Core-shell structure copper-based molecular sieve monolithic SCR catalyst and preparation method thereof

The copper-based molecular sieve SCR catalyst with a core-shell structure utilizes transition metal oxides to coat the copper-based molecular sieve, avoiding phosphorus poisoning, improving low-temperature denitrification performance and service life, and solving the shortcomings of existing catalysts in phosphorus poisoning. It is suitable for the treatment of automobile exhaust and power plant waste gas.

CN119034798APending Publication Date: 2024-11-29KAILONG HIGH TECH CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411157086.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Existing SCR catalysts have insufficient resistance to phosphorus poisoning in exhaust gases, resulting in denitrification performance degradation, difficult regeneration, and high cost, making it difficult to meet the needs of industrial applications.

Method used

The core-shell structure design uses a copper-based molecular sieve as the core and a porous shell structure formed by coating with transition metal oxides to avoid direct contact between the active center and phosphorus-containing substances. It is then coated on a ceramic support to form an integral catalyst.

Benefits of technology

It significantly improves the catalyst's resistance to phosphorus poisoning, maintains its low-temperature denitrification performance, extends its service life, reduces costs, and is suitable for large-scale treatment of automobile exhaust and power plant waste gas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119034798A_ABST
    Figure CN119034798A_ABST
Patent Text Reader

Abstract

The invention provides a core-shell structure copper-based molecular sieve monolithic SCR catalyst and a preparation method thereof.The catalyst comprises an active component and a carrier, the active component is of a core-shell structure and comprises a copper-based molecular sieve and a transition metal oxide, the copper-based molecular sieve serves as a core, the transition metal oxide serves as a porous shell structure, and the carrier comprises a ceramic carrier. The preparation method comprises the following steps: respectively preparing a copper-based molecular sieve and a transition metal precursor sol; uniformly mixing the two components, drying and roasting to obtain an active component with a core-shell structure; mixing with an adhesive and a thickening agent, coating a ceramic carrier with the slurry, and drying and roasting to obtain the catalyst. Through the design of the core-shell structure, the copper-based molecular sieve is used as the core, and the shell is designed into a porous shell structure, so that the low-temperature denitration performance is excellent; the core-shell junction can prevent active species in the copper-based molecular sieve from being in direct contact with phosphorus-containing substances, so that the phosphorus poisoning resistance of the catalyst is improved, and the service life of the catalyst is prolonged; the preparation method is simple, low in cost and wide in application range.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalyst preparation, and relates to a core-shell structure copper-based molecular sieve integral SCR catalyst and a preparation method thereof. Background Art

[0002] With the rapid economic development and the acceleration of industrialization, the production and ownership of automobiles have shown a high-speed growth trend. Nitrogen oxides in automobile exhaust have a significant impact on the environment and are an important factor causing air pollution problems such as haze. Among all types of motor vehicles, diesel vehicles have the largest proportion of nitrogen oxide emissions. In addition, there are also significant nitrogen oxide emissions in the fuel combustion process of industrial production, as well as nitric acid production, nitration process, explosive production and metal surface nitric acid treatment processes. Since nitrogen oxides can easily cause a variety of diseases and affect human health, it is also necessary to control the emission of nitrogen oxides from this aspect. Therefore, reducing the content of nitrogen oxides in motor vehicle exhaust and fixed source exhaust has become an important measure to control pollution sources and protect the atmospheric environment.

[0003] The SCR catalytic reaction is a reaction process that uses ammonia to selectively catalytically reduce nitrogen oxides to harmless nitrogen. The catalyst used is the SCR catalyst. Currently, commonly used SCR catalysts include vanadium-tungsten-titanium catalysts, copper / iron-based molecular sieve catalysts, etc. Among them, copper-based molecular sieve catalysts are one of the most widely used SCR catalysts in nitrogen oxide emission reduction due to their excellent low-temperature performance and good hydrothermal stability. Depending on the source of the exhaust gas, impurity elements such as phosphorus and sulfur will inevitably exist, which may cause catalyst poisoning. For example, when phosphorus-containing compounds are present, copper-based molecular sieve catalysts are prone to poisoning, resulting in a significant decrease in denitrification performance, and once poisoned, it is difficult to regenerate and restore the catalyst performance.

[0004] At present, although the prior art also involves the preparation of core-shell structure SCR catalyst, its anti-poisoning ability is not mentioned, but the poisoned catalyst is regenerated. CN 110639609A discloses a core-shell structure Cu / SAPO-34@meso-TiO2 catalytic material and its preparation method and application. The catalyst material is a meso-TiO2 shell layer coated on the surface of Cu / SAPO-34 molecular sieve, and the meso-TiO2 shell layer is composed of TiO2, WO3, and SiO2. The content of TiO2 is 0.5-2% of the total mass of the catalytic material, and the content of WO3 and SiO2 accounts for 3-10% and 3-6% of the total mass of the meso-TiO2 shell layer respectively. The focus of the catalytic material is the shell layer coated on the surface and its composition, rather than the composition and structure of the core in the core-shell structure. It is also not clear that the catalytic material is loaded on a carrier when in use, and the catalytic material has anti-sulfur poisoning performance, but it is not clear that it has the ability to resist phosphorus poisoning.

[0005] CN 113797963A discloses a highly alkali-resistant composite denitrification powder and a preparation method thereof. The composite denitrification powder is obtained by using a solid superacid-modified core-shell structure CHA / AEI molecular sieve and TiO2 as carriers to load denitrification active ingredients and additives. The solid superacid is the shell and the CHA / AEI molecule is the core. Although the composite denitrification powder also includes a core-shell structure, the improved core-shell structure is used as a carrier and does not include a denitrification active ingredient. This is different from the traditional core-shell structure in which the core is used as an active component. According to the composition of the composite denitrification powder, it has a strong ability to resist alkali poisoning, but does not involve whether it has the ability to resist phosphorus poisoning.

[0006] CN 106607106A discloses a method for active regeneration and performance optimization of a sulfur, arsenic and phosphorus poisoned SCR catalyst, which comprises: firstly cleaning the dust of the deactivated SCR denitration catalyst, then ultrasonically cleaning, rinsing with deionized water, immersing in a regeneration liquid, then drying, roasting, crushing, sieving, washing with water, and acid washing; wet crushing and grinding to obtain a catalyst slurry, then mixing the catalyst slurry with a metatitanic acid slurry, filtering, adding water, and bleaching with a trivalent titanium reducing agent, then adding ammonium paratungstate and white carbon black, stirring, filtering, dehydrating, calcining, and crushing to obtain a WO3-SiO2-TiO2 composite powder. This method is mainly used for regenerating deactivated SCR catalysts, and the process is complicated, the reagents used are various, the cost is high, and the activity of the catalyst after regeneration will also be significantly attenuated.

[0007] In summary, the SCR catalyst needs to be selected from the aspects of microstructure and composition, which can not only ensure that it has high catalytic denitrification performance, but also has strong resistance to phosphorus poisoning and improve its service life. Summary of the invention

[0008] In view of the problems existing in the prior art, the purpose of the present invention is to provide a core-shell structured copper-based molecular sieve integral SCR catalyst and a preparation method thereof. The SCR catalyst, through the design of a core-shell structure, coats the copper-based molecular sieve with a transition metal oxide, so that it can have a strong low-temperature denitrification performance, and can avoid direct contact between the active substances in the copper-based molecular sieve and the phosphorus-containing substances in the exhaust gas to be treated, thereby improving the catalyst's resistance to phosphorus poisoning and extending the catalyst's service life.

[0009] To achieve this object, the present invention adopts the following technical solutions:

[0010] On the one hand, the present invention provides a core-shell structured copper-based molecular sieve integral SCR catalyst, wherein the SCR catalyst comprises an active component and a carrier, wherein the active component is in a core-shell structure, comprising a copper-based molecular sieve and a transition metal oxide, wherein the copper-based molecular sieve is a core, and the transition metal oxide is a porous shell structure, and the carrier comprises a ceramic carrier.

[0011] In the present invention, for the treatment of nitrogen oxides in exhaust gas pollutants, an SCR catalyst is usually selected. In the present invention, the catalyst is designed as a core-shell structure, wherein the active center copper-based molecular sieve serves as the core, which is coated by the transition metal oxide coated on the outside, and is designed as a porous shell structure to prevent the active center from being unable to contact the gas to be treated. Overall, the low-temperature denitrification performance is excellent and the activation window is wide. At the same time, the core-shell structure can prevent the active species in the copper-based molecular sieve from directly contacting the phosphorus-containing substances in the exhaust gas, significantly improving the catalyst's ability to resist phosphorus poisoning and increasing the catalyst's service life; and the catalyst is coated on the carrier, the coating has high firmness, which can not only ensure the specific surface area of ​​the catalyst, but also avoid the problem of difficult recovery of granular catalysts, which helps to reduce the cost of the catalyst, and can be applied to the treatment of phosphorus-nitrogen-containing exhaust gases such as automobile exhaust and power plant exhaust.

[0012] The following are preferred technical solutions of the present invention, but are not intended to be limitations of the technical solutions provided by the present invention. Through the following technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0013] As a preferred technical solution of the present invention, the types of molecular sieves in the copper-based molecular sieve include CHA molecular sieve and / or AEI molecular sieve.

[0014] In the present invention, the molecular sieves with CHA structure include SSZ-13 molecular sieve and SAPO-34 molecular sieve, and the molecular sieves with AEI structure include SSZ-39 molecular sieve and SAPO-18 molecular sieve.

[0015] Preferably, the copper content in the copper-based molecular sieve is 2.5-5.0wt%, for example, 2.5wt%, 3.0wt%, 3.5wt%, 4.0wt%, 4.5wt% or 5.0wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] Preferably, the transition metal includes any one of Ti, Mo or Zr or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of Ti and Mo, a combination of Mo and Zr, a combination of Ti, Mo and Zr, and the like.

[0017] Preferably, the content of transition metal oxide in the active component is 5 to 20wt%, for example 5wt%, 6wt%, 8wt%, 10wt%, 12wt%, 15wt%, 18wt% or 20wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0018] As a preferred technical solution of the present invention, the core-shell structure is a copper-based molecular sieve coated with a transition metal oxide, and the overall particle size of the core-shell structure is 5 to 8 μm, for example, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm or 8 μm, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, the particle size of the copper-based molecular sieve as the core is 3 to 7 μm, for example 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm or 7 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] Preferably, the pore size of the porous shell structure of the transition metal oxide is 5 to 20 nm, for example 5 nm, 6 nm, 8 nm, 10 nm, 12 nm, 15 nm, 18 nm or 20 nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] Preferably, the proportion of active components in the SCR catalyst is 80-95wt%, for example, 80wt%, 82wt%, 85wt%, 88wt%, 90wt%, 92wt% or 95wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] Preferably, the ceramic carrier comprises a cordierite honeycomb ceramic carrier.

[0023] In another aspect, the present invention provides a method for preparing the above-mentioned SCR catalyst, the preparation method comprising the following steps:

[0024] (1) preparing a copper-based molecular sieve and a transition metal precursor sol respectively;

[0025] (2) uniformly mixing the copper-based molecular sieve and the transition metal precursor sol, drying and calcining to obtain an active component with a core-shell structure;

[0026] (3) The core-shell structured active component is dissolved and mixed with a binder and a thickener to obtain an active component slurry, and then the active component slurry is coated on a ceramic carrier, and the monolithic SCR catalyst is obtained after drying and calcining.

[0027] As a preferred technical solution of the present invention, the preparation step of the copper-based molecular sieve in step (1) includes: mixing a copper precursor solution with a blank molecular sieve, stirring thoroughly and then heating, maintaining stirring for ion exchange, and then filtering, washing, drying, and calcining in sequence to obtain a copper-based molecular sieve.

[0028] Preferably, the copper precursor includes any one of copper nitrate, copper sulfate, copper chloride or copper acetate, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of copper nitrate and copper sulfate, a combination of copper sulfate and copper chloride, a combination of copper nitrate, copper sulfate and copper acetate, a combination of copper nitrate, copper sulfate and copper chloride, etc.

[0029] Preferably, the blank molecular sieve comprises a CHA structure molecular sieve and / or an AEI structure molecular sieve.

[0030] Preferably, the stirring is performed sufficiently until the molecular sieve is fully dispersed in the solution.

[0031] Preferably, the temperature after heating is 70-90°C, for example 70°C, 72°C, 75°C, 78°C, 80°C, 82°C, 85°C, 88°C or 90°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] Preferably, the ion exchange time is 6 to 24 h, for example 6 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h or 24 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0033] Preferably, the calcination temperature is 500-600°C, for example, 500°C, 520°C, 540°C, 550°C, 560°C, 580°C or 600°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; the calcination time is 1.5-4h, for example, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] Preferably, the copper content in the copper-based molecular sieve is 2.5-5.0wt%, for example, 2.5wt%, 3.0wt%, 3.5wt%, 4.0wt%, 4.5wt% or 5.0wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] As a preferred technical solution of the present invention, the preparation step of the transition metal precursor sol in step (1) includes: mixing the transition metal precursor, the organic complexing agent and water, stirring them thoroughly until they are completely dissolved, and evaporating the water by thermal evaporation until a sol is formed.

[0036] Preferably, the transition metal is any one of Ti, Mo or Zr or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of Ti and Mo, a combination of Mo and Zr, a combination of Ti, Mo and Zr, and the like.

[0037] Preferably, the transition metal precursor comprises any one of the nitrates, sulfates, hydrochlorides or acetates of the above-mentioned transition metals, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of nitrates and sulfates, a combination of sulfates and hydrochlorides, a combination of nitrates, hydrochlorides and acetates, a combination of sulfates, hydrochlorides and acetates, and the like.

[0038] Preferably, the organic complexing agent comprises any one of citric acid, ethylenediaminetetraacetic acid, tartaric acid or oxalic acid, or a combination of at least two thereof. Typical but non-limiting examples of the combination include: a combination of citric acid and ethylenediaminetetraacetic acid, a combination of ethylenediaminetetraacetic acid and tartaric acid, a combination of citric acid, tartaric acid and oxalic acid, a combination of ethylenediaminetetraacetic acid, tartaric acid and oxalic acid, etc.

[0039] Preferably, the molar ratio of the organic complexing agent to the transition metal precursor is 1:1 to 1.5:1, for example 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1 or 1.5:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] Preferably, the temperature of the thermal evaporation is 75-95°C, such as 75°C, 80°C, 85°C, 90°C or 95°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] Preferably, the water evaporated during the thermal evaporation process accounts for 60-90% of the initial water volume, for example 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95% or 100%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Preferably, the transition metal precursor sol is viscous and has low fluidity, and its water content is less than 40%, for example 40%, 35%, 30%, 25%, 20% or 15%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] As a preferred technical solution of the present invention, the mass ratio of the copper-based molecular sieve and the transition metal precursor sol mixed in step (2) is 0.8:1 to 3.4:1, for example, 0.8:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1 or 3.4:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] Preferably, the mixing method in step (2) includes grinding mixing, preferably ball milling.

[0045] Preferably, the drying temperature in step (2) is 80-120°C, for example 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C or 120°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] Preferably, the calcination temperature in step (2) is 500-600°C, for example, 500°C, 520°C, 540°C, 550°C, 560°C, 580°C or 600°C, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; the time is 1.5-4h, for example, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0047] Preferably, after calcination in step (2), the transition metal precursor sol forms a transition metal oxide as a shell structure in the core-shell structure.

[0048] In the present invention, a transition metal oxide and a complexing agent undergo a coordination reaction to form a complex, and the complex connects metal ions and ligands in the complexing agent molecules through coordination bonds; during the evaporation of water, the complexes approach each other and gradually form a network structure; the active component molecular sieve and the transition metal precursor sol are fully contacted during the ball milling process, and the latter forms a film to completely wrap the molecular sieve particles, and after roasting, the complex undergoes oxidative decomposition to form oxide-coated molecular sieve particles with a network structure. The obtained product has a core-shell structure, with the copper-based molecular sieve as the core and the transition metal oxide as the porous shell.

[0049] Preferably, the content of transition metal oxide in the core-shell structure in step (2) is 5 to 20 wt%, for example 5 wt%, 6 wt%, 8 wt%, 10 wt%, 12 wt%, 15 wt%, 18 wt% or 20 wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0050] As a preferred technical solution of the present invention, the active component in step (3) is dissolved in water and stirred until fully dispersed, and then a binder and a thickener are added to obtain an active component slurry after the active component is fully dissolved and dispersed.

[0051] Preferably, the binder in step (3) comprises aluminum sol and / or silica sol.

[0052] Preferably, the content of the binder in step (3) is 3 to 10 wt% of the dry weight of the active component slurry, for example 3 wt%, 4 wt%, 5 wt%, 6 wt%, 7 wt%, 8 wt%, 9 wt% or 10 wt%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0053] Preferably, the thickener in step (3) comprises any one of carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose or xanthan gum, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of carboxymethyl cellulose and hydroxyethyl cellulose, a combination of hydroxyethyl cellulose and hydroxypropyl methyl cellulose, a combination of carboxymethyl cellulose and xanthan gum, a combination of carboxymethyl cellulose, hydroxyethyl cellulose and hydroxypropyl methyl cellulose, etc.

[0054] Preferably, the content of the thickener in step (3) is 1 to 5 wt‰ of the dry weight of the active component slurry, for example, 1 wt‰, 1.5 wt‰, 2 wt‰, 2.5 wt‰, 3 wt‰, 3.5 wt‰, 4 wt‰, 4.5 wt‰ or 5 wt‰, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0055] As a preferred technical solution of the present invention, the ceramic carrier in step (3) includes a cordierite honeycomb ceramic carrier.

[0056] Preferably, the coating amount of the active component slurry in step (3) is 100-150 g / L, for example, 100 g / L, 105 g / L, 110 g / L, 115 g / L, 120 g / L, 125 g / L, 130 g / L, 140 g / L or 150 g / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0057] In the present invention, the coating amount of the active component slurry refers to the mass of the slurry coated on each liter of the carrier, and is mainly coated on the inner wall of the pores of the honeycomb carrier.

[0058] Preferably, the drying temperature in step (3) is 80-120°C, for example 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C or 120°C, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0059] Preferably, the calcination temperature in step (3) is 500-600°C, for example, 500°C, 520°C, 540°C, 550°C, 560°C, 580°C or 600°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; the time is 1.5-4h, for example, 1.5h, 2h, 2.5h, 3h, 3.5h or 4h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0060] Preferably, the proportion of active components in the integral SCR catalyst in step (3) is 80-95wt%, for example 80%, 85%, 90%, 95%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0061] As a preferred technical solution of the present invention, the preparation method comprises the following steps:

[0062] (1) preparing a copper-based molecular sieve and a transition metal precursor sol respectively; wherein the preparation step of the copper-based molecular sieve comprises: mixing a copper precursor solution with a blank molecular sieve, wherein the copper precursor comprises any one of copper nitrate, copper sulfate, copper chloride or copper acetate or a combination of at least two thereof, and the blank molecular sieve comprises a CHA structure molecular sieve and / or an AEI structure molecular sieve, stirring the mixture until the molecular sieve is fully dispersed in the solution, and then heating the mixture to 70 to 90° C. and maintaining stirring for ion exchange, wherein the ion exchange time is 6 to 24 hours, and then filtering, washing, drying and calcining the mixture in sequence, wherein the calcination temperature is 500 to 600° C. and the time is 1.5 to 4 hours, to obtain a copper-based molecular sieve, wherein the copper content of the copper-based molecular sieve is 2.5 to 5.0 wt %;

[0063] The preparation step of the transition metal precursor sol comprises: mixing a transition metal precursor, an organic complexing agent and water, wherein any one or a combination of at least two of the transition metals Ti, Mo or Zr, the transition metal precursor comprises any one or a combination of at least two of the nitrates, sulfates, hydrochlorides or acetates of the above transition metals, the organic complexing agent comprises any one or a combination of at least two of citric acid, ethylenediaminetetraacetic acid, tartaric acid or oxalic acid, the molar ratio of the amount of the organic complexing agent added to the transition metal precursor is 1:1 to 1.5:1, stirring fully until completely dissolved, evaporating water by thermal evaporation, the thermal evaporation temperature is 75 to 95° C., and the evaporated water accounts for 60 to 90% of the initial water content, until a viscous sol is formed;

[0064] (2) uniformly mixing the copper-based molecular sieve and the transition metal precursor sol, wherein the mass ratio of the two is 0.8:1 to 3.4:1, and the mixing method includes grinding and mixing, and then drying and calcining. The drying temperature is 80 to 120° C., and the calcining temperature is 500 to 600° C. for 1.5 to 4 hours to obtain an active component of a core-shell structure. After the calcination, the transition metal precursor sol forms a transition metal oxide as a shell structure in the core-shell structure, and the content of the transition metal oxide in the core-shell structure is 5 to 20 wt %;

[0065] (3) The active component of the core-shell structure is dissolved in water and stirred until fully dispersed, and mixed with a binder and a thickener until fully dissolved and dispersed to obtain an active component slurry, wherein the binder includes aluminum sol and / or silica sol, and its content accounts for 3-10wt% of the dry weight of the active component slurry; the thickener includes any one of carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose or xanthan gum or a combination of at least two thereof, and its content accounts for 1-5wt‰ of the dry weight of the active component slurry; and then the active component slurry is coated on a cordierite honeycomb ceramic carrier, and the coating amount of the active component slurry is 100-150g / L, and then dried and calcined, the drying temperature is 80-120°C, the calcination temperature is 500-600°C, and the time is 1.5-4h to obtain the integral SCR catalyst, and the proportion of the active component in the integral SCR catalyst is 80-95wt%.

[0066] Compared with the prior art, the present invention has the following beneficial effects:

[0067] (1) The catalyst of the present invention is designed with a core-shell structure, wherein the active center copper-based molecular sieve is used as the core, which is coated by the transition metal oxide coated on the outside and is designed as a porous shell structure, so that the active site is protected and the surface is modified, and the low-temperature denitrification performance is excellent and the activation window temperature is wide;

[0068] (2) The core-shell structure of the catalyst of the present invention can prevent the active species in the copper-based molecular sieve from directly contacting with the phosphorus-containing substances in the exhaust gas, significantly improving the catalyst's ability to resist phosphorus poisoning, and can still maintain catalytic activity after phosphorus poisoning, effectively increasing the service life of the catalyst;

[0069] (3) The catalyst of the present invention is coated on a carrier, and the coating has high firmness, which can not only ensure the specific surface area of ​​the catalyst, but also avoid the problem that the granular catalyst is difficult to recover;

[0070] (4) The catalyst structure and preparation method of the present invention are simple and low in cost, and can be applied to the large-scale treatment of phosphorus- and nitrogen-containing waste gases such as automobile exhaust and power plant exhaust. BRIEF DESCRIPTION OF THE DRAWINGS

[0071] Figure 1 It is the denitration performance of the SCR catalyst in fresh state provided by Example 1 of the present invention and Comparative Example 1;

[0072] Figure 2 The denitration performance of the SCR catalyst after phosphorus poisoning provided in Example 1 of the present invention and Comparative Example 1 is shown. DETAILED DESCRIPTION

[0073] In order to better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below. However, the following embodiments are only simple examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0074] The following are typical but non-limiting embodiments of the present invention:

[0075] Embodiment 1:

[0076] This embodiment provides a method for preparing a core-shell structured copper-based molecular sieve monolithic SCR catalyst, the preparation method comprising the following steps:

[0077] (1) preparing a copper-based molecular sieve and a transition metal precursor sol respectively; wherein the preparation step of the copper-based molecular sieve comprises: mixing a copper acetate solution with a CHA-structured H-SSZ-13 molecular sieve, stirring sufficiently until the molecular sieve is fully dispersed in the solution, then heating to 80° C., maintaining stirring for ion exchange, wherein the ion exchange time is 16 hours, and then filtering, washing, drying, and calcining in sequence, wherein the calcination temperature is 550° C., and the time is 2.5 hours, to obtain a copper-based Cu-SSZ-13 molecular sieve, wherein the copper content in the copper-based molecular sieve is 3.09wt%;

[0078] The preparation steps of the transition metal precursor sol include: mixing zirconium nitrate, an organic complexing agent citric acid and water, wherein the molar ratio of the organic complexing agent to the zirconium nitrate is 1:1, stirring until completely dissolved, evaporating water by thermal evaporation, wherein the thermal evaporation temperature is 80° C., and the evaporated water accounts for 60% of the initial water content, until a sol is formed;

[0079] (2) The copper-based molecular sieve and zirconium nitrate sol are uniformly mixed in a mass ratio of 1.4:1, and the mixing method is ball milling for 30 minutes, followed by drying and calcining. The drying temperature is 110°C, and the calcination temperature is 500°C for 2 hours to obtain a core-shell structure active component Cu-SSZ-13@ZrO2. After calcination, the zirconium nitrate sol forms zirconium dioxide as a shell structure in the core-shell structure. The content of zirconium dioxide in the core-shell structure is 8.97wt%, and the content of copper-based molecular sieve is 91.03wt%;

[0080] (3) The core-shell structured active component is dissolved in water and stirred until fully dispersed, and then mixed with a binder and a thickener until fully dissolved and dispersed to obtain an active component slurry, wherein the binder is aluminum sol, and its content accounts for 6.2wt% of the dry weight of the active component slurry; the thickener is carboxymethyl cellulose, and its content accounts for 3.6wt‰ of the dry weight of the active component slurry; and then the active component slurry is coated on a cordierite honeycomb ceramic carrier, and the coating amount of the active component slurry is 120g / L. Then, it is dried and calcined, and the drying temperature is 80°C, and the calcination temperature is 500°C, and the time is 2h to obtain the integral SCR catalyst.

[0081] Embodiment 2:

[0082] This embodiment provides a method for preparing a core-shell structured copper-based molecular sieve monolithic SCR catalyst, the preparation method comprising the following steps:

[0083] (1) preparing a copper-based molecular sieve and a transition metal precursor sol respectively; wherein the preparation step of the copper-based molecular sieve comprises: mixing a copper nitrate solution with a CHA-structured H-SAPO-34 molecular sieve, stirring sufficiently until the molecular sieve is fully dispersed in the solution, then heating to 70° C., maintaining stirring for ion exchange, wherein the ion exchange time is 24 hours, and then filtering, washing, drying, and calcining in sequence, wherein the calcination temperature is 500° C., and the time is 4 hours, to obtain a copper-based Cu-SAPO-34 molecular sieve, wherein the copper content in the copper-based molecular sieve is 2.5 wt%;

[0084] The preparation steps of the transition metal precursor sol include: mixing zirconium nitrate, an organic complexing agent ethylenediaminetetraacetic acid and water, wherein the molar ratio of the organic complexing agent to the zirconium nitrate is 1.25:1, stirring the mixture until it is completely dissolved, evaporating water by thermal evaporation, wherein the thermal evaporation temperature is 95° C., and the evaporated water accounts for 70% of the initial water content, until a sol is formed;

[0085] (2) The copper-based molecular sieve and zirconium nitrate sol are uniformly mixed in a mass ratio of 1.7:1, and the mixing method is ball milling mixing, the ball milling time is 40 minutes, and then dried and calcined, the drying temperature is 100°C, the calcination temperature is 550°C, and the time is 3 hours, to obtain the active component Cu-SAPO-34@ZrO2 of the core-shell structure, the zirconium nitrate sol after calcination forms zirconium dioxide as the shell structure in the core-shell structure, the content of zirconium dioxide in the core-shell structure is 9.5wt%, and the content of copper-based molecular sieve is 90.5wt%;

[0086] (3) The core-shell structured active component is dissolved in water and stirred until fully dispersed, and then mixed with a binder and a thickener until fully dissolved and dispersed to obtain an active component slurry, wherein the binder is aluminum sol, and its content accounts for 3.6wt% of the dry weight of the active component slurry; the thickener is carboxymethyl cellulose, and its content accounts for 2.1wt‰ of the dry weight of the active component slurry; and then the active component slurry is coated on a cordierite honeycomb ceramic carrier, and the coating amount of the active component slurry is 130g / L. Then, it is dried and calcined, and the drying temperature is 90°C, and the calcination temperature is 550°C, and the time is 3h to obtain the integral SCR catalyst.

[0087] Embodiment 3:

[0088] This embodiment provides a method for preparing a core-shell structured copper-based molecular sieve monolithic SCR catalyst, the preparation method comprising the following steps:

[0089] (1) preparing a copper-based molecular sieve and a transition metal precursor sol respectively; wherein the preparation step of the copper-based molecular sieve comprises: mixing a copper acetate solution with an H-SSZ-39 molecular sieve with an AEI structure, stirring sufficiently until the molecular sieve is fully dispersed in the solution, then heating to 90° C., maintaining stirring for ion exchange, wherein the ion exchange time is 6 hours, and then filtering, washing, drying, and calcining in sequence, wherein the calcination temperature is 600° C., and the calcination time is 1.5 hours, to obtain a copper-based Cu-SSZ-39 molecular sieve, wherein the copper content in the copper-based molecular sieve is 4.0 wt%;

[0090] The preparation steps of the transition metal precursor sol include: mixing zirconium nitrate, an organic complexing agent tartaric acid and water, wherein the molar ratio of the organic complexing agent to the zirconium nitrate is 1.3:1, stirring until completely dissolved, evaporating water by thermal evaporation, wherein the thermal evaporation temperature is 85° C., and the evaporated water accounts for 80% of the initial water content, until a sol is formed;

[0091] (2) The copper-based molecular sieve and zirconium nitrate sol are uniformly mixed in a mass ratio of 0.8:1, and the mixing method is ball milling for 20 minutes, followed by drying and calcining. The drying temperature is 120°C, and the calcination temperature is 600°C for 1.5 hours to obtain a core-shell structure active component Cu-SSZ-39@ZrO2. After calcination, the zirconium nitrate sol forms zirconium dioxide as a shell structure in the core-shell structure. The content of zirconium dioxide in the core-shell structure is 18.6wt%, and the content of copper-based molecular sieve is 81.4wt%;

[0092] (3) The core-shell structured active component is dissolved in water and stirred until fully dispersed, and mixed with a binder and a thickener until fully dissolved and dispersed to obtain an active component slurry, wherein the binder is silica sol, and its content accounts for 8.5wt% of the dry weight of the active component slurry; the thickener is hydroxyethyl cellulose, and its content accounts for 5wt‰ of the dry weight of the active component slurry; the active component slurry is then coated on a cordierite honeycomb ceramic carrier, and the coating amount of the active component slurry is 100g / L; and then dried and calcined, the drying temperature is 100°C, the calcination temperature is 600°C, and the time is 1.5h, to obtain the integral SCR catalyst.

[0093] Embodiment 4:

[0094] This embodiment provides a method for preparing a core-shell structured copper-based molecular sieve monolithic SCR catalyst, the preparation method comprising the following steps:

[0095] (1) preparing a copper-based molecular sieve and a transition metal precursor sol respectively; wherein the preparation step of the copper-based molecular sieve comprises: mixing a copper sulfate solution with an H-SAPO-18 molecular sieve of AEI structure, stirring sufficiently until the molecular sieve is fully dispersed in the solution, then heating to 75° C., maintaining stirring for ion exchange, wherein the ion exchange time is 12 hours, and then filtering, washing, drying, and calcining in sequence, wherein the calcination temperature is 520° C., and the time is 3.5 hours, to obtain a copper-based Cu-SAPO-18 molecular sieve, wherein the copper content in the copper-based molecular sieve is 4.65wt%;

[0096] The preparation steps of the transition metal precursor sol include: mixing titanium sulfate, an organic complexing agent tartaric acid and water, wherein the molar ratio of the organic complexing agent to titanium sulfate is 1.41:1, stirring until completely dissolved, evaporating water by thermal evaporation, wherein the thermal evaporation temperature is 75° C., and the evaporated water accounts for 65% of the initial water content, until a sol is formed;

[0097] (2) The copper-based molecular sieve and titanium sulfate sol are uniformly mixed in a mass ratio of 3.4:1, and the mixing method is ball milling for 25 minutes, followed by drying and calcining. The drying temperature is 105°C, and the calcination temperature is 520°C for 3.5 hours to obtain a core-shell structure active component Cu-SAPO-18@TiO2. After calcination, the titanium sulfate sol forms titanium dioxide as a shell structure in the core-shell structure. The content of titanium dioxide in the core-shell structure is 5.5wt%, and the content of copper-based molecular sieve is 94.5wt%;

[0098] (3) The core-shell structured active component is dissolved in water and stirred until fully dispersed, and then mixed with a binder and a thickener until fully dissolved and dispersed to obtain an active component slurry, wherein the binder is silica sol, and its content accounts for 10wt% of the dry weight of the active component slurry; the thickener is hydroxypropyl methylcellulose, and its content accounts for 1wt‰ of the dry weight of the active component slurry; and then the active component slurry is coated on a cordierite honeycomb ceramic carrier, and the coating amount of the active component slurry is 140g / L, and then dried and calcined, the drying temperature is 110°C, the calcination temperature is 520°C, and the time is 4h to obtain the integral SCR catalyst.

[0099] Embodiment 5:

[0100] This embodiment provides a method for preparing a core-shell structured copper-based molecular sieve monolithic SCR catalyst, the preparation method comprising the following steps:

[0101] (1) preparing a copper-based molecular sieve and a transition metal precursor sol respectively; wherein the preparation step of the copper-based molecular sieve comprises: mixing a copper sulfate solution with a CHA-structured H-SSZ-13 molecular sieve, stirring sufficiently until the molecular sieve is fully dispersed in the solution, then heating to 90° C., maintaining stirring for ion exchange, wherein the ion exchange time is 8 hours, and then filtering, washing, drying, and calcining in sequence, wherein the calcination temperature is 580° C., and the time is 2.5 hours, to obtain a copper-based Cu-SSZ-13 molecular sieve, wherein the copper content in the copper-based molecular sieve is 5.0 wt%;

[0102] The preparation steps of the transition metal precursor sol include: mixing titanium nitrate, an organic complexing agent oxalic acid and water, wherein the molar ratio of the organic complexing agent to the titanium nitrate is 1.5:1, stirring fully until completely dissolved, evaporating water by thermal evaporation, wherein the thermal evaporation temperature is 90° C., and the evaporated water accounts for 90% of the initial water content, until a sol is formed;

[0103] (2) The copper-based molecular sieve and titanium nitrate sol are uniformly mixed in a mass ratio of 1.5:1, and the mixing method is ball milling for 35 minutes, followed by drying and calcining. The drying temperature is 80°C, and the calcination temperature is 580°C for 2.5 hours to obtain a core-shell structure active component Cu-SSZ-13@TiO2. After calcination, the titanium nitrate sol forms titanium dioxide as a shell structure in the core-shell structure. The content of titanium dioxide in the core-shell structure is 16.3wt%, and the content of copper-based molecular sieve is 83.7wt%;

[0104] (3) The core-shell structured active component is dissolved in water and stirred until fully dispersed, and then mixed with a binder and a thickener until fully dissolved and dispersed to obtain an active component slurry, wherein the binder is silica sol, and its content accounts for 3wt% of the dry weight of the active component slurry; the thickener is xanthan gum, and its content accounts for 3.5wt‰ of the dry weight of the active component slurry; and then the active component slurry is coated on a cordierite honeycomb ceramic carrier, and the coating amount of the active component slurry is 150g / L. Then, it is dried and calcined, the drying temperature is 120°C, the calcination temperature is 580°C, and the time is 2.5h to obtain the integral SCR catalyst.

[0105] Embodiment 6:

[0106] This embodiment provides a method for preparing a core-shell structured copper-based molecular sieve monolithic SCR catalyst, the preparation method comprising the following steps:

[0107] (1) preparing a copper-based molecular sieve and a transition metal precursor sol respectively; wherein the preparation step of the copper-based molecular sieve comprises: mixing a cupric chloride solution with an H-SSZ-39 molecular sieve of an AEI structure, stirring sufficiently until the molecular sieve is fully dispersed in the solution, then heating to 85° C., maintaining stirring for ion exchange, wherein the ion exchange time is 10 hours, and then filtering, washing, drying, and calcining in sequence, wherein the calcination temperature is 560° C., and the time is 3.5 hours, to obtain a copper-based Cu-SSZ-39 molecular sieve, wherein the copper content in the copper-based molecular sieve is 4.2wt%;

[0108] The preparation step of the transition metal precursor sol comprises: mixing molybdenum nitrate, an organic complexing agent citric acid and water, wherein the molar ratio of the organic complexing agent to the molybdenum nitrate is 1.2:1, stirring the mixture until it is completely dissolved, evaporating water by thermal evaporation, wherein the thermal evaporation temperature is 80° C., and the evaporated water accounts for 90% of the initial water content, until a sol is formed;

[0109] (2) The copper-based molecular sieve and the molybdenum nitrate sol are uniformly mixed, the mass ratio of the two is 1.25:1, the mixing method is ball milling, the ball milling time is 30 minutes, and then dried and calcined, the drying temperature is 90°C, the calcination temperature is 560°C, and the time is 3.5 hours, to obtain the active component Cu-SSZ-39@MoO2 of the core-shell structure, the molybdenum nitrate sol after calcination forms molybdenum dioxide as the shell structure in the core-shell structure, the content of molybdenum dioxide in the core-shell structure is 10.5wt%, and the content of copper-based molecular sieve is 89.5wt%;

[0110] (3) The core-shell structured active component is dissolved in water and stirred until fully dispersed, and mixed with a binder and a thickener until fully dissolved and dispersed to obtain an active component slurry, wherein the binder is aluminum sol, and its content accounts for 3.2wt% of the dry weight of the active component slurry; the thickener is xanthan gum, and its content accounts for 4wt‰ of the dry weight of the active component slurry; the active component slurry is then coated on a cordierite honeycomb ceramic carrier, and the coating amount of the active component slurry is 110g / L; and then dried and calcined, the drying temperature is 115°C, the calcination temperature is 560°C, and the time is 3.5h to obtain the integral SCR catalyst.

[0111] Embodiment 7:

[0112] This embodiment provides a method for preparing a core-shell structured copper-based molecular sieve monolithic SCR catalyst, the preparation method comprising the following steps:

[0113] (1) preparing a copper-based molecular sieve and a transition metal precursor sol respectively; wherein the preparation step of the copper-based molecular sieve comprises: mixing a copper acetate solution with an H-SAPO-18 molecular sieve with an AEI structure, stirring sufficiently until the molecular sieve is fully dispersed in the solution, then heating to 75° C., maintaining stirring for ion exchange, wherein the ion exchange time is 18 hours, and then filtering, washing, drying, and calcining in sequence, wherein the calcination temperature is 540° C., and the time is 3 hours, to obtain a copper-based Cu-SAPO-18 molecular sieve, wherein the copper content in the copper-based molecular sieve is 3.5wt%;

[0114] The preparation steps of the transition metal precursor sol include: mixing molybdenum sulfate, an organic complexing agent oxalic acid and water, wherein the molar ratio of the organic complexing agent to molybdenum sulfate is 1.3:1, stirring until completely dissolved, evaporating water by thermal evaporation, wherein the thermal evaporation temperature is 88° C., and the evaporated water accounts for 85% of the initial water content, until a sol is formed;

[0115] (2) The copper-based molecular sieve and the molybdenum sulfate sol are uniformly mixed, the mass ratio of the two is 2.4:1, the mixing method is ball milling, the ball milling time is 30 minutes, and then dried and calcined, the drying temperature is 100°C, the calcination temperature is 540°C, and the time is 3 hours, to obtain the active component Cu-SAPO-18@MoO2 of the core-shell structure, the molybdenum sulfate sol after calcination forms molybdenum dioxide as the shell structure in the core-shell structure, the content of molybdenum dioxide in the core-shell structure is 8.8wt%, and the content of copper-based molecular sieve is 91.2wt%;

[0116] (3) The core-shell structured active component is dissolved in water and stirred until fully dispersed, and then mixed with a binder and a thickener until fully dissolved and dispersed to obtain an active component slurry, wherein the binder is silica sol, and its content accounts for 6wt% of the dry weight of the active component slurry; the thickener is xanthan gum, and its content accounts for 1.5wt‰ of the dry weight of the active component slurry; and then the active component slurry is coated on a cordierite honeycomb ceramic carrier, and the coating amount of the active component slurry is 120g / L. Then, it is dried and calcined, the drying temperature is 105°C, the calcination temperature is 540°C, and the time is 3h to obtain the integral SCR catalyst.

[0117] Comparative Example 1:

[0118] This comparative example provides a method for preparing a copper-based molecular sieve integral SCR catalyst. The preparation method refers to the preparation method in Example 1, with the only difference being that the preparation of the transition metal precursor sol in step (1) and the preparation of the active component of the core-shell structure in step (2) are not included, but the copper-based molecular sieve is directly used in step (3).

[0119] The catalysts in Examples 1-7 and Comparative Example 1 were tested for their anti-phosphorus poisoning performance. The performance test was carried out in a fixed bed reactor. A small sample of φ24*50 mm was obtained using a sampler. The denitration performance of the catalysts in each example in the fresh state and after phosphorus poisoning treatment was tested. The results are shown in Table 1. The fresh denitration performance of the catalysts in Example 1 and Comparative Example 1 is shown in Table 1. Figure 1 As shown in Figure 2, the denitrification performance after phosphorus poisoning treatment is as follows: Figure 2 shown.

[0120] The conditions for performance testing are: NO x The concentration is 500ppm, the NH3 concentration is 500ppm, the O2 concentration is 8%, the CO2 concentration is 5%, the H2O concentration is 7%, N2 is used as the balance gas, and the volume space velocity is 60000h -1 , respectively, at 190℃, 200℃, 225℃ and 250℃, until the reaction is balanced, and the NO x Conversion rate; among them, NO x The conversion rate was calculated according to the following formula: x Conversion rate = (C 进口 -C 出口 ) / C 进口 × 100%, where C 进口 With C 出口 NO x Inlet and outlet concentrations (ppm).

[0121] The conditions for the phosphorus poisoning treatment are as follows: prepare 1L of 0.05mol / L phosphoric acid solution in a beaker, completely immerse the sample to be treated in the solution, take it out after soaking for 12 hours, dry it at 110°C, and calcine it at 500°C for 2 hours. The phosphorus poisoning treatment of the sample is completed.

[0122] Table 1 Denitrification performance of the catalysts in fresh state and after phosphorus poisoning treatment in Examples 1-7 and Comparative Example 1

[0123]

[0124] From Table 1 and Figure 1-2 The activity test results show that the transition metal oxide coated copper-based molecular sieve forms a core-shell structure, which improves the low-temperature performance of the fresh catalyst to a certain extent. The NO x The conversion rate was increased by 2.3% compared with that of comparative example 1. The transition metal oxide coating modification in other examples also had similar effects. After 12h of phosphorus poisoning treatment, the denitration performance of the SCR catalyst with a core-shell structure was much higher than that of the catalyst in comparative example 1. The NO x The conversion rate is 52.8% higher than that in Comparative Example 1, and the transition metal oxide-coated copper-based molecular sieves in other embodiments also obtain similar high resistance to phosphorus poisoning. It can be seen that the copper-based molecular sieve SCR catalyst with a core-shell structure obtained by the preparation method of the present invention has high resistance to phosphorus poisoning and improves the SCR activity in the low temperature zone.

[0125] From the above embodiments and comparative examples, it can be seen that the catalyst of the present invention is designed with a core-shell structure, wherein the active center copper-based molecular sieve serves as the core, which is coated by the transition metal oxide coated on the outside, and is designed as a porous shell structure to protect the active site and modify the surface, and has excellent low-temperature denitrification performance and a wide activation window temperature; the core-shell structure of the catalyst can avoid direct contact between the active species in the copper-based molecular sieve and the phosphorus-containing substances in the exhaust gas, significantly improve the catalyst's ability to resist phosphorus poisoning, and can still maintain catalytic activity after phosphorus poisoning, effectively improving the service life of the catalyst; the catalyst is coated on a carrier, and the coating has high firmness, which can not only ensure the specific surface area of ​​the catalyst, but also avoid the problem of difficulty in recovering the granular catalyst; the catalyst structure and preparation method are simple, low cost, and can be suitable for large-scale treatment of phosphorus-nitrogen exhaust gases such as automobile exhaust and power plant exhaust.

[0126] The applicant declares that the present invention illustrates the detailed products and methods of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed products and methods, that is, it does not mean that the present invention must rely on the above-mentioned detailed products and methods to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the method of the present invention, addition of auxiliary steps, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A core-shell structure copper-based molecular sieve monolithic SCR catalyst, It is characterized in that The SCR catalyst comprises an active component and a carrier. The active component is in a core-shell structure, comprising a copper-based molecular sieve and a transition metal oxide. The copper-based molecular sieve is a core, the transition metal oxide is a porous shell structure, and the carrier comprises a ceramic carrier.

2. The SCR catalyst according to claim 1, It is characterized in that The types of molecular sieves in the copper-based molecular sieve include CHA molecular sieve and / or AEI molecular sieve; Preferably, the copper content in the copper-based molecular sieve is 2.5-5.0 wt%; Preferably, the transition metal includes any one of Ti, Mo or Zr or a combination of at least two thereof; Preferably, the content of transition metal oxide in the active component is 5 to 20 wt%.

3. The SCR catalyst according to claim 1 or 2, It is characterized in that The core-shell structure is a copper-based molecular sieve coated with a transition metal oxide, and the overall particle size of the core-shell structure is 5 to 8 μm; Preferably, the particle size of the copper-based molecular sieve as a core is 3 to 7 μm; Preferably, the pore size of the porous shell structure of the transition metal oxide is 5 to 20 nm; Preferably, the proportion of active components in the SCR catalyst is 80-95wt%; Preferably, the ceramic carrier comprises a cordierite honeycomb ceramic carrier.

4. The method for preparing the SCR catalyst according to any one of claims 1 to 3, It is characterized in that The preparation method comprises the following steps: (1) preparing a copper-based molecular sieve and a transition metal precursor sol respectively; (2) uniformly mixing the copper-based molecular sieve and the transition metal precursor sol, drying and calcining to obtain an active component with a core-shell structure; (3) The core-shell structured active component is dissolved and mixed with a binder and a thickener to obtain an active component slurry, and then the active component slurry is coated on a ceramic carrier, and the monolithic SCR catalyst is obtained after drying and calcining.

5. The preparation method according to claim 4, It is characterized in that The preparation steps of the copper-based molecular sieve in step (1) include: mixing a copper precursor solution with a blank molecular sieve, stirring thoroughly and then heating, maintaining stirring to perform ion exchange, and then filtering, washing, drying, and roasting in sequence to obtain the copper-based molecular sieve; Preferably, the copper precursor includes any one of copper nitrate, copper sulfate, copper chloride or copper acetate, or a combination of at least two thereof; Preferably, the blank molecular sieve comprises a CHA structure molecular sieve and / or an AEI structure molecular sieve; Preferably, the stirring is sufficient until the molecular sieve is fully dispersed in the solution; Preferably, the temperature after heating is 70-90°C; Preferably, the ion exchange time is 6 to 24 hours; Preferably, the calcination temperature is 500-600°C, and the calcination time is 1.5-4h; Preferably, the copper content in the copper-based molecular sieve is 2.5-5.0 wt%.

6. The preparation method according to claim 4 or 5, It is characterized in that The preparation step of the transition metal precursor sol in step (1) comprises: mixing the transition metal precursor, the organic complexing agent and water, stirring them fully until they are completely dissolved, and evaporating the water by thermal evaporation until a sol is formed; Preferably, the transition metal is any one or a combination of at least two of Ti, Mo or Zr; Preferably, the transition metal precursor comprises any one or a combination of at least two of the nitrates, sulfates, hydrochlorides or acetates of the above transition metals; Preferably, the organic complexing agent comprises any one of citric acid, ethylenediaminetetraacetic acid, tartaric acid or oxalic acid, or a combination of at least two thereof; Preferably, the molar ratio of the amount of the organic complexing agent added to the transition metal precursor is 1:1 to 1.5:1; Preferably, the temperature of the thermal evaporation is 75-95°C; Preferably, the water evaporated during the thermal evaporation process accounts for 60% to 90% of the initial water volume; Preferably, the transition metal precursor sol is viscous and has a water content of less than 40%.

7. The preparation method according to any one of claims 4 to 6, It is characterized in that The mass ratio of the copper-based molecular sieve and the transition metal precursor sol in step (2) is 0.8:1 to 3.4:1; Preferably, the mixing method in step (2) includes grinding mixing, preferably ball milling; Preferably, the drying temperature in step (2) is 80-120°C; Preferably, the calcination temperature in step (2) is 500-600° C. and the calcination time is 1.5-4 h; Preferably, after calcination in step (2), the transition metal precursor sol forms a transition metal oxide as a shell structure in the core-shell structure; Preferably, the content of transition metal oxide in the core-shell structure in step (2) is 5 to 20 wt%.

8. The preparation method according to any one of claims 4 to 7, It is characterized in that Step (3) the active component is dissolved in water and stirred until fully dispersed, and then a binder and a thickener are added until fully dissolved and dispersed to obtain an active component slurry; Preferably, the binder in step (3) comprises aluminum sol and / or silica sol; Preferably, the content of the binder in step (3) is 3-10 wt% of the dry weight of the active component slurry; Preferably, the thickener in step (3) comprises any one of carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose or xanthan gum, or a combination of at least two thereof; Preferably, the content of the thickener in step (3) is 1 to 5 wt‰ of the dry weight of the active component slurry.

9. The preparation method according to any one of claims 4 to 8, It is characterized in that The ceramic carrier in step (3) comprises a cordierite honeycomb ceramic carrier; Preferably, the coating amount of the active component slurry in step (3) is 100-150 g / L; Preferably, the drying temperature in step (3) is 80-120°C; Preferably, the calcination temperature in step (3) is 500-600° C. and the calcination time is 1.5-4 h; Preferably, the proportion of active components in the monolithic SCR catalyst in step (3) is 80-95 wt%.

10. The preparation method according to any one of claims 4 to 9, It is characterized in that The preparation method comprises the following steps: (1) preparing a copper-based molecular sieve and a transition metal precursor sol respectively; wherein the preparation step of the copper-based molecular sieve comprises: mixing a copper precursor solution with a blank molecular sieve, wherein the copper precursor comprises any one of copper nitrate, copper sulfate, copper chloride or copper acetate or a combination of at least two thereof, and the blank molecular sieve comprises a CHA structure molecular sieve and / or an AEI structure molecular sieve, stirring the mixture until the molecular sieve is fully dispersed in the solution, and then heating the mixture to 70 to 90° C. and maintaining stirring for ion exchange, wherein the ion exchange time is 6 to 24 hours, and then filtering, washing, drying and calcining the mixture in sequence, wherein the calcination temperature is 500 to 600° C. and the time is 1.5 to 4 hours, to obtain a copper-based molecular sieve, wherein the copper content of the copper-based molecular sieve is 2.5 to 5.0 wt %; The preparation step of the transition metal precursor sol comprises: mixing a transition metal precursor, an organic complexing agent and water, wherein any one or a combination of at least two of the transition metals Ti, Mo or Zr, the transition metal precursor comprises any one or a combination of at least two of the nitrates, sulfates, hydrochlorides or acetates of the above transition metals, the organic complexing agent comprises any one or a combination of at least two of citric acid, ethylenediaminetetraacetic acid, tartaric acid or oxalic acid, the molar ratio of the amount of the organic complexing agent added to the transition metal precursor is 1:1 to 1.5:1, stirring fully until completely dissolved, evaporating water by thermal evaporation, the thermal evaporation temperature is 75 to 95° C., and the evaporated water accounts for 60% to 90% of the initial water, until a viscous sol is formed; (2) uniformly mixing the copper-based molecular sieve and the transition metal precursor sol, wherein the mass ratio of the two is 0.8:1 to 3.4:1, and the mixing method includes grinding and mixing, and then drying and calcining. The drying temperature is 80 to 120° C., and the calcining temperature is 500 to 600° C. for 1.5 to 4 hours to obtain an active component of a core-shell structure. After the calcination, the transition metal precursor sol forms a transition metal oxide as a shell structure in the core-shell structure, and the content of the transition metal oxide in the core-shell structure is 5 to 20 wt %; (3) The active component of the core-shell structure is dissolved in water and stirred until fully dispersed, and mixed with a binder and a thickener until fully dissolved and dispersed to obtain an active component slurry, wherein the binder includes aluminum sol and / or silica sol, and its content accounts for 3-10wt% of the dry weight of the active component slurry; the thickener includes any one of carboxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl methyl cellulose or xanthan gum or a combination of at least two thereof, and its content accounts for 1-5wt‰ of the dry weight of the active component slurry; and then the active component slurry is coated on a cordierite honeycomb ceramic carrier, and the coating amount of the active component slurry is 100-150g / L, and then dried and calcined, the drying temperature is 80-120°C, the calcination temperature is 500-600°C, and the time is 1.5-4h to obtain the integral SCR catalyst, and the proportion of the active component in the integral SCR catalyst is 80-95wt%.

Citation Information

Cited By

  • Anti-HCs poisoning SCR catalyst and preparation method thereof

    CN121513946A

  • Low-temperature NH3-SCR denitration catalyst with low N2O selectivity and preparation method thereof

    CN122479801A

  • A low-temperature NH3-SCR denitration catalyst with low N2O selectivity and its preparation method