Preparation method of cobalt-chromium-molybdenum bar

Through vacuum smelting, atomization powder making, and thermal isostatic pressure and forging of cobalt powder, chromium powder and molybdenum powder, the poor component uniformity and insufficient mechanical properties of cobalt chromium molybdenum rods in the prior art are solved. Problem, the preparation of high-performance cobalt chromium molybdenum rods has been achieved, with good composition uniformity and excellent mechanical properties.

CN119035531APending Publication Date: 2024-11-29NINGBO FENGKE JINGCHENG ELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411177392.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

The existing cobalt chromium molybdenum materials have defects in poor component uniformity, grain distribution uniformity and mechanical properties during the production process.

Method used

Vacuum smelting and atomizing powder is used to mix cobalt powder, chromium powder and molybdenum powder, followed by hot isostatic pressing, forging and heat treatment. Cobalt chromium is enhanced through the coordinated coupling of powdering, hot isostatic pressing and forging. The composition uniformity and mechanical properties of molybdenum rods.

Benefits of technology

The high-performance preparation of cobalt chromium molybdenum rods has been achieved, with good composition uniformity, tensile strength ≥1020MPa, yield strength ≥690MPa, and elongation ≥17%, which significantly improves the mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005011079210000111
    Figure BDA0005011079210000111
  • Figure BDA0005011079210000121
    Figure BDA0005011079210000121
Patent Text Reader

Abstract

The invention relates to a preparation method of a cobalt-chromium-molybdenum bar, in particular to the technical field of medical alloys.The preparation method comprises the steps that cobalt powder, chromium powder and molybdenum powder are mixed, and mixed powder is obtained; the mixed powder is sequentially subjected to vacuum melting and atomization powder making, and intermediate powder is obtained; and the intermediate powder is subjected to hot isostatic pressing, forging and heat treatment, and the cobalt-chromium-molybdenum bar is obtained. According to the preparation method provided by the invention, the preparation of the high-performance cobalt-chromium-molybdenum alloy bar is realized through the design of the preparation process of the cobalt-chromium-molybdenum bar and the cooperative coupling of powder preparation, hot isostatic pressing and forging, and the component uniformity, the grain distribution uniformity and the mechanical property are favorably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of medical alloys, and in particular to a method for preparing a cobalt-chromium-molybdenum rod. Background Art

[0002] Currently, cobalt, chromium, and molybdenum are widely used in medical devices, usually (hot) forged and precision processed. Cast CoCrMo alloys have been used in dentistry for decades and are currently used to make artificial joints, while forged CoCrMo alloys are used to make heavy joints that bear large loads, such as knee and hip joints.

[0003] For example, CN110129591A discloses a method for producing CoCrMo alloy for artificial joints. The method first obtains a forging blank by vacuum induction furnace smelting and electroslag remelting. The blank is then heated to 1150°C-1250°C for insulation and then forged. During the forging process, the temperature of the blank is strictly controlled within a certain temperature range. The insulation temperature of the last fire is 1150°C, and the temperature of each final forging is not less than 1000°C to ensure that the CoCrMo forging blank can be in a good plastic processing state. After forging, diffusion annealing is performed at a temperature of 1000°C-1050°C.

[0004] CN214387786U discloses a forged cobalt-chromium-molybdenum alloy artificial hip joint, comprising a femoral ball head and a femoral stem, wherein one end of the femoral ball head is slidably connected to the acetabulum cup and the other end is plug-connected to the femoral stem, the femoral ball head comprises an outer spherical shell and an inner sphere, the inner sphere is matched and embedded in the outer spherical shell, an acetabulum liner that slides relative to the outer spherical shell is disposed outside the outer spherical shell, an acetabulum cup is matched and disposed outside the acetabulum liner, and a femoral stem is plug-connected in the inner sphere; the femoral stem comprises a stem neck, a stem body, and an elastic connector arranged at the connection between the stem neck and the stem body, the stem body comprises a stem proximal portion and a stem distal portion, the stem proximal portion is provided with a plurality of wavy water-patterned grooves, and the front and rear side surfaces of the stem distal portion are provided with vertical grooves.

[0005] However, the existing cobalt-chromium-molybdenum material mainly adopts the vacuum melting-atomization powder method in its production process, and the prepared cobalt-chromium-molybdenum alloy material still has the defects of poor component uniformity, uniform grain distribution and poor mechanical properties. Summary of the invention

[0006] In view of the problems existing in the prior art, the object of the present invention is to provide a method for preparing a cobalt-chromium-molybdenum rod to solve the defects of the cobalt-chromium-molybdenum alloy rod, such as poor component uniformity, uniform grain distribution and poor mechanical properties.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] The present invention provides a method for preparing a cobalt-chromium-molybdenum rod, the preparation method comprising:

[0009] Mixing cobalt powder, chromium powder and molybdenum powder to obtain mixed powder;

[0010] The mixed powder is subjected to vacuum melting and atomization powder making in sequence to obtain an intermediate powder;

[0011] The intermediate powder is subjected to hot isostatic pressing, forging and heat treatment to obtain cobalt-chromium-molybdenum rods.

[0012] The preparation method provided by the present invention realizes the preparation of high-performance cobalt-chromium-molybdenum alloy bars by designing the preparation process of cobalt-chromium-molybdenum bars and by the coordinated coupling of powder making, hot isostatic pressing and forging, which is beneficial to improving component uniformity, grain distribution uniformity and mechanical properties.

[0013] As a preferred technical solution of the present invention, the particle size of the cobalt powder is 2-10 μm.

[0014] Preferably, the particle size of the chromium powder is 2-10 μm.

[0015] Preferably, the particle size of the molybdenum powder is 2-10 μm.

[0016] As a preferred technical solution of the present invention, the mixing is carried out under an inert atmosphere.

[0017] Preferably, the rotation speed during the mixing is 10-15 r / min.

[0018] Preferably, the mixing time is 12-24 hours.

[0019] As a preferred technical solution of the present invention, the mass ratio of cobalt powder, chromium powder and molybdenum powder in the mixed powder is (60-65):(25-30):(5-10).

[0020] As a preferred technical solution of the present invention, the absolute vacuum degree of the vacuum melting is ≤0.001Pa.

[0021] Preferably, the vacuum melting temperature is 1500-1600°C.

[0022] Preferably, the vacuum melting time is 2-2.5 hours.

[0023] As a preferred technical solution of the present invention, the operating pressure in the atomization powder making is 10-15 MPa.

[0024] As a preferred technical solution of the present invention, the temperature of the hot isostatic pressing is 850-1100°C.

[0025] Preferably, the hot isostatic pressing pressure is 80-120 MPa.

[0026] Preferably, the hot isostatic pressing time is 2-7 hours.

[0027] As a preferred technical solution of the present invention, the forging includes: a first forging and a second forging performed sequentially.

[0028] Preferably, the temperature of the first forging is greater than the temperature of the second forging.

[0029] As a preferred technical solution of the present invention, the temperature of the first forging is 1200-1250°C.

[0030] Preferably, the deformation amount of the first forging pass is 15-25%.

[0031] Preferably, the temperature of the second forging is 1000-1050°C.

[0032] Preferably, the deformation amount of the second forging pass is 15-25%.

[0033] As a preferred technical solution of the present invention, the temperature of the heat treatment is 1000-1200°C.

[0034] Preferably, the heat treatment time is 0.5-3h.

[0035] Compared with the prior art solutions, the present invention has the following beneficial effects:

[0036] The preparation method provided by the present invention realizes the preparation of high-performance cobalt-chromium-molybdenum alloy rods by adopting a specially designed preparation process and the coordinated coupling of powder making, hot isostatic pressing and forging. The obtained cobalt-chromium-molybdenum alloy rods have good composition uniformity, tensile strength ≥1020MPa, yield strength ≥690MPa, and elongation ≥17%. DETAILED DESCRIPTION

[0037] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0038] This embodiment provides a method for preparing a cobalt-chromium-molybdenum rod, the preparation method comprising:

[0039] Mixing cobalt powder, chromium powder and molybdenum powder to obtain mixed powder;

[0040] The mixed powder is subjected to vacuum melting and atomization powder making in sequence to obtain an intermediate powder;

[0041] The intermediate powder is subjected to hot isostatic pressing, forging and heat treatment to obtain cobalt-chromium-molybdenum rods.

[0042] Wherein, the particle size of the cobalt powder is 2-10 μm.

[0043] In the present invention, the purity of the cobalt powder used is ≥99.96%.

[0044] Wherein, the particle size of the chromium powder is 2-10 μm.

[0045] In the present invention, the purity of the chromium powder used is ≥99.96%.

[0046] Wherein, the particle size of the molybdenum powder is 2-10 μm.

[0047] In the present invention, the purity of the molybdenum powder used is ≥99.96%.

[0048] In the present invention, the particle size of the metal powder is defined as an aggregate of particles of any particle size within a limited range, or an aggregate of all particles within a certain range, exemplified by an aggregate of particles with a particle size of 2 μm, an aggregate of particles with a particle size of 4 μm, an aggregate of particles with a particle size of 6 μm, an aggregate of particles with a particle size of 8 μm, an aggregate of particles with a particle size of 10 μm, or an aggregate of all particles within a particle size range of 3-6 μm, or an aggregate of all particles within a particle size range of 5-8 μm, or an aggregate of all particles within a particle size range of 7-10 μm, etc.

[0049] Wherein, the mixing is carried out under an inert atmosphere.

[0050] In the present invention, the inert atmosphere refers to a gas that does not affect the properties of the obtained alloy, such as nitrogen, helium, argon or neon, etc., which are commonly used inert gases in the art.

[0051] The rotation speed during the mixing is 10-15 r / min, for example, it can be 10 r / min, 11 r / min, 12 r / min, 13 r / min, 14 r / min or 15 r / min, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0052] The mixing time is 12-24 hours, for example, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0053] Among them, the mass ratio of cobalt powder, chromium powder and molybdenum powder in the mixed powder is (60-65):(25-30):(5-10), for example, it can be 60:25:5, 61:26:6, 62:27:7, 63:28:8, 64:29:9, 65:30:10, 60:25:10, 65:25:10 or 60:30:5, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0054] The absolute vacuum degree of the vacuum melting is ≤0.001Pa, for example, it can be 0.001Pa, 0.0008Pa, 0.0006Pa, 0.0004Pa, 0.0002Pa or 0.0001Pa, etc., but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0055] The temperature of the vacuum melting is 1500-1600°C, for example, it can be 1500°C, 1520°C, 1540°C, 1560°C, 1580°C or 1600°C, but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0056] The vacuum melting time is 2-2.5 h, for example, 2 h, 2.1 h, 2.2 h, 2.3 h, 2.4 h or 2.5 h, but is not limited to the listed values, and other values ​​not listed within the range also meet the requirements.

[0057] Among them, the operating pressure in the atomization powder making is 10-15MPa, for example, it can be 10MPa, 11MPa, 12MPa, 13MPa, 14MPa or 15MPa, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0058] Wherein, the temperature of the hot isostatic pressing is 850-1100°C, for example, it can be 850°C, 860°C, 880°C, 900°C, 920°C, 940°C, 960°C, 980°C, 1000°C, 1020°C, 1040°C, 1060°C, 1080°C or 1100°C, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0059] Among them, the hot isostatic pressing pressure is 80-120MPa, for example, it can be 80MPa, 83MPa, 87MPa, 90MPa, 93MPa, 97MPa, 100MPa, 103MPa, 107MPa, 110MPa, 113MPa, 117MPa or 120MPa, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0060] Among them, the time of hot isostatic pressing is 2-7h, for example, it can be 2h, 2.3h, 2.7h, 3h, 3.3h, 3.7h, 4h, 4.3h, 4.7h, 5h, 5.3h, 5.7h, 6h, 6.3h, 6.7h or 7h, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0061] In the present invention, the hot isostatic pressing needs to be combined with the jacketing and degassing treatments for the intermediate powder.

[0062] Among them, the sheath treatment can be carried out according to the conventional requirements in the field of hot isostatic pressing, and the material used for the sheath is cobalt-based steel plate and other materials.

[0063] The degassing treatment is to degas the assembly obtained by the sheathing treatment, illustratively, the degassing is performed at a temperature of 500-600° C. under an absolute vacuum degree of ≤0.005 Pa for 1-3 hours.

[0064] Among them, the absolute vacuum degree in the degassing treatment is ≤0.005Pa, for example, it can be 0.005Pa, 0.0045Pa, 0.004Pa, 0.0035Pa, 0.003Pa, 0.0025Pa, 0.002Pa, 0.0015Pa, 0.001Pa or 0.0001Pa, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0065] Among them, the temperature in the degassing treatment is 500-600℃, for example, it can be 500℃, 510℃, 520℃, 530℃, 540℃, 550℃, 560℃, 570℃, 580℃, 590℃ or 600℃, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0066] The degassing time is 1-3h, for example, it can be 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, 2.2h, 2.4h, 2.6h, 2.8h or 3h, but is not limited to the listed values. Other values ​​not listed within the range also meet the requirements.

[0067] Wherein, the forging includes: a first forging and a second forging performed sequentially.

[0068] Among them, the temperature of the first forging is 1200-1250℃, for example, it can be 1200℃, 1205℃, 1210℃, 1215℃, 1220℃, 1225℃, 1230℃, 1235℃, 1240℃, 1245℃ or 1250℃, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0069] Among them, the deformation amount of the first forging pass is 15-25%, for example, it can be 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24% or 25%, etc., but is not limited to the listed values, and other unlisted values ​​within this range also meet the requirements.

[0070] Among them, the temperature of the second forging is 1000-1050℃, for example, it can be 1000℃, 1005℃, 1010℃, 1015℃, 1020℃, 1025℃, 1030℃, 1035℃, 1040℃, 1045℃ or 1050℃, but is not limited to the listed values, and other unlisted values ​​within this range also meet the requirements.

[0071] Among them, the deformation amount of the second forging pass is 15-25%, for example, it can be 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24% or 25%, etc., but is not limited to the listed values, and other unlisted values ​​within this range also meet the requirements.

[0072] Wherein, the temperature of the heat treatment is 1000-1200°C, for example, it can be 1000°C, 1020°C, 1040°C, 1060°C, 1080°C, 1100°C, 1120°C, 1140°C, 1160°C, 1180°C or 1200°C, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0073] The heat treatment time is 0.5-3h, for example, it can be 0.5h, 0.6h, 0.7h, 0.8h, 0.9h, 1h, 1.3h, 1.7h, 2h, 2.3h, 2.7h or 3h, but is not limited to the listed values, and other unlisted values ​​within the range also meet the requirements.

[0074] Further, in order to illustrate the excellent performance that can be achieved by the cobalt-chromium-molybdenum rod obtained by the present invention, actual examples are used for illustration, as follows:

[0075] Example 1

[0076] This embodiment provides a method for preparing a cobalt-chromium-molybdenum rod, the preparation method comprising:

[0077] Mixing cobalt powder, chromium powder and molybdenum powder to obtain mixed powder;

[0078] The mixed powder is subjected to vacuum melting and atomization powder making in sequence to obtain an intermediate powder;

[0079] The intermediate powder is subjected to hot isostatic pressing, forging and heat treatment to obtain cobalt-chromium-molybdenum rods;

[0080] The particle size of the cobalt powder is 4-8 μm, and the purity is 99.96%; the particle size of the chromium powder is 5-10 μm, and the purity is 99.96%; the particle size of the molybdenum powder is 2-7 μm, and the purity is 99.96%;

[0081] The mixing is carried out under an inert atmosphere (helium); the rotation speed during the mixing is 14 r / min; the mixing time is 16 h; the mass ratio of cobalt powder, chromium powder and molybdenum powder in the mixed powder is 62:27:8;

[0082] The absolute vacuum degree of the vacuum melting is 0.001 Pa; the temperature of the vacuum melting is 1560° C.; the time of the vacuum melting is 2.4 h;

[0083] The operating pressure in the atomization powder making process is 13 MPa;

[0084] The temperature of the hot isostatic pressing is 1000°C; the pressure of the hot isostatic pressing is 100MPa; and the time of the hot isostatic pressing is 5h;

[0085] The forging includes: a first forging and a second forging performed sequentially; the temperature of the first forging is 1230°C; the deformation amount of the first forging pass is 20%; the temperature of the second forging is 1020°C; the deformation amount of the second forging pass is 18%;

[0086] The temperature of the heat treatment is 1100° C.; the time of the heat treatment is 2 hours.

[0087] Example 2

[0088] This embodiment provides a method for preparing a cobalt-chromium-molybdenum rod, the preparation method comprising:

[0089] Mixing cobalt powder, chromium powder and molybdenum powder to obtain mixed powder;

[0090] The mixed powder is subjected to vacuum melting and atomization powder making in sequence to obtain an intermediate powder;

[0091] The intermediate powder is subjected to hot isostatic pressing, forging and heat treatment to obtain cobalt-chromium-molybdenum rods;

[0092] The particle size of the cobalt powder is 2-5 μm, and the purity is 99.99%; the particle size of the chromium powder is 3-7 μm, and the purity is 99.98%; the particle size of the molybdenum powder is 6-10 μm, and the purity is 99.97%;

[0093] The mixing is carried out under an inert atmosphere (neon gas); the rotation speed during the mixing is 12 r / min; the mixing time is 20 h; the mass ratio of cobalt powder, chromium powder and molybdenum powder in the mixed powder is 62:28:7;

[0094] The absolute vacuum degree of the vacuum melting is 0.001 Pa; the temperature of the vacuum melting is 1540° C.; the time of the vacuum melting is 2.2 h;

[0095] The operating pressure in the atomization powder making process is 12MPa;

[0096] The temperature of the hot isostatic pressing is 900°C; the pressure of the hot isostatic pressing is 90MPa; and the time of the hot isostatic pressing is 4h;

[0097] The forging includes: a first forging and a second forging performed sequentially; the temperature of the first forging is 1220°C; the deformation amount of the first forging pass is 18%; the temperature of the second forging is 1030°C; the deformation amount of the second forging pass is 20%;

[0098] The temperature of the heat treatment is 1150° C.; the time of the heat treatment is 1 hour.

[0099] Example 3

[0100] This embodiment provides a method for preparing a cobalt-chromium-molybdenum rod, the preparation method comprising:

[0101] Mixing cobalt powder, chromium powder and molybdenum powder to obtain mixed powder;

[0102] The mixed powder is subjected to vacuum melting and atomization powder making in sequence to obtain an intermediate powder;

[0103] The intermediate powder is subjected to hot isostatic pressing, forging and heat treatment to obtain cobalt-chromium-molybdenum rods;

[0104] The particle size of the cobalt powder is 3-8 μm, and the purity is 99.96%; the particle size of the chromium powder is 6-10 μm, and the purity is 99.99%; the particle size of the molybdenum powder is 2-7 μm, and the purity is 99.98%;

[0105] The mixing is carried out under an inert atmosphere (argon); the rotation speed during the mixing is 10 r / min; the mixing time is 24 hours; the mass ratio of cobalt powder, chromium powder and molybdenum powder in the mixed powder is 60:30:10;

[0106] The absolute vacuum degree of the vacuum melting is 0.0001Pa; the temperature of the vacuum melting is 1500°C; the time of the vacuum melting is 2.5h;

[0107] The operating pressure in the atomization powder making process is 10MPa;

[0108] The temperature of the hot isostatic pressing is 850°C; the pressure of the hot isostatic pressing is 120MPa; and the time of the hot isostatic pressing is 2h;

[0109] The forging includes: a first forging and a second forging performed sequentially; the temperature of the first forging is 1200° C.; the deformation amount of the first forging pass is 25%; the temperature of the second forging is 1000° C.; the deformation amount of the second forging pass is 25%;

[0110] The temperature of the heat treatment is 1000° C.; the time of the heat treatment is 3 hours.

[0111] Example 4

[0112] This embodiment provides a method for preparing a cobalt-chromium-molybdenum rod, the preparation method comprising:

[0113] Mixing cobalt powder, chromium powder and molybdenum powder to obtain mixed powder;

[0114] The mixed powder is subjected to vacuum melting and atomization powder making in sequence to obtain an intermediate powder;

[0115] The intermediate powder is subjected to hot isostatic pressing, forging and heat treatment to obtain cobalt-chromium-molybdenum rods;

[0116] The particle size of the cobalt powder is 2-10 μm, and the purity is 99.99%; the particle size of the chromium powder is 2-10 μm, and the purity is 99.99%; the particle size of the molybdenum powder is 2-10 μm, and the purity is 99.99%;

[0117] The mixing is carried out under an inert atmosphere (neon); the rotation speed during the mixing is 15 r / min; the mixing time is 12 h; the mass ratio of cobalt powder, chromium powder and molybdenum powder in the mixed powder is 65:25:5;

[0118] The absolute vacuum degree of the vacuum melting is 0.0005 Pa; the temperature of the vacuum melting is 1600° C.; the time of the vacuum melting is 2 hours;

[0119] The operating pressure in the atomization powder making process is 15 MPa;

[0120] The temperature of the hot isostatic pressing is 1100° C.; the pressure of the hot isostatic pressing is 80 MPa; and the time of the hot isostatic pressing is 7 hours;

[0121] The forging includes: a first forging and a second forging performed sequentially; the temperature of the first forging is 1250°C; the deformation amount of the first forging pass is 15%; the temperature of the second forging is 1050°C; the deformation amount of the second forging pass is 15%;

[0122] The temperature of the heat treatment is 1200° C.; the time of the heat treatment is 0.5 h.

[0123] Comparative Example 1

[0124] The only difference from Example 1 is that atomization powder making is not performed, but casting is used instead, and the ingot obtained by casting is subsequently processed.

[0125] Comparative Example 2

[0126] The only difference from Example 1 is that hot isostatic pressing is replaced by hot pressing sintering under isostatic conditions.

[0127] Comparative Example 3

[0128] The only difference from Example 1 is that the mixed powder is directly subjected to hot isostatic pressing and subsequent treatment.

[0129] Comparative Example 4

[0130] The only difference from Example 1 is that no forging is performed.

[0131] Comparative Example 5

[0132] The only difference from Example 1 is that the temperature of the first forging is 1020°C and the temperature of the second forging is 1230°C.

[0133] Comparative Example 6

[0134] The only difference from Example 1 is that only the first forging is performed.

[0135] Comparative Example 7

[0136] The only difference from Example 1 is that only the second forging is performed.

[0137] In the above-mentioned embodiments and comparative examples, the degassing treatment before hot isostatic pressing was carried out at an absolute vacuum degree of 0.005 Pa and a temperature of 550° C. for degassing for 2 h.

[0138] The bars obtained in the examples and comparative examples were subjected to mechanical property testing according to GB / T 228.1-2010 (Tensile test of metallic materials - Part 1: Room temperature test method). At the same time, 15 sampling points were evenly distributed along the axial direction of the bar, and the composition was tested and the relative standard error RSD of the 15 sampling points was calculated to evaluate the composition uniformity. The results are shown in Table 1 below.

[0139] Table 1

[0140]

[0141]

[0142] As can be seen from Table 1, in the solution provided by the present invention, by increasing the vacuum degree of the smelting process and appropriately increasing the molybdenum content in the alloy, the mechanical properties of the bar can be improved and a certain elongation can be maintained; large variable processing of the billet and specific heat treatment are combined to obtain more ideal mechanical properties. In Comparative Example 1, atomization powder making was not performed, and direct casting was performed, so the grains were relatively coarse and the powder uniformity was poor. After forging, the grains were refined, but the mechanical properties were poor; in Comparative Example 2, hot isostatic pressing was replaced by hot pressing sintering, and the density was low. After forging, the densification was improved, but the mechanical properties were general. In Comparative Example 3, the powder was directly hot isostatically pressed, and its molding was poor, the powder uniformity was poor, and its mechanical properties were unstable after forging. In Comparative Example 4, no forging was performed, and its strength and elongation were low; in Comparative Example 5, due to the low temperature of the first forging, the deformation was uneven, and microcracks existed in the forging process, which were compensated by the second forging, but the mechanical properties were low, and the uniformity of the composition was also reduced; in Comparative Example 6, only the first forging was performed, the forging temperature was high, and its strength was low, and the uniformity of the composition was also reduced; in Comparative Example 7, only the second forging was performed, the forging temperature was low, the deformation was uneven, microcracks existed, the mechanical properties were low, and the uniformity of the composition was also reduced.

[0143] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.

[0144] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0145] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing cobalt-chromium-molybdenum rods, characterized in that: The preparation method comprises: Mixing cobalt powder, chromium powder and molybdenum powder to obtain mixed powder; The mixed powder is subjected to vacuum melting and atomization powder making in sequence to obtain an intermediate powder; The intermediate powder is subjected to hot isostatic pressing, forging and heat treatment to obtain cobalt-chromium-molybdenum rods.

2. The preparation method according to claim 1, characterized in that The particle size of the cobalt powder is 2-10 μm; The particle size of the chromium powder is 2-10 μm; The particle size of the molybdenum powder is 2-10 μm.

3. The preparation method according to claim 1, characterized in that: The mixing is carried out under an inert atmosphere; The rotation speed during the mixing is 10-15 r / min; The mixing time is 12-24h.

4. The preparation method according to claim 1, characterized in that: The mass ratio of cobalt powder, chromium powder and molybdenum powder in the mixed powder is (60-65):(25-30):(5-10).

5. The preparation method according to claim 1, characterized in that: The absolute vacuum degree of the vacuum melting is ≤0.001Pa; The temperature of the vacuum melting is 1500-1600°C; The vacuum melting time is 2-2.5h.

6. The preparation method according to claim 1, characterized in that: The operating pressure in the atomization powder making process is 10-15 MPa.

7. The preparation method according to claim 1, characterized in that: The temperature of the hot isostatic pressing is 850-1100°C; The hot isostatic pressing pressure is 80-120 MPa; The hot isostatic pressing time is 2-7h.

8. The preparation method according to claim 1, characterized in that: The forging includes: a first forging and a second forging performed sequentially; The temperature of the first forging is greater than the temperature of the second forging.

9. The preparation method according to claim 8, characterized in that: The temperature of the first forging is 1200-1250℃; The deformation of the first forging pass is 15-25%; The temperature of the second forging is 1000-1050°C; The deformation of the second forging pass is 15-25%.