Composite resin foaming sheet, adhesive tape, display assembly and electronic product

By combining the porous layer of the composite resin foamed sheet with the reinforcement layer, the problems of low cohesion strength and large impact deformation of foam tape are solved, and better tear and impact resistance in electronic products are achieved, ensuring the equipment stability and service life.

CN119036977AActive Publication Date: 2024-11-29HUBEI XIANGYUAN HIGH-TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411326577.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-29
Estimated Expiration
2044-09-23

AI Technical Summary

Technical Problem

Existing foam tapes have problems in electronic products with insufficient cohesion strength and excessive impact deformation, resulting in material failure and structural integrity damage.

Method used

Using composite resin foamed sheets, the reinforcement layer provides rigid support by combining the porous layer with the reinforcement layer, the conversion point impact is to surface impact, and the cohesion and shear strength of the material are enhanced by controlling the diameter and cross-linking of the bubble cell. Ensure that there is no interlayer separation under high and low temperature cycles and thermal aging conditions.

Benefits of technology

The tear resistance and impact deformation control of foamed sheets are improved, while maintaining the buffering performance, enhancing the bonding firmness and impact resistance, extending the service life, and ensuring the structural integrity of electronic equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119036977A_ABST
    Figure CN119036977A_ABST
Patent Text Reader

Abstract

The invention provides a resin foamed sheet, a preparation method thereof, an adhesive tape and application. The resin foaming sheet is obtained by compounding a porous layer and a reinforcing layer, the cohesive force of the porous layer is 1000-4000 gf, the difference value between the melting endothermic peak temperature (Tpm) in the heating process of the porous layer and the exothermic peak temperature (Tpc) in the cooling process of the reinforcing layer is 5-25 DEG C, the reinforcing layer is attached to the porous layer after being melted and is shaped after being cooled, and the interlayer binding force is high. The invention further provides a preparation method of the resin foamed sheet, an adhesive tape formed by the sheet and application of the sheet. The resin foamed sheet provided by the invention improves the problems of low cohesion strength, low shear strength, large impact deformation and the like of a flexible foam tape in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electronic display products, in particular to a sealing tape providing buffering performance in display components and electronic products. Background Art

[0002] With the rapid development of modern industry, especially the rapid growth of the electronics and automotive industries, the demand for high-performance adhesive materials is increasing. In these application areas, foam tapes have been widely used due to their unique cushioning properties and softness. These characteristics enable foam tapes to effectively absorb impact forces and protect equipment from damage caused by vibration and impact, while also being able to adhere well to various uneven surfaces. In addition, the application of foam tapes in electronic devices, especially high-precision, lightweight products such as smartphones, tablets, and wearable devices, also demonstrates its unique design flexibility and functional advantages, overcoming the limitations of traditional fixing methods such as screws, buckles, and glue in lightweight designs.

[0003] However, despite the excellent performance of foam tape in terms of cushioning and softness, there are still some problems that need to be solved in practical applications. One of the main problems is insufficient cohesive strength. Cohesive strength refers to the ability of the material itself to resist damage. It is an important indicator to measure whether the material will not break or tear when subjected to external force. If the cohesive strength is too low, the foam tape is prone to tearing when subjected to external force, resulting in material failure. This not only affects the service life of the tape, but may also cause damage to the bonded components. In electronic products, especially display components, the application process is usually accompanied by heating and cooling of the device. In each power-on application cycle, there is a cycle of hot and cold changes. The rapid change of temperature will cause thermal stress inside the material, especially between different material layers. Due to the difference in thermal expansion coefficient, the stress concentration phenomenon is more obvious. In the cycle of rapid changes in extreme temperature, if there is a loose bond between the layers of multi-layer composite materials, interlayer separation or delamination is prone to occur.

[0004] Another problem is excessive deformation under impact. Ideally, foam tape should be able to absorb impact energy while maintaining a small deformation to avoid adverse effects on sensitive components such as electronic components. However, existing foam tapes may deform significantly when subjected to a large impact, which may damage the structural integrity of electronic devices and even affect their normal operation.

[0005] Therefore, how to maintain the good cushioning performance of the foam tape while improving its cohesive strength and reducing impact deformation during the application process has become a key challenge in the current technological development. Summary of the invention

[0006] In order to improve the above problems, the present invention provides a composite resin foam sheet, a tape comprising the foam sheet, and downstream applications, aiming to improve the problems of low cohesive strength, low shear strength, large impact deformation, etc. of the flexible foam tape in the prior art.

[0007] The inventors conducted in-depth research and found that by compounding a foam sheet with a specific porous layer and a reinforcement layer, the reinforcement layer provides greater rigidity, converts point impact into surface impact, and at the same time improves the cohesion of the porous layer, which can solve the problems of low cohesive strength of the foam sheet, especially low cohesive strength when subjected to high and low temperature changes in application, low shear strength, large impact deformation, etc. At the same time, due to the presence of the reinforcement layer, the overall tensile strength and elongation at break of the material are improved, and the reinforcement layer and the porous layer are firmly combined and still have excellent performance after high and low temperature cycles and thermal aging.

[0008] That is, the gist of the present invention is as follows:

[0009] The present invention discloses a display assembly, comprising a display panel 1, a middle frame 2 and a back cover 3, wherein the middle frame 2 is used to support the display panel 1, the back cover 3 is buckled on the middle frame 2, a buffer sealing tape 4 is provided between the display panel 1 and the middle frame 2 and / or between the middle frame 2 and the back cover 3, and the buffer sealing tape 4 comprises a composite resin foam sheet as a tape substrate, wherein:

[0010] The composite resin foam sheet comprises a porous layer and at least one reinforcing layer; the composite resin foam sheet is peeled off and damaged without appearing at the interface between the porous layer and the reinforcing layer during the cohesion test; the porous layer is formed by foaming a cross-linked polyolefin resin, the cross-linking degree is 15-60%, and the average cell diameter D p 90-200 μm; the reinforcing layer is an uncrosslinked or slightly crosslinked polyolefin resin, the degree of crosslinking is less than 10%; and the average cell diameter D of the porous layer p With the thickness of the single-sided reinforcement layer H r and the cell wall thickness H of the porous layer adjacent to the single-sided reinforcement layer b The following relationship exists:

[0011] 1.4≤D p / (H r +H b )≤6.6;

[0012] Furthermore, the melting endothermic peak temperature T pm The peak temperature T of the heat release peak during the cooling process of the reinforcement layer pc The following relationship exists:

[0013] 5℃≤T pm -T pc ≤25;

[0014] And, the melting endothermic peak temperature T pm The exothermic peak temperature T during the cooling process of the reinforcement layer is: 80-120℃; pc is: 60-115℃.

[0015] The present invention also provides a composite resin foam sheet, comprising a porous layer and at least one reinforcing layer; the composite resin foam sheet is peeled off and damaged during the cohesion test without appearing at the interface between the porous layer and the reinforcing layer; the porous layer is formed by foaming a cross-linked polyolefin resin, the cross-linking degree is 15-60%, and the average cell diameter D p 90-200 μm; the reinforcing layer is an uncrosslinked or slightly crosslinked polyolefin resin, the degree of crosslinking is less than 10%; and the average cell diameter D of the porous layer p With the thickness of the single-sided reinforcement layer H r and the cell wall thickness H of the porous layer adjacent to the single-sided reinforcement layer b The following relationship exists:

[0016] 1.4≤D p / (H r +H b )≤6.6;

[0017] Furthermore, the melting endothermic peak temperature T pm The peak temperature T of the heat release peak during the cooling process of the reinforcement layer pc The following relationship exists:

[0018] 5℃≤T pm -T pc ≤25;

[0019] And, the melting endothermic peak temperature T pm The exothermic peak temperature T during the cooling process of the reinforcement layer is: 80-120℃; pc is: 60-115℃.

[0020] In one of the schemes, the cohesion of the composite resin foam sheet is 1000-4000 gf, and the cohesion is tested by 180° peeling;

[0021] Moreover, after the composite resin foam sheet has undergone 100 cycles of high and low temperatures from -40°C to 80°C, its cohesive force remains above 1000gf, and no interface separation between the porous layer and the reinforcement layer occurs during the high and low temperature cycles.

[0022] In one of the solutions, the composite resin foam sheet has a thickness of 0.3 mm to 2.0 mm and an overall density of 0.060 to 0.125 g / cm 3 , the elongation at break is greater than 250%.

[0023] In one embodiment, the cell density in the porous layer is 15-100 cells / mm 2 The average number of cells in the ZD direction is 2-10, and the reinforcing layer does not contain cells.

[0024] In one of the schemes, the infrared similarity between the porous layer and the reinforcing layer is greater than 80%, and the analysis method of the infrared similarity and infrared identification similarity includes a peak area comparison method, a spectrum fitting method or a correlation coefficient method.

[0025] In one embodiment, the deformation amount of the composite resin foam sheet when the compressive stress is 0.1 MPa is 30%-70%.

[0026] In one embodiment, the thickness of the reinforcement layer is 20-100 μm, and the density of the porous layer is 0.05-0.125 g / cm 3 The density of the reinforcement layer is 0.910-0.920g / cm 3 .

[0027] In one of the schemes, the porous layer of the composite resin foam sheet is made of polyolefin resin using azodicarbonamide as a foaming agent and foaming by thermal decomposition; the reinforcing layer of the foam sheet is composed of polyolefin resin without foaming agent and its decomposition residue.

[0028] In one embodiment, the porous layer of the composite resin foam sheet includes the following components in parts by weight:

[0029] Polyolefin plastomer 20-80 parts

[0030] Polyolefin elastomer 20-80 parts

[0031] 5-10 parts of foaming agent.

[0032] In one embodiment, the composite resin foam sheet reinforcement layer includes the following components, calculated in parts by weight:

[0033]

[0034] In one embodiment, the composite resin foam sheet is laminated to the foaming layer after the reinforcing layer is heated to a completely molten or partially molten state, including but not limited to hot lamination, melt coating, and melt rolling lamination.

[0035] In one embodiment, the reinforcing layer is attached to one or both sides of the porous layer.

[0036] Furthermore, the present invention also provides a sealing buffer tape, comprising the composite resin foam sheet of the present invention as a tape substrate, and an acrylic adhesive is coated on both sides of the tape substrate after corona treatment.

[0037] Furthermore, the present invention also provides a use of a composite resin foam sheet, which is used as a tape substrate in the fields of household appliances, automobiles, and electronic products that require component bonding and / or component protection.

[0038] Furthermore, the present invention also provides an electronic product, comprising the composite resin foam sheet of the present invention or the sealing buffer tape of the present invention.

[0039] Beneficial effects of the present invention:

[0040] The present invention forms a composite structure foam sheet by compounding a porous layer and a reinforcing layer, and reasonably controls the pore diameter and cross-linking degree of the porous layer, so that the foam material maintains overall softness while having excellent tear resistance. At the same time, the presence of the reinforcing layer improves the hardness and flatness of the foam sheet surface, making it easier for the foam sheet to adhere firmly when it is attached to the glue, and shortening the aging time. In addition, the reinforcing layer has rigid support, and forms a "dispersed" large-area absorption of the impact force at the moment of force, and controls the deformation in the thickness direction to an ideal state that can meet the buffering requirements and maintain no excessive deformation.

[0041] At the same time, by regulating the DSC melting and crystallization peak temperatures of the porous layer and the reinforcement layer, the melting endothermic peak temperature (T pm ) and the exothermic peak temperature (T pc ) is within a specific range, so that the porous layer and the reinforcement layer are well combined, and the interface separation of the porous layer and the reinforcement layer is difficult to occur under various test conditions such as shear in different directions or glass, peeling after high and low temperature cycles, and thermal aging, etc., which further compensates for the impact defects caused by the composite, so that the composite resin foam sheet can take into account softness, tear resistance, impact deformation and peeling damage after impact in a variety of application scenarios. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 It is a schematic diagram of the structure of the display assembly of the present invention;

[0043] Description of reference numerals: 1-display panel; 2-middle frame; 21-blocking portion; 22-bearing portion; 3-back cover; 4-buffer sealing tape;

[0044] Figure 2 It is a schematic diagram of the overall cross section of the composite resin foam sheet;

[0045] Figure 3 Schematic diagram of the lamination process of the porous layer and the reinforcement layer (single-sided).

[0046] Among them, 5. reinforcement layer; 6. porous layer; 7. heating roller; 8. cooling and shaping roller; 9. composite resin foam sheet. DETAILED DESCRIPTION

[0047] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art in this field can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.

[0048] The composite resin foam sheet of the present invention comprises a porous layer and a reinforcing layer which are laminated to each other to form a multi-layer composite layer structure, wherein the reinforcing layer is laminated to one side or both sides of the porous layer.

[0049] [Porous layer]

[0050] The porous layer of the present invention, i.e., in the layer, has a porous structure, and the polymer matrix is ​​separated by pores, which give the porous layer excellent cushioning and impact absorption properties, can effectively disperse and absorb energy, and reduce damage to sensitive components. In addition, the air permeability and lightness of the porous layer also bring additional advantages to the composite resin foam sheet, such as reducing weight and improving the comfort of use of the material. The crosslinking degree of the polyolefin resin in the porous layer is 15-60%, preferably 20-50%, and further preferably 25-45%. When it is within this range, it is more conducive to forming a foam material with moderate pore size and high independent porosity, and the foam layer has good tear resistance, which is an important factor affecting the cohesion of the material.

[0051] Furthermore, the average diameter D of the cells in the porous layer is p It is 90-200μm, preferably, and further preferably, when it is within the above range, it can give the material excellent cushioning and impact absorption properties, can effectively disperse and absorb energy, reduce damage to sensitive components, and at the same time ensure high cohesion, avoiding the problem of insufficient cohesion due to excessive pore size, so it is also an important factor affecting the cohesion of the material.

[0052] The average cell diameter D of the porous layer is p With the thickness of the single-sided reinforcement layer H r and the cell wall thickness H of the porous layer adjacent to the single-sided reinforcement layer b The following relationship exists:

[0053] 1.4≤D p / (H r +H b )≤6.6; for details, please refer to Figure 2 A schematic diagram of the overall cross-section of a composite resin foam sheet, showing H r and H bThe meaning of H r is the thickness of the single-sided reinforcement layer, H b is the thickness of the cell wall of the porous layer adjacent to the single-sided reinforcement layer, and the cell wall of the porous layer adjacent to the single-sided reinforcement layer is as follows: Figure 2 As shown, it is the maximum area when the lower end of the single-sided reinforcement layer extends and no bubbles appear in the porous layer, and its thickness is the thickness of this maximum area.

[0054] Preferably 2≤D p / (H r +H b )≤6, more preferably 3≤D p / (H r +H b )≤5; when the above relationship exists, it is found that the reinforcement layer can better ensure the dispersion of impact force as a rigid support, and establish an ideal balance between impact force dispersion and cushioning performance. If it is less than 1.4, it is found that the cushioning performance is poor, the bubble deformation in the porous layer is insufficient, and the energy absorption is poor, resulting in brittle damage to the foamed sheet; if it exceeds 6.6, it is found that the rigid support effect is not good, and it is impossible to form a "dispersed" large-area absorption of the impact force at the moment of force, and it is easy to form a large deformation in the local area of ​​the impact while other parts are less deformed, resulting in unevenness of the tape under impact.

[0055] <Component>

[0056] The porous layer of the composite resin foam sheet comprises the following components, in parts by weight:

[0057] Polyolefin plastomer 20-80 parts

[0058] Polyolefin elastomer 20-40 parts

[0059] Foaming agent 4-10 parts

[0060] The polyolefin plastomer is used as the base material of the porous layer to provide structural strength for the porous layer and maintain overall shape and dimensional stability. The weight content of the polyolefin plastomer is preferably 30-70 parts by weight, and more preferably 40-60 parts by weight. The selection of specific polyolefin plasticizers is not specifically limited, including but not limited to other polyethylene resins except linear low-density polyethylene, such as low-density polyethylene (LDPE), medium-density polyethylene (MDPE), high-density polyethylene (HDPE), and modified polyethylene; ethylene-α-olefin copolymers with ethylene as the main component can also be selected, wherein the α-olefin is selected from α-olefins such as propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 3-methyl-1-pentene, 4-methyl-1-pentene, 3-ethyl-1-pentene, 1-octene, 1-decene, and 1-undecene, each having 2-12 carbon atoms, and the number of such α-olefins can be only one, or can be more than two; polypropylene resins can also be selected, such as propylene homopolymers, propylene-ethylene copolymers, propylene-ethylene-α-olefin copolymers, and propylene-α-olefin copolymers; and ethylene-vinyl acetate copolymers, etc. Based on mechanical properties and cost considerations, polyethylene resins (different from polyolefin elastomers and linear low-density polyethylene) are preferred.

[0061] Among them, the polyolefin elastomer can increase the resilience of the porous layer and give the final composite resin foam sheet shape tracking properties, and is further preferably 30-70 parts by weight, and more preferably 40-60 parts by weight. Specifically listed are: natural rubber, polyisobutylene, isoprene rubber, butyl rubber, chloroprene rubber, nitrile rubber and other natural or synthetic rubbers; olefin elastomers such as ethylene-vinyl acetate copolymer, polybutylene, polyisobutylene and chlorinated polyethylene; styrene elastomers such as styrene-isoprene-styrene copolymer (SIS), styrene-butadiene-styrene copolymer (SBS), styrene-isoprene-butadiene-styrene copolymer (SIBS), and hydrogenated polymers thereof; thermoplastic polyester elastomers; thermoplastic polyurethane elastomers; and thermoplastic acrylic elastomers. The number of types of these rubbers and / or thermoplastic elastomers can be only one, or can be more than two.

[0062] The choice of the foaming agent is not particularly limited, and an inorganic foaming agent or an organic foaming agent can be used. Examples of the inorganic foaming agent include ammonium carbonate, ammonium bicarbonate, sodium bicarbonate, ammonium nitrite, sodium borohydride, and various azides. In addition, as organic foaming agents, for example, fluorinated alkane compounds such as trichloromonofluoromethane and dichloromonofluoromethane; azo compounds such as azobisisobutyronitrile, azodicarbonamide, and barium azodicarboxylate; hydrazine compounds such as p-toluenesulfonylhydrazine, diphenylsulfone-3,3'-disulfonylhydrazine, 4,4'-oxybis(benzenesulfonylhydrazine), and allylbis(sulfonylhydrazine); semicarbazide compounds such as p-toluenesulfonylsemicarbazide and 4,4'-oxybis(benzenesulfonylsemicarbazide); triazole compounds such as 5-morpholinyl-1,2,3,4-thiazole; N,N'-dinitrosopentamethylenetetramine, N,N'-dimethyl-N,N'-dinitrosoterephthalamide; and other N-nitroso compounds. From the perspective of high efficiency and uniform controllable foaming, azodicarbonamide is preferably used as the foaming agent. The content of the foaming agent is 4-10 parts by weight.

[0063] Optionally, the porous layer also contains carbon black, which plays a light shielding role in some application scenarios, and the content is 0.05-1 parts by weight, preferably 0.2-0.8 parts by weight. Based on considerations during the processing, other additives such as antioxidants, cross-linking agents, etc. may also be contained.

[0064] <Cells>

[0065] The average pore size of the porous layer of the composite resin foam sheet is 60-200 μm, preferably 70-180 μm, further preferably 80-160 μm, and more preferably 90-150 μm. Within this size range, it helps to provide good cushioning performance without excessively increasing the density of the material.

[0066] In addition, the cell density, i.e., the number of cells per unit area formed by the MD or TD direction and the thickness direction obtained by the test method of the present invention, is between 15 and 100 cells / mm 2 , preferably 30 to 90, more preferably 35 to 80, and more preferably 40 to 70. Within this range, the porous layer is ensured to have sufficient structural strength while maintaining the necessary softness, which helps to maintain the cohesion of the porous layer and prevent internal tearing when subjected to force.

[0067] And in the porous layer, the average number of cells in the ZD direction is 2-10, and the ZD direction refers to the direction perpendicular to the surface of the porous layer in the composite resin foam sheet, that is, the thickness direction, in which the polymer matrix and the cells are arranged alternately to form a multilayer structure. Observe in the ZD direction, and record 1 cell from the upper surface to the lower surface of the same cell. The number of cells in the thickness distance range of the porous layer ZD direction is counted as the number of cells in the ZD direction, and statistics are performed at several measurement positions to calculate the average value of the number of cells in these measurement areas. This average value is the average number of cells in the ZD direction. Preferably 3-9, more preferably 4-8. In this range, it is ensured that the porous layer, while maintaining the necessary softness, helps to disperse and absorb energy when the plane is impacted, and reduces the impact damage to the interface of the reinforcing layer, thereby optimizing the cushioning effect. If the number is too small, there will be no cushioning effect; if the number is too large, the pore size is too dense, and only the bubbles close to the surface play the role of energy absorption, while the internal pores do not play their role, resulting in the impact energy not being better conducted and the deformation being uneven.

[0068] <Cohesion of composite resin foam sheet>

[0069] The composite resin foam sheet of the present invention does not peel off and fail at the interface between the porous layer and the reinforcing layer during the cohesion test, nor does it occur at the reinforcing layer. Therefore, the cohesion of the composite resin foam sheet is actually the cohesion of the porous layer, that is, the peeling force that the porous layer withstands when it breaks when the 180° peeling method is used for testing. That is to say, the cohesion of the composite resin foam sheet of the present invention is 1000-4000gf, which is also the cohesion of the porous layer. The cohesion of the porous layer depends on the raw material components, pore size and distribution, crosslinking degree, and molding heat treatment mentioned above.

[0070] [Enhancement Layer]

[0071] The reinforcing layer of the present invention, that is, in this layer, basically does not contain pores or unfoamed foaming agent, provides additional strength and rigidity of the composite resin foam sheet, and provides a certain degree of flatness, so that the foam sheet is easier to adhere firmly when it is attached to the glue, and shortens the aging time. The thickness of the reinforcing layer is 20-100μm, preferably 30-80μm, and more preferably 40-70μm. Within the above range, the strength and softness of the composite resin foam sheet can be better taken into account. Of course, when the thickness range is specifically selected, the thickness of the overall composite resin foam sheet also needs to be considered to avoid the thickness of the reinforcing layer from being too high. The tensile strength and elongation at break are mainly provided by the reinforcing layer. The reinforcing layer is an uncrosslinked or slightly crosslinked polyolefin resin with a crosslinking degree of less than 10%. The uncrosslinked or slightly crosslinked polyolefin resin has a higher elongation at break. Excessive crosslinking will affect the ductility of the polyolefin resin, reduce the elongation of the reinforcing layer, and the residual stress after film formation is large, which is not conducive to the firm combination of the porous layer and the reinforcing layer of the composite resin foam sheet.

[0072] In addition to providing strength and rigidity in the horizontal direction of the foam sheet, the reinforcing layer also provides rigid support in the thickness direction. When it receives impact in the thickness direction, it forms a "dispersed" large-area absorption and then transmits it to the internal porous layer, thereby effectively playing an impact resistance and buffering role, and also avoiding local protruding deformation.

[0073] <Component>

[0074] The components of the reinforcement layer are similar to those of the porous layer, and also include polyolefin plastomers and polyolefin elastomers. The similarity between the two is greater than 80% through infrared similarity identification, which proves that although there are differences in the material components, based on the principle of similar compatibility, the functional functional groups are still consistent, that is, the specific material selection of polyolefin plastomers and polyolefin elastomers is basically consistent with that of the porous layer.

[0075] <Linear Low Density Polyethylene>

[0076] Compared with the porous layer, linear low-density polyethylene is mainly used in the reinforcement layer to increase tensile strength, stiffness and rigidity. The linear molecular chains of LLDPE tend to be arranged more closely to form a more regular crystal structure. This orderly arrangement increases the overall strength and deformation resistance of the material. And its molecular chain still maintains a certain flexibility, which helps to absorb and disperse the force applied to the material, thereby improving its overall mechanical properties. The content of linear low-density polyethylene is 40-80 parts by weight, preferably 50-70 parts by weight. It should be noted that although the porous layer does not contain linear low-density polyethylene, linear low-density polyethylene (LLDPE) and other types of polyethylene are very similar in chemical structure, and are polymers formed by polymerization of ethylene monomers, so they have little effect on infrared similarity.

[0077] The reinforcing layer does not contain any foaming agent, so its density is 0.910-0.920 g / cm 3 And the layer does not contain cells larger than 0.1 μm. If there are cells larger than 0.1 μm, it means that there are defects in the reinforcement layer, which is not conducive to providing greater rigidity, and the defects will become stress points in the impact, resulting in an inability to ideally convert into surface impact.

[0078] The reinforcing layer may also contain stearate and antioxidants to ensure the fluidity and anti-oxidation of the reinforcing layer during high-temperature bonding.

[0079] <Bonding strength between the reinforcement layer and the porous layer>

[0080] In the present invention, the bonding force between the reinforcing layer and the porous layer is greater than the cohesive force of the porous layer, which requires that the reinforcing layer and the porous layer penetrate each other at the interface. According to the principle of like dissolves like, the infrared similarity of the two layers reflecting the material difference must be greater than 80%. In addition, the hot pressing temperature and hot pressing pressure must be kept within a controlled range to ensure that the bonding force between the reinforcing layer and the porous layer is within an ideal range.

[0081] [Composite resin foam sheet]

[0082] < Melting endothermic peak temperature T pm The exothermic peak temperature T during cooling pc >

[0083] In the present invention, the peak temperature T of the melting endothermic peak of the porous layer is controlled pm The peak temperature T of the heat release peak during the cooling process of the reinforcement layer pc The difference between 5 and T is used to control the melting of the porous layer under heating conditions and the lossless bonding of the reinforcement layer. pm -T pc When the temperature is ≤25℃, it can ensure that the reinforcement layer will not be unable to melt the porous layer due to too fast cooling speed, resulting in failure to bond; nor will the porous layer be too melted during bonding due to too high temperature, causing severe damage and deformation, thereby reducing the thickness and compressive stress. Preferably, 8℃≤T pm -T pc ≤23℃, more preferably 10℃≤T pm -T pc ≤20℃, more preferably 12℃≤T pm -T pc ≤18℃.

[0084] The peak temperature of the porous layer melting endothermic peak T pm The peak temperature T of the heat release peak during the cooling process of the reinforcement layer pcThe control of is related to the material composition, crystallinity, molecular weight, crosslinking degree, and thermal history. In the present invention, the infrared similarity between the porous layer and the reinforcing layer is greater than 80%, which means that the functional groups are highly similar. The peak temperature of the melting endothermic peak of the porous layer is T pm The peak temperature T of the heat release peak during the cooling process of the reinforcement layer pc The control of the porous layer and the reinforcing layer can be realized by adjusting the crystallinity, molecular weight, crosslinking degree and other factors of the porous layer and the reinforcing layer based on the specific polyolefin material with high similarity, and those skilled in the art also know on the basis of the present invention that the peak temperature T of the melting endothermic peak of the porous layer can be controlled. pm The peak temperature T of the heat release peak during the cooling process of the reinforcement layer pc That is, it can solve the technical problem of this link in the invention, and the control factors for realizing this means are also clearly defined here, so there is no need to list and limit the specific details.

[0085] <High and low temperature cycle T-type peel test and dynamic shear test>

[0086] The composite resin foam sheet described in the present invention is subjected to a tear resistance test by means of a T-type peel test and a dynamic shear test before and after high and low temperature cycles. The T-type peel test before high and low temperature cycles reflects the static peeling force between layers, that is, the tear resistance in the thickness direction, that is, the interlayer cohesion F0. The T-type peel test after high and low temperature cycles reflects the peeling force under environmental changes, that is, the tear resistance in the thickness direction; and the dynamic shear test reflects the tear resistance in the horizontal direction of the layer. Subsequent experiments proved that the two tear resistance tests of the composite resin foam sheet of the present invention were both torn at the porous layer rather than at the junction of the porous layer and the reinforcement layer. The corresponding maximum tear force in the T-type peeling test before high and low temperature cycling, that is, the cohesive force F0 of the porous layer, ranged from 1000-4000 gf, preferably from 1500-3500 gf, further preferably from 2000-3000 gf, and more preferably from 2200-2800 gf. The maximum shear force range when the porous layer is torn in the shear test is from 100-400 gf, preferably from 130-380 gf, further preferably from 150-350 gf, and more preferably from 200-300 gf.

[0087] Furthermore, through the T-peel test under the high and low temperature cold and hot cycles of the present invention, the composite resin foam sheet of the present invention is still maintained above 1000gf, and there is no interface separation between the porous layer and the reinforcing layer. This shows that the reinforcing layer and the porous layer of the present invention still maintain good bonding under the influence of alternating hot and cold on the material; it is speculated that the main reason is that the present invention controls the infrared similarity and DSC difference. When the infrared similarity is high, the difference in thermal expansion coefficient between the materials of each layer is small. When the DSC difference is within the range specified by the present invention, the material is firmly composited and the residual internal stress is small, and the rapid change of temperature will not weaken the bonding force between the layers.

[0088] [Compound Process]

[0089] The preparation process of the composite resin foam sheet of the present invention comprises:

[0090] 1. Preparation of porous layer;

[0091] According to the previously disclosed porous layer raw material components, the sheet is made after being uniformly kneaded with a limited weight portion, and after irradiation cross-linking, high-temperature foaming is performed to obtain a porous layer of a composite resin foam sheet; wherein the irradiation cross-linking is not particularly limited, and is performed according to the conventional irradiation cross-linking method in the art, and the porous layer sheet can be cross-linked by ionizing radiation such as electron beams, α-rays, β-rays, and γ-rays, preferably electron beam irradiation cross-linking; single-sided irradiation or double-sided irradiation can be performed, preferably double-sided irradiation; the irradiation amount of the above ionizing radiation is adjusted in a manner such that the cross-linking degree of the obtained foam sheet becomes the desired range, such as 10Mrad-30Mrad, preferably 12Mrad-28Mrad, and more preferably 15Mrad-25Mrad. The energy of irradiation cross-linking will affect the rate of cross-linking, and is usually selected as 1.0Mev-3.0Mev, preferably 1.2Mev-2.8Mev, and more preferably 1.5Mev-2.5Mev.

[0092] The porous layer of the foamed sheet obtained by high-temperature foaming after cross-linking treatment is foamed at normal pressure and high temperature. The temperature for heating and foaming varies depending on the decomposition temperature of the thermal decomposition type foaming agent. When an azo compound foaming agent is used, it is usually 140-300°C, preferably 160-260°C.

[0093] 2. Composite materials of porous layer and reinforcement layer:

[0094] Since the porous layer is a soft and easily deformable porous structure, it is necessary to avoid directly heating the porous layer during compounding to avoid destroying the pore structure. The present invention uses the composite of the porous layer and the reinforcing layer material to heat the reinforcing layer to a molten state and press it with the porous layer. The reinforcing layer releases heat during cooling to melt the surface of the porous layer, and the composite resin foam sheet is tightly fitted under appropriate pressure. The method of heating the reinforcing layer to a molten state includes: 1) directly laminating the reinforcing layer after the extruder melts the reinforcing layer into a film; 2) after the reinforcing layer is made into a film by means of film blowing, film lamination, double-drawing film formation, etc., it is heated and compounded by a hot roller; 3) after the reinforcing layer is coated on the foam surface by a coating machine, it is cooled and formed.

[0095] One of the methods can refer to the present invention Figure 3 As shown, the formed reinforcement layer 5 is laminated to the porous layer 6 by a heating roller 7 and then shaped by a cooling shaping roller 8 to obtain a composite resin foam sheet 9.

[0096] Regardless of the method, the reinforcing layer must be in a molten state before contacting the porous layer, with a temperature of 150-250°C, preferably 160-220°C; a certain pressure must be applied during lamination, with a hot pressing pressure of 0.2-1.5 MPa, preferably 0.5-1.2 MPa.

[0097] [application]

[0098] The composite resin foam sheet of the present invention is used as a tape substrate in the fields of home appliances, automobiles, and electronic products that require bonding and component protection. Specifically, it includes:

[0099] 1. Window, LCD module fixation and protection: In modern smart devices, multi-layered flexible foam tape is directly attached to the back of the display module as a buffer component. The multi-layer foam support layer has sufficient support capacity and anti-deformation ability to ensure the precise alignment and stable connection between the display module and the shell. It can effectively absorb the impact of falling or squeezing without affecting the display clarity, protecting the fragile display panel from damage.

[0100] 2. Camera module fixation: For precise fixation of camera modules, flexible foam can be designed into a sandwich structure with precise size and shape, which fits precisely around the periphery of the camera. This structure not only provides the necessary physical support to ensure the module is firmly positioned in the device and reduce image blur caused by vibration, but may also contain a shock-absorbing layer to absorb the tiny vibrations generated during the use of the device and improve the image quality.

[0101] 3. FPCB (flexible printed circuit board) fixing: When fixing FPCB, the multi-layer structure foam can be designed as a clamping structure with a specific shape and thickness. Using its softness and self-adhesiveness, it gently and firmly wraps the edge of the circuit board to prevent movement inside the device or deformation due to force. This design can ensure the stability of the electrical connection of the circuit board, while reducing the requirements for the bending of the FPCB, which is conducive to the efficient use of space and simplification of the assembly process.

[0102] 4. Built-in antenna module fixation: In antenna design, multi-layer foam can integrate a conductive layer or an electromagnetic shielding layer to fix the antenna module while providing the necessary electromagnetic interference (EMI) shielding. This design helps optimize the radiation performance of the antenna, reduce signal interference, and ensure the quality of wireless communication. Through precise layout, the foam can also serve as an isolation layer to avoid mutual interference between the antenna and other electronic components.

[0103] 5. Dustproof, cushioning and waterproofing of electronic equipment casing: In the dustproof, cushioning and waterproofing design of electronic equipment, multi-layer foam is used as a dustproof pad to fill the gap in the shell to prevent dust and particles from entering; the highly elastic cushioning layer can effectively absorb impact and protect internal sensitive components; at the same time, a specific waterproof foam layer is designed around the interface and buttons to form a sealing ring to prevent moisture intrusion and ensure the waterproof performance of the equipment.

[0104] When used as an adhesive tape, the composite resin foam sheet of the present invention is used as an adhesive tape substrate, and both sides of the adhesive tape substrate are subjected to corona treatment and coated with an acrylic adhesive to obtain the adhesive tape.

[0105] The composite resin foam sheet of the present invention forms an electronic product sealing tape, which is attached between a printed circuit board and a cover plate of an electronic product, or between an image display component and a display glass plate, especially in the limited space between a bearing unit, a housing and a display panel, and then is sealed and shaped to play a buffering and impact-resistant role. At the same time, it is not easy to peel off and has little deformation when impacted, which is beneficial to maintaining the dimensional stability of display devices and electronic products.

[0106] The electronic products include: intelligent mobile communication devices, laptop computers, liquid crystal displays, OLED displays, e-books, tablet terminals, gaming devices, cameras, and wearable electronic devices.

[0107] Take the display component as an example, Figure 1As shown in the figure, it is the structure of the polyolefin-based buffer foamed sheet of the present invention applied to a display component. The display component includes a display panel 1, a middle frame 2, and a rear cover 3. The middle frame 2 is used to support the display panel 1, and the rear cover 3 is buckled to the middle frame 2. The middle frame 2 has a blocking portion 21 and a bearing portion 22 perpendicular to the blocking portion 21. The display panel 1 is disposed on the bearing portion 22 and is fixedly connected to the display panel 1 through a buffer sealing tape 4. The rear cover 3 and the middle frame 2 can also be hermetically connected through a buffer and yield-resistant sealing tape. In addition, other electronic components in the display component, such as a PCB board, a battery, etc., are disposed in an accommodation space formed by the display panel 1, the middle frame 2, and the rear cover 3. A buffer sealing tape can also be disposed on the side of the rear cover facing the display panel to play a role in buffering and protecting the electronic components.

[0108] [Test Conditions]

[0109] The methods for measuring the performance indicators involved in the present invention are as follows:

[0110] <Average Pore Diameter / Pore Density>

[0111] Cut the composite resin foamed sheet into 50 mm × 50 mm square samples as the foamed body samples for measurement. After soaking it in liquid nitrogen for 1 minute, cut it along the MD direction, TD direction, and ZD direction in the thickness direction with a blade. Use a digital microscope to take magnified photos of the cross-section, measure the bubble diameters of all independent bubbles existing on the cut surfaces of each 2 mm length in the MD direction, TD direction, and ZD direction. The incomplete holes caused by sampling are not included in the statistics, and repeat this operation 5 times. Take the average value of all bubbles as the average bubble diameter of the foamed material.

[0112] For the TD or MD direction, 2 mm × the sample thickness direction t is the observation area, count the total number of pores m in this area, and calculate according to the following formula (unit: number / mm 2 ):

[0113] Pore density = m / 2t

[0114] <Average Number of Pores in the ZD Direction>

[0115] Make 3 samples by the above method for testing pores. Randomly take 5 places for each sample to observe the number of pores in the thickness direction, and find the average value.

[0116] <Infrared Similarity>

[0117] The infrared spectra of the reinforcing layer and the porous layer are tested by the infrared ATR mode, with 16 scanning times, 4 resolution, and a data interval of 0.482 cm -1 , and the scanning range is 4000 - 600 cm -1After obtaining the infrared spectra of the reinforcement layer and the porous layer, the quality inspection function of the OMNIC software was used to compare the infrared spectra of the reinforcement layer and the porous layer to obtain the infrared spectrum 4000-600cm -1 Similarity within the region.

[0118] <T-type peel test before high and low temperature cycling, F0>

[0119] After corona treatment, the composite resin foam sheet was cut into narrow strips with a width of 25 mm and placed under standard test conditions for 48 hours. 3M 9448A tape and reinforced PET film were pasted on both sides respectively. After being placed under standard test conditions for 48 hours, the PET films pasted on both sides of the composite resin foam sheet were fixed by a tensile testing machine, and the composite resin foam sheet was destroyed by a 180° peeling method. The destruction form of the composite resin foam sheet was observed to obtain the average force value of the test.

[0120] <T-type peeling test under high and low temperature thermal cycle, F1>

[0121] Using a hot and cold cycle test chamber, the test samples were tested according to the GB / T 2423.22 method, and the program settings are as follows:

[0122] TH (test temperature): 70℃±2℃;

[0123] TL (test temperature): -40℃±2℃;

[0124] tc1 (stabilization time after temperature switching): 5min;

[0125] tc2 (sample TH temperature stabilization time): 1h;

[0126] tc3 (sample TL temperature stabilization time): 1h;

[0127] T (number of cycles): 24 cycles;

[0128] After returning to room temperature, perform the test according to <T-type peel test before high and low temperature cycle>.

[0129] <Shear test, maximum shear value>

[0130] 1. Sample surface treatment: After the sample surface is cleaned with alcohol, both sides are primed with 3M 94 primer;

[0131] 2. Adhesive tape: double-sided adhesive tape (Jinghua 903 tape)

[0132] 3. Sample size: 25×25×product thickness mm

[0133] 3. Place the sample between the test steel plates. The sample should be placed in the middle of the narrow sides of the two test steel plates as much as possible. To avoid residual bubbles, press the sample for 4 seconds at a pressure of 0.3 MPa and place it at a temperature of 25°C ± 3 for 3 days.

[0134] 4. The test speed of the electronic universal testing machine is set to 10mm / min, the inlet force is set to 1N, the test is started after the equipment is reset, the tensile testing machine is tested at a constant test speed, and the shear strength is read on the software;

[0135] 5. Observe the damage form of the sample. The tear test results between the foam layers are valid. There should be no detachment of the glue, foam or steel plate.

[0136] 6. Record the maximum force when the sample is sheared;

[0137] 7. Both horizontal and vertical directions need to be tested, 3 groups each, and the average value is taken.

[0138] <Deformation under 0.1MPa compressive stress>

[0139] Test compression according to ASTM D3574, and find the compression ratio corresponding to the deformation under 0.1 MPa compression stress based on the compression curve.

[0140] <Porous layer T pm , enhancement layer T pc >

[0141] The samples were scanned using a Mettler Toledo DSC3 instrument in a temperature range of -70 to 250°C at a heating rate of 10°C / min.

[0142] Test conditions: sample weight 0.8 to 1.2 mg, nitrogen atmosphere, cycle temperature:

[0143] Heating process, 30 to 180, 10 / min, nitrogen 50ml / min, eliminate thermal history;

[0144] Constant temperature process, 180, 2min, nitrogen 50ml / min, buffer;

[0145] Cooling process, 180 to 30, -10 / min, nitrogen 50ml / min, cooling crystallization;

[0146] Constant temperature process, 30, 2min, nitrogen 50ml / min, buffer;

[0147] Heating process, 30 to 180, 10 / min, nitrogen 50ml / min, melting test.

[0148] Take the cooling curve to find the exothermic peak temperature (Tpc )

[0149] Take the DSC melting curve of the second heating and find the melting endothermic peak temperature (T pm )

[0150] When the DSC melting peak has multiple peaks, the peak with the largest area is used as the basis.

[0151] <Falling ball impact evaluation>

[0152] Place the glass test piece on a flat steel plate with a thickness of 10 mm, and place a 20 mm*20 mm foam sheet on the glass test piece with the reinforcement layer of the foam sheet facing upwards;

[0153] A steel ball weighing 30±0.5g is released from above the foam sheet. The steel ball falls freely and hits the center of the foam sheet. After the falling ball hits, observe whether the glass test piece is damaged or cracked;

[0154] During the test, gradually adjust the release height of the steel ball from low to high, increasing by 20 cm, and record the lowest release height at which the glass test piece is damaged and cracked by the drop ball test;

[0155] When the minimum release height at which the glass test piece is damaged and cracked in the drop ball test is 20 cm, the point impact resistance of the foam sheet is evaluated as C; when the release height is below 40 cm, the point impact resistance of the foam sheet is evaluated as B; when the release height is above 40 cm, the point impact resistance of the foam sheet is evaluated as A.

[0156] The conditions of each test are kept consistent, including the weight of the steel ball, the placement of the foam sheet, and the model of the glass test piece. After each test, a new glass test piece and foam sheet are replaced to ensure the accuracy of the results. The glass test piece is a sailboat brand cover glass 24mm*24MM, with a thickness of 0.15±0.02mm.

[0157] The present invention is described below by means of several examples related to the present invention, but there is no intention to limit the present invention to these examples. The “parts” mentioned in the following examples and comparative examples are all “parts by weight”.

[0158] Embodiment 1:

[0159] 50 parts of polyolefin plastomer, 50 parts of polyolefin elastomer, 7 parts of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mixer, the temperature was set at 100°C, the mixing was carried out for 15 minutes, and the resin sheet was extruded and calendered into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 14.3 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0160] 20 parts of polyolefin plastomers, 20 parts of polyolefin elastomers, 60 parts of linear low-density polyethylene, 0.5 parts of carbon black, 0.08 parts of stearate, and 0.08 parts of antioxidants are extruded by a single screw in a molten state at a temperature of 190°C, coated on a porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 0.6 MPa to form a 1.1 mm foamed sheet, wherein the thickness of the reinforcing layer is H r 50μm, prepare samples for performance testing.

[0161] Embodiment 2:

[0162] 80 parts of polyolefin plastomer, 20 parts of polyolefin elastomer, 4 parts of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mixer, the temperature was set at 100°C, and the mixture was mixed for 15 minutes. The mixture was extruded and rolled into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 14.3 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0163] 20 parts of polyolefin plastomers, 20 parts of polyolefin elastomers, 60 parts of linear low-density polyethylene, 0.5 parts of carbon black, 0.08 parts of stearate, and 0.08 parts of antioxidants are extruded by a single screw in a molten state at a temperature of 220°C, coated on a porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 0.6MPa to form a 0.3mm foamed sheet, wherein the thickness of the reinforcement layer is H r 50μm, prepare samples for performance testing.

[0164] Embodiment 3:

[0165] 20 parts of polyolefin plastomer, 80 parts of polyolefin elastomer, 10 parts of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mixer, the temperature was set at 100°C, and the mixture was mixed for 15 minutes. The mixture was extruded and rolled into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 14.3 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0166] 20 parts of polyolefin plastomers, 20 parts of polyolefin elastomers, 60 parts of linear low-density polyethylene, 0.5 parts of carbon black, 0.08 parts of stearate, and 0.08 parts of antioxidants are extruded by a single screw in a molten state at a temperature of 160°C, coated on a porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 0.6MPa to form a 2.0mm foamed sheet, wherein the thickness of the reinforcing layer is H r 30μm, prepare samples for performance testing.

[0167] Embodiment 4:

[0168] 50 parts of polyolefin plastomer, 50 parts of polyolefin elastomer, 7 parts of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mixer, the temperature was set at 100°C, and the mixture was mixed for 15 minutes. The mixture was extruded and rolled into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 14.3 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0169] 20 parts of polyolefin plastomer, 20 parts of polyolefin elastomer, 60 parts of linear low-density polyethylene, 0.5 parts of carbon black, 0.08 parts of stearate, and 0.08 parts of antioxidant are extruded by a single screw in a molten state at a temperature of 220°C, coated on a porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 1.0 MPa to form a 0.57 mm foamed sheet, wherein the thickness of the reinforcing layer is H r 60μm, prepare samples for performance testing.

[0170] Embodiment 5:

[0171] 50 parts of polyolefin plastomer, 50 parts of polyolefin elastomer, 7 parts of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mixer, the temperature was set at 100°C, and the mixture was mixed for 15 minutes. The mixture was extruded and rolled into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 14.3 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0172] 20 parts of polyolefin plastomer, 80 parts of linear low-density polyethylene, 0.5 parts of carbon black, 0.08 parts of stearate, and 0.08 parts of antioxidant are extruded by a single screw in a molten state at a temperature of 190°C, coated on a porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 0.6MPa to form a 1.13mm foamed sheet, wherein the thickness of the reinforcement layer is H r 80μm, prepare samples for performance testing.

[0173] Embodiment 6:

[0174] 50 parts of polyolefin plastomer, 50 parts of polyolefin elastomer, 7 parts of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mixer, the temperature was set at 100°C, and the mixture was mixed for 15 minutes. The mixture was extruded and rolled into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 14.3 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0175] 20 parts of polyolefin plastomer, 40 parts of polyolefin elastomer, 40 parts of linear low-density polyethylene, 0.5 parts of carbon black, 0.08 parts of stearate, and 0.08 parts of antioxidant are extruded by a single screw in a molten state at a temperature of 190°C, coated on a porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 0.6MPa to form a 1.14mm foamed sheet, wherein the thickness of the reinforcing layer is H r 25μm, prepare samples for performance testing.

[0176] Embodiment 7:

[0177] 50 parts of polyolefin plastomer, 50 parts of polyolefin elastomer, 7 parts of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mixer, the temperature was set at 100°C, and the mixture was mixed for 15 minutes. The mixture was extruded and rolled into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 14.3 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0178] 20 parts of polyolefin plastomer, 20 parts of radiation-modified polyolefin elastomer, 60 parts of linear low-density polyethylene, 0.5 parts of carbon black, and 0.08 parts of stearate are extruded by a single screw in a molten state at a temperature of 160°C, coated on a porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 0.6MPa to form a 1.17mm foamed sheet, wherein the thickness of the reinforcement layer is H r 40μm, prepare samples for performance testing.

[0179] Embodiment 8:

[0180] 50 parts of polyolefin plastomer, 50 parts of polyolefin elastomer, 7 parts of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mixer, the temperature was set at 100°C, and the mixture was mixed for 15 minutes. The mixture was extruded and rolled into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 12.1 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0181] 20 parts of radiation-modified polyolefin plastomers, 20 parts of polyolefin elastomers, 60 parts of linear low-density polyethylene, 0.5 parts of carbon black, 0.08 parts of stearate, and 0.08 parts of antioxidants are extruded by a single screw in a molten state at a temperature of 220°C, coated on a porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 1.0 MPa to form a 1.01 mm foamed sheet, wherein the thickness of the reinforcing layer is H r 20μm, prepare samples for performance testing.

[0182] Embodiment 9:

[0183] 50 parts of polyolefin plastomer, 50 parts of polyolefin elastomer, 7 parts of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mixer, the temperature was set at 100°C, and the mixture was mixed for 15 minutes. The mixture was extruded and rolled into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 19.7 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0184] 20 parts of polyolefin plastomers, 20 parts of polyolefin elastomers, 60 parts of linear low-density polyethylene, 0.5 parts of carbon black, 0.08 parts of stearate, and 0.08 parts of antioxidants are extruded by a single screw in a molten state at a temperature of 190°C, coated on a porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 0.6MPa to form a 1.2mm foamed sheet, wherein the thickness of the reinforcement layer is H r 100μm, prepare samples for performance testing.

[0185] Comparative Example 1:

[0186] 50 parts of polyolefin plastomer, 50 parts of polyolefin elastomer, 7 parts of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mixer, the temperature was set at 100°C, and the mixture was mixed for 15 minutes. The mixture was extruded and rolled into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 14.3 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0187] 20 parts of polyolefin plastomer, 20 parts of polyolefin elastomer, 60 parts of linear low-density polyethylene, 0.5 parts of carbon black, 0.08 parts of stearate, and 0.08 parts of antioxidant are extruded by a single screw in a molten state at a temperature of 190°C, coated on a porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 0.1MPa to form a 1.36mm foamed sheet, wherein the thickness of the reinforcement layer is H r 50μm, prepare samples for performance testing.

[0188] Comparative Example 2:

[0189] 100 parts of polyolefin elastomer, 7 parts of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mill, the temperature was set at 100°C, and the mixture was mixed for 15 minutes. The mixture was extruded and rolled into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 19.7 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0190] 20 parts of polyolefin plastomer, 20 parts of polyolefin elastomer, 60 parts of linear low-density polyethylene, 0.5 parts of carbon black, 0.08 parts of stearate, and 0.08 parts of antioxidant are extruded by a single screw in a molten state at a temperature of 190°C, coated on a porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 0.6MPa to form a 0.83mm foamed sheet, wherein the thickness of the reinforcing layer is H r 20μm, prepare samples for performance testing.

[0191] Comparative Example 3:

[0192] 100 parts of polyolefin plastomer, 7 parts of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mixer, the temperature was set at 100°C, and the mixture was mixed for 15 minutes. The mixture was extruded and rolled into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 14.3 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0193] 20 parts of polyolefin plastomer, 20 parts of polyolefin elastomer, 60 parts of linear low-density polyethylene, 0.5 parts of carbon black, 0.08 parts of stearate, and 0.08 parts of antioxidant are extruded by a single screw in a molten state at a temperature of 190°C, coated on a porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 0.6MPa to form a 1.15mm foamed sheet, wherein the thickness of the reinforcement layer is H r 60μm, prepare samples for performance testing.

[0194] Comparative Example 4:

[0195] 50 parts of polyolefin plastomer, 50 parts of polyolefin elastomer, 7 parts of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mixer, the temperature was set at 100°C, and the mixture was mixed for 15 minutes. The mixture was extruded and rolled into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 14.3 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0196] 20 parts of radiation-modified polyolefin plastomer, 20 parts of radiation-modified polyolefin elastomer, 60 parts of linear low-density polyethylene, 0.5 parts of carbon black, 0.08 parts of stearate, after single-screw extrusion, the molten state temperature is 230°C, coated on the porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 0.6MPa to form a 0.98mm foamed sheet, wherein the thickness of the reinforcement layer is H r 30μm, prepare samples for performance testing.

[0197] Comparative Example 5:

[0198] 50 parts of polyolefin plastomer, 50 parts of polyolefin elastomer, 15 parts of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mixer, the temperature was set at 100°C, and the mixture was mixed for 15 minutes. The mixture was extruded and rolled into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 14.3 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0199] 20 parts of radiation modified polyolefin plastomer, 20 parts of radiation modified polyolefin elastomer, 60 parts of linear low density polyethylene, 0.5 parts of carbon black, 0.08 parts of stearate, and 0.08 parts of antioxidant are extruded by a single screw in a molten state at a temperature of 150°C, coated on a porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 0.1MPa to form a 2.3mm foamed sheet, wherein the thickness of the reinforcement layer is H r 10μm, prepare samples for performance testing.

[0200] Comparative Example 6:

[0201] 50 parts of polyolefin plastomer, 50 parts of polyolefin elastomer, 1 part of AC foaming agent, 0.5 parts of carbon black and 0.5 parts of zinc oxide were added into a closed plastic mixer, the temperature was set at 100°C, and the mixture was mixed for 15 minutes. The mixture was extruded and rolled into a 0.45 mm resin sheet by a single screw extruder. The sheet was cross-linked and modified by irradiation with an ELV accelerator (2.5 Mev, 50 mA, 100 kW) at a dose of 14.3 Mrad. The modified resin sheet was foamed in a hot air environment at 280°C for 1.5 minutes to obtain a porous layer of a foamed sheet.

[0202] 20 parts of polyolefin plastomer, 20 parts of polyolefin elastomer, 60 parts of linear low-density polyethylene, 0.5 parts of carbon black, 0.08 parts of stearate, and 0.08 parts of antioxidant are extruded by a single screw in a molten state at a temperature of 250°C, coated on a porous layer, pressed by a heating roller at 85°C, then cooled by a cooling shaping roller and calendered at a hot composite pressure of 1.2MPa to form a 0.35mm foamed sheet, wherein the thickness of the reinforcement layer is H r 110μm, prepare samples for performance testing.

[0203] The structural characteristics of the composite resin foamed sheet samples obtained in Examples 1-9 and Comparative Examples 1-6 (D1-D6) are summarized in Tables 1 and 2 below:

[0204] Table 1:

[0205]

[0206] Table 2:

[0207]

[0208] The performance characteristics of the composite resin foamed sheet samples obtained in Examples 1-9 and Comparative Examples 1-6 (D1-D6) are summarized in Tables 3 and 4 below:

[0209] Table 3:

[0210]

[0211]

[0212] Table 4:

[0213]

[0214] It can be seen that in Comparative Example 1, due to insufficient lamination pressure when the two layers are laminated, the composite resin foam sheet is peeled off and damaged at the interface between the porous layer and the reinforcing layer during the cohesion test. It is also easy to fall off during high and low temperature cycles, and the effect is not good. Comparative Examples 2-6 do not meet 1.4≤D p / (Hr +H b )≤6.6 and 5℃≤T pm -T pc When the temperature is ≤25℃, there will be problems such as the reinforcement layer falling off, insufficient cushioning performance or insufficient elongation at break. However, Examples 1-9 that meet the conditions can have the above advantages and achieve the ideal target effect. Compared with the composite layer with thinner reinforcement layers in Comparative Examples 2 and 5, Examples 1-9 have better falling ball impact test results, proving that a reinforcement layer of a certain thickness has the effect of converting point impact into surface impact and fully dispersing the impact force.

[0215] The present invention can be implemented in other forms than those described above without departing from the spirit and scope of the present invention. The embodiments disclosed in the present application are examples and are not limited to these.

Claims

1. A display assembly, comprising a display panel (1), a middle frame (2) and a back cover (3), wherein the middle frame (2) is used to support the display panel (1), the back cover (3) is buckled on the middle frame (2), and a buffer sealing tape (4) is provided between the display panel (1) and the middle frame (2) and / or between the middle frame (2) and the back cover (3). It is characterized in that The buffer sealing tape (4) comprises a composite resin foam sheet as a tape substrate, wherein: The composite resin foam sheet comprises a porous layer and at least one reinforcing layer; The composite resin foam sheet does not undergo peeling failure at the interface between the porous layer and the reinforcement layer during a cohesion test; The porous layer is formed by foaming a cross-linked polyolefin resin, the cross-linking degree of which is 15-60%, and the average cell diameter D p 90-200 μm; the reinforcing layer is an uncrosslinked or slightly crosslinked polyolefin resin, the degree of crosslinking is less than 10%; and the average pore diameter D of the porous layer p , thickness of single-sided reinforcement layer H r and the cell wall thickness H of the porous layer adjacent to the single-sided reinforcement layer b The following relationship exists: 1.4≤D p / (H r +H b )≤6.6; Furthermore, the melting endothermic peak temperature T pm The peak temperature T of the heat release peak during the cooling process of the reinforcement layer pc The following relationship exists: 5℃≤T pm -T pc ≤25℃; Furthermore, the melting endothermic peak temperature Tpm during the heating process of the porous layer is 80-120°C; the exothermic peak temperature Tpc during the cooling process of the reinforcement layer is 60-115°C.

2. A composite resin foam sheet, It is characterized in that The composite resin foam sheet comprises a porous layer and at least one reinforcing layer; The composite resin foam sheet does not undergo peeling failure at the interface between the porous layer and the reinforcement layer during a cohesion test; The porous layer is formed by foaming a cross-linked polyolefin resin, the cross-linking degree of which is 15-60%, and the average cell diameter D p 90-200μm; The reinforcing layer is an uncrosslinked or slightly crosslinked polyolefin resin, and its crosslinking degree is less than 10%; The average cell diameter D of the porous layer is p The thickness of the single-sided reinforcement layer H r and the cell wall thickness H of the porous layer adjacent to the single-sided reinforcement layer b The following relationship exists: 1.4≤D p / (H r +H b )≤6.6; Furthermore, the melting endothermic peak temperature T pm The peak temperature T of the heat release peak during the cooling process of the reinforcement layer pc The following relationship exists: 5℃≤T pm -T pc ≤25℃; And, the melting endothermic peak temperature T pm The exothermic peak temperature T of the reinforcing layer during cooling is 80-120°C. pc is: 60-115℃.

3. The composite resin foam sheet according to claim 2, It is characterized in that The cohesive force of the composite resin foam sheet is 1000-4000 gf, and the cohesive force is tested by 180° peeling; Furthermore, after the composite resin foam sheet has been subjected to 100 high and low temperature cycles from -40°C to 80°C, its cohesive force is still maintained above 1000 gf, and no interface separation between the porous layer and the reinforcing layer occurs during the high and low temperature cycles.

4. The composite resin foam sheet according to claim 2, It is characterized in that The composite resin foam sheet has a thickness of 0.3 mm to 2.0 mm and an overall density of 0.060 to 0.125 g / cm 3 , the elongation at break is greater than 250%.

5. The composite resin foam sheet according to claim 2, It is characterized in that The cell density in the porous layer is 15-100 cells / mm 2 The average number of cells in the ZD direction is 2-10, and the reinforcing layer does not contain cells.

6. The composite resin foam sheet according to claim 2, It is characterized in that The infrared similarity between the porous layer and the reinforcing layer is greater than 80%, and the infrared similarity and infrared identification similarity analysis methods include peak area comparison method, spectrum fitting method or correlation coefficient method.

7. The composite resin foam sheet according to claim 2, It is characterized in that The deformation amount of the composite resin foam sheet is 30%-70% when the compressive stress is 0.1 MPa.

8. The composite resin foam sheet according to claim 2, It is characterized in that The thickness of the reinforcement layer is 20-100 μm, and the density of the porous layer is 0.05-0.125 g / cm 3 The density of the reinforcement layer is 0.910-0.920g / cm 3 .

9. The composite resin foam sheet according to claim 2, It is characterized in that The porous layer of the composite resin foam sheet is made of polyolefin resin using azodicarbonamide as a foaming agent through thermal decomposition and foaming; the reinforcing layer of the foam sheet is composed of polyolefin resin without the foaming agent and its decomposition residue.

10. The composite resin foam sheet according to claim 2, It is characterized in that The porous layer of the composite resin foam sheet comprises the following components, in parts by weight: Polyolefin plastomer 20-80 parts Polyolefin elastomer 20-80 parts 4-10 parts of foaming agent.

11. The composite resin foam sheet according to claim 2, It is characterized in that The foam sheet reinforcement layer comprises the following components, in parts by weight:

12. The composite resin foam sheet according to claim 2, It is characterized in that The composite resin foam sheet is laminated with the foaming layer after the reinforcing layer is heated to a completely molten or partially molten state, and the laminating method includes thermal lamination, melt coating, and melt rolling lamination.

13. The composite resin foam sheet according to claim 12, It is characterized in that The reinforcing layer of the foam sheet is attached to one or both sides of the porous layer.

14. A sealing cushioning tape, It is characterized in that The composite resin foam sheet according to claim 2 to 13 is used as a tape substrate, and an acrylic adhesive is coated on one or both sides of the tape substrate after corona treatment.

15. Use of the composite resin foamed sheet according to claim 2, It is characterized in that The composite resin foam sheet is used as a tape substrate in the fields of household appliances, automobiles, and electronic products that require component bonding and / or component protection.

16. An electronic product, It is characterized in that The composite resin foam sheet comprises any one of claims 2 to 13 or the sealing and buffering tape comprises claim 14.

Citation Information

Patent Citations

  • Foamed composite sheet, adhesive tape, cushioning material for electronic components, and adhesive tape for electronic components

    CN112074403A

  • Multilayer foam sheet and adhesive tape

    CN116348292A

  • Manufacturing method for foamed sheet, and foamed sheet

    JP2004181933A

  • Polyolefin based resin laminated foam sheet and method of manufacturing the same

    JP2009184181A

  • Expanded sheet and adhesive tape

    JP2019137795A