Functional group-introduced membrane pore dynamic telescopic composite nanofiltration membrane and preparation method thereof

By introducing functional groups into the membrane pores and utilizing voltage regulation, the problem of limited adjustment range of the pore size of the electrically responsive membrane pores is solved, and the wide adjustment of membrane desalination performance and cost reduction are achieved, which improves the stability and application prospects of the membrane.

CN119034516APending Publication Date: 2024-11-29RES CENT FOR ECO ENVIRONMENTAL SCI THE CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411391045.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The pore size adjustment range of existing electrically responsive membrane pore telescopic membranes is limited, and the carbon materials used in the preparation process are expensive and have poor stability, which limits their application and large-scale production in the field of water treatment.

Method used

A porous polymer base membrane and a membrane pore dynamic telescopic composite nanofiltration membrane containing a polypyrrole functional layer containing functional groups are used to introduce functional groups through vacuum filtration and gas-phase polymerization reaction, and the membrane pore size is regulated by voltage to enhance the adjustment range of membrane desalination performance.

Benefits of technology

A large-scale dynamic regulation of membrane pore size is achieved, the range of adjustment of desalination performance is improved, the preparation cost is reduced, the stability and expansion potential of the membrane are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034516A_ABST
    Figure CN119034516A_ABST
Patent Text Reader

Abstract

The invention provides a functional group-introduced membrane pore dynamic telescopic composite nanofiltration membrane and a preparation method thereof. The functional group-introduced membrane pore dynamic telescopic composite nanofiltration membrane comprises a porous polymer substrate membrane and a functional group-containing polypyrrole functional layer, the polypyrrole functional layer containing the functional group is positioned on the surface of the porous polymer basement membrane and inside membrane pores; the preparation method comprises the following steps: uniformly dispersing an oxidizing agent into the membrane surface and membrane pores of a basement membrane through vacuum filtration so that functional groups can be introduced into the membrane pores by a doping agent, and obtaining the functional group-introduced membrane pore dynamic telescopic composite nanofiltration membrane by utilizing a gas-phase polymerization reaction of a pyrrole monomer. The functional group is introduced into the aperture expansion membrane for the first time, the function of the functional group is coupled with aperture expansion, the size effect of the functional group is utilized, the adjustment range of the membrane desalination performance is greatly enhanced, the preparation process is simple, the cost of the used reagent is low, the prepared composite membrane is stable in strength, and the scale is easy to expand.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water treatment, and in particular to a composite nanofiltration membrane with dynamic expansion and contraction of membrane pores with functional groups introduced therein and a preparation method thereof. Background Art

[0002] At present, membrane technology is an important technology in the field of water treatment, and is widely used in wastewater treatment, resource recovery, and seawater desalination. Among them, the pore size range of nanofiltration membranes is at the nanometer and sub-nanometer level, and is often used for the selective separation of ions or molecules in the above fields. However, once the nanofiltration membrane is prepared, the size of its membrane pores remains fixed. When faced with new demands such as dynamic separation of multiple substances, multiple nanofiltration membranes are usually required, which not only increases costs and processes, but also fails to achieve ideal results, limiting the development and application prospects of nanofiltration membranes.

[0003] Membrane pore expansion and contraction responsive membranes can adjust the size of membrane pores by external stimuli, thereby achieving timed separation or gradient separation of ions and molecules, and are one of the development directions of the next generation of membrane technology. Among them, electroresponsive membrane pore expansion and contraction membranes organically combine membrane technology and electrochemistry, and can accurately control the membrane pore size with electrode potential, so they have the most application prospects. The preparation of electroresponsive membranes is to embed conductive polymers whose volume changes with electrode potential into the membrane matrix. Conductive polymer polypyrrole is a common material for artificial muscles and actuators. It has good volume relaxation function and environmentally friendly properties, and is a common material for the preparation of electroresponsive membranes. For example, CN116459685A discloses a nanofiltration membrane with dynamic membrane pore expansion and contraction, and a preparation method, a use method and an application thereof. The nanofiltration membrane with dynamic membrane pore expansion and contraction comprises a porous polymer matrix membrane and a graphene-polypyrrole composite membrane covering the surface of the porous polymer matrix membrane; the nanofiltration membrane with dynamic membrane pore expansion and contraction is prepared by successively subjecting a mixed solution containing polypyrrole nanoparticles and graphene oxide to suction filtration and reduction reaction on the porous polymer matrix membrane; by selecting and adjusting the electrode potential applied to the nanofiltration membrane with dynamic membrane pore expansion and contraction, the dynamic membrane pore expansion and contraction can be achieved by electrochemical regulation, thereby adjusting the desalination performance of the nanofiltration membrane in situ, and can be applied to water treatment. CN110237713A discloses an electroresponsive polymer membrane and its preparation method, use method and purpose, wherein the electroresponsive polymer membrane comprises a porous polymer membrane substrate, and a polypyrrole membrane covering the pore walls and surface of the porous polymer membrane substrate, wherein the polypyrrole membrane is doped with a large volume anion; the large volume anion comprises any one or a combination of at least two of alkylbenzene sulfonate ions, alkyl sulfonate ions, alkyl sulfate ions and dioctyl dibutyrate sulfonate ions; the alkyl group is a C7-C12 alkyl group. The electroresponsive polymer membrane has the function of membrane pore expansion and contraction, can realize the removal of membrane pollutants and the selective retention of organic pollutants, and has good mechanical properties and stability.

[0004] However, the electro-responsive membrane pore stretching membrane prepared based on polypyrrole has a limited volume relaxation range of polypyrrole itself, so the pore size adjustment range of the electro-responsive membrane is limited. The control range of the retention rate of divalent salt sodium sulfate is about 5%, which cannot meet the requirements of precise separation in practical applications. In addition, its preparation process requires the use of expensive and unstable carbon materials such as graphene, which hinders subsequent large-scale production. Therefore, it is necessary to develop a preparation path for electro-responsive membrane pore stretching membranes with simple process, strong stability, low cost, and easy scalability, while solving the problem of its small adjustment range. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention provides a method for preparing a composite nanofiltration membrane with dynamic expansion and contraction of membrane pores with the introduction of functional groups, wherein the composite nanofiltration membrane with dynamic expansion and contraction of membrane pores with the introduction of functional groups comprises a porous polymer substrate membrane and a polypyrrole functional layer containing functional groups, wherein the polypyrrole functional layer containing functional groups is located on the surface of the porous polymer substrate membrane and inside the membrane pores; the preparation method comprises: by vacuum filtration, the oxidant is evenly dispersed to the membrane surface and membrane pores of the substrate membrane, so that the dopant can complete the introduction of functional groups in the membrane pores, and the composite nanofiltration membrane with dynamic expansion and contraction of membrane pores with the introduction of functional groups is obtained by utilizing the gas phase polymerization reaction of pyrrole monomers. The present invention introduces functional groups into the aperture expansion and contraction membrane for the first time, and couples the action of functional groups with aperture expansion and contraction, and utilizes the size effect of functional groups to greatly enhance the adjustment range of membrane desalination performance; the preparation method has the advantages of simple preparation process, low cost, strong stability, and potential for expansion.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] One of the purposes of the present invention is to provide a composite nanofiltration membrane with dynamic expansion and contraction of membrane pores introduced with functional groups, wherein the composite nanofiltration membrane with dynamic expansion and contraction of membrane pores introduced with functional groups comprises a porous polymer base membrane and a polypyrrole functional layer containing functional groups, wherein the polypyrrole functional layer containing functional groups is located on the surface of the porous polymer base membrane and inside the membrane pores.

[0008] The composite nanofiltration membrane with dynamic expansion and contraction of membrane pores with the introduction of functional groups described in the present invention utilizes a membrane assembly capable of applying voltage to the membrane surface, and realizes dynamic regulation of the desalination performance of the nanofiltration membrane by switching the working voltage, thereby enhancing the dynamic adjustment range of the desalination performance of the membrane pore expansion and contraction thin film composite membrane. This is because the external voltage applied to the membrane surface can control the migration of cations in the solution, so that the cations are embedded from the solution into the polypyrrole, or are removed from the polypyrrole. When the cations are embedded, the volume of the polypyrrole increases and the membrane pores decrease; when the cations are removed, the volume of the polypyrrole decreases and the membrane pores increase. At the same time, the functional groups on the polypyrrole will also change the interaction between the ions and the membrane pores, thereby affecting the transmission of ions. This effect is more significant when the membrane pore size is small. The functional group effect is coupled with the pore expansion and contraction, and the synergistic effect of the two can be used to prepare a composite nanofiltration membrane with a wide range of dynamic regulation. The specific regulation and use methods include method (i) and / or method (ii):

[0009] The method (i) comprises: in a solution containing an electrolyte, applying a reduction potential to the dynamic expansion and contraction composite nanofiltration membrane with functional groups introduced therein to reduce the pore size, lower the salt rejection rate, and increase the flux;

[0010] The method (ii) comprises: in a solution containing an electrolyte, applying an oxidation potential to the dynamic expansion and contraction composite nanofiltration membrane with functional groups introduced therein to enlarge the pore size, increase the salt rejection rate, and reduce the flux.

[0011] As a preferred technical solution of the present invention, the thickness of the porous polymer matrix membrane is 100-200 μm, for example, 100 μm, 110 μm, 130 μm, 150 μm, 170 μm, 180 μm or 200 μm.

[0012] Preferably, the pore size of the porous polymer substrate membrane is 10 to 30 nm, for example, 10 nm, 15 nm, 20 nm, 25 nm or 30 nm.

[0013] Preferably, the polymer of the porous polymer substrate membrane includes any one of polyvinylidene fluoride, polyethersulfone, cellulose acetate and polyamide, preferably polyethersulfone.

[0014] The second object of the present invention is to provide a method for preparing the composite nanofiltration membrane with dynamic expansion and contraction of membrane pores with introduced functional groups as described in the first object, the preparation method comprising the following steps:

[0015] (1) preparing an oxidant composite solution, wherein the oxidant composite solution contains an oxidant and a dopant with a functional group, wherein the functional group of the dopant with a functional group includes at least one of a hydroxyl group, a carboxyl group, a benzenesulfonic acid group or a sulfonic acid group; coating the oxidant composite solution on a porous polymer substrate membrane, and performing vacuum filtration;

[0016] (2) placing the substrate film treated in step (1) in a vacuum dryer and performing a gas phase polymerization reaction in an atmosphere of pyrrole monomer to form a polypyrrole functional layer containing functional groups, thereby obtaining a composite nanofiltration membrane with dynamic membrane pore expansion and contraction and introducing functional groups.

[0017] The preparation method of the present invention prepares an oxidant composite solution containing an oxidant and a dopant with a functional group according to the functional group to be introduced, and the functional group can be simply introduced into the membrane pore expansion membrane by replacing the dopant in the solution, and the introduced functional group includes at least one of a hydroxyl group, a carboxyl group, a benzenesulfonic acid group or a sulfonic acid group. The present invention introduces functional groups into the aperture expansion membrane for the first time, and utilizes the regulating effect of the functional group on ion transmission to couple the aperture expansion, so that the regulating effect of the functional group is more obvious in the small-sized membrane pores, solves the problem of limited volume relaxation of polypyrrole, can break through the limited salt interception adjustment range of the polypyrrole response membrane, and greatly enhances the desalination performance adjustment range of the membrane pore expansion membrane.

[0018] The preparation method of the present invention uses vacuum filtration to adjust the binding sites of pyrrole for the second time after coating the oxidant solution on the basement membrane, so that the oxidant is evenly dispersed on the membrane surface and in the membrane pores, and the polymerization of pyrrole is successfully completed. On the one hand, the method dredges the polypyrrole on the membrane surface, reduces the blockage of the membrane pores on the basement membrane surface, and improves the membrane flux; on the other hand, pyrrole is polymerized in the pores, and its volume change directly regulates the expansion and contraction of the membrane pores compared to the polypyrrole on the membrane surface. The preparation method of the present invention has a simple preparation process, low cost of reagents, stable membrane structure, and is easy to scale up.

[0019] The preparation method of the present invention can realize the introduction of different functional groups of the thin film composite nanofiltration membrane by adjusting the type of the oxidant composite solution, and secondary adjust the binding site of pyrrole by vacuum filtration, so that the oxidant is evenly dispersed on the membrane surface and in the membrane pores, and the dynamic adjustment of the membrane pores can be realized by the working voltage. When a reduction potential is applied to the membrane surface, the volume of polypyrrole increases and the membrane pore size decreases; when an oxidation potential is applied to the membrane surface, the volume of polypyrrole decreases and the membrane pore size increases. At the same time, due to the coupling effect of pore size expansion and contraction and the action of functional groups, the adjustment range of the desalination performance of the membrane is greatly enhanced, the range of variation of the retention rate exceeds 13%, and the range of variation of the flux exceeds 3.5LMH.

[0020] It should be noted that in step (1) of preparing the oxidant composite solution, the oxidant is first added into deionized water to be completely dissolved, and then the dopant with a functional group is added and completely dissolved.

[0021] As a preferred technical solution of the present invention, the oxidant in step (1) includes at least one of ferric chloride, ammonium persulfate, potassium persulfate or sodium persulfate.

[0022] As a preferred technical solution of the present invention, the doping agent with a functional group in step (1) includes at least one of β-cyclodextrin, lauric acid, sodium dodecylbenzene sulfonate or sodium dodecyl sulfonate.

[0023] As a preferred technical solution of the present invention, in the oxidant composite solution of step (1), the oxidant content is 0-1 mol / L, excluding 0 mol / L, for example, 0.1 mol / L, 0.2 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.8 mol / L or 1.0 mol / L, etc., and the dopant content with a functional group is 0-100 mmol / L, excluding 0 mmol / L, for example, 10 mmol / L, 20 mmol / L, 40 mmol / L, 50 mmol / L, 60 mmol / L, 80 mmol / L or 100 mmol / L, etc.

[0024] As a preferred technical solution of the present invention, in step (1), after the coating and before the vacuum filtration, it also includes standing.

[0025] Preferably, the standing time is 60 to 120 s, for example, 60 s, 70 s, 80 s, 90 s, 100 s, 110 s or 120 s.

[0026] As a preferred technical solution of the present invention, the time of the vacuum filtration in step (1) is 20 to 40 minutes, for example, 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes.

[0027] Preferably, the pressure of the vacuum filtration in step (1) is 0.5-0.9 MPa, for example, 0.5 MPa, 0.6 MPa, 0.7 MPa, 0.8 MPa or 0.9 MPa.

[0028] It is worth noting that the present invention uses a vacuum filtration method to adjust the reaction sites for the second time, and the uniformity of the distribution of the reaction sites is related to the time pressure of the filtration process. If the filtration time is too long and the filtration pressure is too large, it is easy to reduce the residence time of the oxidant and the dopant in the membrane pores, and the composite solution is not easy to be coated inside the membrane pores; if the filtration time is too short and the filtration pressure is too small, the composite solution on the membrane surface cannot be successfully filtered to the inside of the membrane pores. The membrane surface after the vacuum filtration secondary adjustment reaction site is light yellow, and at this time, the composite solution of the oxidant and the dopant is evenly distributed on the membrane surface and the membrane pores, so that the polymerization reaction of pyrrole can occur in the membrane pores and the membrane surface, especially the polypyrrole generated by the reaction in the membrane pores, and its volume change can directly affect the change in the membrane pore size, and improve the contribution efficiency of the polypyrrole volume change to the dynamic expansion and contraction of the membrane pore size change. This method of secondary adjustment of the reaction site has the characteristics of simple operation and easy adjustment of parameters.

[0029] As a preferred technical solution of the present invention, in step (2), the porous polymer substrate membrane treated in step (1) is first placed in a vacuum dryer, and then the pyrrole solution is placed in the vacuum dryer, and finally the vacuum dryer is sealed and evacuated.

[0030] Preferably, the concentration of the pyrrole solution is 7 to 14 mol / L, for example, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, 13 mol / L or 14 mol / L.

[0031] Preferably, the gas phase polymerization reaction time in step (2) is 8 to 15 min, for example, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min or 15 min.

[0032] Preferably, the temperature of the gas phase polymerization reaction in step (2) is 10-30°C, for example, 10°C, 15°C, 20°C, 25°C or 30°C.

[0033] As a preferred technical solution of the present invention, after the gas phase polymerization reaction in step (2), the obtained thin film composite film is dried, for example, the obtained thin film composite film is placed in an oven for drying, so that the gas phase polymerization reaction is complete and the film is fully dried.

[0034] Preferably, the drying temperature is 50-80°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C.

[0035] Preferably, the drying time is 8 to 15 min, for example, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min or 15 min.

[0036] As a preferred technical solution of the present invention, the composite nanofiltration membrane with dynamic expansion and contraction of membrane pores and functional groups introduced therein obtained in step (2) is placed in ultrapure water for standby use.

[0037] Compared with the prior art solutions, the present invention has at least the following beneficial effects:

[0038] (1) The preparation method of the present invention can simply introduce functional groups into the membrane pore stretching membrane by replacing the dopant in the solution. The introduced functional groups include at least one of hydroxyl, carboxyl, benzenesulfonic acid group or sulfonic acid group, and the functional group effect is coupled with the pore size expansion phase. By utilizing the size effect of the functional group, the functional group's hindering effect on ion transport is more effectively exerted in small-sized pores, thereby breaking through the bottleneck of insufficient dynamic adjustment range of desalination performance caused by the volume relaxation range limitation of polypyrrole itself, and greatly enhancing the adjustment range of desalination performance of the membrane pore stretching membrane;

[0039] (2) The preparation method of the present invention innovatively uses vacuum filtration to secondary adjust the binding sites of pyrrole after coating the oxidant solution, so that the oxidant is evenly dispersed on the membrane surface and in the membrane pores. On the one hand, the polypyrrole on the membrane surface is unblocked, the blockage of polypyrrole is reduced, and the membrane flux is improved; on the other hand, the pyrrole is polymerized in the pores, and its volume change directly regulates the expansion and contraction of the membrane pores;

[0040] (3) The preparation method of the present invention has a simple preparation process, which only includes coating, vacuum filtration and gas phase polymerization processes. The materials used are mainly low-cost chemical reagents such as pyrrole and ferric chloride, which are easy to scale up. The membrane obtained by the preparation method of the present invention has strong stability and has the potential for large-scale preparation. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 It is a schematic flow chart of the preparation method of the composite nanofiltration membrane with dynamic expansion and contraction of membrane pores with introduced functional groups according to the present invention;

[0042] Figure 2 is a SEM cross-sectional view of the composite nanofiltration membrane with dynamic expansion and contraction of membrane pores and functional groups introduced therein prepared in Example 1;

[0043] Figure 3 This is a SEM cross-sectional view of the composite nanofiltration membrane with dynamic membrane pore expansion and contraction prepared in Comparative Example 1;

[0044] Figure 4 This is a SEM cross-sectional view of the composite nanofiltration membrane with dynamic expansion and contraction of membrane pores and functional groups introduced therein prepared in Comparative Example 2;

[0045] Figure 5 The dynamic expansion and contraction of the composite nanofiltration membrane of Example 1 to sodium sulfate (Na 2 SO 4 ) retention rate and flux change curve;

[0046] Figure 6 The dynamic expansion and contraction of the composite nanofiltration membrane of Example 1 for sodium sulfate (Na 2 SO 4 ) retention rate and flux change curve;

[0047] Figure 7 The dynamic expansion and contraction of the composite nanofiltration membrane of Example 2 for sodium sulfate (Na 2 SO 4 ) retention rate and flux change curve. DETAILED DESCRIPTION

[0048] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0049] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0050] The present invention provides a method for preparing a composite nanofiltration membrane with dynamic expansion and contraction of membrane pores by introducing functional groups. Figure 1 A schematic flow chart of the preparation method is shown, and the preparation method comprises the following steps:

[0051] (1) preparing an oxidant composite solution, wherein the oxidant composite solution contains an oxidant and a dopant with a functional group, wherein the functional group of the dopant with a functional group includes at least one of a hydroxyl group, a carboxyl group, a benzenesulfonic acid group or a sulfonic acid group; coating the oxidant composite solution on a porous polymer substrate membrane, and performing vacuum filtration;

[0052] (2) placing the substrate film treated in step (1) in a vacuum dryer and performing a gas phase polymerization reaction in an atmosphere of pyrrole monomer to form a polypyrrole functional layer containing functional groups, thereby obtaining a composite nanofiltration membrane with dynamic membrane pore expansion and contraction and introducing functional groups.

[0053] Example 1

[0054] This embodiment provides a method for preparing a composite nanofiltration membrane with dynamic expansion and contraction of membrane pores with introduced functional groups, the preparation method comprising the following steps:

[0055] (1) Uniform dispersion of pyrrole binding sites

[0056] First, ferric chloride as an oxidant is added into deionized water to completely dissolve it, and a corresponding dopant (β-cyclodextrin) is added according to the introduced functional group to obtain an oxidant composite solution; in the oxidant composite solution, the oxidant content is 0.5 mol / L, and the content of the dopant with a functional group is 50 mmol / L;

[0057] The oxidant composite solution was coated on a polyethersulfone substrate membrane with a thickness of 150 μm and a pore size of 20 nm, and allowed to stand for 90 seconds, and then vacuum filtered until the membrane surface was completely dry. The vacuum filtration time was controlled to be 30 minutes and the pressure was 0.7 MPa, so that the oxidant was evenly dispersed on the membrane surface and in the membrane pores, and the membrane surface was yellow at this time;

[0058] (2) Preparation of membrane hole stretch film composite membrane

[0059] The substrate film treated in step (1) is placed in a vacuum dryer, and then a pyrrole solution with a concentration of 10 mol / L is placed in the vacuum dryer. Finally, the vacuum is sealed and evacuated to carry out a gas phase polymerization reaction. After reacting at 25°C for 10 minutes, the pyrrole will polymerize into polypyrrole in the presence of the oxidant. At this time, the membrane surface is black. The prepared thin film composite membrane is placed in a 60°C oven for drying for 10 minutes, and then soaked in ultrapure water for standby use, thereby obtaining a dynamic expansion and contraction composite nanofiltration membrane with membrane pores introduced with functional groups.

[0060] Figure 2 The SEM cross-sectional image of the dynamic expansion and contraction composite nanofiltration membrane with introduced functional groups obtained in this embodiment shows the pore structure of the basement membrane cross-section, and the membrane pores are evenly distributed. In addition, there are evenly distributed polypyrrole round particles in the pores, indicating that the binding sites of pyrrole have successfully entered the membrane pores and are very uniform.

[0061] Example 2

[0062] This embodiment provides a method for preparing a composite nanofiltration membrane with dynamic expansion and contraction of membrane pores with introduced functional groups, the preparation method comprising the following steps:

[0063] (1) Uniform dispersion of pyrrole binding sites

[0064] First, ferric chloride as an oxidant is added into deionized water to completely dissolve it, and a corresponding dopant (β-cyclodextrin) is added according to the introduced functional group to obtain an oxidant composite solution; in the oxidant composite solution, the oxidant content is 1 mol / L, and the dopant content with a functional group is 100 mmol / L;

[0065] The oxidant composite solution was coated on a polyethersulfone substrate membrane with a thickness of 200 μm and a pore size of 30 nm, and allowed to stand for 120 seconds, and then vacuum filtered until the membrane surface was completely dry. The vacuum filtration time was controlled to be 40 minutes and the pressure was 0.9 MPa, so that the oxidant was evenly dispersed on the membrane surface and in the membrane pores, and the membrane surface was yellow at this time;

[0066] (2) Preparation of membrane hole stretch film composite membrane

[0067] The substrate film treated in step (1) is placed in a vacuum dryer, and then a pyrrole solution with a concentration of 14 mol / L is placed in the vacuum dryer. Finally, the vacuum is sealed and evacuated to carry out a gas phase polymerization reaction. After reacting at 30°C for 15 minutes, the pyrrole will polymerize into polypyrrole in the presence of the oxidant. At this time, the membrane surface is black. The prepared thin film composite membrane is placed in an oven at 80°C for drying for 15 minutes, and then soaked in ultrapure water for standby use, thereby obtaining a dynamic expansion and contraction composite nanofiltration membrane with membrane pores introduced with functional groups.

[0068] Example 3

[0069] This embodiment provides a method for preparing a composite nanofiltration membrane with dynamic expansion and contraction of membrane pores with introduced functional groups, the preparation method comprising the following steps:

[0070] (1) Uniform dispersion of pyrrole binding sites

[0071] First, ferric chloride as an oxidant is added into deionized water to completely dissolve it, and a corresponding dopant (β-cyclodextrin) is added according to the introduced functional group to obtain an oxidant composite solution; in the oxidant composite solution, the oxidant content is 0.1 mol / L, and the content of the dopant with a functional group is 10 mmol / L;

[0072] The oxidant composite solution was coated on a polyethersulfone substrate membrane with a thickness of 100 μm and a pore size of 10 nm, and allowed to stand for 60 seconds, and then vacuum filtered until the membrane surface was completely dry. The vacuum filtration time was controlled to be 20 minutes and the pressure was 0.5 MPa, so that the oxidant was evenly dispersed on the membrane surface and in the membrane pores, and the membrane surface was yellow at this time;

[0073] (2) Preparation of membrane hole stretch film composite membrane

[0074] The substrate film treated in step (1) is placed in a vacuum dryer, and then a pyrrole solution with a concentration of 7 mol / L is placed in the vacuum dryer. Finally, the vacuum is sealed and evacuated to carry out a gas phase polymerization reaction. After reacting at 10°C for 8 minutes, the pyrrole will polymerize into polypyrrole in the presence of the oxidant. At this time, the membrane surface is black. The prepared thin film composite membrane is placed in a 50°C oven for drying for 8 minutes, and then soaked in ultrapure water for standby use, thereby obtaining a dynamic expansion and contraction composite nanofiltration membrane with membrane pores introduced with functional groups.

[0075] Example 4

[0076] This embodiment provides a method for preparing a composite nanofiltration membrane with dynamic expansion and contraction of membrane pores by introducing functional groups. Compared with Example 1, the only difference is that β-cyclodextrin is replaced by lauric acid of equimolar concentration, that is, the content of dopants with functional groups in the oxidant composite solution is still 50 mmol / L.

[0077] Example 5

[0078] This embodiment provides a method for preparing a composite nanofiltration membrane with dynamic expansion and contraction of membrane pores by introducing functional groups. Compared with Example 1, the only difference is that β-cyclodextrin is replaced with sodium dodecylbenzenesulfonate of equimolar concentration, that is, the content of dopants with functional groups in the oxidant composite solution is still 50 mmol / L.

[0079] Example 6

[0080] This embodiment provides a method for preparing a composite nanofiltration membrane with dynamic expansion and contraction of membrane pores by introducing functional groups. Compared with Example 1, the only difference is that β-cyclodextrin is replaced by sodium dodecyl sulfate of equimolar concentration, that is, the content of dopants with functional groups in the oxidant composite solution is still 50 mmol / L.

[0081] Comparative Example 1

[0082] This comparative example provides a method for preparing a composite nanofiltration membrane with dynamic membrane pore expansion and contraction. Compared with Example 1, the only difference is that the dopant with a functional group (β-cyclodextrin) in step (1) is completely omitted, that is, an oxidant solution containing only an oxidant is prepared.

[0083] Figure 3 The SEM cross-sectional view of the dynamic expansion and contraction composite nanofiltration membrane obtained in this comparative example shows that the polypyrrole successfully enters the pores and is evenly distributed in the pores, which is basically the same as Example 1. This shows that after the pyrrole reaction sites are adjusted twice by vacuum filtration, polypyrrole can be successfully polymerized in the pores, regardless of the specific components of the oxidant composite solution used.

[0084] Comparative Example 2

[0085] This comparative example provides a method for preparing a composite nanofiltration membrane with dynamic membrane pore expansion and contraction. Compared with Example 1, the only difference is that the vacuum filtration described in step (1) is completely omitted, that is, the polyethersulfone substrate membrane coated with the oxidant composite solution is allowed to stand for 90 seconds and directly placed in a vacuum dryer, and then a pyrrole solution with a concentration of 10 mol / L is placed in the vacuum dryer, and finally the vacuum is sealed and evacuated to carry out a gas phase polymerization reaction.

[0086] Figure 4 The SEM cross-sectional view of the composite nanofiltration membrane with dynamic membrane pore expansion obtained in this comparative example shows that the pore structure profile of the base membrane shows that the membrane pores are evenly distributed, but there is no polypyrrole in the pores. This is because the pyrrole polymerization sites are not adjusted by vacuum filtration after the oxidant is coated, resulting in almost all pyrrole polymerizing on the membrane surface and blocking the membrane pores, so there is no polypyrrole in the pores. Although the polypyrrole accumulated on the membrane surface will undergo volume relaxation under electrochemical action, the effect of its volume change on the membrane pore size is very limited.

[0087] The membrane pore dynamic expansion and contraction composite nanofiltration membranes prepared in the above examples and comparative examples were tested for desalination performance, and the specific contents are as follows:

[0088] A specific membrane assembly is used to test the desalination performance of the dynamic expansion and contraction composite nanofiltration membrane. Two electrodes extend from the inside of the membrane assembly, one of which is connected to the membrane surface and the other is opposite to the membrane surface. When the membrane surface is connected to the negative electrode, the membrane acts as a cathode and a reduction reaction occurs; when the membrane surface is connected to the positive electrode, the membrane acts as an anode and an oxidation reaction occurs. By switching between the positive and negative electrodes, the membrane undergoes an oxidation-reduction reaction and adjusts the in-situ change of the membrane pore size. During the test, 1g / L Na 2 SO 4 The solution was used as the inlet solution to measure the dynamic expansion and contraction of the composite nanofiltration membrane after applying the redox potential to sodium sulfate (Na 2 SO 4 ) retention rate and flux changes.

[0089] Figure 5 The corresponding sodium sulfate (Na 2 SO 4 ) shows the retention rate and flux change curves. It can be seen that when the reduction potential is applied, the salt rejection rate of the membrane increases and the flux decreases. When the oxidation potential is applied, the salt rejection rate of the membrane decreases and the flux increases. In the cyclic switching cycles of several working potentials, the salt rejection rate and flux of the membrane change periodically with the potential switching, where the retention rate changes in the range of 14.5% and the flux changes in the range of about 4.5LMH. Figure 6 The sodium sulfate (Na 2 SO 4 ) shows that the salt rejection and flux of the membrane also change periodically with the potential switching, where the range of the rejection rate is 10.3% and the range of the flux is 3.1LMH; Figure 7 The sodium sulfate (Na 2 SO 4 ), it can be seen from the retention rate and flux variation curve of Example 1 that the membrane prepared at this time has almost no ability to change the desalination performance with the potential switching, wherein the retention rate variation range is 1.5%, and the flux variation range is 0.5LMH, that is, the retention rate and flux variation range corresponding to Example 1 are higher than the retention rate and flux variation range corresponding to Comparative Example 1 and Comparative Example 2, indicating that the desalination performance of the electrochemical membrane pore expansion and contraction thin film composite nanofiltration membrane prepared in Example 1 is greatly enhanced.

[0090] The specific experimental results are summarized in Table 1.

[0091] Table 1

[0092]

[0093]

[0094] From Table 1, we can see the following points:

[0095] (1) The membrane pore dynamic expansion and contraction composite nanofiltration membranes provided in Examples 4 to 6 respectively introduce carboxyl groups, benzenesulfonic acid groups and sulfonic acid groups. Compared with the β-cyclodextrin in Example 1, the functional group abundance introduced in Examples 4 to 6 is lower, and the dopants are all long-chain structures, and the regulation ability of ion transport is not as good as that of the macrocyclic β-cyclodextrin;

[0096] (2) Comparing Example 1 with Comparative Example 1, since the dopant with functional groups (β-cyclodextrin) is completely omitted in Comparative Example 1, the membrane pore dynamic expansion and contraction composite nanofiltration membrane prepared in Comparative Example 1 does not contain functional groups, and only regulates the transmission of ions through the effect of pore expansion and contraction, and the desalination performance is poor;

[0097] (3) Comparing Example 1 with Comparative Example 2, since vacuum filtration was completely omitted in Comparative Example 2, the pyrrole polymerization sites were not adjusted by vacuum filtration after the oxidant coating, resulting in the pyrrole being almost entirely polymerized on the membrane surface and blocking the membrane pores, so there was no polypyrrole in the pores; although the polypyrrole accumulated on the membrane surface would undergo volume relaxation under electrochemical action, the effect of its volume change on the membrane pore size was very limited; the corresponding desalination performance was significantly reduced;

[0098] (4) The preparation method of the present invention can achieve the introduction of different functional groups into the thin film composite nanofiltration membrane by adjusting the type of the oxidant composite solution, and secondary adjust the binding sites of pyrrole by vacuum filtration, so that the oxidant is evenly dispersed on the membrane surface and in the membrane pores. The membrane pores can be dynamically adjusted by the working voltage. Due to the coupling effect of pore size expansion and contraction and the action of functional groups, the adjustment range of the desalination performance of the membrane is greatly enhanced, the range of retention rate variation exceeds 13%, and the range of flux variation exceeds 3.5LMH.

[0099] The present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0100] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0101] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0102] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A composite nanofiltration membrane with dynamic expansion and contraction of membrane pores with functional groups introduced, characterized in that: The composite nanofiltration membrane with dynamic expansion and contraction of membrane pores with introduced functional groups comprises a porous polymer substrate membrane and a polypyrrole functional layer containing functional groups, wherein the polypyrrole functional layer containing functional groups is located on the surface of the porous polymer substrate membrane and inside the membrane pores.

2. The composite nanofiltration membrane with dynamic expansion and contraction of membrane pores with introduced functional groups according to claim 1, characterized in that: The thickness of the porous polymer substrate membrane is 100 to 200 μm; Preferably, the pore size of the porous polymer substrate membrane is 10 to 30 nm; Preferably, the polymer of the porous polymer substrate membrane includes any one of polyvinylidene fluoride, polyethersulfone, cellulose acetate and polyamide, preferably polyethersulfone.

3. A method for preparing a composite nanofiltration membrane with dynamic expansion and contraction of membrane pores with introduced functional groups as claimed in claim 1 or 2, characterized in that: The preparation method comprises the following steps: (1) preparing an oxidant composite solution, wherein the oxidant composite solution contains an oxidant and a dopant with a functional group, wherein the functional group of the dopant with a functional group includes at least one of a hydroxyl group, a carboxyl group, a benzenesulfonic acid group or a sulfonic acid group; coating the oxidant composite solution on a porous polymer substrate membrane, and performing vacuum filtration; (2) placing the substrate film treated in step (1) in a vacuum dryer and performing a gas phase polymerization reaction in an atmosphere of pyrrole monomer to form a polypyrrole functional layer containing functional groups, thereby obtaining a composite nanofiltration membrane with dynamic membrane pore expansion and contraction and introducing functional groups.

4. The preparation method according to claim 3, characterized in that: The oxidant in step (1) comprises at least one of ferric chloride, ammonium persulfate, potassium persulfate or sodium persulfate; Preferably, the dopant with a functional group includes at least one of β-cyclodextrin, lauric acid, sodium dodecylbenzene sulfonate or sodium dodecyl sulfonate.

5. The preparation method according to claim 3 or 4, characterized in that: In the oxidant composite solution of step (1), the oxidant content is 0 to 1 mol / L, excluding 0 mol / L, and the dopant content with a functional group is 0 to 100 mmol / L, excluding 0 mmol / L.

6. The preparation method according to any one of claims 3 to 5, characterized in that: In step (1), after the coating and before the vacuum filtration, the method further comprises standing; Preferably, the standing time is 60 to 120 seconds.

7. The preparation method according to any one of claims 3 to 6, characterized in that: The vacuum filtration time in step (1) is 20 to 40 minutes; Preferably, the pressure of the vacuum filtration in step (1) is 0.5-0.9 MPa.

8. The preparation method according to any one of claims 3 to 7, characterized in that: In step (2), the porous polymer substrate membrane treated in step (1) is first placed in a vacuum dryer, and then the pyrrole solution is placed in the vacuum dryer, and finally the vacuum dryer is sealed and evacuated; Preferably, the concentration of the pyrrole solution is 7 to 14 mol / L; Preferably, the gas phase polymerization reaction time in step (2) is 8 to 15 minutes; Preferably, the temperature of the gas phase polymerization reaction in step (2) is 10 to 30°C.

9. The preparation method according to any one of claims 3 to 8, characterized in that: After the gas phase polymerization reaction in step (2), the obtained thin film composite membrane is dried; Preferably, the drying temperature is 50-80°C; Preferably, the drying time is 8 to 15 minutes.

10. The preparation method according to any one of claims 3 to 9, characterized in that: The composite nanofiltration membrane with dynamic expansion and contraction of membrane pores and functional groups introduced therein obtained in step (2) is placed in ultrapure water for standby use.

Citation Information

Cited By

  • A loose nanofiltration membrane and a method for preparing the same

    CN122806302A