Porous catalyst for desulfurization and denitrification
By using porous manganese oxide-loaded catalysts for V2O5 and CeO2 in flue gas treatment, the problems of low flue gas desulfurization and denitrification efficiency and complex material preparation in the prior art are solved, and efficient flue gas treatment and material stability are achieved.
Patent Information
- Application Number
- CN202411139966.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The existing flue gas desulfurization and denitrification technology has problems such as low efficiency and complex material preparation process, especially the activity of manganese oxide catalysts is limited by the load amount and load method.
Porous manganese oxide MO is used as the matrix, supported by V2O5 and CeO2, and a porous structure is formed through high-temperature calcination and microwave ultrasonic reaction. It is used as a desulfurization and denitrification catalyst to increase the specific surface area and porosity of the catalyst and enhance catalytic activity.
The desulfurization efficiency of more than 85% and the desulfurization efficiency of more than 94% is achieved, the efficiency of flue gas treatment is improved, and the structural stability and dispersion of the catalyst are good, and the material preparation is relatively simplified.
Smart Images

Figure CN119034720A_ABST
Abstract
Description
[Technical field]
[0001] The invention belongs to the field of industrial catalysis, and in particular relates to a desulfurization and denitrification porous catalyst for flue gas treatment.
Technical Background
[0002] Excessive emission of SO2 and NOx in industrial production processes can lead to various environmental problems such as acid rain, photochemical smog, ozone layer destruction and greenhouse effect, affecting human life, health and safety. Therefore, countries have put forward strict requirements on the control technology of atmospheric pollutant emissions from coal-fired power plants. Most coal-fired power plants are equipped with dust removal, desulfurization and denitrification staged treatment devices. This process has the advantages of strong selectivity and relative stability in treating pollutants. In order to improve the treatment effect and shorten the process, researchers have invented the flue gas simultaneous desulfurization and denitrification technology, which can remove SO2 and NOx simultaneously in the flue gas treatment unit. Among them, the more representative methods are adsorption regeneration technology, plasma technology, catalytic reduction technology and catalytic oxidation technology.
[0003] Catalytic reduction technology is to install the activated reduction catalyst in the reactor and introduce reducing gases such as H2, CH4, NH3, CO, etc. When the polluted flue gas passes through, the reduction catalyst combines with the reducing gas to react with SO2 and NOx in the polluted flue gas. SO2 in the polluted flue gas will be reduced to S element, which can be recycled after treatment. NOx in the polluted flue gas will be reduced to N2, which will not pollute the atmosphere and can be directly discharged into the atmosphere after the reaction. Commonly used catalysts are precious metal elements such as Pd, Pt, etc., transition metals, rare earth element catalysts, and perovskite-type and solid solution-type catalysts.
[0004] Catalytic oxidation technology is to oxidize SO2 in polluted flue gas into SO3 and NO into higher valence NOx, which are then absorbed and removed in subsequent devices. In the process of catalytic reaction, reducing gas is not used, and the oxidation catalyst currently used does not use precious metal elements, saving a lot of costs. Commonly used catalysts include iron oxide catalysts and manganese oxide catalysts.
[0005] Manganese oxide catalysts show good activity in the process of oxidative denitrification mainly because manganese has variable chemical valence states (Mn2+, Mn3+, Mn4+). The preparation of manganese oxide catalysts is often loaded onto Al2O3 carriers as active components, and their activity is subject to factors such as loading amount and loading method. Although the existing flue gas desulfurization and denitrification technologies have many active components, they still have problems such as low efficiency and complex material preparation processes. [Summary of the invention]
[0006] To achieve the above purpose, the present invention provides a porous catalyst for desulfurization and denitration, wherein the catalyst uses manganese oxide MO as a porous carrier for denitration, and the porous carrier provides loading sites for active desulfurization catalyst vanadium oxide and cerium oxide. The catalyst is represented by MO / Ce, V, and MO is obtained by high-temperature calcination of a metal organic framework compound. The specific scheme of the present invention is:
[0007] A porous catalyst for desulfurization and denitrification, the catalyst MO / Ce, V, takes porous manganese oxide MO as a matrix and loads V2O5 and CeO2.
[0008] The molar contents of V2O5 and CeO2 relative to the porous manganese oxide MO are 0.01-0.05 and 0.01-0.05.
[0009] The porous manganese oxide matrix is a honeycomb-like porous structure.
[0010] The V2O5 and CeO2 are loaded on the surface of the porous manganese oxide.
[0011] The specific surface area of the catalyst is 65.1 m 2 / g, porosity is 0.52cm 3 / g.
[0012] The desulfurization efficiency and denitrification efficiency of the porous catalyst are respectively above 85% and 94%.
[0013] The present invention also provides a method for preparing a porous desulfurization and denitrification catalyst, which includes preparing a porous manganese oxide MO matrix, dissolving an organic manganese source and terephthalic acid in a solvent, then subjecting the mixture to a solvent thermal reaction in a high-pressure reactor, and separating the product and calcining it in a high-temperature furnace.
[0014] The preparation method also includes loading of a porous manganese oxide MO matrix, wherein the loading method comprises dispersing the calcined product in a vanadium salt solution, heating and stirring, and then calcining; dispersing the calcined product in a cerium salt solution, subjecting the solution to microwave ultrasonic reaction, and then calcining to obtain the catalyst.
[0015] The organic manganese source is selected from manganese nitrate, manganese chloride, and manganese acetate; the solvent is selected from DMF, ethanol, and methanol; the solvent thermal temperature is 100-180° C., and the solvent thermal time is 10-18 hours; and the molar ratio of the organic manganese source to terephthalic acid is 1:2 to 2:1.
[0016] The vanadium salt solution is a mixed solution of ammonium metavanadate and oxalic acid, and the molar ratio of the two is 1:1.
[0017] The heating and stirring conditions are heating and stirring at 60°C for 3h;
[0018] The roasting and calcining process conditions are the same, both of which are to increase the temperature to 300° C. at a heating rate of 5° C. / min and keep the temperature for 4 hours.
[0019] The porous manganese oxide MO of the present invention is an organic metal framework structure formed by organic manganese salt and ligand terephthalic acid under high temperature and high pressure. The framework structure compound is calcined to form a porous morphology. The manganese oxide actually exists mainly in the form of Mn3O4 and Mn2O3. As a catalyst component for flue gas denitration, it has the characteristics of ultra-high specific surface area, hierarchical pore size distribution and chemical stability. The nanoparticles prepared after calcination have more uniform size and better dispersibility, and maintain the original porosity and morphology of the template. The porous structure is used as a carrier for subsequent loading of desulfurization active components, and the porous structure is used as a catalytic channel for denitration.
[0020] The desulfurization active component of the present invention uses V2O5 mainly because V2O5 has an activated coordination site and thus has a strong redox ability, and can oxidize SO2 to SO3 and then reduce itself to keep its own properties unchanged. The V element easily reacts with metal oxides on the surface of MO. The desulfurization active component V2O5 is prepared by the reaction of ammonium metavanadate and oxalic acid. The active component V2O5 and the auxiliary agent CeO2 are loaded by a partial impregnation method, rather than directly mixing vanadium salts and cerium salts, to avoid the reaction of oxalic acid with CeO2.
[0021] The present invention selects CeO2 as an auxiliary agent for the desulfurization catalyst based on the fact that cerium oxide has good oxygen storage properties, which makes the catalyst have good redox ability. After V2O5 reacts with CeO2, the Ce element exists in the form of Ce3+. Compared with CeO2, the valence of the Ce element has changed. At the same time, the V element easily reacts with CeO2 to form a VO-Ce bond, which improves the catalytic activity of the V-based catalyst and greatly improves the catalytic ability of the catalyst. In addition, when the framework structure of MO is used as the matrix, V2O5 and CeO2 can be evenly distributed on the framework structure of MO, the catalyst has good dispersibility inside, the overall structure is stable, the addition of auxiliary agents is conducive to the loading of vanadium elements, and the improvement of the MO catalyst is further improved, which helps to improve the efficiency of SO2 removal.
[0022] The MO catalyst was prepared by thermal decomposition: first, organic manganese and terephthalic acid were dissolved in DMF respectively. After ultrasonic treatment and stirring, the mixed solution was transferred to a polytetrafluoroethylene reactor for high temperature reaction for a certain period of time. After completion, the precipitate was collected by centrifugation, washed and dried. The white powder of the obtained metal organic framework compound was placed in a tube furnace and heated to 300°C for insulation. A black powder was obtained, namely the manganese oxide catalyst MO.
[0023] Weigh the manganese oxide catalyst MO, disperse it in deionized water, add the solution of vanadate and oxalic acid, heat and stir to mix thoroughly, vacuum dry and grind, place in a dry and clean ceramic crucible and calcine in a muffle furnace.
[0024] Weigh the calcined product and evenly disperse it in deionized water, then weigh a certain amount of cerium metal salt and add it to the above dispersion, and stir continuously after ultrasonic treatment at room temperature. After standing at room temperature, remove the supernatant. Place the obtained lower solid precipitate in an oven. After drying, grind the sample into powder and calcine it in a tube furnace. After the reaction is completed, cool the sample to room temperature to obtain a black powder, which is the catalyst MO / Ce,V.
[0025] One of the improvements of the present invention is to use denitrification manganese oxide as a carrier, combined with a desulfurization catalyst, to achieve simultaneous desulfurization and denitrification.
[0026] The improvement of the present invention is that the porous structure of manganese oxide MO provides more loading sites for active components, which can generate more active sites during the reaction process, increase the contact opportunities with pollutants, and improve the reaction efficiency. The three metals have a synergistic effect, which improves the desulfurization and denitrification effects of the catalyst as a whole, and the desulfurization efficiency and denitrification efficiency of flue gas are 85% and 94% or more respectively.
Brief Description of the Drawings
[0027] Figure 1 XRD characterization diagram of the product
[0028] Figure 2 SEM morphology of the product
[0029] [Example 1]
[0030] Step 1: Dissolve 1.42g of manganese acetate and 1.08g of terephthalic acid in 30ml of DMF, respectively. Ultrasonic treatment for 20min, stirring for 30min, transfer the mixed solution to a 50ml polytetrafluoroethylene reactor, react at 100℃ for 10h, collect the precipitate by centrifugation after the reaction is completed, wash three times with deionized water and anhydrous ethanol respectively, and dry at 80℃ overnight. Finally, a white powder is obtained.
[0031] Step 2: Place the synthesized white powder in a tube furnace, heat it to 300° C. at a heating rate of 5° C. / min, and keep it at that temperature for 4 hours to obtain the desired black powder, i.e., the manganese oxide catalyst matrix MO.
[0032] Step 3: Weigh 1.014g of manganese oxide catalyst matrix MO and evenly disperse it in 10mL of deionized water. The molar ratio of addition is 1:1. Weigh 0.4592g of ammonium metavanadate and 0.25g of oxalic acid (the molar ratio of vanadium to the matrix is 2.5%). Heat and stir at 60°C for 3h until it is fully mixed; dry the heated and stirred catalyst at 105°C in a vacuum drying oven for 12 hours; take out the dried catalyst, grind it, place it in a dry and clean ceramic crucible, and roast it in a muffle furnace for 5h.
[0033] Step 4: Weigh 1.014g of the product prepared in step 3 and evenly disperse it in 10mL of deionized water. Then weigh 0.85g of Ce(NO3)3·6H2O (the molar ratio of cerium to the matrix is 2.5%) and add it to the dispersion of the above powder. Ultrasonic treatment is carried out at room temperature for 30min, and then continuous stirring is carried out for 2h. After standing at room temperature for 30min, the supernatant is removed. The obtained lower solid precipitate is placed in an oven and dried at 100℃ for 12h. After drying, the sample is ground into powder and placed in a tube furnace. It is calcined in an air atmosphere with an initial temperature of 20℃, a heating rate of 5℃ / min, and a calcination temperature of 300℃ for 4h. After the reaction is completed, the sample is cooled to room temperature to obtain a black powder, which is the desulfurization and denitrification catalyst MO / Ce,V.
[0034] [Example 2]
[0035] Step 1: Dissolve 1.42g of manganese acetate and 1.08g of terephthalic acid in 30ml of DMF, respectively. Ultrasonic treatment for 20min, stirring for 30min, transfer the mixed solution to a 50ml polytetrafluoroethylene reactor, react at 180℃ for 18h, collect the precipitate by centrifugation after the reaction is completed, wash three times with deionized water and anhydrous ethanol respectively, and dry at 80℃ overnight. Finally, a white powder product is obtained.
[0036] Step 2: Place the synthesized white powder in a tube furnace, heat it to 300° C. at a heating rate of 5° C. / min, and keep it at that temperature for 4 hours to obtain the desired black powder, i.e., the manganese oxide catalyst matrix MO.
[0037] Step 3: Weigh 1.014g of manganese oxide catalyst matrix MO and evenly disperse it in 10mL of deionized water. The molar ratio of addition is 1:1. Weigh 0.4592g of ammonium metavanadate and 0.4949g of oxalic acid (the molar ratio of vanadium to the matrix is 5%). Heat and stir at 60°C for 3h until it is fully mixed; dry the heated and stirred catalyst at 105°C in a vacuum drying oven for 12 hours; take out the dried catalyst, grind it, place it in a dry and clean ceramic crucible, and roast it in a muffle furnace for 5h.
[0038] Step 4: Weigh 1.014g of the product prepared in step 3 and evenly disperse it in 10mL of deionized water. Then weigh 1.71g of Ce(NO3)3·6H2O (the molar ratio of cerium to the matrix is 5%) and add it to the dispersion of the above powder. Ultrasonic treatment is carried out at room temperature for 30min, and then continuous stirring is carried out for 2h. After standing at room temperature for 30min, the supernatant is removed. The obtained lower solid precipitate is placed in an oven and dried at 100℃ for 12h. After drying, the sample is ground into powder and placed in a tube furnace. It is calcined for 4h in an air atmosphere with an initial temperature of 20℃, a heating rate of 5℃ / min, and a calcination temperature of 300℃. After the reaction is completed, the sample is cooled to room temperature to obtain a black powder, which is the desulfurization and denitrification catalyst MO / Ce,V.
[0039] [Comparative Example 1]
[0040] Step 1 and step 2 are the same as in Examples 1 and 2.
[0041] Step 3: Weigh 1.014g of manganese oxide catalyst matrix MO and evenly disperse it in 10mL of deionized water. The molar ratio of addition is 1:1. Weigh 0.4592g of ammonium metavanadate and 0.4949g of oxalic acid (the molar ratio of vanadium to the matrix is 5%). Heat and stir at 60°C for 3h until it is fully mixed; dry the heated and stirred catalyst at 105°C in a vacuum drying oven for 12 hours; take out the dried catalyst, grind it, place it in a dry and clean ceramic crucible, and roast it in a muffle furnace for 5h to obtain the product catalyst MO / V.
[0042] [Comparative Example 2]
[0043] Step 1 and step 2 are the same as in Examples 1 and 2.
[0044] Step 3, weigh 1.014g of the product prepared in step 2, disperse it evenly in 10mL of deionized water, then weigh 1.71g of Ce(NO3)3·6H2O (the molar ratio of cerium to the matrix is 5%) and add it to the dispersion of the above powder, ultrasonically treat at room temperature for 30min, and then stir continuously for 2h. After standing at room temperature for 30min, remove the supernatant. Place the obtained lower solid precipitate in an oven and dry it at 100℃ for 12h. After drying, grind the sample into powder and place it in a tube furnace, and calcine it in an air atmosphere with an initial temperature of 20℃, a heating rate of 5℃ / min, and a calcination temperature of 300℃ for 4h. After the reaction is completed, cool the sample to room temperature to obtain a black powder, and obtain the product catalyst MO / Ce.
[0045] [Comparative Example 3]
[0046] Step 1 and step 2 are the same as in Examples 1 and 2.
[0047] Step 3: Weigh 1.014g of manganese oxide catalyst matrix and evenly disperse it in 10mL of deionized water. The molar ratio of addition is 1:1. Weigh 0.4592g of ammonium metavanadate, 0.4949g of oxalic acid, and 1.71g of Ce(NO3)3·6H2O. Heat and stir at 60℃ for 3h until it is fully mixed; dry the heated and stirred catalyst at 105℃ in a vacuum drying oven for 12h; take out the dried catalyst, grind it, place it in a dry and clean ceramic crucible, and calcine it in a muffle furnace for 5h.
[0048] Effect detection:
[0049] Figure 1 The XRD spectrum of the product is shown in the figure. The XRD spectrum of MnO derived from the manganese metal organic framework can be seen from the figure. As can be seen from the figure, diffraction peaks appear at 2θ of 18.3°, 29.2°, 32.7°, 36.4°, 44.7°, 51.1°, 60.2°, etc. After consulting the relevant data analysis, it can be obtained that they correspond to the characteristic diffraction peaks of Mn3O4 (JCPDS24-0734). The diffraction peaks at 23.0°, 32.8°, 38.1°, 45.2°, 49.2°, 55.0°, and 67.4° can well correspond to the characteristic diffraction peaks of the standard Mn2O3 sample (JCPDS41-1442). 28.549°, 33.083°, 46.486°, 56.346°, and 59.093° are weak diffraction peak patterns of CeO2, and 26.759°, 34.742°, 36.23°, and 41.289 are weak diffraction peak patterns of V2O5. This shows that the manganese oxide catalyst mainly exists in the form of Mn3O4 and Mn2O3, with a small amount of CeO2 and V2O5.
[0050] Figure 2 This is the SEM image of the product. It can be seen from the image that the surface of the matrix is a porous structure with high porosity. A large number of particles are loaded in the gaps of the matrix. The small particles are CeO2 and V2O5 particles. Figure 1 and 2 It can be seen that the catalyst achieves effective loading of vanadium oxide and cerium oxide, and the specific surface area of the catalyst is 65.1m 2 / g, porosity is 0.52cm 3 / g.
[0051] As for the catalytic effect, the product catalyst obtained in the embodiment of the present invention was passed through flue gas containing NO and SO2, and the conversion rate was measured after catalysis at 260°C for 8 hours. The results are shown in the following table.
[0052]
[0053]
[0054] The gas after the reaction was tested by a flue gas analyzer. NO2 was detected in the gas product after the denitrification experiment, indicating that the catalytic reaction oxidized NO to NO2; the gas after the desulfurization experiment was passed into HCl+BaCl2 solution, and a white precipitate was produced after a period of time, indicating that SO2 was oxidized to SO3 through the catalytic reaction, and the generated SO3 reacted with the BaCl2 solution to generate BaSO4 precipitate.
[0055] The present invention selects CeO2 to react with V2O5 to form CeVO4 with higher oxidation activity, which can further promote the oxidation process of SO2 to SO3 and improve the desulfurization efficiency. The denitrification reaction mainly uses MnOx as the active component, because the metal oxide has good oxidation activity and can oxidize NO into higher valence NOx. When the auxiliary agent CeO2 is added, at a higher calcination temperature, the cerium oxide keeps the internal lattice of the catalyst stable, prevents the crystal form from changing in other directions, and allows the grains to remain in a finer state, which also allows more active sites to be retained. The synergistic effect between vanadium and manganese is mainly manifested in the process of co-impregnation. Vanadium and manganese will form a VO-Mn bond. During the reaction, the highly active MnVOx will undergo an oxidation reaction and eventually generate Mn(I)V (4+) O x-1 In addition, in the presence of manganese, it can promote the reduction of vanadium, thus improving the overall desulfurization and denitrification effect of the catalyst. It can also improve the regeneration capacity of Mn, thereby promoting the denitrification of the catalyst, and ultimately improving the catalytic efficiency of simultaneous desulfurization and denitrification.
[0056] Although the present invention is described herein with reference to a number of illustrative embodiments of the present invention, it will be appreciated that those skilled in the art will be able to devise many other modifications and implementations that will fall within the scope and spirit of the principles disclosed herein. More specifically, within the scope of the present disclosure and claims, a variety of variations and improvements can be made to the components and / or layout of the subject combination layout. In addition to the variations and improvements made to the components and / or layout, other uses will also be apparent to those skilled in the art.
Claims
1. A porous catalyst for desulfurization and denitrification, It is characterized in that The catalyst is based on porous manganese oxide MO and loaded with V 2 O 5 and CeO 2 .
2. A desulfurization and denitrification porous catalyst according to claim 1, It is characterized in that The V 2 O 5 and CeO 2 The molar content of MO relative to the porous manganese oxide is 0.01-0.05, 0.01-0.
05.
3. A porous catalyst for desulfurization and denitrification according to claim 1, It is characterized in that The porous manganese oxide matrix is a honeycomb-like porous structure. 2 O 5 and CeO 2 Loaded on the surface of porous manganese oxide.
4. A desulfurization and denitrification porous catalyst according to claim 1, It is characterized in that The specific surface area of the catalyst is 65.1 m 2 / g, porosity is 0.52cm 3 / g.
5. A method for preparing a porous catalyst for desulfurization and denitrification as claimed in claim 1, It is characterized in that The method includes, Preparation of porous manganese oxide MO matrix: organic manganese source and terephthalic acid are dissolved in a solvent, and then solvent thermal reaction is carried out in a high-pressure reactor, and the product is separated and calcined in a high-temperature furnace; Loading of porous manganese oxide MO matrix: The loading method is to disperse the calcined product in a vanadium salt solution, heat and stir, and then calcine; disperse the calcined product in a cerium salt solution, perform microwave ultrasonic reaction, and then calcine to obtain the catalyst.
6. The method for preparing a porous catalyst for desulfurization and denitration according to claim 5, It is characterized in that The organic manganese source is selected from manganese nitrate, manganese chloride, and manganese acetate; and the solvent is selected from DMF, ethanol, and methanol.
7. The method for preparing a porous catalyst for desulfurization and denitration according to claim 5, It is characterized in that The solvent thermal temperature is 100-180° C., and the solvent thermal time is 10-18 hours. The molar ratio of the organic manganese source to terephthalic acid is 1:2 to 2:
1.
8. The method for preparing a porous catalyst for desulfurization and denitration according to claim 5, It is characterized in that The vanadium salt solution is a mixed solution of ammonium metavanadate and oxalic acid, and the molar ratio of the two is 1:1; The heating and stirring conditions are heating and stirring at 60° C. for 3 hours.
9. The method for preparing a porous catalyst for desulfurization and denitration according to claim 5, It is characterized in that The roasting and calcining process conditions are the same, both of which are to increase the temperature to 300° C. at a heating rate of 5° C. / min and keep the temperature for 4 hours.
10. A method for preparing a porous catalyst for desulfurization and denitration according to any one of claims 1 to 4, It is characterized in that The application of the preparation method in flue gas desulfurization and denitrification conversion.
Citation Information
Patent Citations
Composite smoke denitration catalyst capable of oxidizing zero-valence mercury
CN102350340A
Load type cobalt and manganese compound oxide catalyst and preparation method of load type cobalt and manganese compound oxide catalyst
CN105251506A
Manganese oxide nanotube loading type denitration catalyst and preparation method therefor
CN106179326A
Manganese oxide loaded cerium oxide catalyst, preparation and application
CN106693954A
Preparation method of novel porous carbon nanosheets
CN107032407A
Cited By
Preparation process of low-nitrogen-content reagent-grade sulfuric acid
CN121672428A
Process for the preparation of a reagent grade sulfuric acid with low nitrogen content
CN121672428B