Borosilicate glass as well as preparation method and application thereof

By adjusting the composition of borosilicate glass, increasing Al2O3, reducing B2O3, and replacing Na2O and CaO with Li2O, the problem of low molybdenum solubility in borosilicate glass is solved, and high molybdenum tolerance and stability of high radioactive nuclear waste is achieved It avoids the precipitation of the yellow phase of molybdate and improves the safety of nuclear waste solidification.

CN119038873AActive Publication Date: 2024-11-29QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES) +1

Patent Information

Application Number
CN202411195534.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-29
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The low solubility of molybdenum in borosilicate glass causes the cured glass to easily produce the yellow phase of molybdate, which reduces chemical stability and safety, and limits its application in the curing of high radioactive nuclear waste.

Method used

By adjusting the composition of borosilicate glass, increasing the Al2O3 content, reducing the B2O3 content, and replacing Na2O and CaO with Li2O, a new borosilicate glass composition was designed to increase the solubility of molybdenum and add up to 11 mol% MoO3 There is no yellow phase of molybdate.

Benefits of technology

It significantly improves the solubility of molybdenum and the chemical stability of glass, avoids the precipitation of the yellow phase of molybdate, and enhances the tolerance and safety of high radioactive nuclear waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119038873A_ABST
    Figure CN119038873A_ABST
Patent Text Reader

Abstract

The invention discloses borosilicate glass as well as a preparation method and application thereof. High-radioactivity waste liquid generated in the nuclear energy industry has huge environmental risks and must be treated stably and safely, borosilicate glass is widely adopted as basic glass internationally to solidify the high-radioactivity waste liquid, but molybdenum in nuclear waste is low in solubility in the borosilicate basic glass, and therefore the high-radioactivity waste liquid is solidified. Therefore, the problem that molybdate yellow phase precipitation is easy to occur in solidified glass is solved. According to the invention, the base glass with high molybdenum inclusion rate is prepared by adjusting the composition of the borosilicate glass. The preparation method specifically comprises the following steps: firstly, gradually replacing B2O3 with Al2O3 to obtain an optimal composition in which 8mol% of MoO3 can be added at most without generating devitrification, then replacing Na2O and CaO with Li2O on the basis, and in the process, keeping the molar ratio of Na2O to CaO unchanged to obtain borosilicate glass in which 11mol% of MoO3 can be added at most without generating devitrification. And the phenomenon of low inclusion rate of the high-radioactivity nuclear waste in the glass curing treatment process is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of nuclear waste treatment, and mainly relates to borosilicate glass for solidifying highly radioactive nuclear waste, and a preparation method and application thereof. Background Art

[0002] Energy issues have always been one of the focal issues that countries continue to pay attention to. The use of fossil fuels will cause serious air pollution and greenhouse gas emissions. Nuclear energy is a supplement to fossil energy, but the spent fuel treatment process will produce a large amount of highly radioactive waste liquid. These nuclear wastes have major safety risks. Once an accident occurs, it will cause catastrophic damage to humans and the environment. At present, the most effective way to dispose of these nuclear wastes is to solidify them and then dispose of them in deep geological conditions.

[0003] Using glass as a matrix for solidifying high-level radioactive nuclear waste is a method that has been successfully applied. Among them, borosilicate glass is widely used as a basic glass for solidifying high-level radioactive nuclear waste due to its good chemical stability, but it also has its shortcomings. For example, the molybdenum content in the high-level radioactive nuclear waste liquid produced by the nuclear power industry is high, while its solubility in borosilicate glass is low. 3 The maximum solubility of molybdenum indicated by (hereinafter the same) does not exceed 5 mol% (usually less than 2 mol%). Once the molybdenum content exceeds its solubility in the glass, the solidified glass formed is very easy to produce phase separation and crystallization, especially the precipitation of molybdate yellow phase (especially soluble Na 2 MoO 4 ), thereby reducing the chemical stability of the solidified glass, causing an increase in the leaching rate of nuclear waste elements, and posing a serious safety hazard. Therefore, borosilicate glass with low molybdenum solubility is difficult to use in the solidification of high-level nuclear waste. Adjusting the basic glass composition is a possible way to increase the solubility of molybdenum in borosilicate glass. Table 1 summarizes the existing results in the literature, showing that the solubility of molybdenum in borosilicate glass is still relatively low.

[0004] Table 1 Data on the solubility of molybdenum in borosilicate glass in the literature

[0005]

[0006] Summary of the invention

[0007] The purpose of the present invention is to solve the problem of yellow phase precipitation of solidified glass due to low solubility of molybdenum in borosilicate glass, and to further improve the solubility of molybdenum in borosilicate glass through innovative composition design. Specifically, Al is added to the composition of borosilicate glass. 2 O 3 and reduce the content of B 2 O3 The content of Li 2 O replaces [Na 2 O+CaO]. The results show that by designing the composition of the base glass, up to 11 mol% of MoO can be added to the borosilicate glass developed by the present invention. 3 The obtained solid body has no molybdate yellow phase precipitation, and the effect of improving molybdenum solubility is significant.

[0008] In order to achieve the above purpose, a group of borosilicate glass compositions are designed. The specific oxide content (mol%) range is shown in Table 2. It should be noted that B 2 O 3 With Al 2 O 3 The total amount remained unchanged at 19.78%, with an increase in Al 2 O 3 When the content is 2 O 3 The content of Li in the basic glass composition is reduced accordingly; 2 O、Na 2 The sum of O and CaO is 16.79%, and Na 2 O, CaO molar ratio 1.02 remains unchanged; or Na 2 O and CaO are both 0, and Li in the base 2 The highest O content is 16.79%.

[0009] The following steps are required to prepare borosilicate glass according to the composition given in Table 2:

[0010] (1) According to the molar content of each oxide in the basic glass composition, the raw materials required for preparing the glass are weighed accordingly. The specific raw materials and introduced oxides are: silica sand introduces SiO 2 ;Na 2 B 4 O 7 10H 2 O introduces Na 2 O and B 2 O 3 , such as B introduced by borax 2 O 3 If insufficient, use H 3 BO 3 Supplement, such as the introduction of Na 2 If O is insufficient, use Na 2 CO 3 Complement; Al(OH) 3 Introduction of Al 2 O 3 ; CaCO 3Introduction of CaO; ZnO Introduction of ZnO; Li 2 CO 3 Introducing Li 2 O; ZrO 2 Introducing ZrO 2 .

[0011] (2) The weighed raw materials are thoroughly mixed until uniform, and then placed in a suitable corundum crucible for melting.

[0012] (3) Place the crucible containing the batch material into a melting furnace, heat it to 1550°C at a rate of 5°C / min, and melt it at this temperature for 2 h.

[0013] (4) After melting, the glass liquid is cast onto a copper plate and allowed to cool freely to room temperature.

[0014] Table 2 Designed composition of borosilicate glass of the present invention (mol%)

[0015] Components <![CDATA[SiO 2 ]]> <![CDATA[Al 2 THE 3 ]]> <![CDATA[B 2 THE 3 ]]> <![CDATA[Na 2 The]]> CaO ZnO <![CDATA[Li 2 The]]> <![CDATA[ZrO 2 ]]> percentage 60.28 7-10 9.78-12.78 0-5.8 0-5.7 2.45 5.29-16.79 0.7

[0016] When preparing solidified glass, 1-11 mol% MoO is added on the basis of the designed basic glass oxide ratio. 3 , directly from MoO 3 The raw materials are introduced; each raw material is weighed according to step (1), and the remaining experimental steps are the same as (2)-(4). It should be noted that the experiment uses XRD and Raman spectroscopy technology to determine whether there is molybdate yellow phase precipitation in the solidified glass. The obtained part contains MoO 3 The XRD patterns and Raman spectra of the solidified glass (including samples of Examples 1-4 and Comparative Examples 1-3 within the protection scope of the present invention) are as follows: Figure 1 and Figure 2 As shown. Among them, Figure 1 The XRD curves corresponding to the four examples in the experiment have only one mantou peak spanning 15-35° 2θ, proving that no crystals have been precipitated in these four examples, while the XRD curves corresponding to the three comparative examples all have some sharp peaks, among which the strongest peak is located at 28.775° 2θ, from which it can be retrieved that CaMoO has been precipitated in the samples. 4 (PDF#29-0351) phase. Figure 2 The Raman spectra of the four samples in the examples are at 970 cm -1 There is a broad peak and 322cm -1 The weak peaks indicate that the four samples contain only free [MoO 4 ] 2- Without CaMoO 4Crystal; The Raman spectra of all the samples corresponding to Comparative Examples 1-3 are at 322, 389, 790, 845, 878 cm -1 There are sharp peaks, which indicates the presence of CaMoO in these samples. 4 Based on these two test results, it can be determined that when the solidified glass has no yellow phase precipitation, the maximum MoO 3 Amount. For example: Al 2 O 3 When the added MoO 3 The amount can reach 6 mol%; Al 2 O 3 When the maximum added MoO is 10 mol%, and there is no sodium oxide or calcium oxide in the glass, or the sum of the two is less than or equal to 3.5 mol%, 3 The amount can reach 11 mol%.

[0017] High-level radioactive liquid waste generated by the nuclear power industry poses a huge environmental risk and must be handled safely and securely. Glass solidification of high-level radioactive liquid waste is an internationally practical method, in which borosilicate glass is a widely used basic glass. However, the solubility of molybdenum in nuclear waste in borosilicate basic glass is low, which leads to the problem of yellow phase precipitation of molybdate in the solidified glass. The present invention obtains a basic glass with a high molybdenum inclusion rate by adjusting the composition of borosilicate glass. Specifically: First, Al 2 O 3 Gradually replace B 2 O 3 , and a maximum of 8 mol% MoO 3 Without producing the best composition of crystallization, Li 2 O replaces Na 2 O and CaO, in this process Na 2 The molar ratio of O to CaO remains unchanged, and a maximum of 11 mol% MoO can be added. 3 Borosilicate glass, which does not produce crystallization, improves the low inclusion rate of high-level radioactive nuclear waste during the glass solidification process.

[0018] Compared with the prior art, the present invention has a higher molybdenum solubility. In the borosilicate base glass, up to 11 mol% MoO can be added. 3 This allows the inclusion rate of high-level radioactive nuclear waste in borosilicate glass to be further increased. In addition, two situations occurred during the development of the glass composition of this patent. First, when MoO 3 When the addition amount is lower than the maximum solubility, there is neither Na 2 MoO 4 There is no CaMoO precipitation4 The glass is completely amorphous. 3 When the addition amount exceeds the maximum solubility, CaMoO will precipitate in the glass. 4 No Na will be precipitated 2 MoO 4 , CaMoO 4 It is not a water-soluble substance. Compared with Na 2 MoO 4 This water-soluble substance has little effect on the chemical stability of the glass solid body. Therefore, the borosilicate glass of the present invention has potential wide practical value. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The XRD patterns of the samples of the embodiments and comparative examples are shown in FIG.

[0020] Figure 2 The Raman spectra of the samples of the embodiments and comparative examples are shown in FIG. DETAILED DESCRIPTION

[0021] The present invention is further described below through specific examples. It should be understood that the following description is only for explaining the present invention and does not limit its content. Table 3 shows the oxide design composition of the base glasses of Examples 1-4 and Comparative Examples 1-3. The preparation of these borosilicate base glasses includes the following steps:

[0022] (1) According to the oxide contents given in Table 3, weigh the raw materials required for preparing glass, totaling 30 g. The specific raw materials and introduced oxides are: silica sand introduces SiO 2 ;Na 2 B 4 O 7 10H 2 O introduces Na 2 O and B 2 O 3 , such as B introduced by borax 2 O 3 If insufficient, use H 3 BO 3 Supplement, such as the introduction of Na 2 If O is insufficient, use Na 2 CO 3 Complement; Al(OH) 3 Introduction of Al 2 O 3 ; CaCO 3 Introduction of CaO; ZnO Introduction of ZnO; Li 2 CO 3 Introducing Li 2 O; ZrO2 Introducing ZrO 2 .

[0023] (2) The weighed raw materials are thoroughly mixed until uniform, and then placed in a suitable corundum crucible for melting.

[0024] (3) Place the crucible containing the batch material into a melting furnace, heat it to 1550°C at a rate of 5°C / min, and melt it at this temperature for 2 h.

[0025] (4) After melting, the glass liquid is cast onto a copper plate and allowed to cool freely to room temperature.

[0026] When preparing solidified glass, 1-11 mol% MoO is added on the basis of the designed basic glass oxide ratio. 3 , directly from MoO 3 The raw materials are introduced; the raw materials are weighed according to step (1), and the remaining experimental steps are the same as (2) to (4). The obtained solidified glass is subjected to XRD and Raman spectroscopy techniques to determine whether molybdate yellow phase is precipitated in the solidified glass.

[0027] Table 3 Basic glass design composition of the embodiments and comparative examples, added MoO 3 (mol%) / solidified body

[0028]

[0029]

[0030] To determine the maximum amount of MoO that can be added to the above base glass 3 Based on the designed composition in Table 3, different amounts of MoO 3 The MoO-containing 3 The solidified glass was confirmed to contain MoO by XRD and Raman spectroscopy analysis. 3 The results are as follows:

[0031] The base glass of Example 1 can be added with up to 6 mol% MoO 3 There is no yellow phase precipitation in the obtained solidified glass.

[0032] The base glass of Example 2 can be added with up to 8 mol% MoO 3 There is no yellow phase precipitation in the obtained solidified glass.

[0033] Comparative Example 1 Compared with Examples 1 and 2, the Al content in the base glass is 2 O 3 When the content is reduced to 5 mol%, 5 mol% MoO is added 3, a yellow phase has precipitated in the obtained solidified glass.

[0034] Comparative Example 2 Compared with Examples 1 and 2, the Al content in the base glass is 2 O 3 The content is reduced to 3.7 mol%, and 3 mol% MoO is added to the base glass. 3 , a yellow phase has precipitated in the obtained solidified glass.

[0035] The base glass of Example 3 can be added with up to 11 mol% MoO 3 There is no yellow phase precipitation in the obtained solidified glass.

[0036] The base glass of Example 4 can be added with up to 11 mol% MoO 3 , no yellow phase is precipitated in the obtained solidified glass. 2 The O content was reduced to 9.29 mol%, of which 11 mol% MoO 3 , a yellow phase has precipitated in the obtained solidified glass.

Claims

1. A borosilicate base glass for solidifying high-level nuclear waste, Features: The oxides in the glass and their molar contents are SiO 2 60.28%, Al 2 O 3 7-10%, B 2 O 3 9.78-12.78%, Na 2 O 0-5.8%, CaO 0-5.7%, ZnO2.45%, Li 2 O 5.29-16.79%, ZrO 2 0.7%.

2. The base glass according to claim 1, Features: Glass composition B 2 O 3 With Al 2 O 3 The total amount remained unchanged at 19.78%, with an increase in Al 2 O 3 When the content is 2 O 3 The content is reduced accordingly.

3. The base glass according to claim 1, Features: Composition of Li in glass 2 O、Na 2 The sum of O and CaO is 16.79%. 2 The molar ratio of O and CaO remains unchanged at 1.02, or the content of both is 0% at the same time. 2 The highest O content is 16.79%.

4. A method for preparing the base glass according to claim 1, Its characteristics are: The following steps are involved: (1) According to the content of each oxide in the glass composition, the raw materials required for preparing the glass are weighed accordingly. The specific raw materials and introduced oxides are: silica sand introduces SiO 2 ;Na 2 B 4 O 7 10H 2 O introduces Na 2 O and B 2 O 3 , such as B introduced by borax 2 O 3 If insufficient, use H 3 BO 3 Supplement, such as the introduction of Na 2 If O is insufficient, use Na 2 CO 3 Complement; Al(OH) 3 Introduction of Al 2 O 3 ; CaCO 3 Introduction of CaO; ZnO Introduction of ZnO; Li 2 CO 3 Introducing Li 2 O; ZrO 2 Introducing ZrO 2 ; (2) Mix the weighed raw materials thoroughly until they are uniform, and place them in a suitable corundum crucible to be melted; (3) Place the crucible containing the batch material into a melting furnace, heat it to 1550 °C at a rate of 5 °C / min, and melt it at this temperature for 2 h; (4) After melting, the glass liquid is cast onto a copper plate and allowed to cool freely to room temperature.

5. A MoO-containing 3 Borosilicate cured glass, Its characteristics are: Based on the composition of the base glass according to any one of claims 1 to 3, 6-11 mol% of MoO 3 .

6. A method for preparing the solidified glass according to claim 5, Its characteristics are: The following steps are involved: (1) According to the content of each oxide in the glass composition, the raw materials required for preparing the glass are weighed accordingly. The specific raw materials and introduced oxides are: silica sand introduces SiO 2 ;Na 2 B 4 O 7 10H 2 O introduces Na 2 O and B 2 O 3 , such as B introduced by borax 2 O 3 If insufficient, use H 3 BO 3 Supplement, such as the introduction of Na 2 If O is insufficient, use Na 2 CO 3 Complement; Al(OH) 3 Introduction of Al 2 O 3 ; CaCO 3 Introduction of CaO; ZnO Introduction of ZnO; Li 2 CO 3 Introducing Li 2 O; ZrO 2 Introducing ZrO 2, MoO 3 Introducing MoO 3 ; (2) Mix the weighed raw materials thoroughly until they are uniform, and place them in a suitable corundum crucible to be melted; (3) Place the crucible containing the batch material into a melting furnace, heat it to 1550 °C at a rate of 5 °C / min, and melt it at this temperature for 2 h; (4) After melting, the glass liquid is cast onto a copper plate and allowed to cool freely to room temperature.

Citation Information

Patent Citations

  • Method for confining a substance by vitrification

    CN101218182A

  • Glass composition for vitrifying flammable waste products and method for vitrifying flammable waste product using same

    CN105813999A

  • Glass solidified body capable of improving solubility of molybdenum element and preparation method of glass solidified body

    CN115583796A

  • Reducing agents for increasing dissolving capacity of molybdenum in borosilicate glass bodies and methods of use thereof

    CN118420217A

Cited By

  • Preparation method and application of power stack high-level liquid waste glass curing electric melting furnace starting glass