Nano magnesium hydroxide prepared from magnesite tailings as well as preparation method and application of nano magnesium hydroxide
Through the calcination, hydration and hydrothermal treatment of magnesite tailings, high-purity nanomagnesium hydroxide was prepared, which solved the problem that magnesium hydroxide could not reach the nano level and poor purity in the prior art, and realized magnesium hydroxide High added value utilization of mineral tailings and improved performance of flame-retardant PE materials.
Patent Information
- Application Number
- CN202411152761.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-29
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art cannot effectively utilize magnesite tailings, resulting in the preparation of magnesium hydroxide that cannot reach the nano-level, and its purity and yield are poor, making it impossible to achieve high added value utilization.
After calcining the magnesite tailings at a constant temperature of 700-1100°C, the calcined product is obtained, and hydrogen peroxide, sulfuric acid and ammonia water are added to convert them into MgSO4. Then, nanomagnesium hydroxide is prepared by hydrothermal reaction, and dispersant is used to improve the Dispersibility.
Successfully prepared high-purity nanomagnesium hydroxide with particle sizes of 80-120nm, which increased the added value of magnesite, and when used in flame retardant PE materials, it improved flame retardant and mechanical properties, and the electrical properties did not change much .
Smart Images

Figure CN119038581A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of functional material preparation, and in particular to nano magnesium hydroxide prepared from magnesite tailings, and a preparation method and application thereof. Background Art
[0002] Magnesite is a high-quality mineral source for the preparation of magnesium-containing compounds, but how to comprehensively utilize coal mine tailings is an urgent problem to be solved.
[0003] Nano magnesium hydroxide has attracted much attention with its excellent performance and has been increasingly used in various fields. Especially in terms of flame retardancy, in recent years, magnesium hydroxide as a flame retardant can not only improve the flame retardant effect of materials, but also, compared with halogen flame retardants, magnesium hydroxide does not generate toxic gases such as smoke and hydrogen halides, and has received extensive attention at home and abroad. How to use magnesite with high added value to prepare nano magnesium hydroxide is very meaningful. However, the magnesium hydroxide prepared from magnesite tailings as raw materials in the prior art cannot reach the nano level and the purity and yield of magnesium hydroxide in the product are not good. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides nano magnesium hydroxide prepared from magnesite tailings and a preparation method and application thereof, which effectively solves the technical problems that the prior art cannot comprehensively utilize the magnesite tailings, thereby improving the added value of magnesite, and the purity and yield of the magnesium hydroxide prepared from magnesite as a raw material are not good. At the same time, a nano magnesium hydroxide with a simple preparation process and good dispersibility is provided. The flame retardancy of the flame-retardant PE material prepared by using the nano magnesium hydroxide is improved, and the electrical properties do not change much. At this time, the tensile strength is 10.58MPa, the elongation at break is 334%, the dielectric constant is 2.7-2.7, and the volume resistivity is 4.5×10 13 Ω·m, oxygen index 24%.
[0005] The present invention provides a method for preparing nano magnesium hydroxide from magnesite tailings, comprising the following steps:
[0006] The magnesite tailings are calcined at a constant temperature of 700-1100°C to obtain a calcined product;
[0007] The water is heated to reflux at a constant temperature of 25 to 45° C., and the calcined product is added under stirring to undergo a hydration reaction to obtain a suspension containing MgO, Fe2O3, Al2O3, CaO and SiO2, and the suspension is aged to obtain a hydrated product; hydrogen peroxide is added to the hydrated product, and then sulfuric acid and ammonia water are added to the hydrated product, and Fe2O3, Al2O3 and CaO in the hydrated product are converted into precipitates to be filtered out, and MgO is converted into MgSO4 to be separated from SiO2;
[0008] Add OH to the MgSO4- A solution is prepared by adding a dispersant and hydrothermally reacting the magnesium sulfate at 130-160° C. to prepare nano-magnesium hydroxide.
[0009] As a preferred implementation manner, the mass concentration of the hydrogen peroxide is 3%, and the mass ratio of the hydrogen peroxide to the hydration product is 0.3-0.5:1.
[0010] As a preferred embodiment, the mass concentration of the ammonia water is 25%, and the mass ratio of the ammonia water to the hydration product is 4-8:1; the concentration of the sulfuric acid is 65%, and the mass ratio of the sulfuric acid to the hydration product is 3-5:1.
[0011] As a preferred embodiment, the OH-containing - The solution is a NaOH solution, and the mass ratio of MgSO4 to NaOH is 1:6-12.
[0012] As a preferred embodiment, the mass ratio of water to calcined product is 6 to 10:1.
[0013] As a preferred embodiment, the hydration reaction time is 1 to 3 hours, the hydrothermal reaction time is 14 to 76 hours, and the constant temperature calcination time is 100 to 200 minutes.
[0014] As a preferred embodiment, the dispersant is a mixture of APG and SDS in a mass ratio of 1:1, and the amount of the dispersant is 4% to 10% of the mass of the nano-magnesium hydroxide.
[0015] The second object of the present invention is to provide a nano-magnesium hydroxide obtained by the method described above, wherein the particle size of the nano-magnesium hydroxide is 80 to 120 nm.
[0016] The third object of the present invention is to provide an application of the above-mentioned nano magnesium hydroxide in the preparation of a flame-retardant polyethylene composite material, characterized in that the application is: the nano magnesium hydroxide is modified by a silane coupling agent to obtain a modified nano magnesium hydroxide; polyethylene and the modified nano magnesium hydroxide are smelted at 70-100° C. for 10-20 min, triangularly packaged 9 times, and tableted at 160-190° C. to obtain a flame-retardant PE composite material.
[0017] As a preferred embodiment, the mass ratio of the modified magnesium hydroxide to polyethylene is 2 to 5:10; the silane coupling agent is γ-aminopropyltriethoxysilane, and the amount of the silane coupling agent is 1.5% to 3% based on the mass of polyethylene.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The invention provides a nano magnesium hydroxide prepared from magnesite tailings and a preparation method and application thereof. The magnesite tailings are calcined at a constant temperature of 700-1100°C to obtain a calcined product; water is heated to reflux at a constant temperature, and the calcined product is added under stirring conditions to undergo a hydration reaction to obtain a suspension, which is aged to obtain a hydrated product; hydrogen peroxide is added to the hydrated product, and then sulfuric acid and ammonia water are added, and Fe2O3, Al2O3, and CaO in the hydrated product are converted into precipitates to be filtered out, and MgO is converted into MgSO4 to be separated from SiO2 in the magnesite tailings; OH-containing precipitate is added to the MgSO4, and the precipitate is filtered out. - The present invention solves the technical problems that the prior art cannot comprehensively utilize magnesium ore tailings to increase the added value of magnesite, and the prepared magnesium hydroxide cannot reach the nanometer level, and the purity and yield of the magnesium hydroxide in the product are poor. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a SEM image of nano magnesium hydroxide prepared in Example 1 of the present invention;
[0021] Figure 2 This is the XRD diagram of nano magnesium hydroxide prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0022] In order to enable those skilled in the art to better understand the technical solution of the present invention and implement it, the present invention is further described below in conjunction with specific examples, but the examples are not intended to limit the present invention. The following test methods and detection methods, unless otherwise specified, are conventional methods; the reagents and raw materials, unless otherwise specified, are commercially available.
[0023] Magnesite, which is mentioned in the background technology of the present invention as a superior mineral in my country, is a high-quality ore source for preparing magnesium-containing compounds. However, how to comprehensively utilize coal mine tailings is an urgent problem to be solved. How to make good use of my country's magnesite tailings resources, improve its resource economic benefits, and prepare high-quality magnesium-containing compounds is currently the main research direction for magnesite tailings resources. And how to prepare nano magnesium hydroxide using magnesite tailings as raw materials, so as to use magnesium hydroxide as a flame retardant, improve the flame retardant effect of the material, and make high value-added use of magnesite is of great significance. In the prior art, magnesium hydroxide prepared using magnesite tailings as raw materials cannot reach the nano level and agglomeration phenomenon is serious, and the purity and yield of magnesium hydroxide in the product are not enough. Based on the above technical background, the present invention provides a nano magnesium hydroxide prepared from magnesite tailings and its preparation method and application.
[0024] The technical solution of the present invention is analyzed and explained in detail below.
[0025] The present invention first provides a method for preparing nano magnesium hydroxide from magnesite tailings, comprising the following steps:
[0026] The magnesite tailings are calcined at a constant temperature of 700-1100°C to obtain a calcined product; since the main component of magnesite is MgCO3, after high-temperature calcination in a box-type resistance furnace, volatile impurities such as CO2 are released to generate active MgO;
[0027] The water is heated to reflux at a constant temperature of 25 to 45° C., and the calcined product is added under stirring to undergo a hydration reaction to obtain a suspension containing MgO, Fe2O3, Al2O3, CaO and SiO2, and the suspension is aged to obtain a hydrated product; hydrogen peroxide is added to the hydrated product, and then sulfuric acid and ammonia water are added to the hydrated product, and Fe2O3, Al2O3 and CaO in the hydrated product are converted into precipitates to be filtered out, and MgO is converted into MgSO4 to be separated from SiO2;
[0028] Add OH to the MgSO4 - A solution is prepared by adding a dispersant and hydrothermally reacting the magnesium sulfate at 130-160° C. to prepare nano-magnesium hydroxide.
[0029] The invention uses magnesite tailings as raw materials and prepares nano magnesium hydroxide with good yield and purity through the above-mentioned treatment means, and the nano magnesium hydroxide reaches the nano level with a particle size of 80 to 120 nm, which effectively solves the technical problems that the magnesium hydroxide prepared using magnesite tailings as raw materials cannot reach the nano level and has serious agglomeration phenomenon, and the purity and yield of the magnesium hydroxide in the product are poor.
[0030] It should be noted that the constant temperature calcination time is 100 to 200 minutes. If the calcination time is insufficient, the conversion efficiency of MgCO3 in the magnesite tailings will inevitably be reduced, thereby affecting the MgO yield and the removal rate of impurities.
[0031] In order to further remove the remaining metal elements in the hydration product, the mass concentration of the hydrogen peroxide is 3%, and the mass ratio of the hydrogen peroxide to the hydration product is 0.3-0.5:1.
[0032] It should be emphasized that the mass concentration of the ammonia water is 25%, and the mass ratio of the ammonia water to the hydration product is 4 to 8:1; the concentration of the sulfuric acid is 65%, and the mass ratio of the sulfuric acid to the hydration product is 3 to 5:1. If the amount of sulfuric acid used is too low, it will inevitably lead to the inability to completely convert the oxides in the hydration product into sulfate substances, thereby affecting the yield and purity of the final nano magnesium hydroxide. If the amount of sulfuric acid used is too much, although it can ensure that the metal magnesium oxide in the hydration product is completely converted into sulfate substances, excessive sulfuric acid will inevitably lead to a waste of raw materials.
[0033] In order to completely dissolve the metal ions in the calcined product, the mass ratio of the water to the calcined product is 6 to 10:1.
[0034] In order to completely convert the magnesium ions in magnesium sulfate into magnesium hydroxide precipitates, thereby improving the yield and purity of nano magnesium hydroxide, the OH - The solution is a NaOH solution, and the mass ratio of MgSO4 to NaOH is 1:6-12.
[0035] In order to completely convert the metal ions in the calcined product into metal oxides, and convert magnesium oxide into magnesium sulfate and finally generate nano magnesium hydroxide, the hydration reaction time is 1 to 3 hours, and the hydrothermal reaction time is 14 to 76 hours.
[0036] In order to improve the degree of dispersion, the dispersant is a mixture of APG and SDS in a mass ratio of 1:1, and the amount of the dispersant is 4% to 10% of the mass of the nano magnesium hydroxide.
[0037] The technical effects of the present invention are described below through specific embodiments and comparative examples.
[0038] Example 1
[0039] A method for preparing nano magnesium hydroxide from magnesite tailings comprises the following steps:
[0040] S1. Use an electronic balance to weigh 15.00 g of Dashiqiao magnesite powder tailings and place it in an open porcelain crucible. Place the crucible in a muffle furnace, raise the temperature to 1100° C. at a rate of 15° C. / min, and calcine at a constant temperature for 100 min to obtain a calcined product for later use.
[0041] S2, take 100mL of deionized water and place it in a three-necked flask, heat it to reflux at a constant temperature of 35°C, weigh 10.00g of the calcined product and place it in a three-necked flask, stir it at 1400r / min, and react for 3 hours. After the reaction is completed, the suspension is cooled and aged at room temperature for 30 minutes, then filtered, washed with water 3 times and ethanol 3 times in sequence. The filter cake is placed in a forced air drying oven, the temperature of the drying oven is controlled at 110°C, and dried to obtain a hydrated product. According to the mass ratio of hydrogen peroxide to hydration product of 0.3:1, hydrogen peroxide with a mass concentration of 3% is added to the hydration product. After reacting for 0.3 hours, sulfuric acid with a mass concentration of 65% and ammonia with a mass concentration of 25% are added according to the mass ratio of sulfuric acid or ammonia to hydration product of 5:1, and react for 1 hour to obtain MgSO4;
[0042] S3, according to the mass ratio of MgSO4 to NaOH being 1:10, NaOH solution is added to the MgSO4, and 4% of a composite dispersant (APG and SDS in a mass ratio of 1:1) is added at the same time, and the mixture is reacted at 140°C for 20 hours, and then cooled and aged at room temperature, filtered, and washed with water 2 times and ethanol 3 times in sequence. The filter cake is placed in a 120°C blast drying oven, dried, and cooled to obtain nano magnesium hydroxide with a particle size of 80 to 120 nm.
[0043] The nano magnesium hydroxide prepared above is applied to prepare a flame retardant polyethylene composite material, specifically:
[0044] S1, adding silane coupling agent 550 of 1.5% by weight of polyethylene to the nano-magnesium hydroxide for modification to obtain modified nano-magnesium hydroxide.
[0045] S2, adding 20 parts of modified nano magnesium hydroxide to 100 parts of PE, then adding the above mixture into a double-roll mill, refining at 80°C for 20 minutes, then making 9 triangle packages, and finally pressing into sheets at 180°C on a flat vulcanizer to obtain a flame-retardant PE composite material.
[0046] Example 2
[0047] A method for preparing nano magnesium hydroxide from magnesite tailings comprises the following steps:
[0048] S1. Use an electronic balance to weigh 10.00 g of Dashiqiao magnesite powder tailings and place it in an open porcelain crucible. Place the crucible in a muffle furnace, raise the temperature to 900°C at a rate of 15°C / min, and calcine at a constant temperature for 100 min to obtain a calcined product for later use.
[0049] S2, take 80mL of deionized water and place it in a three-necked flask, heat and reflux at a constant temperature of 25°C, weigh 8.00g of the calcined product and place it in a three-necked flask and stir at 1200r / min, react for 3 hours, after the reaction is completed, cool and age the suspension at room temperature for 30 minutes, then filter it, wash it with water 3 times, and wash it with ethanol 3 times. Place the filter cake in a forced air drying oven, control the temperature of the drying oven at 110°C, dry it, and obtain a hydration product. According to the mass ratio of hydrogen peroxide to hydration product of 0.4:1, add 3% hydrogen peroxide to the hydration product, react for 0.3 hours, then add 65% sulfuric acid and 25% ammonia according to the mass ratio of sulfuric acid or ammonia to hydration product of 4:1, react for 1 hour, and obtain MgSO4;
[0050] S3, according to the mass ratio of MgSO4 to NaOH being 1:12, NaOH solution is added to the MgSO4, and 4% of a composite dispersant (APG and SDS in a mass ratio of 1:1) is added at the same time, and the mixture is reacted at 140°C for 18 hours, and then cooled and aged at room temperature, filtered, and washed with water 2 times and ethanol 3 times in sequence. The filter cake is placed in a 120°C blast drying oven, dried, and cooled to obtain nano magnesium hydroxide with a particle size of 80 to 120 nm.
[0051] The nano magnesium hydroxide prepared above is applied to prepare a flame retardant polyethylene composite material, specifically:
[0052] Adding 2.0% of the mass of polyethylene silane coupling agent 550 to the nano magnesium hydroxide for modification, thereby obtaining modified nano magnesium hydroxide;
[0053] 25 parts of modified nano magnesium hydroxide were added to 100 parts of PE, and then the mixture was added to a double-roll mill, and smelted at 90°C for 20 minutes, and then triangular-wrapped 9 times, and finally pressed into sheets at 185°C on a flat vulcanizer to obtain a flame-retardant PE composite material.
[0054] Example 3
[0055] A method for preparing nano magnesium hydroxide from magnesite tailings comprises the following steps:
[0056] S1. Use an electronic balance to weigh 20.00 g of Dashiqiao magnesite powder and place it in an open porcelain crucible. Place the crucible in a muffle furnace, heat it to 1100°C at a rate of 15°C / min, and calcine it at a constant temperature for 100 min to obtain a calcined product for later use.
[0057] S2, take 120mL of deionized water and place it in a three-necked flask, heat it to reflux at a constant temperature of 45°C, weigh 12.00g of the calcined product and place it in a three-necked flask, stir it at 1600r / min, and react for 2.5 hours. After the reaction is completed, the suspension is cooled and aged at room temperature for 30 minutes, then filtered, washed with water 3 times, and washed with ethanol 3 times. The filter cake is placed in a forced air drying oven, the temperature of the drying oven is controlled at 120°C, and dried to obtain a hydration product. According to the mass ratio of hydrogen peroxide to hydration product of 0.5:1, 3% hydrogen peroxide is added to the hydration product. After reacting for 0.3 hours, sulfuric acid with a mass concentration of 65% and ammonia with a mass concentration of 25% are added according to the mass ratio of sulfuric acid or ammonia to hydration product of 6:1. React for 1 hour to obtain MgSO4;
[0058] S3, according to the mass ratio of MgSO4 to NaOH being 1:6, NaOH solution is added to the MgSO4, and 4% of a composite dispersant (APG and SDS in a mass ratio of 1:1) is added at the same time, and the mixture is reacted at 140°C for 28 hours, and then cooled and aged at room temperature, filtered, and washed with water 2 times and ethanol 3 times in sequence. The filter cake is placed in a 120°C blast drying oven, dried, and cooled to obtain nano magnesium hydroxide with a particle size of 80 to 120 nm.
[0059] The nano magnesium hydroxide prepared above is applied to prepare a flame retardant polyethylene composite material, specifically:
[0060] Adding 2.5% of the mass of polyethylene silane coupling agent 550 to the nano magnesium hydroxide for modification, thereby obtaining modified nano magnesium hydroxide;
[0061] 25 parts of modified nano magnesium hydroxide were added to 100 parts of PE, and then the mixture was added to a double-roll mill, and smelted at 70°C for 20 minutes, and then triangular-packaged 9 times, and finally pressed on a flat vulcanizer at 170°C to obtain a flame-retardant PE composite material.
[0062] Example 4
[0063] A method for preparing nano magnesium hydroxide from magnesite tailings comprises the following steps:
[0064] S1. Use an electronic balance to weigh 20.00 g of Dashiqiao magnesite powder and place it in an open porcelain crucible. Place the crucible in a muffle furnace, heat it to 800°C at a rate of 15°C / min, and calcine it at a constant temperature for 120 min to obtain a calcined product for later use.
[0065] S2, take 120mL of deionized water and place it in a three-necked flask, heat it to reflux at a constant temperature of 35°C, weigh 12.00g of the calcined product and place it in a three-necked flask, stir it at 1600r / min, and react for 2.5 hours. After the reaction is completed, the suspension is cooled and aged at room temperature for 30 minutes, then filtered, washed with water 3 times and ethanol 3 times in sequence, and the filter cake is placed in a blast drying oven, the temperature of the drying oven is controlled at 120°C, and dried to obtain a hydrated product, according to a mass ratio of hydrogen peroxide to hydrated product of 0.3:1, add 3% hydrogen peroxide by mass concentration to the hydrated product, after reacting for 0.3 hours, then add 65% sulfuric acid by mass concentration and 25% ammonia by mass concentration according to a mass ratio of sulfuric acid or ammonia to hydrated product of 7:1, react for 1 hour, and obtain MgSO4;
[0066] S3, according to the mass ratio of MgSO4 to NaOH being 1:8, NaOH solution is added to the MgSO4, and 4% of a composite dispersant (APG and SDS in a mass ratio of 1:1) is added at the same time, and the mixture is reacted at 140°C for 28 hours, and then cooled and aged at room temperature, filtered, and washed with water 2 times and ethanol 3 times in sequence. The filter cake is placed in a 115°C blast drying oven, dried, and cooled to obtain nano magnesium hydroxide with a particle size of 80 to 120 nm.
[0067] The nano magnesium hydroxide prepared above is applied to prepare a flame retardant polyethylene composite material, specifically:
[0068] Adding 2.0% of the mass of polyethylene silane coupling agent 550 to the nano magnesium hydroxide for modification, thereby obtaining modified nano magnesium hydroxide;
[0069] 30 parts of modified nano magnesium hydroxide were added to 100 parts of PE, and then the mixture was added to a double-roll mill, and smelted at 70°C for 20 minutes, and then triangular-packaged 9 times, and finally pressed on a flat vulcanizer at 180°C to obtain a flame-retardant PE composite material.
[0070] Example 5
[0071] A method for preparing nano magnesium hydroxide from magnesite tailings comprises the following steps:
[0072] S1. Use an electronic balance to weigh 15.00 g of Dashiqiao magnesite powder and place it in an open porcelain crucible. Place the crucible in a muffle furnace, heat it to 850°C at a rate of 15°C / min, and calcine it at a constant temperature for 200 min to obtain a calcined product for later use.
[0073] S2, take 110mL of deionized water and place it in a three-necked flask, heat it under reflux at a constant temperature of 35°C, weigh 11.00g of the calcined product and place it in a three-necked flask, stir it at 1600r / min, and react for 1 hour. After the reaction is completed, the suspension is cooled and aged at room temperature for 30min and then filtered, washed with water 3 times and ethanol 3 times in sequence, and the filter cake is placed in a blast drying oven, the temperature of the drying oven is controlled at 120°C, and dried to obtain a hydrated product, according to a mass ratio of hydrogen peroxide to hydrated product of 0.4:1, add 3% hydrogen peroxide by mass concentration to the hydrated product, react for 0.3 hour, then add 65% sulfuric acid and 25% ammonia by mass concentration according to a mass ratio of sulfuric acid or ammonia to hydrated product of 6:1, react for 1 hour, and obtain MgSO4;
[0074] S3, according to the mass ratio of MgSO4 to NaOH being 1:10, NaOH solution is added to the MgSO4, and 4% of a composite dispersant (APG and SDS in a mass ratio of 1:1) is added at the same time, and the mixture is reacted at 130°C for 76 hours, and then cooled and aged at room temperature, filtered, and washed with water 2 times and ethanol 3 times in sequence. The filter cake is placed in a blast drying oven at 115°C, dried, and cooled to obtain nano magnesium hydroxide with a particle size of 80 to 120 nm.
[0075] The nano magnesium hydroxide prepared above is applied to prepare a flame retardant polyethylene composite material, specifically:
[0076] Adding 3.0% of the mass of polyethylene silane coupling agent 550 to the nano magnesium hydroxide for modification, thereby obtaining modified nano magnesium hydroxide;
[0077] Add 50 parts of modified nano magnesium hydroxide to 100 parts of PE, then add the mixture into a double-roll mill, refine at 75°C for 20 minutes, then make 9 triangle packages, and finally press into sheets on a flat vulcanizer at 165°C to obtain a flame-retardant PE composite material.
[0078] Example 6
[0079] A method for preparing nano magnesium hydroxide from magnesite tailings comprises the following steps:
[0080] S1. Use an electronic balance to weigh 15.00 g of Dashiqiao magnesite powder and place it in an open porcelain crucible. Place the crucible in a muffle furnace, heat it to 750°C at a rate of 15°C / min, and calcine it at a constant temperature for 150 min to obtain a calcined product for later use.
[0081] S2, take 90mL of deionized water and place it in a three-necked flask, heat it to reflux at a constant temperature of 35°C, weigh 9.00g of the calcined product and place it in a three-necked flask, stir it at 1600r / min, and react for 2 hours. After the reaction is completed, the suspension is cooled and aged at room temperature for 30min and then filtered, washed with water 3 times and ethanol 3 times in sequence, and the filter cake is placed in a blast drying oven, the temperature of the drying oven is controlled at 120°C, and dried to obtain a hydrated product, according to a mass ratio of hydrogen peroxide to hydrated product of 0.3:1, add 3% hydrogen peroxide by mass concentration to the hydrated product, react for 0.3 hours, and then add 65% sulfuric acid and 25% ammonia by mass concentration according to a mass ratio of sulfuric acid or ammonia to hydrated product of 5:1, react for 1 hour, and obtain MgSO4;
[0082] S3, according to the mass ratio of MgSO4 to NaOH being 1:12, NaOH solution is added to the MgSO4, and 4% of a composite dispersant (APG and SDS in a mass ratio of 1:1) is added at the same time, and the mixture is reacted at 150°C for 14 hours, and then cooled and aged at room temperature, filtered, and washed with water 2 times and ethanol 3 times in sequence. The filter cake is placed in a 115°C blast drying oven, dried, and cooled to obtain nano magnesium hydroxide with a particle size of 80 to 120 nm.
[0083] The nano magnesium hydroxide prepared above is applied to prepare a flame retardant polyethylene composite material, specifically:
[0084] Adding 2.0% of the mass of polyethylene silane coupling agent 550 to the nano magnesium hydroxide for modification, thereby obtaining modified nano magnesium hydroxide;
[0085] 35 parts of modified nano magnesium hydroxide were added to 100 parts of PE, and then the mixture was added to a double-roll mill, and smelted at 85°C for 10 minutes, and then triangular-wrapped 9 times, and finally pressed on a flat vulcanizer at 170°C to obtain a flame-retardant PE composite material.
[0086] Example 7
[0087] A method for preparing nano magnesium hydroxide from magnesite tailings comprises the following steps:
[0088] S1. Use an electronic balance to weigh 15.00 g of Dashiqiao magnesite powder and place it in an open porcelain crucible. Place the crucible in a muffle furnace, heat it to 950°C at a rate of 15°C / min, and calcine it at a constant temperature for 180 min to obtain a calcined product for later use.
[0089] S2, take 100mL of deionized water and place it in a three-necked flask, heat it under reflux at a constant temperature of 35°C, weigh 12.00g of the calcined product and place it in a three-necked flask, stir it at 1600r / min, and react for 1.5 hours. After the reaction is completed, the suspension is cooled and aged at room temperature for 30 minutes, then filtered, washed with water 3 times and ethanol 3 times in sequence, and the filter cake is placed in a blast drying oven, the temperature of the drying oven is controlled at 120°C, and dried to obtain a hydrated product, and hydrogen peroxide with a mass concentration of 3% is added to the hydrated product according to a mass ratio of hydrogen peroxide to hydrated product of 0.5:1, after reacting for 0.3 hours, sulfuric acid with a mass concentration of 65% and ammonia with a mass concentration of 25% are added according to a mass ratio of sulfuric acid or ammonia to hydrated product of 4:1, and reacted for 1 hour to obtain MgSO4;
[0090] S3, according to the mass ratio of MgSO4 to NaOH being 1:8, NaOH solution is added to the MgSO4, and 4% of a composite dispersant (APG and SDS in a mass ratio of 1:1) is added at the same time, and the mixture is reacted at 160°C for 40 hours, and then cooled and aged at room temperature, filtered, and washed with water 2 times and ethanol 3 times in sequence. The filter cake is placed in a blast drying oven at 115°C, dried, and cooled to obtain nano magnesium hydroxide with a particle size of 80 to 120 nm.
[0091] The nano magnesium hydroxide prepared above is applied to prepare a flame retardant polyethylene composite material, specifically:
[0092] Adding 2.5% of the mass of polyethylene silane coupling agent 550 to the nano magnesium hydroxide for modification, thereby obtaining modified nano magnesium hydroxide;
[0093] 25 parts of modified nano magnesium hydroxide were added to 100 parts of PE, and then the mixture was added to a double-roll mill, smelted at 80°C for 12 minutes, then triangular-packaged 9 times, and finally pressed on a flat vulcanizer at 190°C to obtain a flame-retardant PE composite material.
[0094] Example 8
[0095] A method for preparing nano magnesium hydroxide from magnesite tailings comprises the following steps:
[0096] S1. Use an electronic balance to weigh 20.00 g of Dashiqiao magnesite powder and place it in an open porcelain crucible. Place the crucible in a muffle furnace, heat it to 1000°C at a rate of 15°C / min, and calcine it at a constant temperature for 160 min to obtain a calcined product for later use.
[0097] S2, take 120mL of deionized water and place it in a three-necked flask, heat it to reflux at a constant temperature of 35°C, weigh 10.00g of the calcined product and place it in a three-necked flask, stir it at 1600r / min, and react for 2.5 hours. After the reaction is completed, the suspension is cooled and aged at room temperature for 30 minutes, then filtered, washed with water 3 times and ethanol 3 times in sequence, and the filter cake is placed in a forced air drying oven, the temperature of the drying oven is controlled at 120°C, and dried to obtain a hydrated product, and hydrogen peroxide with a mass concentration of 3% is added to the hydrated product according to a mass ratio of hydrogen peroxide to hydrated product of 0.4:1, after reacting for 0.3 hours, sulfuric acid with a mass concentration of 65% and ammonia with a mass concentration of 25% are added according to a mass ratio of sulfuric acid or ammonia to hydrated product of 7:1, and reacted for 1 hour to obtain MgSO4;
[0098] S3, according to the mass ratio of MgSO4 to NaOH being 1:6, NaOH solution is added to the MgSO4, and 4% of a composite dispersant (APG and SDS in a mass ratio of 1:1) is added at the same time, and the mixture is reacted at 140°C for 50 hours, and then cooled and aged at room temperature, filtered, and washed with water 2 times and ethanol 3 times in sequence. The filter cake is placed in a 115°C blast drying oven, dried, and cooled to obtain nano magnesium hydroxide with a particle size of 80 to 120 nm.
[0099] The nano magnesium hydroxide prepared above is applied to prepare a flame retardant polyethylene composite material, specifically:
[0100] Adding 1.5% of the mass of polyethylene silane coupling agent 550 to the nano magnesium hydroxide for modification, thereby obtaining modified nano magnesium hydroxide;
[0101] 20 parts of modified nano magnesium hydroxide were added to 100 parts of PE, and then the mixture was added to a double-roll mill, and smelted at 80°C for 15 minutes, and then triangular-wrapped 9 times, and finally pressed on a flat vulcanizer at 160°C to obtain a flame-retardant PE composite material.
[0102] The morphology and performance of the nano magnesium hydroxide obtained in Examples 1 to 8 of the present invention were characterized, and Example 1 was used as an example to illustrate the effect. The test results are as follows: Figure 1 and Figure 2 shown.
[0103] Depend on Figure 1 and Figure 2 It can be seen that nano magnesium hydroxide is obtained by adding composite dispersants APG and SDS through the calcination-hydration-hydrothermal process. The dispersant can improve the dispersibility of the product and reduce the adhesion and agglomeration of the product.
[0104] After the prepared nano magnesium hydroxide was added to PE, as the amount of magnesium hydroxide flame retardant increased, the mechanical properties of PE decreased but the effect was small, the flame retardancy was improved, and the electrical properties did not change much. At this time, the tensile strength was 10.58MPa, the elongation at break was 334%, the dielectric constant was 2.7-4.1, and the volume resistivity was 4.5×10 13 Ω·m, oxygen index 24%.
[0105] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for preparing nano magnesium hydroxide from magnesite tailings, characterized in that: The following steps are involved: The magnesite tailings are calcined at a constant temperature of 700-1100° C. to obtain a calcined product; The water is heated to reflux at a constant temperature of 25 to 45° C., and the calcined product is added under stirring to undergo a hydration reaction to obtain a suspension containing MgO, Fe2O3, Al2O3, CaO and SiO2, and the suspension is aged to obtain a hydrated product; hydrogen peroxide is added to the hydrated product, and then sulfuric acid and ammonia water are added to the hydrated product, and Fe2O3, Al2O3 and CaO in the hydrated product are converted into precipitates to be filtered out, and MgO is converted into MgSO4 to be separated from SiO2; Add OH to the MgSO4 - A solution is prepared by adding a dispersant and hydrothermally reacting the magnesium sulfate at 130-160° C. to prepare nano-magnesium hydroxide.
2. The method according to claim 1, characterized in that The mass concentration of the hydrogen peroxide is 3%, and the mass ratio of the hydrogen peroxide to the hydration product is 0.3-0.5:
1.
3. The method according to claim 1, characterized in that The mass concentration of the aqueous ammonia is 25%, and the mass ratio of the aqueous ammonia to the hydration product is 4-8:1; the concentration of the sulfuric acid is 65%, and the mass ratio of the sulfuric acid to the hydration product is 3-5:
1.
4. The method according to claim 1, characterized in that: The OH-containing - The solution is a NaOH solution, and the mass ratio of MgSO4 to NaOH is 1:6-12.
5. The method according to claim 1, characterized in that: The mass ratio of the water to the calcined product is 6 to 10:
1.
6. The method according to claim 1, characterized in that The time of the hydration reaction is 1 to 3 hours, the time of the hydrothermal reaction is 14 to 76 hours, and the time of the constant temperature calcination is 100 to 200 minutes.
7. The method according to claim 1, characterized in that The dispersant is a mixture of APG and SDS in a mass ratio of 1:1, and the amount of the dispersant is 4% to 10% of the mass of the nano magnesium hydroxide.
8. Nano magnesium hydroxide obtained by the method according to any one of claims 1 to 7, characterized in that: The particle size of the nano magnesium hydroxide is 80-120 nm.
9. Use of the nano magnesium hydroxide according to claim 8 in preparing a flame retardant polyethylene composite material, characterized in that: The application is as follows: modifying the nano magnesium hydroxide with a silane coupling agent to obtain modified nano magnesium hydroxide; refining polyethylene and the modified nano magnesium hydroxide at 70-100° C. for 10-20 minutes, making triangle packages 9 times, and pressing the sheets at 160-190° C. to obtain a flame-retardant PE composite material.
10. The use according to claim 9, characterized in that: The mass ratio of the modified magnesium hydroxide to polyethylene is 2-5:10; the silane coupling agent is γ-aminopropyltriethoxysilane, and the amount of the silane coupling agent is 1.5%-3% based on the mass of polyethylene.