A2B2O7 type high entropy oxide ceramic and its preparation method and application
Through the design and preparation of A2B2O7 high-entropy oxide ceramics, the dissolution corrosion and preparation instability of glass curing technology when dealing with high radioactive nuclear waste is solved, and the safe curing and long-term stable storage of high-level waste is achieved.
Patent Information
- Application Number
- CN202311462163.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-06
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-11-06
AI Technical Summary
The existing glass curing technology has problems such as harmful gases and waste generation, dissolution and corrosion, uncontrolled preparation process and easy breakage when dealing with high radioactive nuclear waste. It is difficult to cure low-solution elements and volatile nuclides, affecting the safety of nuclear waste. Store.
A2B2O7 type high-entropy oxide ceramics, with specific components as (Gd0.2Sm0.2Dy0.2Er0.2Yb0.2)2Ti2O7, was prepared by high-energy ball milling and discharge sintering method to form a uniform single-phase BCC structure to enhance the mechanical properties of the material. Radiation resistance and thermal stability.
It has achieved safe curing of high-level waste, provided good radiation resistance and corrosion resistance, ensured the long-term and stable storage of nuclear waste, and reduced environmental risks during the curing process.
Smart Images

Figure CN117510206B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nuclear waste solidification, and specifically relates to an A2B2O7 type high entropy oxide ceramic and a preparation method and application thereof. Background Art
[0002] Currently, the most popular method for solidifying high-level radioactive waste is vitrification. However, there are some problems in the application of vitrification in engineering practice: (1) A large amount of harmful gases and waste will be produced during the vitrification process, which greatly increases the cost and difficulty of handling high-level radioactive waste; (2) The glass phase is a metastable state, and it will dissolve and corrode in a certain humid and high-temperature environment, resulting in the release of high-level radioactive waste; (3) The preparation of the glass solid body is also a difficult point. Glass crystallization is an uncontrolled process, which leads to the fact that stress cannot appear during the preparation of the glass solid body. Even after successful preparation, the glass solid body can easily break due to external force, which is extremely unfavorable for the long-term stable storage of the solid body. (4) Elements and compounds with low solubility in glass melt are not suitable for entering the glass structure as network structure formers or modifiers. At the same time, some highly radioactive nuclides that are volatile (such as 129I and 36Cl) or have low compatibility with silicate glass (such as 135Cs) are difficult to solidify through glass.
[0003] During geological storage, the complex thermal and radiation environment may cause the radioactive nuclides in the solidified body to be released into the surrounding environment, so the solidified body of nuclear waste must have good radiation resistance and excellent corrosion resistance. Ceramics are considered to have higher chemical durability and thermal stability than glass, and radioactive nuclides do not react with many silicate minerals and rocks. Therefore, it is of great significance to develop new ceramic solidification materials to improve the safety of high-level waste placement. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides an A2B2O7 type high entropy oxide ceramic and its preparation method and application. Taking into account the specific conditions that the solidified nuclear waste must meet, such as large packaging capacity, high mechanical properties, high leaching resistance, high thermal stability, excellent radiation resistance and technical feasibility, the proportion of each component is determined, and the high entropy ceramic is prepared by a method of high-energy ball milling followed by discharge sintering to obtain a single-phase BCC structure with uniform organizational structure (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 high entropy oxide ceramics.
[0005] The present invention is specifically achieved through the following technical solutions.
[0006] The high entropy oxide ceramics designed as the high-level radioactive waste solidification material in the present invention are A2B2O7 type high entropy oxide ceramics, and the specific composition is (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7.
[0007] (1) The selection of high-level radioactive waste solidification material components mainly considers the mechanical properties and radiation resistance of the solidified matrix: when A is Gd and B is Ti or Zr, the A2B2O7 type oxide has excellent structural stability and excellent radiation resistance; oxides of rare earth elements with similar ionic radius are selected to ensure the formation of a stable single-phase solid solution in the high-entropy ceramic material. Taking the above into consideration, Gd2O3, Sm2O3, Dy2O3, Er2O3, Yb2O3 and TiO2 are selected to prepare A2B2O7 type high-entropy oxide ceramics.
[0008] (2) Design high entropy materials using oxides with equal atomic ratios to maximize the structural entropy of the material.
[0009] The high entropy oxide ceramic provided by the invention has high density, a single-phase body-centered cubic structure, and good organizational and component uniformity.
[0010] The present invention also provides a method for preparing an A2B2O7 type high entropy oxide ceramic, which is used to prepare the A2B2O7 type high entropy oxide ceramic, comprising the following steps:
[0011] According to (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 proportion: weigh Gd2O3, Sm2O3, Dy2O3, Er2O3, Yb2O3 and TiO2 raw material powders;
[0012] The weighed raw material mixture is ball-milled, and then the ball-milled powder is spark plasma sintered to prepare the A2B2O7 type high entropy oxide ceramic.
[0013] In some embodiments of the present invention, Gd2O3, Sm2O3, Dy2O3, Er2O3, Yb2O3 and TiO2 are all made of raw materials with a purity of 99wt.% or above.
[0014] In some embodiments of the present invention, in order to prevent the raw material powder from being oxidized or deteriorated during powder processing, the raw material powder is pre-placed in a glove box, and the oxygen concentration in the glove box is less than 4 ppm and the H2O content is less than 0.01 ppm.
[0015] In some embodiments of the present invention, the mass ratio of the mixture to the grinding balls is 1:10, the ball mill speed is set to 500 rpm, and the forward and reverse rotation modes are adopted. Each cycle runs for 20 minutes with an interval of 10 minutes to prevent overheating of the powder during ball milling and increase of pressure in the ball mill jar, for a total of 15 ball milling cycles.
[0016] In some embodiments of the present invention, during spark plasma sintering, the target sintering temperature is 1100-1400°C.
[0017] In some embodiments of the present invention, during spark plasma sintering, the temperature changes as follows: during the heating process, the sample heating rate is initially 100°C / min, and the heating rate is reduced to 50°C / min when approaching 100°C before the target sintering temperature. After reaching the target sintering temperature, the temperature is kept for 6 minutes, and then the temperature is lowered at a rate of 100°C / min. The program ends when the temperature drops to 600°C, and the sample is taken out after cooling to room temperature.
[0018] In some embodiments of the present invention, during spark plasma sintering, the pressure at both ends of the spark plasma sintering equipment mold is set to 50 MPa, the spark plasma sintering chamber is continuously kept in a vacuum state, and the temperature is monitored by an infrared thermometer aligned with the mold temperature measuring hole.
[0019] The invention provides a nuclear waste solidification material, which is prepared from the A2B2O7 type high entropy oxide ceramic.
[0020] The high entropy effect, lattice distortion effect, hysteresis diffusion effect and cocktail effect of high entropy ceramics make them have extremely high melting point, high hardness, high oxidation resistance, corrosion resistance and good radiation resistance compared with traditional ceramics, and have attracted widespread attention, becoming a candidate material for nuclear energy applications with great development prospects. The high entropy oxide ceramic component of the nuclear waste solidification material of the present invention is scientifically designed, the preparation method is simple, and compared with the existing high-level waste solidification materials, it has the following advantages:
[0021] 1. The A2B2O7 type high entropy oxide material ceramic of the present invention has a reasonable and scientific composition ratio and is suitable for high-level radioactive waste solidification conditions. The A-site metal elements Gd, Sm, Dy, Er, and Yb are in an equiatomic ratio, and B is an A2B2O7 type oxide formed by the Ti element, which has excellent structural stability and excellent radiation resistance; oxides of rare earth elements with similar ionic radii are selected to ensure the formation of a stable single-phase solid solution in the high entropy ceramic material. Compared with single-component oxides, high entropy oxide ceramics have lattice distortion, which can improve the radiation resistance of high entropy oxide ceramic solidification materials.
[0022] 2. The high entropy ceramic of the present invention adopts conventional high-energy ball milling and spark plasma sintering, and the preparation method is simple. The prepared high entropy oxide ceramic (Gd 0.2 Sm0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 has high density, a single-phase body-centered cubic (BCC) structure, and good organizational and composition uniformity.
[0023] 3. The high entropy oxide ceramic solidified material of the present invention has good radiation resistance and mechanical properties, with a maximum Vickers hardness exceeding 13.3 GPa and a density exceeding 98.46%. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 X-ray diffraction patterns (XRD) of the materials prepared in Examples 1 to 4.
[0025] Figure 2 XRD patterns of the materials prepared in Example 3, Comparative Example 1 and Comparative Example 2.
[0026] Figure 3 These are scanning electron microscope morphology images of the materials prepared in Examples 1 to 4.
[0027] Figure 4 Hardness and grain size of the materials prepared in Examples 1 to 4.
[0028] Figure 5 These are the radiation resistance test results of the materials prepared in Example 3, Comparative Example 1 and Comparative Example 2. DETAILED DESCRIPTION
[0029] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the present invention is further described below in conjunction with specific embodiments and drawings, but the embodiments are not intended to limit the present invention.
[0030] The experimental methods and detection methods described in the following embodiments are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified.
[0031] High entropy ceramics have become a promising candidate material for nuclear energy applications due to their high entropy effect that can improve thermodynamic properties, lattice distortion effect that can improve mechanical properties, hysteresis diffusion effect that improves high temperature stability, and cocktail effect that integrates the advantages of each component. High entropy alloys / ceramics not only open up new areas of material design, but also provide new possibilities for the selection of high-level radioactive waste solidification materials.
[0032] A2B2O7-type oxides have a large adjustable composition space, so they exhibit a variety of interesting physical and chemical properties. The A and B cations of A2B2O7-type oxides can be occupied by lanthanides, transition metals, actinides and minor actinides, with ordered pyrochlore structures and disordered fluorite structures, which show different waste loading capacities and chemical flexibility. If A is Gd and B is Ti, the A2B2O7-type oxide has excellent structural stability and excellent radiation resistance. Therefore, A2B2O7-type high entropy oxide ceramics (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 has great potential as a candidate material for new high-level radioactive waste solidification materials.
[0033] During geological storage, the complex thermal and radiation environment may cause the radioactive nuclides in the solidified body to be released into the surrounding environment. Therefore, the solidified body of nuclear waste must have good radiation resistance and excellent corrosion resistance. The uniformity of the dense structure is conducive to improving the radiation resistance and corrosion resistance. The present invention comprehensively considers that the solidified body of nuclear waste must meet the conditions of large packaging capacity, high mechanical properties, high anti-leaching, high thermal stability, excellent radiation resistance and technical feasibility, and designs and prepares (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 high entropy oxide ceramics. 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 has high density, a single-phase body-centered cubic (BCC) structure, good organizational and compositional uniformity, a maximum Vickers hardness of over 13.3 GPa, and a density of over 98.46%.
[0034] The A2B2O7 high entropy oxide ceramic (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 preparation method comprises the following steps:
[0035] (1) Prepare raw materials: Weigh the required Gd2O3, Sm2O3, Dy2O3, Er2O3, Yb2O3 and TiO2 raw material powders according to the ratio of oxide high entropy ceramics. The raw materials are all raw materials with a purity of more than 99wt.%. In order to prevent the raw material powders from oxidation or deterioration during powder processing, the raw material powders are pre-placed in a glove box. The oxygen concentration in the glove box is less than 4ppm and the H2O content is less than 0.01ppm.
[0036] (2) High-energy ball milling: 30 g of powdered raw materials weighed by weight and 300 g of tungsten carbide grinding balls were placed in a ball mill. The ball mill speed was set to 500 rpm, with a forward and reverse rotation mode. Each cycle was run for 20 minutes, with an interval of 10 minutes to prevent the powder from overheating during the ball milling and causing the pressure in the ball milling jar to increase. A total of 15 ball milling cycles were performed.
[0037] (3) Densification sintering: The powder after high-energy ball milling is densified and sintered in the LABOX-325R spark plasma sintering equipment (SPS). During the sintering process, the pressure at both ends of the mold is set to 50MPa, and the SPS chamber is continuously kept in a vacuum state. The temperature is monitored by an infrared thermometer aligned with the temperature measuring hole of the mold. During the heating process, the sample heating rate is initially 100℃ / min. When it is close to 100℃ before the target temperature, the heating rate is reduced to 50℃ / min to prevent the residual stress inside the sample caused by excessive heating, which will cause the sample to crack after cooling. After reaching the target temperature, keep warm for 6 minutes, and then start cooling after keeping warm. The cooling rate is 100℃ / min. The program ends when it drops to 600℃. The sample is taken out after cooling to room temperature. A2B2O7 type high entropy oxide ceramics (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 The target temperatures of )2Ti2O7 were set to 1100℃, 1200℃, 1300℃ and 1400℃, respectively, and the performance tests were carried out on the blocks prepared by sintering.
[0038] The present invention is specifically described below by means of the following examples and comparative examples.
[0039] Example 1
[0040] According to the ratio of oxide high entropy ceramics, the required Gd2O3 (4.09g), Sm2O3 (3.93g), Dy2O3 (4.21g), Er2O3 (4.31g), Yb2O3 (4.45g) and TiO2 (9.01g) raw material powders are weighed. The raw materials have a purity of more than 99wt.%.
[0041] In order to prevent the raw powder from oxidation or deterioration during powder handling, the raw powder was placed in a glove box with a H2O content of less than 0.01ppm and an oxygen concentration of less than 4ppm. 30g of powdered raw material weighed by weight and 300g of tungsten carbide grinding balls were loaded into the ball mill. The ball mill speed was set to 500 rpm, with a forward and reverse rotation mode, and each cycle was run for 20 minutes with an interval of 10 minutes to prevent the powder from overheating during the ball mill and causing the pressure in the ball mill to increase. A total of 15 ball milling cycles were performed.
[0042] The powder after high-energy ball milling was densified and sintered in the LABOX-325R spark plasma sintering equipment (SPS). A graphite mold with an inner diameter of 10 mm was used for sintering. The pressure at both ends of the mold was set to 50 MPa. The SPS chamber was kept in a vacuum state. The temperature was monitored by an infrared thermometer aligned with the temperature measuring hole of the mold. During the heating process, the sample heating rate was initially 100 ° C / min. When it was close to 100 ° C before the target temperature, the heating rate was reduced to 50 ° C / min to prevent the residual stress inside the sample from being caused by excessive heating, which would cause the sample to crack after cooling. After reaching the target temperature of 1100 ° C, keep it warm for 6 minutes, and then start cooling after keeping warm. The cooling rate is 100 ° C / min. The program ends when it drops to 600 ° C. The sample is taken out after cooling to room temperature.
[0043] Example 2
[0044] According to the ratio of oxide high entropy ceramics, the required Gd2O3 (4.09g), Sm2O3 (3.93g), Dy2O3 (4.21g), Er2O3 (4.31g), Yb2O3 (4.45g) and TiO2 (9.01g) raw material powders are weighed. The raw materials have a purity of more than 99wt.%.
[0045] In order to prevent the raw powder from oxidation or deterioration during powder handling, the raw powder was placed in a glove box with a H2O content of less than 0.01ppm and an oxygen concentration of less than 4ppm. 30g of powdered raw material weighed by weight and 300g of tungsten carbide grinding balls were loaded into the ball mill. The ball mill speed was set to 500 rpm, with a forward and reverse rotation mode, and each cycle was run for 20 minutes with an interval of 10 minutes to prevent the powder from overheating during the ball mill and causing the pressure in the ball mill to increase. A total of 15 ball milling cycles were performed.
[0046] The powder after high-energy ball milling was densified and sintered in the LABOX-325R spark plasma sintering equipment (SPS). A graphite mold with an inner diameter of 10 mm was used for sintering. The pressure at both ends of the mold was set to 50 MPa. The SPS chamber was kept in a vacuum state. The temperature was monitored by an infrared thermometer aligned with the temperature measuring hole of the mold. During the heating process, the sample heating rate was initially 100 ° C / min. When it was 100 ° C before the target temperature, the heating rate was reduced to 50 ° C / min to prevent the residual stress inside the sample from being caused by excessive heating, which would cause the sample to crack after cooling. After reaching the target temperature of 1200 ° C, keep the temperature for 6 minutes, and then start cooling after keeping the temperature. The cooling rate was 100 ° C / min. The program ended when it dropped to 600 ° C, and the sample was taken out after cooling to room temperature.
[0047] Example 3
[0048] According to the ratio of oxide high entropy ceramics, the required Gd2O3 (4.09g), Sm2O3 (3.93g), Dy2O3 (4.21g), Er2O3 (4.31g), Yb2O3 (4.45g) and TiO2 (9.01g) raw material powders are weighed. The raw materials have a purity of more than 99wt.%.
[0049] In order to prevent the raw powder from oxidation or deterioration during powder handling, the raw powder was placed in a glove box with a H2O content of less than 0.01ppm and an oxygen concentration of less than 4ppm. 30g of powdered raw material weighed by weight and 300g of tungsten carbide grinding balls were loaded into the ball mill. The ball mill speed was set to 500 rpm, with a forward and reverse rotation mode, and each cycle was run for 20 minutes with an interval of 10 minutes to prevent the powder from overheating during the ball mill and causing the pressure in the ball mill to increase. A total of 15 ball milling cycles were performed.
[0050] The powder after high-energy ball milling was densified and sintered in the LABOX-325R spark plasma sintering equipment (SPS). A graphite mold with an inner diameter of 10 mm was used for sintering. The pressure at both ends of the mold was set to 50 MPa. The SPS chamber was kept in a vacuum state. The temperature was monitored by an infrared thermometer aligned with the temperature measuring hole of the mold. During the heating process, the sample heating rate was initially 100 ° C / min. When it was close to 100 ° C before the target temperature, the heating rate was reduced to 50 ° C / min to prevent the residual stress inside the sample from being caused by excessive heating, which would cause the sample to crack after cooling. After reaching the target temperature of 1300 ° C, keep it warm for 6 minutes, and then start cooling after keeping warm. The cooling rate is 100 ° C / min. The program ends when it drops to 600 ° C. The sample is taken out after cooling to room temperature.
[0051] Example 4
[0052] According to the ratio of oxide high entropy ceramics, the required Gd2O3 (4.09g), Sm2O3 (3.93g), Dy2O3 (4.21g), Er2O3 (4.31g), Yb2O3 (4.45g) and TiO2 (9.01g) raw material powders are weighed. The raw materials have a purity of more than 99wt.%.
[0053] In order to prevent the raw powder from oxidation or deterioration during powder handling, the raw powder was placed in a glove box with a H2O content of less than 0.01ppm and an oxygen concentration of less than 4ppm. 30g of powdered raw material weighed by weight and 300g of tungsten carbide grinding balls were loaded into the ball mill. The ball mill speed was set to 500 rpm, with a forward and reverse rotation mode, and each cycle was run for 20 minutes with an interval of 10 minutes to prevent the powder from overheating during the ball mill and causing the pressure in the ball mill to increase. A total of 15 ball milling cycles were performed.
[0054] The powder after high-energy ball milling was densified and sintered in the LABOX-325R spark plasma sintering equipment (SPS). A graphite mold with an inner diameter of 10 mm was used for sintering. The pressure at both ends of the mold was set to 50 MPa. The SPS chamber was kept in a vacuum state. The temperature was monitored by an infrared thermometer aligned with the temperature measuring hole of the mold. During the heating process, the sample heating rate was initially 100 ° C / min. When it was close to 100 ° C before the target temperature, the heating rate was reduced to 50 ° C / min to prevent the residual stress inside the sample from being caused by excessive heating, which would cause the sample to crack after cooling. After reaching the target temperature of 1400 ° C, keep it warm for 6 minutes, and then start cooling after keeping warm. The cooling rate is 100 ° C / min. The program ends when it drops to 600 ° C. The sample is taken out after cooling to room temperature.
[0055] The blocks in Examples 1-4 prepared by sintering were tested for their organizational structure and performance, and the specific contents are as follows:
[0056] (1) Phase structure analysis
[0057] The sintered samples were surface-grinded using 400# to 4000# mesh SiC sandpaper, then polished using 3μm to 1μm alumina suspension, and finally water-polished to clean the samples. The polished samples were subjected to XRD testing, such as Figure 1 As shown, the high entropy oxide ceramics (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 XRD spectrum, at the SPS sintering temperature of 1100℃-1400℃, the five components (Gd 0.2 Sm 0.2 Dy 0.2Er 0.2 Yb 0.2 )2Ti2O7 has a characteristic peak position between those of Gd2Ti2O7, Sm2Ti2O7, Dy2Ti2O7, Er2Ti2O7 and Yb2Ti2O7, and its peak shape is the same as that of A2B2O7 type ceramic Gd2Ti2O7, indicating that at an SPS sintering temperature of 1100℃-1400℃, the mixed powder forms a single-phase high-entropy oxide ceramic with a BCC structure through solid-phase reaction.
[0058] (2) Microstructure analysis
[0059] The sintered samples were surface-grinded using 400# to 4000# mesh SiC sandpaper, then polished using 3μm to 1μm alumina suspension, and finally water-polished to clean the samples. Figure 3 As shown, the high entropy oxide ceramics (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 cross-sectional SEM morphology. Figure 3 As shown in (a), at a sintering temperature of 1100°C, high entropy oxide ceramics (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 has a density of 91.10% and a grain size of 1.32 μm; Figure 3 As shown in (b), at a sintering temperature of 1200°C, high entropy carbide ceramics (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 has a density of 95.17% and a grain size of 0.4 μm; Figure 3 As shown in (c), at a sintering temperature of 1300°C, high entropy carbide ceramics (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 has a density of 98.46% and a grain size of 0.72 μm; Figure 3 As shown in (d), at a sintering temperature of 1400℃, high entropy carbide ceramics (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2)2Ti2O7 has a grain size of 2.21 μm. The high entropy carbide ceramics (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 has the highest density.
[0060] (3) Thermal performance analysis
[0061] The sintered samples were surface-grinded using 400# to 4000# mesh SiC sandpaper, then polished with 3μm to 1μm alumina suspension, and finally water-polished to clean the samples. The hardness was measured using a Vickers hardness tester. Under a load of 9.8N, a diamond indenter was pressed into the sample surface and held for 10s to obtain the Vickers hardness of the prepared high entropy oxide ceramic sample. The test was repeated ten times for each sample. At the SPS sintering temperature of 1100℃-1400℃, the five components (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7, the average hardness values are 9.03GPa, 11.41GPa, 13.27GPa and 11.99GPa respectively. Figure 4 As shown, the high entropy oxide ceramics (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 hardness and grain size, where at 1300℃ SPS sintering temperature, (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 has the highest hardness, which is 13.27GPa.
[0062] In order to illustrate the (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 high entropy oxide ceramics have excellent properties, and the following comparative examples are also set up.
[0063] Comparative Example 1
[0064] (Gd 1 / 3 Sm 1 / 3 Dy 1 / 3 )2Ti2O7 preparation, comprising the following steps:
[0065] According to the ratio of oxide high entropy ceramics, the required Gd2O3 (6.96g), Sm2O3 (6.69g), Dy2O3 (7.16g), Er2O3 (0g), Yb2O3 (0g) and TiO2 (9.2g) raw material powders are weighed. The raw materials have a purity of more than 99wt.%.
[0066] In order to prevent the raw powder from oxidation or deterioration during powder handling, the raw powder was placed in a glove box with a H2O content of less than 0.01ppm and an oxygen concentration of less than 4ppm. 30g of powdered raw material weighed by weight and 300g of tungsten carbide grinding balls were loaded into the ball mill. The ball mill speed was set to 500 rpm, with a forward and reverse rotation mode, and each cycle was run for 20 minutes with an interval of 10 minutes to prevent the powder from overheating during the ball mill and causing the pressure in the ball mill to increase. A total of 15 ball milling cycles were performed.
[0067] The powder after high-energy ball milling was densified and sintered in the LABOX-325R spark plasma sintering equipment (SPS). A graphite mold with an inner diameter of 10 mm was used for sintering. The pressure at both ends of the mold was set to 50 MPa. The SPS chamber was kept in a vacuum state. The temperature was monitored by an infrared thermometer aligned with the temperature measuring hole of the mold. During the heating process, the sample heating rate was initially 100 ° C / min. When it was close to 100 ° C before the target temperature, the heating rate was reduced to 50 ° C / min to prevent the residual stress inside the sample from being caused by excessive heating, which would cause the sample to crack after cooling. After reaching the target temperature of 1300 ° C, keep it warm for 6 minutes, and then start cooling after keeping warm. The cooling rate is 100 ° C / min. The program ends when it drops to 600 ° C. The sample is taken out after cooling to room temperature.
[0068] Comparative Example 2
[0069] The preparation of Gd2Ti2O7 comprises the following steps:
[0070] The required Gd2O3 (20.82g), Sm2O3 (0g), Dy2O3 (0g), Er2O3 (0g), Yb2O3 (0g) and TiO2 (9.18g) raw material powders are weighed according to the ratio of oxide high entropy ceramics. The raw materials have a purity of more than 99wt.%.
[0071] In order to prevent the raw powder from oxidation or deterioration during powder handling, the raw powder was placed in a glove box with a H2O content of less than 0.01ppm and an oxygen concentration of less than 4ppm. 30g of powdered raw material weighed by weight and 300g of tungsten carbide grinding balls were loaded into the ball mill. The ball mill speed was set to 500 rpm, with a forward and reverse rotation mode, and each cycle was run for 20 minutes with an interval of 10 minutes to prevent the powder from overheating during the ball mill and causing the pressure in the ball mill to increase. A total of 15 ball milling cycles were performed.
[0072] The powder after high-energy ball milling was densified and sintered in the LABOX-325R spark plasma sintering equipment (SPS). A graphite mold with an inner diameter of 10 mm was used for sintering. The pressure at both ends of the mold was set to 50 MPa. The SPS chamber was kept in a vacuum state. The temperature was monitored by an infrared thermometer aligned with the temperature measuring hole of the mold. During the heating process, the sample heating rate was initially 100 ° C / min. When it was close to 100 ° C before the target temperature, the heating rate was reduced to 50 ° C / min to prevent the residual stress inside the sample from being caused by excessive heating, which would cause the sample to crack after cooling. After reaching the target temperature of 1300 ° C, keep it warm for 6 minutes, and then start cooling after keeping warm. The cooling rate is 100 ° C / min. The program ends when it drops to 600 ° C. The sample is taken out after cooling to room temperature.
[0073] Taking Example 3 as an example, it is compared with Comparative Example 1 and Comparative Example 2, and the results are as follows:
[0074] like Figure 2 As shown, Example 3 (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7, Comparative Example 1 (Gd 1 / 3 Sm 1 / 3 Dy 1 / 3 )2Ti2O7 and Comparative Example 2Gd2Ti2O7 at an SPS sintering temperature of 1300℃XRD patterns show that the characteristic diffraction peaks correspond to the peaks of A2B2O7 type ceramic Gd2Ti2O7, indicating that at an SPS sintering temperature of 1300℃, the mixed powders of Comparative Example 1 and Comparative Example 2 form a single-phase oxide ceramic with a BCC structure through a solid phase reaction.
[0075] Similarly, the density and grain size of the materials in Comparative Examples 1 and 2 were characterized. 1 / 3Sm 1 / 3 Dy 1 / 3The densities of the sintered samples of Example 3 and Comparative Example 2Gd2Ti2O7 at 1300°C SPS temperature were 97.76% and 95.44%, respectively, and the grain sizes were 1.46 μm and 0.36 μm, respectively. 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 has a density of 98.46% and a grain size of 0.72 μm, which is better than that of Comparative Examples 1 and 2. It has good uniformity of organization and composition, and is beneficial to improving the radiation resistance and corrosion resistance of the material.
[0076] In Comparative Example 1, (Gd 1 / 3 Sm 1 / 3 Dy 1 / 3 )2Ti2O7 and Gd2Ti2O7 in Comparative Example 2 were subjected to thermal property analysis using the same method. 1 / 3 Sm 1 / 3 Dy 1 / 3 The hardness of the entropy carbide ceramic (Gd2Ti2O7) in Example 3 and the Gd2Ti2O7 in Comparative Example 2 at 1300°C SPS sintering temperature are 12.69 GPa and 12.8 GPa respectively. 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 has a hardness of 13.27 GPa, which is better than Comparative Example 1 and Comparative Example 2.
[0077] In addition, the radiation resistance of the materials in Example 3, Comparative Example 1 and Comparative Example 2 was analyzed respectively. The specific method was as follows: the sintered samples were surface polished with 400# to 4000# mesh SiC sandpaper, then polished with 3μm to 1μm alumina suspension, and finally water polished to clean the samples. 17 ions / cm 2 , He with energy of 400keV 2+ Irradiation experiments were performed on Example 3, Comparative Example 1 and Comparative Example 2, respectively, and grazing-incidence-angle X-ray diffraction (GIXRD) analysis was performed on the unirradiated and irradiated samples. Figure 5 As shown, the GIXRD analysis results of the samples of Example 3, Comparative Example 1 and Comparative Example 2 before and after irradiation are compared. It can be seen that after irradiation, most of the characteristic peaks of Gd2Ti2O7 in Comparative Example 2 disappear, and the sample is seriously amorphous; while in Example 3 (Gd 0.2 Sm 0.2 Dy 0.2 Er0.2 Yb 0.2 )2Ti2O7 and Comparative Example 1 (Gd 1 / 3 Sm 1 / 3 Dy 1 / 3 )2Ti2O7 has most of its characteristic peaks, and a small part of the sample is amorphous. 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 and (Gd 1 / 3 Sm 1 / 3 Dy 1 / 3 )2Ti2O7 has better radiation resistance than Gd2Ti2O7. In addition, considering the above characterization results, it can be seen that the present invention (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 high entropy oxide ceramic solidified material has good density and hardness, and has excellent radiation resistance. This is because, compared with Comparative Examples 1 and 2, the material composition design prepared by the present invention is more scientific, and the prepared high entropy oxide ceramic is A2B2O7 type high entropy oxide ceramic, wherein the A-position and B-position cations of the A2B2O7 type oxide can be occupied by lanthanide elements, transition metal elements, actinides and sub-actinides, and have an ordered pyrochlore structure and a disordered fluorite structure, which shows different waste loading capacity and chemical flexibility. Wherein if A is Gd element and B is Ti element, the A2B2O7 type oxide has excellent structural stability and excellent radiation resistance. Oxides of rare earth elements with similar ionic radii are selected to ensure the formation of a stable single-phase solid solution in the high entropy ceramic material. Taking all factors into consideration, Gd2O3, Sm2O3, Dy2O3, Er2O3, Yb2O3 and TiO2 are selected to prepare A2B2O7 type high entropy oxide ceramics. The data also proves the rationality of the designed ingredients.
[0078] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, they are also intended to be included.
Claims
1. A nuclear waste solidification material, characterized in that: It is prepared from A2B2O7 type high entropy oxide ceramics, the molecular formula of which is (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7; The preparation method of the A2B2O7 type high entropy oxide ceramic comprises the following steps: According to (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 proportion Weigh Gd2O3, Sm2O3, Dy2O3, Er2O3, Yb2O3 and TiO2 raw material powders; The weighed raw material powders are mixed and ball-milled, and then the ball-milled powders are subjected to spark plasma sintering to prepare the A2B2O7 type high entropy oxide ceramic; During spark plasma sintering, the target sintering temperature is 1300-1400°C; During spark plasma sintering, the temperature changes as follows: during the heating process, the sample heating rate is initially 100 °C / min, and the heating rate is reduced to 50 °C / min when it is 100 °C before the target sintering temperature. After reaching the target sintering temperature, it is kept warm for 6 min, and then the temperature is lowered at a rate of 100 °C / min. The program ends when the temperature drops to 600 °C, and the sample is taken out after cooling to room temperature. During spark plasma sintering, the pressure at both ends of the spark plasma sintering equipment mold is set to 50 MPa, and the spark plasma sintering chamber is continuously maintained in a vacuum state.
2. The nuclear waste solidification material according to claim 1, characterized in that: The high entropy oxide ceramic is a single-phase body-centered cubic structure.
3. A method for preparing A2B2O7 type high entropy oxide ceramics, characterized in that: The method for preparing the A2B2O7 type high entropy oxide ceramics in claim 1 comprises the following steps: According to (Gd 0.2 Sm 0.2 Dy 0.2 Er 0.2 Yb 0.2 )2Ti2O7 proportion Weigh Gd2O3, Sm2O3, Dy2O3, Er2O3, Yb2O3 and TiO2 raw material powders; The weighed raw material powders are mixed and ball-milled, and then the ball-milled powders are spark plasma sintered to prepare the A2B2O7 type high entropy oxide ceramics.
4. The preparation method according to claim 3, characterized in that: Gd2O3, Sm2O3, Dy2O3, Er2O3, Yb2O3 and TiO2 all use raw materials with a purity of more than 99 wt.%.
5. The preparation method according to claim 3, characterized in that: Each raw material powder is pre-placed in a glove box, and the oxygen concentration in the glove box is less than 4 ppm and the H2O content is less than 0.01 ppm.
6. The preparation method according to claim 3, characterized in that: During ball milling, the mass ratio of the mixture to the grinding balls was 1:10, the ball mill speed was 500 rpm, and a forward and reverse rotation mode was adopted. A total of 15 ball milling cycles were performed, each cycle ran for 20 minutes, and the interval between two adjacent cycles was 10 minutes.
7. The preparation method according to claim 3, characterized in that: During spark plasma sintering, the target sintering temperature is 1300-1400°C.
8. The preparation method according to claim 7, characterized in that: During spark plasma sintering, the temperature changes as follows: during the heating process, the sample heating rate is initially 100 °C / min, and the heating rate is reduced to 50 °C / min when it is 100 °C before the target sintering temperature. After reaching the target sintering temperature, it is kept warm for 6 min, and then the temperature is lowered at a rate of 100 °C / min. The program ends when the temperature drops to 600 °C, and the sample is taken out after cooling to room temperature.
9. The preparation method according to claim 7, characterized in that: During spark plasma sintering, the pressure at both ends of the spark plasma sintering equipment mold is set to 50 MPa, and the spark plasma sintering chamber is continuously maintained in a vacuum state.
Citation Information
Patent Citations
Ultrafine nano A2B2O7 structure high-entropy ceramic and preparation method thereof
CN116102353A
High-entropy ceramic material and coating for high-energy electron protection and preparation method of high-entropy ceramic material and coating
CN116606132A