Method for producing liquid salt and co-producing anhydrous sodium sulphate by utilizing mirabilite tailings
By combining cryogenic denitrification process and quicklime-sodium bicarbonate purification method with membrane filtration and cryogenic crystallization technology, the problem of insufficient utilization of mirabilite tailings resources has been solved, and the co-production of liquid salt and sodium sulfate has been achieved, improving resource utilization and product quality.
Patent Information
- Application Number
- CN202410735125.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-11-29
AI Technical Summary
The current technology does not adequately develop and utilize mirabilite tailings resources, resulting in the waste of sodium chloride and sodium sulfate resources in the brine, and the recycling of mother liquor leads to a decline in product quality.
By employing a cryogenic denitrification process combined with a quicklime-sodium bicarbonate purification method, and through membrane filtration and cryogenic crystallization technology, liquid salt co-produced with sodium sulfate is generated. This utilizes the sodium chloride and sodium sulfate resources in the low-nitrate brine, avoiding the infinite recycling of the mother liquor.
It improved resource utilization, reduced production costs, achieved efficient production of liquid salt, avoided product quality decline, and increased the added value of frozen low-nitrate brine.
Smart Images

Figure FT_1
Abstract
Description
Technical Field
[0001] The invention relates to a method for producing liquid salt and alum from mirabilite tailings, belonging to the technical field of comprehensive resource utilization. Background Art
[0002] Glauber's salt ore is formed by the intergeneration of anhydrous Glauber's salt and rock salt. Glauber's salt ore layers often contain thin layers of rock salt or the roof and floor are rock salt layers. In addition, after the ore layer is mined, the roof collapses and the rock salt layer above the roof is dissolved, resulting in a gradual increase in the salt content in the Glauber's salt brine after the mine has been mined for a period of time. In recent years, with the exploitation of resources, there are more and more tailings resources, the sodium sulfate content in the tailings is getting lower and lower, while the salt content is getting higher and higher, and the separation cost is getting higher and higher. The main components of the tailings are: Na2SO4 content: 50 g / L~180 g / L; NaCl content: 260 g / L~320 g / L. At present, there is a patent that uses tailings brine as raw material and uses the freezing method to produce decahydrated nitrate, which is sent to the existing nitrate salt evaporation system to produce alum. However, the mother liquor after the nitrate reduction is recycled into the system, and the infinite circulation in the system causes the product quality to become low. At present, no matter which mother liquor treatment method is used, the sodium chloride resources in the mother liquor cannot be effectively utilized, resulting in a waste of resources.
[0003] Liquid salt refers to a solution with a certain level of sodium chloride, which is the basic raw material for producing alkali and other products. Compared with solid salt, liquid salt has many advantages, such as convenient transportation, simplified production process, low cost, energy saving, and investment saving. In China, liquid salt is currently mainly produced from well salt. This is because well salt contains very little calcium and magnesium ions, and the saturated sodium chloride solution produced after dissolving in water has few impurities, and the purity of liquid salt is very high.
[0004] CN113526530A discloses a system and method for preparing large-particle sodium sulfate as a by-product of nitrate-containing brine. The brine is separated into a sodium sulfate concentrate and a filtered clear solution by a membrane concentration unit, and then the sodium sulfate concentrate is sent to a continuous flow salting-out unit. The sodium sulfate suspension brine material obtained by the salting-out unit is graded, and large-particle sodium sulfate is removed from the system, and fine sodium sulfate particles are returned to the salting-out unit. The removed large-particle sodium sulfate is then centrifuged and dried to obtain the by-product large-particle sodium sulfate. At the same time, the fine particles of sodium sulfate crystals carried by the airflow during the drying process are collected and used in the salting-out unit.
[0005] CN109534362A discloses a lime-sodium bicarbonate brine purification process, wherein the high-nitrate raw material brine rich in sodium bicarbonate is: NaCl: 50-280 g / l, NaSO4: 50-260 g / l, NaHCO3: 1-5 g / l, Ca 2+ :30~60ppm,Mg 2+:15~30ppm. To purify this brine, dry slaked lime (Ca(OH)2) particles with a particle size range of less than 100 mesh are used to carry out a series of purification reactions with sodium bicarbonate (NaHCO3) inherent in the brine to produce Ca 2+ and Mg 2+ Total nitrate brine ≤ 40ppm. Summary of the invention
[0006] The purpose of the present invention is to provide a method for producing liquid salt and alum by freezing and denitrification in view of the insufficient development and utilization of the current mirabilite tailings resources, which combines the production of liquid salt with the co-production of alum, has a simple production process, reduces investment and production costs, improves resource utilization, increases the added value of low-nitrate brine after freezing, and maximizes benefits.
[0007] A method for producing liquid salt and co-producing sodium sulfate by using mirabilite tailings, the method comprising the following steps: (1) Low-grade brine, i.e., low-nitrate brine, is extracted from the mirabilite tailings, and the low-nitrate brine is purified to precipitate calcium and magnesium in the brine, so that the total amount of calcium and magnesium ions in the brine after purification is ≤6 mg / L, the upper clear liquid, i.e., the purified brine, is refined low-nitrate brine, and the lower mud is calcium and magnesium mud; (2) The refined low-nitrate brine in step (1) is filtered through a membrane to remove suspended solids to obtain refined brine; (3) A portion of the refined brine in step (2) enters the nitrate-salt co-production system, where nitrate is first separated and dried in the nitrate evaporation system to obtain a glauber salt product. The remaining mother liquor from the production of glauber salt enters the salt evaporation system to produce solid salt; (4) Another part of the refined brine in step (2) enters the freezing crystallization system, cools down and crystallizes to precipitate sodium sulfate decahydrate, and the sodium sulfate decahydrate enters the nitrate evaporation system in step (3) as a supplementary nitrate source, and evaporates together with the refined brine to obtain a glauber salt product; (5) The supernatant in the crystallization process in step (4) is filtered to remove the sodium sulfate contained therein to obtain a liquid salt product.
[0008] Furthermore, the calcium magnesium mud obtained in step (1) is used for power generation and desulfurization.
[0009] Furthermore, in the purification of step (1), an appropriate amount of a sedimentation aid is optionally added. The sedimentation aid includes, for example, polyacrylamide, which is a polymer water treatment flocculant product that can be used to adsorb suspended particles in water, play a linking and bridging role between particles, make fine particles form relatively large flocs, and accelerate the precipitation rate. The amount is not particularly limited, as long as it is an amount that can fully flocculate the suspended particles in the water.
[0010] Furthermore, the composition of the low nitrate brine in step (1) is as follows: Na2SO4 content: 50 g / L~180 g / L; NaCl content: 260 g / L~320 g / L; CaSO4 content: 0.2 g / L~0.5 g / L; MgSO4 content: 0.12 g / L~0.32 g / L. For example, the Na2SO4 content in low nitrate brine can be 60 g / L~170 g / L, 70 g / L~160 g / L, 80 g / L~150 g / L, or 90 g / L~140 g / L; the NaCl content can be 265 g / L~315 g / L, 270 g / L~310 g / L, 272 g / L~300 g / L, 280 g / L~295 g / L, or 285 g / L~290 g / L; the CaSO4 content can be 0.25 g / L~0.45 g / L, 0.28 g / L~0.42 g / L, or 0.30 g / L~0.40 g / L; the MgSO4 content can be 0.15 g / L~0.30 g / L, 0.18 g / L~0.28 g / L or 0.20g / L~0.25g / L.
[0011] Furthermore, in step (1), a slaked lime-sodium bicarbonate purification method is used to remove calcium and magnesium ions, and 0.1-0.3% (preferably about 0.2%) of slaked lime and 0.1-0.3% (preferably about 0.2%) of sodium bicarbonate relative to the mass of the low nitrate brine are added to the low nitrate brine. After stirring for reaction, the mixture is allowed to settle for 1-3 hours (preferably 1.5-2.5 hours), and excess caustic soda (for example, 0.25-0.4% (preferably about 0.3%) relative to the mass of the low nitrate brine) is added to obtain purified brine.
[0012] Furthermore, the type of membrane in the membrane filtration system in step (2) is any one of a ceramic membrane, a Gore membrane, and an organic membrane, and the pore size of the membrane is 20-60 nm, preferably 30-50 nm, and more preferably 35-45 nm.
[0013] Furthermore, in the refined brine in step (2), the content of Na2SO4 is 50 g / L~180 g / L; the content of NaCl is 260 g / L~320 g / L, preferably, the content of Na2SO4 is 60 g / L~170 g / L; the content of NaCl is 265 g / L~315 g / L, more preferably, the content of Na2SO4 is 80 g / L~150 g / L; the content of NaCl is 270 g / L~310 g / L.
[0014] Furthermore, the volume ratio of the refined brine entering the nitrate co-production system in step (3) and the refined brine entering the freezing crystallization system in step (4) is 1:3-7, preferably 1:4-6, more preferably 1:4.5-5.5, such as 1:5. A portion of the refined brine is sent to the nitrate co-production system to produce solid salt and sodium sulfate, and the remaining portion enters the freezing crystallization system to produce liquid salt and sodium sulfate. When the volume ratio of the two is in the range of 1:4-6, the yield of sodium sulfate and liquid salt is higher.
[0015] Furthermore, in step (3), the nitration is carried out at 120-150°C, preferably 125-145°C, preferably 130-140°C.
[0016] Furthermore, in step (4), the evaporation is performed at 120-150°C, preferably at 130-140°C.
[0017] Further, in step (4), the cooling crystallization includes: the temperature of the refined brine after purification, sedimentation and filtration is generally 35-45°C, and it first enters a closed cooling tower at 35-45°C for pre-cooling to 25-30°C, preferably 25-29°C, and more preferably 25-28°C, and then enters a feed barrel, and after being pressurized by a pump, it passes through a precooler, and is pumped to a cooler with the deep-cooled nitre mother liquor coming out of the freezing crystallization tank, and performs a two-stage cold exchange, wherein the temperature of the nitre mother liquor is -6~-7°C. The precooling outlet temperature of the brine is controlled at 16~25°C, preferably 16-23°C, and enters a single-stage freezing crystallization tank for freezing, and the temperature in the freezing crystallization tank is -8~-14°C, further -10-~13°C, preferably about -13°C, and the brine is cooled at -6~-7°C in the freezing crystallization tank to precipitate sodium sulfate decahydrate, and the remaining nitre mother liquor is sent to the precooler as a refrigerant.
[0018] Furthermore, the upper clear liquid in the freezing crystallization tank enters the buffer mother liquid tank, the mother liquid in the tank is pumped into a vacuum belt filter to filter the sodium sulfate decahydrate mixed in the solution, the clear filtrate falls into the clear mother liquid barrel, the clear liquid goes to the precooler as a refrigerant for heat exchange and then goes to the liquid salt storage tank for storage to obtain a liquid salt product.
[0019] Furthermore, the liquid salt obtained in step (5) is 300 g / L to 350 g / L, preferably 310 g / L to 340 g / L, and more preferably 320 g / L to 330 g / L NaCl.
[0020] Furthermore, the crystallization tank discharges nitrate through the lower nitrate leg, and centrifuges to obtain sodium sulfate decahydrate. The sodium sulfate decahydrate is slurried by refined brine and enters the nitrate evaporation system of step (3) as a supplementary nitrate source to evaporate at 120-150°C to obtain the glauber powder product.
[0021] In the present application, "optionally" means with or without.
[0022] The beneficial effects of the present invention are: The invention provides a method for producing liquid salt and alum by freezing and denitrifying mirabilite tailings, which can fully develop and utilize the sodium chloride and sodium sulfate resources in low-nitrate brine and improve the resource utilization rate.
[0023] A method for producing liquid salt and alum by freezing and denitrifying mirabilite tailings is provided. Sodium sulfate in low-nitrate brine is developed through the freezing and denitrifying process and added to the nitrate evaporation system, thereby increasing the sodium sulfate content in the system and reducing energy consumption.
[0024] Provided is a method for producing liquid salt and sodium sulfate by freezing and denitrifying mirabilite tailings. Liquid salt and sodium sulfate products are produced through slaked lime-sodium bicarbonate purification, refrigeration, freezing crystallization, centrifugal separation, drying and other processes, thereby avoiding the problem of low-nitrate brine circulating endlessly in the system and causing product quality degradation.
[0025] Liquid salt products do not require a salting process: because the raw brine has a high sodium chloride content (260 g / L~320 g / L), the brine after freezing takes away water due to the crystallization water of decahydrate, directly increasing the salt content in the brine to 300 g / L~350 g / L, directly eliminating the need for a salting system. However, the liquid salt production of traditional chlor-alkali enterprises requires a salting system for salting because the concentration requirement for nanofiltration membranes is relatively low (the salt content of light brine is usually 280g / L~290g / L). Therefore, in comparison, the present invention can effectively reduce the consumption of refined salt, save investment, and expand benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 The present invention is a process flow chart for producing liquid salt and alum from mirabilite tailings. DETAILED DESCRIPTION
[0027] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. In this application, unless otherwise specified, % generally refers to mass percentage.
[0028] like Figure 1 As shown, a sedimentation aid (main component: polyacrylamide) is optionally added to the low-nitrate brine for slaked lime-sodium bicarbonate purification, and the lower mud is calcium-magnesium mud for desulfurization. The upper clear liquid is sent to the refined nitrate water barrel and filtered with a ceramic membrane to obtain refined brine. A part of the refined brine enters the nitrate-salt co-production system, first entering the nitrate evaporation system for nitrate separation to obtain the sodium sulfate product. The remaining mother liquor from the production of sodium sulfate enters the salt evaporation system to produce solid salt.
[0029] The other part of the refined brine is cooled and then sent to the crystallization tank for crystallization. The precipitate (sodium sulfate decahydrate) precipitated out of the frozen crystallization tank is discharged through the lower nitrate leg and centrifuged to obtain sodium sulfate decahydrate. The sodium sulfate decahydrate is slurried through the refined brine and enters the nitrate evaporation system together with the refined brine as a supplementary nitrate source to be evaporated to obtain the alum product.
[0030] The upper clear liquid of the crystallization tank enters the buffer mother liquid tank, and the mother liquid in the tank is pumped into the vacuum belt filter to filter the sodium sulfate decahydrate mixed in the solution. The clear filtrate falls into the clear mother liquid barrel. The clear liquid goes to the precooler as a refrigerant for heat exchange and then goes to the liquid salt storage barrel for storage to obtain the liquid salt product. Example 1
[0031] like Figure 1 As shown, a method for producing liquid salt and sodium sulfate by freezing and denitrifying mirabilite tailings: (1) Low-grade brine is extracted from the mirabilite tailings and put into a reaction barrel. The composition of the low-nitrate brine is as follows: Na2SO4 content: 60 g / L; NaCl content: 280 g / L; CaSO4 content: 0.2 g / L; MgSO4 content: 0.12 g / L. 0.2% slaked lime and 0.2% sodium bicarbonate relative to the brine are added to the low-nitrate brine. After stirring and reacting, the mixture is allowed to settle for 1-2 hours. 0.3% caustic soda relative to the low-nitrate brine is added to increase the alkalinity in the reaction barrel. The total amount of calcium and magnesium ions in the purified brine is ≤6 mg / L. The slaked lime-sodium bicarbonate purification method is used. NaHCO3 in the brine reacts with Ca(OH)2 to generate Na2CO3. Na2CO3 is then reacted with calcium sulfate in the brine to generate calcium carbonate precipitate to remove calcium ions. Calcium hydroxide reacts with magnesium sulfate to generate magnesium hydroxide precipitate to remove magnesium ions.
[0032] (2) The upper clear liquid in the reaction barrel is refined low-nitrate brine, which is pumped into the refined nitrate water barrel. The lower mud is calcium-magnesium mud, which can be used for power generation and desulfurization.
[0033] (3) The refined low-nitrate brine in the refined nitrate water barrel is filtered through a ceramic membrane with a pore size of 50 nm to remove suspended solids to obtain refined brine. The refined brine has a Na2SO4 content of 60 g / L and a NaCl content of 280 g / L.
[0034] (4) In order to maximize production efficiency, a portion of the refined brine (accounting for 15%) enters the nitrate-salt co-production system. The refined brine first enters the nitrate evaporation system, where it is separated out at 120-150°C and dried to obtain the alum product. The remaining mother liquor from the production of alum enters the salt evaporation system to produce solid salt.
[0035] (5) Another part of the refined brine (accounting for 85%) enters the refrigeration system. After purification, sedimentation and filtration, the initial temperature of the refined brine is 35~45℃. It first enters the closed cooling tower at 35~45℃ to be pre-cooled to 25℃, and then enters the feed barrel. After being pressurized by a pump, it passes through the precooler and is pumped to the cooler with the deep-cooled nitrate mother liquor coming out of the freezing crystallization tank for two-stage cold exchange. The temperature of the nitrate mother liquor is -6~-7℃. The pre-cooling temperature of the brine is controlled at 16℃ and enters the single-stage freezing crystallization tank for freezing. The temperature in the freezing crystallization tank is -13℃. The brine is cooled at -6~-7℃ in the freezing crystallization tank to precipitate sodium sulfate decahydrate.
[0036] (6) The supernatant liquid from the crystallization tank enters the buffer mother liquid tank. The mother liquid in the tank is pumped into a vacuum belt filter to filter out the sodium sulfate decahydrate mixed in the solution. The clear filtrate falls into the clear mother liquid barrel. The clear liquid goes to the precooler as a refrigerant for heat exchange and then goes to the liquid salt storage tank for storage to obtain a liquid salt product. The sodium chloride content of the liquid salt is 301 g / L, and the content of other impurities is 4.7 g / L.
[0037] (7) The precipitate (sodium sulfate decahydrate) precipitated from the freezing crystallization tank in step (5) is discharged through the lower nitrate leg and centrifuged to obtain sodium sulfate decahydrate. The sodium sulfate decahydrate is slurried through refined brine and enters the nitrate evaporation system together with the refined brine in step (4) as a supplementary nitrate source, and evaporated at 140°C to obtain a glauber salt product. The purity of the glauber salt product is 95%. Example 2
[0038] like Figure 1 As shown, a method for producing liquid salt and sodium sulfate by freezing and denitrifying mirabilite tailings: (1) Low-grade brine is extracted from the mirabilite tailings and put into a reaction barrel. The composition of the low-nitrate brine is as follows: Na2SO4 content: 80 g / L; NaCl content: 280 g / L; CaSO4 content: 0.2 g / L; MgSO4 content: 0.12 g / L. 0.2% slaked lime and 0.2% sodium bicarbonate based on the brine are added to the low-nitrate brine. After stirring and reacting, the mixture is allowed to settle for 1-2 hours. 0.3% caustic soda based on the low-nitrate brine is added to increase the alkalinity in the reaction barrel. The total amount of calcium and magnesium ions in the purified brine is ≤5 mg / L.
[0039] (2) The upper clear liquid in the reaction barrel is refined low-nitrate brine, which is pumped into the refined nitrate water barrel. The lower mud is calcium-magnesium mud, which can be used for power generation and desulfurization.
[0040] (3) The refined low-nitrate brine in the refined nitrate water barrel is filtered through a ceramic membrane with a pore size of 45 nm to remove suspended solids to obtain refined brine. The refined brine has a Na2SO4 content of 80 g / L and a NaCl content of 280 g / L.
[0041] (4) In order to maximize production efficiency, a portion of the refined brine (accounting for 17%) enters the nitrate-salt co-production system and then the nitrate evaporation system, where it is separated at 120-150°C and dried to obtain the sodium sulfate product. The remaining mother liquor from the production of sodium sulfate enters the salt evaporation system to produce solid salt.
[0042] (5) Another part of the refined brine (accounting for 83%) enters the refrigeration system. After purification, sedimentation and filtration, the initial temperature of the refined brine is 35~45℃. It first enters the closed cooling tower at 35~45℃ to be pre-cooled to 25℃, and then enters the feed barrel. After being pressurized by a pump, it passes through the precooler and is pumped to the cooler with the deep-cooled nitrate mother liquor from the freezing crystallization tank for two-stage cold exchange. The temperature of the nitrate mother liquor is -6~-7℃. The pre-cooling temperature of the brine is controlled at 16℃ and enters the single-stage freezing crystallization tank for freezing. The temperature in the freezing crystallization tank is -13℃. The brine is cooled at -6~-7℃ in the freezing crystallization tank to precipitate sodium sulfate decahydrate.
[0043] (6) The supernatant liquid from the crystallization tank enters the buffer mother liquid tank. The mother liquid in the tank is pumped into a vacuum belt filter to filter out the sodium sulfate decahydrate mixed in the solution. The clear filtrate falls into the clear mother liquid barrel. The clear liquid goes to the precooler as a refrigerant for heat exchange and then goes to the liquid salt storage tank for storage to obtain a liquid salt product. The sodium chloride content of the liquid salt is 304 g / L, and the content of other impurities is 4.2 g / L.
[0044] (7) The precipitate (sodium sulfate decahydrate) precipitated from the freezing crystallization tank in step (5) is discharged through the lower nitrate leg and centrifuged to obtain sodium sulfate decahydrate. The sodium sulfate decahydrate is slurried through refined brine and enters the nitrate evaporation system together with the refined brine in step (4) as a supplementary nitrate source, and evaporated at 140°C to obtain a glauber salt product with a purity of 96%. Example 3
[0045] like Figure 1 As shown, a method for producing liquid salt and sodium sulfate by freezing and denitrifying mirabilite tailings: (1) Low-grade brine was extracted from the mirabilite tailings. The composition of the low-grade brine was as follows: Na2SO4 content: 100 g / L; NaCl content: 280 g / L; CaSO4 content: 0.2 g / L; MgSO4 content: 0.12 g / L. 0.2% slaked lime and 0.2% sodium bicarbonate were added to the low-grade brine relative to the low-grade brine. After stirring and reacting, the mixture was allowed to settle for 1.5 hours. 0.3% caustic soda was added to increase the alkalinity in the reaction barrel. The total amount of calcium and magnesium ions in the purified brine was ≤5 mg / L.
[0046] (2) The upper clear liquid in the reaction barrel is refined low-nitrate brine, which is pumped into the refined nitrate water barrel. The lower mud is calcium-magnesium mud, which can be used for power generation and desulfurization.
[0047] (3) The refined low-nitrate brine in the refined nitrate water barrel is filtered through a ceramic membrane with a pore size of 40 nm to remove suspended solids to obtain refined brine. The content of Na2SO4 in the refined brine is 100 g / L and the content of NaCl is 280 g / L.
[0048] (4) In order to maximize production efficiency, a portion of the refined brine (accounting for 20%) enters the nitrate-salt co-production system and then the nitrate evaporation system, where it is separated at 120-150°C and dried to obtain the sodium sulfate product. The remaining mother liquor from the production of sodium sulfate enters the salt evaporation system to produce solid salt.
[0049] (5) Another part of the refined brine (accounting for 80%) enters the refrigeration system. After purification, sedimentation and filtration, the initial temperature of the refined brine is 35~45℃. It first enters the closed cooling tower at 35~45℃ to be pre-cooled to 25℃, and then enters the feed barrel. After being pressurized by a pump, it passes through the precooler and is pumped to the cooler with the deep-cooled nitrate mother liquor from the freezing crystallization tank for two-stage cold exchange. The temperature of the nitrate mother liquor is -6~-7℃. The pre-cooling temperature of the brine is controlled at 16℃ and enters the single-stage freezing crystallization tank for freezing. The temperature in the freezing crystallization tank is -13℃. The brine is cooled at -6~-7℃ in the freezing crystallization tank to precipitate sodium sulfate decahydrate.
[0050] (6) The supernatant liquid from the crystallization tank enters the buffer mother liquid tank. The mother liquid in the tank is pumped into a vacuum belt filter to filter out the sodium sulfate decahydrate mixed in the solution. The clear filtrate falls into the clear mother liquid barrel. The clear liquid goes to the precooler as a refrigerant for heat exchange and then goes to the liquid salt storage tank for storage to obtain a liquid salt product. The sodium chloride content of the liquid salt is 303 g / L, and the content of other impurities is 3.4 g / L.
[0051] (7) The precipitate (sodium sulfate decahydrate) precipitated from the freezing crystallization tank in step (5) is discharged through the lower nitrate leg and centrifuged to obtain sodium sulfate decahydrate. The sodium sulfate decahydrate is slurried through refined brine and enters the nitrate evaporation system together with the refined brine in step (4) as a supplementary nitrate source, and evaporated at 140°C to obtain a glauber salt product with a purity of 96%. Comparative Example 1
[0052] (1) Low-grade brine was extracted from the mirabilite tailings. The composition of the low-grade brine was as follows: Na2SO4 content: 100 g / L; NaCl content: 280 g / L; CaSO4 content: 0.2 g / L; MgSO4 content: 0.12 g / L. 0.2% slaked lime and 0.2% sodium bicarbonate were added to the low-grade brine relative to the low-grade brine. After stirring and reacting, the mixture was allowed to settle for 1.5 hours. 0.3% caustic soda was added to increase the alkalinity in the reaction barrel. The total amount of calcium and magnesium ions in the purified brine was ≤5 mg / L.
[0053] (2) The upper clear liquid is refined low-nitrate brine, which is pumped into the refined nitrate water barrel. The lower mud is calcium-magnesium mud, which can be used for power generation and desulfurization.
[0054] (3) The refined low-nitrate brine in the refined nitrate water barrel is filtered through a ceramic membrane with a pore size of 40 nm to remove suspended solids to obtain refined brine. The content of Na2SO4 in the refined brine is 100 g / L and the content of NaCl is 280 g / L.
[0055] (4) The refined brine enters the freezing system and is frozen to below -7°C in a single-stage freezing crystallizer. The brine is cooled in a cooling crystallizer to precipitate sodium sulfate decahydrate.
[0056] (5) The supernatant liquid from the crystallization tank enters the buffer mother liquor tank. The mother liquor in the tank is pumped into a vacuum belt filter to filter out the sodium sulfate decahydrate mixed in the solution. The clear filtrate falls into the clear mother liquor barrel and is then pumped to the refined brine barrel in step (3). Together with the newly prepared refined brine, it enters the refrigeration system for cooling and precipitation of nitrate.
[0057] (6) The crystallization tank discharges nitrate through the lower nitrate leg, and centrifuges to obtain sodium sulfate decahydrate. The sodium sulfate decahydrate is slurried through refined brine and enters the nitrate evaporation system as a supplementary nitrate source. It is evaporated at 140°C to obtain the sodium sulfate product with a purity of 80%.
[0058] Finally, it should be noted that the above content is only for illustrative purposes and not for limiting the scope of protection of the present invention. A person skilled in the art may modify or substitute equivalents for the technical solution of the present invention without departing from the essence of the present invention, and the modifications or equivalent substitutions shall be included in the scope of protection of the claims of the present invention.
Claims
1. A method for producing liquid salt and sodium sulfate by using mirabilite tailings, characterized in that: The method comprises the following steps: (1) Low-grade brine is extracted from the mirabilite tailings, and the low-nitrate brine is purified to precipitate calcium and magnesium in the brine, so that the total amount of calcium and magnesium ions in the brine after purification is ≤6 mg / L. The upper clear liquid, i.e. the purified brine, is refined low-nitrate brine, and the lower mud is calcium and magnesium mud; (2) The refined low-nitrate brine in step (1) is filtered through a membrane to remove suspended solids to obtain refined brine; (3) A portion of the refined brine in step (2) enters the nitrate-salt co-production system, where nitrate is first separated and dried in the nitrate evaporation system to obtain a glauber salt product. The remaining mother liquor from the production of glauber salt enters the salt evaporation system to produce solid salt; (4) Another part of the refined brine in step (2) enters the freezing crystallization system, cools down and crystallizes to precipitate sodium sulfate decahydrate, and the sodium sulfate decahydrate enters the nitrate evaporation system in step (3) as a supplementary nitrate source, and evaporates together with the refined brine to obtain a glauber salt product; (5) The supernatant in the crystallization process in step (4) is filtered to remove the sodium sulfate contained therein to obtain a liquid salt product.
2. The method for producing liquid salt and co-producing sodium sulfate by utilizing mirabilite tailings according to claim 1, characterized in that: The composition of the low nitrate brine in step (1) is as follows: Na2SO4 content: 50 g / L~180 g / L; NaCl content: 260 g / L~320 g / L; CaSO4 content: 0.2 g / L~0.5 g / L; MgSO4 content: 0.12 g / L~0.32 g / L.
3. The method for producing liquid salt and co-producing sodium sulfate by utilizing mirabilite tailings according to claim 1 or 2, characterized in that: In step (1), slaked lime-sodium bicarbonate purification method is used to remove calcium and magnesium ions. Slaked lime and sodium bicarbonate are added to low nitrate brine, stirred for reaction, and then allowed to settle for 1-3 hours, preferably 1.5-2.5 hours, and excess caustic soda is added to obtain purified brine.
4. The method for producing liquid salt and co-producing sodium sulfate using mirabilite tailings according to any one of claims 1 to 3, characterized in that: The type of membrane in the membrane filtration system in step (2) is any one of a ceramic membrane, a Gore membrane, and an organic membrane, and the pore size of the membrane is 20-60 nm, preferably 30-50 nm, and more preferably 35-45 nm.
5. The method for producing liquid salt and co-producing sodium sulfate using mirabilite tailings according to any one of claims 1 to 4, characterized in that: In the refined brine in step (2), the content of Na2SO4 is 50 g / L~180 g / L; the content of NaCl is 260 g / L~320 g / L, preferably, the content of Na2SO4 is 60 g / L~170 g / L; the content of NaCl is 265 g / L~315, more preferably, the content of Na2SO4 is 80 g / L~150 g / L; the content of NaCl is 270 g / L~310.
6. The method for producing liquid salt and co-producing sodium sulfate using mirabilite tailings according to any one of claims 1 to 5, characterized in that: The volume ratio of the refined brine entering the nitrate co-production system and the refined brine entering the freezing crystallization system is 1:4~6.
7. The method for producing liquid salt and alum from mirabilite tailings according to any one of claims 1 to 6, characterized in that: In step (4), the refined brine first enters a closed cooling tower at 35-45°C for pre-cooling to 25-30°C, preferably 25-29°C, more preferably 25-28°C, and then enters a feed barrel, is pressurized by a pump, passes through a pre-cooler, and undergoes a two-stage cold exchange with the deep-frozen nitrate mother liquor from a freezing crystallizer. The pre-cooling outlet temperature of the brine is controlled at 16-25°C, preferably 16-23°C, and then enters a single-stage freezing crystallizer for freezing. The refined brine is cooled in the freezing crystallizer to precipitate sodium sulfate decahydrate.
8. The method for producing liquid salt and co-producing sodium sulfate using mirabilite tailings according to any one of claims 1 to 7, characterized in that: In step (5), the upper clear liquid of the frozen crystallization enters the buffer mother liquid tank, the mother liquid in the tank is pumped into a vacuum belt filter to filter the sodium sulfate decahydrate mixed in the solution, and the clear filtrate falls into the clear mother liquid barrel. The clear liquid goes to the precooler as a refrigerant for heat exchange and then goes to the liquid salt storage tank for storage to obtain a liquid salt product.
9. The method for producing liquid salt and co-producing sodium sulfate using mirabilite tailings according to any one of claims 1 to 8, characterized in that: The concentration of the liquid salt obtained in step (5) is 300 g / L to 350 g / L, preferably 310 g / L to 340 g / L, and more preferably 320 g / L to 330 g / L.
10. The method for producing liquid salt and alum from mirabilite tailings according to any one of claims 1 to 9, characterized in that: The nitration is carried out at 120-150°C, preferably 125-145°C, preferably 130-140°C.