 277c. Next, a conductive film that becomes the conductor 256 is deposited. Next, a CMP process is performed to remove a portion of the conductive film, thereby exposing the insulators 277b, 277c, and 278. As a result, the conductor 256 is formed in the above-mentioned opening (see Fig.21B1 and Fig.21B2 ). Through this CMP process, a portion of the insulator 277b, a portion of the insulator 277c, and a portion of the insulator 278 may be removed.

[0415] Next, an insulator 285 is formed on the insulator 276, the insulator 277b, the insulator 277c, the insulator 278, the conductor 260, and the conductor 256 (see Fig.22A1 and Fig.22A2). The insulator 285 is preferably deposited by sputtering. By using a sputtering method that does not require the use of molecules containing hydrogen as a deposition gas, the hydrogen concentration in the insulator 285 can be reduced. In this embodiment, silicon oxide is deposited as the insulator 285 by sputtering.

[0416] Next, an opening is formed in the insulator 285 (see Fig.22B1 and Fig.22B2 ). By forming the opening, at least the top surface of the insulator 276, the top surface of the conductor 256, and the top surface of the conductor 260 are exposed. When forming the opening, a wet etching method can be used, but a dry etching method is preferred for micro-machining. When the opening is formed in the insulator 285, a part of the insulator 276 is sometimes removed.

[0417] Next, conductive films to become the conductors 262a_1 and 262c_1 and conductive films to become the conductors 262a_2 and 262c_2 are sequentially deposited. In this embodiment, a titanium nitride film is deposited by ALD as the conductive films to become the conductors 262a_1 and 262c_1, and a tungsten film is deposited by CVD as the conductive films to become the conductors 262a_2 and 262c_2.

[0418] Next, the conductive film to be the conductor 262a_1 and the conductor 262c_1 and the conductive film to be the conductor 262a_2 and the conductor 262c_2 are processed by CMP until the insulator 285 is exposed. Thus, the conductor 262a (conductor 262a_1 and conductor 262a_2) and the conductor 262c (conductor 262c_1 and conductor 262c_2) are formed (see Fig.22B1 and Fig.22B2 Note that when the conductor 260 and the conductors 262a_1 and 262c_1 are formed of the same material, it may be difficult to clearly detect the boundaries between the conductor 260 and the conductors 262a_1 and 262c_1.

[0419] Through the above process, it is possible to manufacture FIG. 13A to FIG. 13D The semiconductor device of transistor 200 is shown. FIG. 15A1 to FIG. 22B2 As shown, by using the method for manufacturing a semiconductor device described in this embodiment, the transistor 200 can be manufactured.

[0420] According to one embodiment of the present invention, a semiconductor device capable of miniaturization or high integration can be provided. According to one embodiment of the present invention, a semiconductor device with less uneven electrical characteristics of a transistor can be provided. According to one embodiment of the present invention, a semiconductor device with excellent reliability can be provided. According to one embodiment of the present invention, a semiconductor device with excellent electrical characteristics can be provided. According to one embodiment of the present invention, a semiconductor device with large on-state current can be provided.

[0421] This embodiment mode can be appropriately combined with other embodiment modes. In addition, in this specification, when a plurality of configuration examples are shown in one embodiment mode, the configuration examples can be appropriately combined.

[0422] (Implementation Method 2) In this embodiment, a memory device according to one embodiment of the present invention is described with reference to the drawings. A memory device according to one embodiment of the present invention is a memory device (hereinafter sometimes referred to as an OS memory device) using a transistor using an oxide for a semiconductor (hereinafter sometimes referred to as an OS transistor).

[0423] <Configuration Example of Storage Device> Fig.23A An example of the structure of an OS storage device is shown. The storage device 1400 includes a peripheral circuit 1411 and a memory cell array 1470. The peripheral circuit 1411 is a circuit having the function of writing data to the memory cells in the memory cell array 1470 and reading data from the memory cells in the memory cell array 1470. The peripheral circuit 1411 includes a row circuit 1420, a column circuit 1430, an output circuit 1440, and a control logic circuit 1460.

[0424] The column circuit 1430 includes, for example, a column decoder, a precharge circuit, a sense amplifier, and a write circuit. The precharge circuit has a function of precharging the wiring. The sense amplifier has a function of amplifying the data signal read from the memory cell. Note that the above-mentioned wiring is a wiring connected to the memory cell included in the memory cell array 1470, and its details are described below. The amplified data signal is output as a data signal RDATA to the outside of the memory device 1400 through the output circuit 1440. In addition, the row circuit 1420 includes, for example, a row decoder, a word line driver circuit, etc., and can select the row to be accessed.

[0425] The memory device 1400 is supplied with a low power supply voltage (VSS) as a power supply voltage, a high power supply voltage (VDD) for the peripheral circuit 1411, and a high power supply voltage (VIL) for the memory cell array 1470 from the outside. In addition, control signals (CE, WE, RES), an address signal ADDR, and a data signal WDATA are input from the outside to the memory device 1400. The address signal ADDR is input to a row decoder and a column decoder, and the data signal WDATA is input to a write circuit.

[0426] The control logic circuit 1460 processes the control signals (CE, WE, RES) input from the outside to generate control signals for the row decoder and the column decoder. The control signal CE is a chip enable signal, the control signal WE is a write enable signal, and the control signal RES is a read enable signal. The signals processed by the control logic circuit 1460 are not limited to these, and other control signals can be input as needed.

[0427] The memory cell array 1470 includes a plurality of memory cells MC arranged in rows and columns and a plurality of wirings. Note that the number of wirings connecting the memory cell array 1470 and the row circuit 1420 depends on the structure of the memory cell MC, the number of memory cells MC included in one column, etc. In addition, the number of wirings connecting the memory cell array 1470 and the column circuit 1430 depends on the structure of the memory cell MC, the number of memory cells MC included in one row, etc.

[0428] In addition, although Fig.23A 14 shows an example in which the peripheral circuit 1411 and the memory cell array 1470 are formed on the same plane, but the present embodiment is not limited thereto. Fig. 23B As shown in FIG. 1 , the memory cell array 1470 may be provided so as to overlap with a part of the peripheral circuit 1411. For example, a structure in which a sense amplifier is provided so as to overlap under the memory cell array 1470 may be adopted.

[0429] Reference Fig.24A and Fig. 24B A structural example of a memory cell that can be suitably used for the above-described memory cell MC will be described.

[0430] Fig.24A An example circuit configuration of a two-transistor gain unit type memory cell is shown. Fig.24A The memory cell 1471 shown includes a transistor M1 and a transistor M2. The transistor M1 and the transistor M2 are single-gate transistors.

[0431] The first terminal of the transistor M1 is connected to the gate of the transistor M2, the second terminal of the transistor M1 is connected to the wiring BIL, and the gate of the transistor M1 is connected to the wiring WOL. The first terminal of the transistor M2 is connected to the wiring SL, and the second terminal of the transistor M2 is connected to the wiring BIL.

[0432] The wiring BIL is used as a bit line, and the wiring WOL is used as a word line.

[0433] In the memory cell 1471, the gate capacitance of the transistor M2 is used as a storage capacitance. That is, the memory cell 1471 can also be called a capacitor-free memory cell. Therefore, it can be called a gain unit type memory cell with 2 transistors and 0 capacitors.

[0434] When an OS transistor is used as the transistor M1, by turning off the transistor M1, the charge of the node electrically connecting one of the source and drain of the transistor M1 and the gate of the transistor M2 can be retained for a long time, thereby realizing a nonvolatile memory cell.

[0435] As Fig.24A The memory cell 1471 shown in FIG. 2 or the memory cell 100 shown in FIG. 13 can be used. In this case, the transistor M1 corresponds to the transistor 200a, and the transistor M2 corresponds to the transistor 200b. In addition, the wiring BIL corresponds to the conductor 244, the wiring WOL corresponds to the conductor 262a, and the wiring SL corresponds to the conductor 246b.

[0436] Fig. 24B Another example of the circuit configuration of a two-transistor gain unit type memory cell is shown. Fig. 24B The memory cell 1472 shown includes a transistor M1 and a transistor M2. The transistor M1 and the transistor M2 are single-gate transistors.

[0437] A first terminal of transistor M1 is connected to a gate of transistor M2, a second terminal of transistor M1 is connected to wiring WBL, and a gate of transistor M1 is connected to wiring WOL. A first terminal of transistor M2 is connected to wiring SL, and a second terminal of transistor M2 is connected to wiring RBL.

[0438] The wiring WBL is used as a write bit line, the wiring RBL is used as a read bit line, and the wiring WOL is used as a word line.

[0439] Similar to the memory cell 1471, in the memory cell 1472, the gate capacitance of the transistor M2 is used as a storage capacitance. When an OS transistor is used as the transistor M1, by turning off the transistor M1, the charge of the node electrically connected to one of the source and drain of the transistor M1 and the gate of the transistor M2 can be retained for a long time. Therefore, a nonvolatile memory cell can be realized.

[0440] As Fig. 24B The memory cell 1472 shown in FIG. 6 can use the memory cell 100A shown in FIG. 6. In this case, the transistor M1 corresponds to the transistor 200a, and the transistor M2 corresponds to the transistor 200b. In addition, the wiring WBL corresponds to the conductor 244a, the wiring RBL corresponds to the conductor 244b, the wiring WOL corresponds to the conductor 262a, and the wiring SL corresponds to the conductor 246b.

[0441] Or, as Fig. 24B The memory cell 1472 shown in FIG. 8 may use the memory cell 100B shown in FIG. 8 or the memory cell 100C shown in FIG. 10 . In this case, the transistor M1 corresponds to the transistor 200 a, and the transistor M2 corresponds to the transistor 200 b. In addition, the wiring WBL corresponds to the conductor 246 a, the wiring RBL corresponds to the conductor 246 b, the wiring WOL corresponds to the conductor 262 a, and the wiring SL corresponds to the conductor 244 b.

[0442] In addition, the memory cell MC is not limited to the memory cell 1471 and the memory cell 1472, and its circuit structure can be changed.

[0443] By using an OS transistor as the transistor M1, the transistor M1 can be formed in the BEOL process of forming the wiring of the memory device. In addition, when a Si transistor is used in the peripheral circuit 1411 overlapping with the memory cell array 1470, the BEOL-Tr technology can be used. By using this technology, a 3D functional circuit can be formed while maintaining the design rules, and high functionality can be achieved with low power consumption and low cost.

[0444] Fig.24C is a perspective view of a storage device 1400. The storage device 1400 includes a layer 1480 and a layer 1490. Fig.24D It is a perspective view for explaining the structure of the storage device 1400 , and shows a layer 1480 and a layer 1490 separately.

[0445] Layer 1480 is a layer including a transistor. The semiconductor layer including the channel formation region of the transistor can be formed using one or a combination of semiconductor materials such as a single crystal semiconductor, a polycrystalline semiconductor, a microcrystalline semiconductor or an amorphous semiconductor. As the semiconductor material, for example, silicon or germanium can be used. In addition, compound semiconductors such as silicon germanium, silicon carbide, gallium arsenide, oxide semiconductors and nitride semiconductors can also be used. In addition, gallium arsenide, aluminum gallium arsenide, indium gallium arsenide, gallium nitride, indium phosphide or silicon germanium that can be used for HEMT (High Electron Mobility Transistor) can also be used.

[0446] Layer 1490 is a layer including a transistor. The semiconductor layer including the channel formation region of the transistor can be formed using a semiconductor material capable of forming a thin film, such as an oxide semiconductor or silicon. By using BEOL-Tr technology, layer 1490 can be provided on layer 1480. Therefore, a miniaturized storage device 1400 can be realized.

[0447] For example, it is assumed that the transistors included in the layer 1480 are Si transistors. In this case, the peripheral circuit 1411 may be provided in the layer 1480. In addition, it is assumed that the transistors included in the layer 1490 are OS transistors. In this case, the memory cell array 1470 may be provided in the layer 1480.

[0448] Thus, the memory device 1400 can be manufactured using BEOL-Tr technology. Therefore, the occupied area of ​​the memory device 1400 can be reduced.

[0449] Note that the structure of the peripheral circuit 1411 and the memory cell array 1470 described in this embodiment is not limited to the above structure. In addition, the arrangement or function of these circuits and wirings connected to the circuits, circuit elements, etc. may be changed, removed, or added as needed.

[0450] Fig.25 Show Fig.23A An example of a cross-sectional structure of a storage device 1400 is shown. Fig.25 Show Fig.23A A portion of storage device 1400 is shown.

[0451] like Fig.25 As shown, the memory device 1400 includes a layer 1480 and a layer 1490 on the layer 1480. The layer 1480 is provided with the peripheral circuit 1411. That is, the layer 1480 can be said to be a layer including the peripheral circuit 1411. In addition, the layer 1490 is provided with the memory cell array 1470. As the memory cell in the memory cell array 1470, the semiconductor device described in the above embodiment mode can be used. That is, the layer 1480 is located below the semiconductor device described in the above embodiment mode.

[0452] Fig.25 The transistor 300 included in the layer 1480 is shown. The transistor 300 is used as a part of the above-mentioned sense amplifier. At this time, the layer 1480 can be regarded as a substrate on which a semiconductor circuit including a transistor is formed.

[0453] in addition, Fig.25 A portion of a memory cell array 1470 disposed in layer 1490 is shown. Specifically, Fig.25 One memory cell MC disposed in layer 1490 is shown.

[0454] The conductor 262a corresponds to the wiring WOL. The conductor 244 corresponds to the wiring BIL. The conductor 246b (not shown) corresponds to the wiring SL.

[0455] Notice, Fig.25 The structure in which one layer of the layer 1490 including the memory cell array 1470 is provided is shown, but the present invention is not limited thereto. For example, a plurality of layers including the memory cell array 1470 may also be provided.

[0456] Fig.26 The structure of stacking a layer 1490_1 including a memory cell array and a layer 1490_2 including a memory cell array is shown. Note that the number of stacked layers may be three or more. In this way, by using OS transistors as transistors constituting the memory cell 100, multiple layers of the memory cell array 1470 can be stacked. That is, the amount of data that can be stored per unit area can be increased.

[0457] <Transistor 300> The transistor 300 is disposed on a substrate 311 and includes a conductor 316 used as a gate, an insulator 315 used as a gate insulator, a semiconductor region 313 formed by a portion of the substrate 311, and a low resistance region 314a and a low resistance region 314b used as a source region or a drain region. The transistor 300 may be a p-channel transistor or an n-channel transistor.

[0458] Here, in Fig.25 In the transistor 300 shown, the semiconductor region 313 (a part of the substrate 311) forming the channel has a convex shape. In addition, a conductor 316 is provided in a manner that covers the side and top surfaces of the semiconductor region 313 via an insulator 315. In addition, a material that adjusts the work function can also be used for the conductor 316. Because the convex portion of the semiconductor substrate is utilized, this transistor 300 is also referred to as a FIN-type transistor. In addition, an insulator having a mask for forming a convex portion in a manner that contacts the upper surface of the convex portion can also be provided. In addition, although a portion of the semiconductor substrate is processed to form a convex portion is shown here, an SOI substrate can also be processed to form a semiconductor film having a convex shape.

[0459] Notice, Fig.25 The structure of the transistor 300 shown is only an example and is not limited to the above structure. An appropriate transistor may be used according to the circuit structure or driving method.

[0460] <Wiring Layer> A wiring layer including an interlayer film, wiring, and plugs may also be provided between each structure. In addition, the wiring layer may be provided in multiple layers according to the design. Here, in a conductor having the function of a plug or wiring, the same symbol is sometimes used to represent multiple structures. In addition, in this specification, wiring and a plug electrically connected to the wiring may also be a component. That is, a part of the conductor is sometimes used as wiring, and a part of the conductor is sometimes used as a plug.

[0461] For example, an insulator 320, an insulator 322, an insulator 324, and an insulator 326 are sequentially stacked as interlayer films on the transistor 300. In addition, a conductor 328 and a conductor 330, etc., which are electrically connected to the transistor 200, are buried in the insulator 320, the insulator 322, the insulator 324, and the insulator 326. In addition, the conductor 328 and the conductor 330 are used as plugs or wiring.

[0462] In addition, the insulator used as an interlayer film can also be used as a planarization film to cover the concavo-convex shape thereunder. For example, in order to improve the flatness of the top surface of the insulator 322, the top surface can also be planarized by a planarization process such as chemical mechanical polishing (CMP).

[0463] Alternatively, a wiring layer may be provided on the insulator 326 and the conductor 330. Fig.25 In the embodiment, an insulator 350, an insulator 352, and an insulator 354 are stacked in this order. In addition, a conductor 356 is formed in the insulator 350, the insulator 352, and the insulator 354. The conductor 356 is used as a plug or wiring.

[0464] As an insulator that can be used as an interlayer film, there are oxides, nitrides, oxynitrides, oxynitrides, metal oxides, metal oxynitrides, metal oxynitrides, and the like having insulating properties.

[0465] For example, by using a material with a low relative dielectric constant for an insulator used as an interlayer film, parasitic capacitance generated between wirings can be reduced. Therefore, it is preferable to select a material according to the function of the insulator.

[0466] For example, insulator 322, insulator 352 and insulator 354 preferably have an insulator with a low relative dielectric constant. For example, the insulator preferably contains silicon oxide added with fluorine, silicon oxide added with carbon, silicon oxide added with carbon and nitrogen, silicon oxide with pores, resin, etc. Alternatively, the insulator preferably has a laminated structure of silicon oxide, silicon oxynitride, silicon nitride oxide, silicon nitride, silicon oxide added with fluorine, silicon oxide added with carbon, silicon oxide added with carbon and nitrogen, or silicon oxide with pores and resin. Since silicon oxide and silicon oxynitride have thermal stability, by combining them with resin, a laminated structure with thermal stability and a low relative dielectric constant can be achieved. As resins, for example, polyesters, polyolefins, polyamides (nylon, aromatic polyamide, etc.), polyimides, polycarbonates or acrylic resins can be cited.

[0467] In addition, by surrounding a transistor using an oxide semiconductor with an insulator having a function of inhibiting the permeation of impurities such as hydrogen and oxygen, the electrical characteristics of the transistor can be stabilized. Therefore, as the insulator 350 or the like, an insulator having a function of inhibiting the permeation of impurities such as hydrogen and oxygen can be used.

[0468] As an insulator having the function of inhibiting the permeation of impurities such as hydrogen and oxygen, for example, an insulator containing boron, carbon, nitrogen, oxygen, fluorine, magnesium, aluminum, silicon, phosphorus, chlorine, argon, gallium, germanium, yttrium, zirconium, lanthanum, neodymium, hafnium or tantalum can be used in a single layer or a stacked layer. Specifically, as an insulator having the function of inhibiting the permeation of impurities such as hydrogen and oxygen, metal oxides such as aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, tantalum oxide, silicon oxynitride, silicon nitride, etc. can be used.

[0469] As the conductor that can be used for wiring and plugs, materials containing one or more metal elements selected from aluminum, chromium, copper, silver, gold, platinum, tantalum, nickel, titanium, molybdenum, tungsten, hafnium, vanadium, niobium, manganese, magnesium, zirconium, beryllium, indium and ruthenium can be used. In addition, semiconductors with high conductivity represented by polycrystalline silicon containing impurity elements such as phosphorus and silicides such as nickel silicide can also be used.

[0470] For example, as the conductor 328, the conductor 330, and the conductor 356, a metal material, an alloy material, a metal nitride material, a metal oxide material, or the like formed of the above materials can be used in a single layer or a stacked layer. It is preferred to use a high melting point material such as tungsten or molybdenum having both heat resistance and conductivity, preferably tungsten. Alternatively, it is preferred to use a low resistance conductive material such as aluminum or copper. By using a low resistance conductive material, the wiring resistance can be reduced.

[0471] This embodiment mode can be appropriately combined with other embodiment modes. In addition, in this specification, when a plurality of configuration examples are shown in one embodiment mode, the configuration examples can be appropriately combined.

[0472] (Implementation 3) In this embodiment, an application example of a semiconductor device using the storage device described in the above embodiment is described. The storage device described in the above embodiment can be applied to various removable storage devices such as a memory card (for example, an SD card), a USB memory, and an SSD (solid state drive). FIG. 27A to FIG. 27E Several structural examples of the removable storage device are schematically shown. For example, the semiconductor device shown in the above embodiment mode is processed into a packaged memory chip and used in various auxiliary storage devices or removable memories.

[0473] Fig.27A 11 is a schematic diagram of a USB memory. The USB memory 1100 includes a housing 1101, a cover 1102, a USB connector 1103, and a substrate 1104. The substrate 1104 is accommodated in the housing 1101. For example, a memory chip 1105 and a controller chip 1106 are mounted on the substrate 1104. The storage device or semiconductor device described in the above embodiment can be assembled to the memory chip 1105, etc.

[0474] Fig.27B This is a schematic diagram of the appearance of an SD card. Fig.27C 11 is a schematic diagram of the internal structure of the SD card. The SD card 1110 includes a housing 1111, a connector 1112, and a substrate 1113. The substrate 1113 is accommodated in the housing 1111. For example, a memory chip 1114 and a controller chip 1115 are mounted on the substrate 1113. By also providing the memory chip 1114 on the back side of the substrate 1113, the capacity of the SD card 1110 can be increased. In addition, a wireless chip with a wireless communication function can also be provided on the substrate 1113. Thus, data of the memory chip 1114 can be read and written through wireless communication between the host device and the SD card 1110. The storage device or semiconductor device shown in the above-mentioned embodiment can be assembled on the memory chip 1114, etc.

[0475] Fig.27D This is a schematic diagram of the appearance of SSD. Fig.27E1150 is a schematic diagram of the internal structure of the SSD. The SSD 1150 includes a housing 1151, a connector 1152, and a substrate 1153. The substrate 1153 is accommodated in the housing 1151. For example, a memory chip 1154, a memory chip 1155, and a controller chip 1156 are mounted on the substrate 1153. The memory chip 1155 is a working memory of the controller chip 1156, and a DOSRAM chip can be used, for example. By also providing the memory chip 1154 on the back side of the substrate 1153, the capacity of the SSD 1150 can be increased. The storage device or semiconductor device shown in the above embodiment can be assembled to the memory chip 1154, etc.

[0476] This embodiment mode can be implemented in combination with the configurations described in other embodiment modes and the like as appropriate.

[0477] (Implementation 4) FIG. 28A to FIG. 28G Specific examples of electronic devices including a storage device or a semiconductor device in which one embodiment of the present invention is implemented are shown.

[0478] <Electronic equipment and systems> The storage device or semiconductor device according to one embodiment of the present invention can be installed in various electronic devices. Examples of electronic devices include information terminals, computers, smart phones, e-book readers, television devices, digital signage, large-scale game machines such as pinball machines, digital cameras, digital video cameras, digital photo frames, mobile phones, portable game machines, recording and reproducing devices, navigation systems, and sound reproducing devices. Here, computers include tablet computers, notebook computers, desktop computers, and large-scale computers such as service systems.

[0479] The electronic device of one embodiment of the present invention may include an antenna. By receiving a signal through the antenna, an image or information can be displayed on the display unit. In addition, when the electronic device includes an antenna and a secondary battery, the antenna can be used for contactless power transmission.

[0480] An electronic device of one embodiment of the present invention may also include a sensor (the sensor has the function of measuring the following factors: force, displacement, position, speed, acceleration, angular velocity, rotation speed, distance, light, liquid, magnetism, temperature, chemical substance, sound, time, hardness, electric field, current, voltage, electricity, radiation, flow, humidity, inclination, vibration, odor or infrared).

[0481] An electronic device of one embodiment of the present invention may have various functions. For example, it may have the following functions: a function of displaying various information (static images, dynamic images, text images, etc.) on a display unit; a function of a touch panel; a function of displaying a calendar, date, or time, etc.; a function of executing various software (programs); a function of wireless communication; a function of reading programs or data stored in a storage medium, etc.

[0482] [Information Terminal] By using the storage device or semiconductor device according to one embodiment of the present invention, a storage device for holding a program of a microcontroller can be formed. Therefore, according to one embodiment of the present invention, the microcontroller can be miniaturized.

[0483] Fig.28A A mobile phone (smartphone) which is one of the information terminals is shown. The information terminal 5100 includes a housing 5101 and a display unit 5102. The display unit 5102 has a touch panel as an input interface, and buttons are provided on the housing 5101. By using a miniaturized microcontroller of one embodiment of the present invention, the limited space in the mobile phone can be effectively utilized. In addition, the storage device of one embodiment of the present invention can also be applied to the auxiliary memory (storage) of the mobile phone. As a result, the storage capacity per unit area of ​​the auxiliary memory can be increased.

[0484] Fig.28B A notebook information terminal 5200 is shown. The notebook information terminal 5200 includes an information terminal body 5201, a display unit 5202, and a keyboard 5203. By using a miniaturized microcontroller of one embodiment of the present invention, the limited space in the notebook information terminal can be effectively utilized. In addition, the storage device of one embodiment of the present invention can also be applied to the auxiliary memory of the notebook information terminal. As a result, the storage capacity per unit area of ​​the auxiliary memory can be increased.

[0485] Note that in the above example, Fig.28A and Fig.28B Although a smartphone and a notebook information terminal are shown as examples of electronic devices, information terminals other than smartphones and notebook information terminals may also be applied. Examples of information terminals other than smartphones and notebook information terminals include PDAs (Personal Digital Assistants), desktop information terminals, and workstations.

[0486] [Game console] Fig.28CA portable game console 5300 is shown as an example of a game console. The portable game console 5300 includes a housing 5301, a housing 5302, a housing 5303, a display unit 5304, a connection unit 5305, and operation keys 5306. The housing 5302 and the housing 5303 can be removed from the housing 5301. By attaching the connection unit 5305 provided in the housing 5301 to another housing (not shown), the image output to the display unit 5304 can be output to another video display device (not shown). In this case, the housing 5302 and the housing 5303 can be used as an operation unit, respectively. Thus, multiple game players can play games at the same time. A storage device or a semiconductor device, etc., of one embodiment of the present invention can be embedded in a chip, etc., provided on a substrate of the housing 5301, the housing 5302, and the housing 5303.

[0487] also, Fig.28D A stationary gaming machine 5400, which is one of the gaming machines, is shown. The stationary gaming machine 5400 is connected to a controller 5402 by wireless or wired connection.

[0488] By using a miniaturized microcontroller according to one embodiment of the present invention in a game console such as a portable game console 5300 or a fixed game console 5400, the limited space in the game console can be effectively utilized. In addition, a storage device or a semiconductor device according to one embodiment of the present invention can also be used in an auxiliary memory of a portable game console. Thus, the storage capacity per unit area of ​​the auxiliary memory can be increased.

[0489] Although Fig.28C and Fig.28D Portable game machines and fixed game machines are shown as examples of game machines, but game machines to which a microcontroller in one embodiment of the present invention is applied are not limited thereto. Game machines to which a microcontroller in one embodiment of the present invention is applied include, for example, arcade game machines installed in entertainment facilities (game centers, amusement parks, etc.), pitching machines for batting practice installed in sports facilities, and the like.

[0490] [Mainframe computer] A storage device or a semiconductor device or the like according to one embodiment of the present invention can be applied to a large computer.

[0491] Fig.28E A supercomputer 5500 is shown as an example of a large-scale computer. Fig.28F A rack mount computer 5502 included in the supercomputer 5500 is shown.

[0492] The supercomputer 5500 includes a rack 5501 and a plurality of rack-mounted computers 5502. Note that the plurality of computers 5502 are housed in the rack 5501. In addition, the computer 5502 is provided with a plurality of substrates 5504, on which a microcontroller of one embodiment of the present invention can be mounted. By using a miniaturized microcontroller of one embodiment of the present invention, a limited space in a large computer can be effectively utilized. In addition, a storage device or a semiconductor device of one embodiment of the present invention can also be used for an auxiliary memory of a large computer. Thus, the storage capacity per unit area of ​​the auxiliary memory can be increased.

[0493] exist Fig.28E and Fig.28F In the embodiment, a supercomputer is shown as an example of a large computer, but a large computer to which a microcontroller in one embodiment of the present invention is applied is not limited to this. As a large computer to which a microcontroller in one embodiment of the present invention is applied, for example, a computer (server) providing a service, a large general-purpose computer (mainframe), etc. can be cited.

[0494] [Electrical products] Figure 28G An electric refrigerator-freezer 5800 is shown as an example of an electric appliance. The electric refrigerator-freezer 5800 includes a housing 5801, a refrigerator door 5802, a freezer door 5803, and the like.

[0495] The storage device or semiconductor device according to one embodiment of the present invention can be used in the electric refrigerator-freezer 5800. For example, by applying a miniaturized microcontroller according to one embodiment of the present invention to the electric refrigerator-freezer 5800, the limited space in the electric refrigerator-freezer can be effectively utilized.

[0496] An electric refrigerator-freezer is described as an example of an electrical product, and other electrical products include vacuum cleaners, microwave ovens, electric ovens, rice cookers, water heaters, IH cookers, water dispensers, air conditioners including air conditioners, washing machines, dryers, audio-visual equipment, etc.

[0497] The electronic device, the function of the electronic device, the effect thereof, and the like described in this embodiment mode can be implemented in combination with the description of other electronic devices as appropriate.

[0498] This embodiment mode can be implemented in combination with the configurations described in other embodiment modes and the like as appropriate. [Explanation of symbols]

[0499] 10: semiconductor device, 100A: memory cell, 100B: memory cell, 100C: memory cell, 100: memory cell, 200a: transistor, 200b: transistor, 200: transistor, 212: insulator, 216: insulator, 230_1: oxide, 230_1A: oxide film, 230_2: oxide, 230_21: region, 230_22: region, 230_2A: oxide film, 230_3: oxide, 230_3A: oxide film, 230: oxide, 242a: conductor, 242A: conductive film, 242b: conductor, 244_1: conductor, 244_2: conductor, 244a: conductor, 244b: conductor, 24 4c: conductor, 244: conductor, 246a: conductor, 246b: conductor, 246b1: convex shape portion, 246c: conductor, 246c1: convex shape portion, 246: conductor, 247: insulator, 250a: insulator, 250A: insulating film, 250b: insulator, 250: insulator, 254a: insulator, 254b: insulator, 256: conductor, 260_1A: conductive film, 260_2A: conductive film, 260: conductor, 262a: conductor, 262a_1: conductor, 262a_2: conductor, 262c: conductor, 262c_1: conductor, 262c_2: conductor, 264b: region, 264c: region, 274A: insulating film, 274c: insulator, 274: insulator, 275a: insulator, 275A: insulating film, 275b: insulator, 276A: insulating film, 276: insulator, 277b: insulator, 277c: insulator, 278: insulator, 285: insulator, 291A: insulating film, 291: insulator, 292: resist mask, 293A: insulating film, 293: insulator, 300: transistor, 311: substrate, 313: semiconductor region, 314a: low resistance region, 314b: low resistance region, 315: insulator, 316: conductor, 320: insulator, 322: insulator, 324: insulator, 326: insulator, 32 8: Conductor, 330: Conductor, 350: Insulator, 352: Insulator, 354: Insulator, 356: Conductor, 1100: USB memory, 1101: Housing, 1102: Cover, 1103: USB connector, 1104: Substrate, 1105: Memory chip, 1106: Controller chip, 1110: SD card, 1111: Housing, 1112: Connector, 1113: Substrate, 1114: Memory chip, 1115: Controller chip, 1150: SSD, 1151: Housing, 1152: Connector, 1153: Substrate, 1154: Memory chip, 1155: Memory chip, 1156: Controller chip, 1400: Storage device,1411: peripheral circuit, 1420: row circuit, 1430: column circuit, 1440: output circuit, 1460: control logic circuit, 1470: memory cell array, 1471: memory cell, 1472: memory cell, 1480: layer, 1490_1: layer, 1490_2: layer, 1490: layer, 5100: information terminal, 5101: housing, 5102: display unit, 5200: notebook information terminal, 5201: main body, 5202: display , 5203: keyboard, 5300: portable game console, 5301: housing, 5302: housing, 5303: housing, 5304: display unit, 5305: connection unit, 5306: operation key, 5400: fixed game console, 5402: controller, 5500: supercomputer, 5501: rack, 5502: computer, 5504: base plate, 5800: electric refrigerator-freezer, 5801: housing, 5802: refrigerator door, 5803: freezer door,

Claims

1. A semiconductor device comprising: a first electrical conductor; A first oxide and a second oxide electrically connected to the first conductor and having an opening; a second conductor electrically connected to the first oxide; a first insulator disposed inside the opening included in the first oxide; a third conductor on the first insulator; a fourth electrical conductor electrically connected to the third electrical conductor; a fifth electrical conductor electrically connected to the second oxide; a second insulator disposed inside the opening included in the second oxide; a sixth conductor on the second insulator; a seventh electrical conductor electrically connected to the sixth electrical conductor; as well as an eighth conductor electrically connected to the second conductor and the seventh conductor, wherein the fourth conductor is arranged in the same layer as the seventh conductor, Furthermore, an extending direction of the fourth conductor is the same as an extending direction of the fifth conductor.

2. The semiconductor device according to claim 1, The extending direction of the first conductor is orthogonal to the extending direction of the fourth conductor.

3. The semiconductor device according to claim 1, further comprising a ninth conductor and a tenth conductor, wherein the ninth conductor is disposed between the first oxide and the second conductor, The side surface of the ninth conductor is consistent with the side surface of the first oxide, The tenth conductor is disposed between the second oxide and the fifth conductor, And the side surface of the tenth conductor is consistent with the side surface of the second oxide.

4. The semiconductor device according to claim 3, wherein the second conductor has a convex shape, And the convex shape portion is in contact with the ninth conductor.

5. The semiconductor device according to claim 1, The side surface of the first oxide has a tapered shape when viewed in cross section.

6. A semiconductor device comprising: A first conductor and a second conductor; A first oxide electrically connected to the first electrical conductor and having an opening; a third electrical conductor electrically connected to the first oxide; a first insulator disposed inside the opening included in the first oxide; a fourth conductor on the first insulator; a fifth electrical conductor electrically connected to the fourth electrical conductor; a second oxide electrically connected to the second electrical conductor and having an opening; a sixth electrical conductor electrically connected to the second oxide; a second insulator disposed inside the opening included in the second oxide; a seventh conductor on the second insulator; an eighth electrical conductor electrically connected to the seventh electrical conductor; as well as a ninth conductor electrically connected to the third conductor and the eighth conductor, wherein the fifth conductor is arranged in the same layer as the eighth conductor, Furthermore, an extending direction of the fifth conductor is the same as an extending direction of the sixth conductor.

7. The semiconductor device according to claim 6, The extending direction of the first conductor is orthogonal to the extending direction of the fifth conductor. Furthermore, an extending direction of the second conductor is orthogonal to an extending direction of the sixth conductor.

8. The semiconductor device according to claim 6, further comprising a tenth conductor and an eleventh conductor, wherein the tenth conductor is disposed between the first oxide and the third conductor, The side surface of the tenth conductor is consistent with the side surface of the first oxide, The eleventh conductor is disposed between the second oxide and the sixth conductor, And the side surface of the eleventh conductor is consistent with the side surface of the second oxide.

9. The semiconductor device according to claim 6, The side surface of the first oxide has a tapered shape when viewed in cross section.

10. A storage device, comprising: The semiconductor device according to any one of claims 1 to 9; as well as Layers including peripheral circuits, wherein the layer is located below the semiconductor device, Furthermore, the peripheral circuit has a function of writing data into the semiconductor device and reading data from the semiconductor device.