Ferric manganese oxide nano material as well as preparation method and application thereof

By adding support frames and ferrous sulfate to the sol-gel method, adding raw materials in batches, stirring and high-temperature calcination, the problem of uneven heat treatment of the solution is solved, and the preparation efficiency and purity of ferromanganese oxygen nanomaterials are improved. Suitable for a variety of applications.

CN119038613APending Publication Date: 2024-11-29BENGBU COLLEGE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411157868.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

When preparing manganese ferrite nanoparticles using the sol-gel method, the raw material dissolves in the solution at a slow rate due to the uneven properties of the raw material itself and the aqueous solution being heated, which affects the preparation efficiency.

Method used

By adding a support frame to the water bath heating to ensure that the bottom of the beaker is in full contact with the heating equipment, and adding a small amount of ferrous sulfate as an auxiliary agent to the aqueous solution, adding iron sulfate and manganese sulfate in batches, and stirring with stirring magnets to adjust pH value and stand in a dust-free cover to reduce dust contact, and finally perform high-temperature calcination.

Benefits of technology

It improves the dissolution efficiency and heat uniformity of the raw materials in aqueous solution, significantly accelerates the preparation process, and obtains high-purity iron-manganese oxygen nanomaterials, suitable for high-frequency inductors, microwave absorbing materials and catalysts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038613A_ABST
    Figure CN119038613A_ABST
Patent Text Reader

Abstract

The invention discloses an iron manganese oxide nano material and a preparation method and application thereof, and relates to the field of nano materials, the preparation method comprises preparation of raw materials for producing the iron manganese oxide nano material, an aqueous solution, manganese sulfate and iron sulfate, the manganese sulfate is manganese sulfate, the manganese sulfate is prepared through the action of metal manganese and sulfuric acid, and the iron sulfate is ferric sulfate. The ferric sulfate is prepared from metal iron and sulfuric acid. Pouring the aqueous solution into a beaker, then putting the beaker into water bath heating equipment, raising the temperature of the beaker and the aqueous solution in the beaker to 60 DEG C, then adding ferric sulfate, manganese sulfate and ferrous sulfate into the beaker in batches according to the proportion, finally adding citric acid for solubilization, and after adding the manganese sulfate and the ferric sulfate into the aqueous solution, stirring uniformly; a small amount of ferrous sulfate is added into the aqueous solution, and meanwhile, the support frame is additionally arranged at the bottom of the beaker, so that the raw materials added into the aqueous solution can be dissolved in the aqueous solution more quickly, and the preparation of the iron-manganese-oxygen nano material is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of nanomaterials, and in particular to an iron-manganese oxide nanomaterial and a preparation method and application thereof. Background Art

[0002] Manganese ferrite nanoparticles are a new type of nanomaterial with broad application prospects. Manganese ferrite is a magnetic material with good magnetic and electrical properties, so it is widely used in electronics, communications, medical treatment, environmental protection and other fields. The development of nanotechnology has further developed the preparation and application of manganese ferrite nanoparticles.

[0003] There are many methods for preparing manganese ferrite nanoparticles, including sol-gel method, coprecipitation method, hydrothermal method, microwave method, etc. Among them, sol-gel method is a more commonly used preparation method. This method dissolves metal ions in a solvent in the form of a sol, and then forms nanoparticles through a gelation reaction. The manganese ferrite nanoparticles prepared by this method have high purity and uniformity, which can meet the needs of different fields.

[0004] When using the sol-gel method to prepare manganese ferrite nanoparticles, the raw materials need to be added to the constant temperature solution in the beaker. When adding the raw materials, the solution will be stirred to allow the raw materials to be fully mixed with the aqueous solution. However, due to the properties of the raw materials themselves and the uneven heating of the aqueous solution, the rate at which the raw materials dissolve in the solution may be slow. Summary of the invention

[0005] The purpose of the present application is to solve the problem raised in the above background technology that the rate at which the raw material itself dissolves into the solution may be slow due to the influence of the properties of the raw material itself and the uneven heating of the aqueous solution. The present application provides an iron manganese oxide nanomaterial and its preparation method and application.

[0006] In order to achieve the above-mentioned purpose, this application specifically adopts the following technical solutions:

[0007] A method for preparing an iron-manganese oxide nanomaterial, the preparation method is as follows:

[0008] S1: raw material preparation, including aqueous solution, manganese sulfate and iron sulfate, manganese sulfate is manganese sulfate, manganese sulfate is prepared by the reaction of metallic manganese and sulfuric acid, iron sulfate is ferric sulfate, ferric sulfate is prepared by the reaction of metallic iron and sulfuric acid;

[0009] S2: Before the experiment begins, soak the beaker and stirring magnet in aqua regia for half an hour to clean them, and then weigh ferric sulfate, ferrous sulfate, manganese sulfate and aqueous solution according to a certain molar ratio of metal particles;

[0010] S3: Add the aqueous solution into a beaker, then place the beaker in a 60°C water bath, then add citric acid into the aqueous solution, and stir the aqueous solution fully with a stirring magnet when adding the citric acid;

[0011] S4: Then add one third of the total amount of ferric sulfate, ferrous sulfate and manganese sulfate to the aqueous solution in sequence, and stir the solution with a stirring magnet during the addition process, and then continue to add one half of the remaining total amount of ferric sulfate, ferrous sulfate and manganese sulfate, and stir the solution thoroughly, and finally add the remaining ferrous sulfate, ferrous sulfate and manganese sulfate to the aqueous solution, and stir the solution thoroughly to obtain a sol;

[0012] S5: After obtaining the sol, ammonia water is added to the sol to adjust the pH value, and then the sol is placed in a dust-free hood and allowed to stand for 12 hours, and then dried at 85° C. to obtain a dry gel, and then the dry gel is calcined at 800° C. to obtain an iron manganese oxide powder.

[0013] Furthermore, the molar ratio of the manganese sulfate to the ferrous sulfate metal ions is 1:4, a small amount of ferrous sulfate is added to the ferric sulfate, and the molar ratio of the metal particles of ferrous sulfate and ferrous sulfate is 10:1.

[0014] Furthermore, the aqueous solution is deionized water. The aqueous solution uses deionized water to remove particulate matter in the aqueous solution, thereby improving the purity of the aqueous solution and reducing the influence of substances in the aqueous solution on the reaction.

[0015] Furthermore, a support frame is provided at the bottom of the beaker containing the aqueous solution for water bath heating, and the support frame abuts against the bottom edge of the beaker.

[0016] A ferromanganese oxide nano material is in the form of nano particles and is prepared by the above-mentioned raw materials and the above-mentioned preparation method.

[0017] An application of an iron-manganese oxide nanomaterial, wherein the iron-manganese oxide nanomaterial can be used to prepare a high-frequency inductor, the iron-manganese oxide nanomaterial can be used to prepare a microwave absorbing material, and the iron-manganese oxide nanomaterial can be used to prepare an adsorbent and a catalyst.

[0018] In summary, the present application includes at least one of the following beneficial effects:

[0019] 1. The present application uses manganese sulfate and ferric sulfate as the materials for producing iron-manganese oxide nanomaterials. When manganese sulfate and ferric sulfate are dissolved in an aqueous solution, a small amount of ferrous sulfate is added to the aqueous solution. The characteristics of the reaction between ferrous sulfate and ferric sulfate are utilized to allow ferrous sulfate to act as an auxiliary agent for dissolving ferric sulfate in the aqueous solution. At the same time, ferric sulfate, ferrous sulfate and manganese sulfate are added to the aqueous solution in batches during preparation, thereby achieving the purpose of improving the efficiency of dissolving the raw materials in the aqueous solution.

[0020] 2. This application. When placing a beaker in a water bath heating device, a support frame is placed at the bottom of the beaker to support the edge of the bottom of the beaker, so that the bottom of the beaker can be fully in contact with the heated solution in the water bath heating device, so that the aqueous solution in the beaker is heated more evenly and manganese sulfate and iron sulfate are dissolved in the aqueous solution more quickly. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the preparation method in this application. DETAILED DESCRIPTION

[0022] The following is combined with Figure 1 This application is described in further detail.

[0023] The embodiments of the present application disclose an iron-manganese oxide nanomaterial and a preparation method and application thereof.

[0024] Reference Figure 1 , a method for preparing an iron-manganese oxide nanomaterial, the preparation method is as follows:

[0025] S1: raw material preparation, including aqueous solution, manganese sulfate and iron sulfate, manganese sulfate is manganese sulfate, manganese sulfate is prepared by the reaction of metallic manganese and sulfuric acid, iron sulfate is ferric sulfate, ferric sulfate is prepared by the reaction of metallic iron and sulfuric acid;

[0026] S2: Before the experiment begins, soak the beaker and stirring magnet in aqua regia for half an hour to clean them, and then weigh ferric sulfate, ferrous sulfate, manganese sulfate and aqueous solution according to a certain molar ratio of metal particles;

[0027] S3: Add the aqueous solution into a beaker, then place the beaker in a 60°C water bath, then add citric acid into the aqueous solution, and stir the aqueous solution fully with a stirring magnet when adding the citric acid;

[0028] S4: Then add one third of the total amount of ferric sulfate, ferrous sulfate and manganese sulfate to the aqueous solution in sequence, and stir the solution with a stirring magnet during the addition process, and then continue to add one half of the remaining total amount of ferric sulfate, ferrous sulfate and manganese sulfate, and stir the solution thoroughly, and finally add the remaining ferrous sulfate, ferrous sulfate and manganese sulfate to the aqueous solution, and stir the solution thoroughly to obtain a sol;

[0029] S5: After obtaining the sol, ammonia water is added to the sol to adjust the pH value, and then the sol is placed in a dust-free hood and allowed to stand for 12 hours, and then dried at 85° C. to obtain a dry gel, and then the dry gel is calcined at 800° C. to obtain an iron manganese oxide powder.

[0030] Before the preparation, first, soak the beaker that needs to hold the aqueous solution and the stirring magnet for stirring in aqua regia, remove the debris on the surface of the beaker and the stirring magnet, then pour the aqueous solution into the beaker, and then put the beaker into a water bath heating device, let the beaker and the aqueous solution in the beaker rise to 60°C and maintain it at 60°C, then add ferric sulfate, manganese sulfate and ferrous sulfate to the beaker in batches according to proportion, ferrous sulfate and ferrous sulfate react with each other, so that ferric sulfate is more integrated into the aqueous solution, and stir with a stirring magnet, finally add citric acid for solution, and adjust the pH value with ammonia water after solution, and then put the obtained sol into a dust-free cover and let it stand for 12 hours, and then dry it, and then calcine it after drying to obtain iron-manganese oxide powder. When adding ferric sulfate to the aqueous solution, adding a small amount of ferrous sulfate can make the ferric sulfate more easily dissolved in the aqueous solution. At the same time, letting the sol stand in a dust-free cover can reduce the contact between dust and sol when the sol is standing.

[0031] The molar ratio of manganese sulfate to ferric sulfate metal ions is 1:4, a small amount of ferrous sulfate is added to ferric sulfate, and the molar ratio of metal particles of ferric sulfate and ferrous sulfate is 10:1.

[0032] The aqueous solution is deionized water. The aqueous solution uses deionized water to remove particulate matter in the aqueous solution, improve the purity of the aqueous solution, and reduce the influence of substances in the aqueous solution on the reaction.

[0033] The bottom of the beaker used for water bath heating is provided with a support frame, which abuts against the bottom edge of the beaker. A support frame is added to the bottom of the beaker, which lifts the bottom of the beaker, allowing the bottom of the beaker to fully contact the water bath heating equipment, so that the beaker is more evenly at the reaction temperature.

[0034] The invention discloses an iron-manganese oxide nano material, which is in the form of nano particles and is prepared by the above raw materials and the above preparation method.

[0035] An application of an iron manganese oxide nanomaterial. The iron manganese oxide nanomaterial can be used to prepare high-frequency inductors, the iron manganese oxide nanomaterial can be used to prepare microwave absorbing materials, and the iron manganese oxide nanomaterial can be used to prepare adsorbents and catalysts.

Claims

1. A method for preparing an iron-manganese oxide nanomaterial, characterized in that: The preparation method is as follows: S1: raw material preparation, including aqueous solution, manganese sulfate and iron sulfate, manganese sulfate is manganese sulfate, manganese sulfate is prepared by the reaction of metallic manganese and sulfuric acid, iron sulfate is ferric sulfate, ferric sulfate is prepared by the reaction of metallic iron and sulfuric acid; S2: Before the experiment begins, soak the beaker and stirring magnet in aqua regia for half an hour to clean them, and then weigh ferric sulfate, ferrous sulfate, manganese sulfate and aqueous solution according to a certain molar ratio of metal particles; S3: Add the aqueous solution into a beaker, then place the beaker in a 60°C water bath, then add citric acid into the aqueous solution, and stir the aqueous solution fully with a stirring magnet when adding the citric acid; S4: Then add one third of the total amount of ferric sulfate, ferrous sulfate and manganese sulfate to the aqueous solution in sequence, and stir the solution with a stirring magnet during the addition process, and then continue to add one half of the remaining total amount of ferric sulfate, ferrous sulfate and manganese sulfate, and stir the solution thoroughly, and finally add the remaining ferrous sulfate, ferrous sulfate and manganese sulfate to the aqueous solution, and stir the solution thoroughly to obtain a sol; S5: After obtaining the sol, ammonia water is added to the sol to adjust the pH value, and then the sol is placed in a dust-free hood and allowed to stand for 12 hours, and then dried at 85° C. to obtain a dry gel, and then the dry gel is calcined at 800° C. to obtain an iron manganese oxide powder.

2. The method for preparing an iron-manganese oxide nanomaterial according to claim 1, characterized in that: The molar ratio of the manganese sulfate to the ferric sulfate metal ions is 1:4, a small amount of ferrous sulfate is added to the ferric sulfate, and the molar ratio of the metal particles of ferric sulfate and ferrous sulfate is 10:

1.

3. The method for preparing an iron-manganese oxide nanomaterial according to claim 1, characterized in that: The aqueous solution is deionized water.

4. The method for preparing an iron-manganese oxide nanomaterial according to claim 1, characterized in that: The bottom of the beaker for holding the aqueous solution in the water bath heating is provided with a support frame, and the support frame abuts against the bottom edge of the beaker.

5. An iron-manganese oxide nanomaterial, characterized in that: The iron manganese oxide nanomaterial is in the form of nanoparticles and is prepared using the raw materials in claims 1 and 2 and the preparation method in any one of claims 3 to 6.

6. An application of an iron-manganese oxide nanomaterial, characterized in that: The iron-manganese oxide nanomaterial can be used to prepare high-frequency inductors, the iron-manganese oxide nanomaterial can be used to prepare microwave absorbing materials, and the iron-manganese oxide nanomaterial can be used to prepare adsorbents and catalysts.