Nano antibacterial ceramic glaze and preparation method thereof
By using composite antibacterial agents coated with copper porous shell powder in ceramic glaze, the problem of insufficient antibacterial and antifouling properties of ceramic glaze is solved, and the excellent antibacterial and antifouling effects of ceramic products are achieved, and the application scope is broadened .
Patent Information
- Application Number
- CN202411179739.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-27
AI Technical Summary
Ordinary ceramic glaze has poor antibacterial and antifouling properties, which makes ceramic products prone to breeding bacteria and mold in humid environments, making it difficult to clean, limiting their application scope.
Porous shell powder is used as the matrix, copper is used as the antibacterial material, silicone oil and biomass alginic acid are used as the antifouling material. By covering the copper-loaded porous shell powder, a composite antimicrobial agent is generated and added to the ceramic glaze to improve antibacterial and antifouling performance.
It effectively improves the antibacterial and anti-fouling properties of ceramic products, avoids the growth of bacteria and mold, and broadens the application scope of ceramic products.
Smart Images

Figure CN119038877A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic glazes, and in particular to a nano antibacterial ceramic glaze and a preparation method thereof. Background Art
[0002] Ceramic products involve all aspects of people's lives, such as tableware, tea sets, washbasins, toilets, bathtubs, etc., and are an indispensable part of modern life. Among them, ceramic glaze is an important component of ceramic products. It is mainly made by applying glaze slurry made of minerals and other raw materials on the ceramic body, and after high-temperature firing, a colorless or colored glassy thin layer is formed on the surface of the ceramic body. The glaze can not only make the porcelain more beautiful and atmospheric, but also protect the surface of the ceramic body.
[0003] In recent years, with the improvement of people's living standards and the intensification of various competitions, the functional requirements for ceramic products are getting higher and higher. Functional ceramic products are mainly achieved by preparing functional glazes. Ordinary ceramic glazes do not have antibacterial properties. In humid environments such as kitchens and bathrooms, the glaze of ceramic products can easily become a breeding ground for microorganisms such as bacteria and mold, forming stains and bacterial communities that are difficult to remove, posing a threat to human health. In addition, scale, food residues, soap bubbles and other substances are easily attached to the concave and convex parts of the glaze or in the micropores under the action of various forces, causing pollution and difficulty in cleaning, which limits the application scope of ceramic products. Therefore, improving the antibacterial and anti-fouling properties of ceramic glazes is of great practical significance.
[0004] In the prior art, in order to improve the antibacterial and antifouling properties of ceramic glazes, most of the methods are to add substances with antibacterial and antifouling properties to the basic glaze, thereby giving the glaze good antibacterial and antifouling properties. For example, the invention patent with publication number CN109970341B discloses an antifouling and antibacterial ceramic glaze and a preparation method thereof. The invention adds an antibacterial agent composed of silver-doped zirconium oxide powder and diatomaceous earth loaded with a small amount of silver to the basic glaze, so that the fired ceramic can continuously and slowly release silver ions in water to achieve a continuous antibacterial effect. At the same time, an aqueous phosphoric acid solution and an aqueous yttrium nitrate solution are added to the glaze, so that the ceramic fired with the glaze has good hydrophobicity, thereby achieving an antifouling effect. Summary of the invention
[0005] The purpose of the present invention is to provide a nano antibacterial ceramic glaze and a preparation method thereof, which solves the following technical problems:
[0006] (1) Solved the problem of poor antibacterial performance of ordinary ceramic glazes;
[0007] (2) Solved the problem of poor anti-fouling performance of ordinary ceramic glazes.
[0008] The purpose of the present invention can be achieved by the following technical solutions:
[0009] A method for preparing a nano antibacterial ceramic glaze comprises the following steps:
[0010] SS1: Place the first glaze and the second glaze in a sand mill and grind them thoroughly until the glaze can pass through a sieve of 800-1000 meshes to obtain a compound glaze;
[0011] SS2: The compound glaze and sodium humate are stirred and mixed, and then aged at 35 to 45° C. for 15 to 25 days to obtain an aged glaze;
[0012] SS3: Add water to the aged glaze and adjust the specific gravity to 1.6-1.8 g / cm 3 , then add methyl cellulose and stir evenly to obtain ceramic glaze;
[0013] The first glaze comprises the following raw materials in parts by weight: 25 to 35 parts of quartz, 15 to 25 parts of potassium feldspar, 8 to 12 parts of calcite, 8 to 10 parts of kaolin, 5 to 8 parts of dolomite, 4 to 6 parts of pyrophyllite, 3 to 5 parts of barium carbonate, 4 to 5 parts of borax, and 5 to 7 parts of aluminum oxide;
[0014] The second glaze comprises the following raw materials in parts by weight: 8 to 12 parts of a composite antibacterial agent and 40 to 50 parts of a frit;
[0015] The composite antibacterial agent is prepared by coating silicone oil and alginic acid on the surface of copper-carrying porous shell powder.
[0016] Furthermore, in step SS1, the weight percentage of the second glaze in the compound glaze is 15-20%.
[0017] Furthermore, the preparation method of the first glaze comprises the following steps:
[0018] S1: adding quartz, potassium feldspar, calcite, kaolin, dolomite, pyrophyllite, barium carbonate, borax and alumina into a pool furnace, the temperature of the pool furnace is 1000-1200°C, the sintering time is 3-5h, the sintered materials are drained into a water pool through a pipeline, and crushed into particles by water flow, the temperature of the water flow is controlled at 20-50°C, and a composite material is obtained;
[0019] S2: Add the composite material into the ball mill for ball milling. After ball milling, pass through a 400-600 mesh screen, and then add water to adjust the specific gravity to 1.75-1.85 g / cm 3 , and obtain the first glaze.
[0020] Furthermore, in step S2, during the ball milling process, the mass ratio of the composite material, the balls and the water is 1:2-3:0.4-0.7, the ball milling speed is 400-600 rpm, and the ball milling time is 5-10 h.
[0021] Furthermore, the preparation method of the second glaze comprises the following steps:
[0022] Add the composite antibacterial agent and frit into the ball mill, mill for 20-40 minutes, then add water to adjust the specific gravity to 1.2-1.6 g / cm 3 , continue ball milling until the slurry can all pass through the 100-200 mesh sieve to obtain the second glaze.
[0023] Furthermore, the preparation method of the composite antibacterial agent comprises the following steps:
[0024] Ⅰ: treating the porous shell powder with an alkali solution to obtain a pretreated porous shell powder;
[0025] II: Disperse the copper salt in deionized water, add the pretreated porous shell powder under stirring at 60-70°C, act with ultrasound for 20-40 minutes, soak for 15-25 hours, discharge the material, and obtain the copper-loaded porous shell powder;
[0026] III: Under the action of tetrabutylammonium bromide, copper-loaded porous shell powder and end-epoxy silicone oil are added to dimethyl sulfoxide solution, ultrasonically dispersed for 20 to 30 minutes, the system temperature is raised to 60 to 70°C, kept warm for 4 to 8 hours, and the solid material is separated by filtration to obtain the intermediate material;
[0027] IV: Add the intermediate material, alginate and N,N-dimethylformamide into the reaction kettle, stir evenly, then add p-toluenesulfonic acid, keep stirring at 90-110°C for 3-6 hours, discharge the material, and obtain the composite antibacterial agent.
[0028] Furthermore, in step I, the alkali solution is any one of sodium hydroxide solution, calcium hydroxide solution or sodium hypochlorite solution.
[0029] Furthermore, in step II, the copper salt is any one of copper sulfate, copper nitrate or copper chloride.
[0030] Furthermore, in step III, the epoxy value of the epoxy-terminated silicone oil is 0.15 to 0.25 mol / 100 g.
[0031] A nano antibacterial ceramic glaze is made by adopting the preparation method.
[0032] Beneficial effects of the present invention: The present invention uses porous shell powder as a matrix, copper as an antibacterial material, silicone oil and biomass alginate as antifouling materials to prepare a composite antibacterial agent. On the one hand, the copper-loaded porous shell powder is coated with silicone oil and biomass alginate, which can effectively prevent copper ions from escaping from the pores during the preparation of ceramic products, resulting in waste of raw materials and reduced antibacterial performance. On the other hand, during the calcination process of ceramic glaze, silicone oil is used as a source of silicon elements, and biomass alginate is used to provide the required oxygen source. The two react at high temperature to generate silicon oxygen. The low surface energy silicon oxide has good hydrophobic properties, making it difficult for water molecules to approach its surface and penetrate into the interior, thereby effectively improving the anti-fouling properties of the ceramic glaze. In addition, after calcination, a tiny pore structure is formed on the surface of the copper-loaded porous shell powder. During the long-term use of ceramic products, the antibacterial material stored in the pores can be continuously released to achieve a slow-release antibacterial effect, thereby giving the ceramic products excellent antibacterial properties, avoiding the growth of bacteria, mold and other microorganisms on the ceramic glaze, posing a threat to human health, and broadening the application range of ceramic products.
[0033] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.
[0035] Figure 1 It is the infrared spectrum test diagram of the intermediate material and the composite antibacterial agent of the present invention. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] The preparation methods of the composite antibacterial agents in the following examples and comparative examples of the present invention are as follows:
[0038] Preparation of composite antibacterial agent
[0039] Ⅰ: 5g of porous shell powder is placed in a sodium hydroxide solution with a mass fraction of 4% and soaked for 24 hours, the material is filtered, the solid sample is collected, washed, and dried to obtain the pretreated porous shell powder;
[0040] Ⅱ: Disperse 2g of copper sulfate in deionized water, add 5g of pretreated porous shell powder under stirring at 65℃, act with ultrasound for 30min, soak for 20h, discharge, wash and dry to obtain copper-loaded porous shell powder;
[0041] The copper content in the copper-loaded porous shell powder was tested using a Z-5000 atomic absorption spectrometer (AAS). The test showed that the mass fraction of copper in the prepared copper-loaded porous shell powder was 5.16%.
[0042] III: Under nitrogen protection, 5 g of copper-loaded porous shell powder was added to a dimethyl sulfoxide solution, and ultrasonic dispersion was performed for 25 min. 2.6 g of terminal epoxy silicone oil with an epoxy value of 0.2 mol / 100 g and 0.1 g of tetrabutylammonium bromide were added. The system temperature was raised to 65°C under stirring conditions, and the temperature was kept for 6 h. The solid material was separated by filtration, and the intermediate material was obtained after washing and vacuum drying.
[0043] IV: Add 5 g of the intermediate material and N,N-dimethylformamide to a nitrogen-protected reactor, stir mechanically, then add 2.8 g of alginate and 0.1 g of p-toluenesulfonic acid, turn on the heating until the temperature in the reactor reaches 100°C, keep stirring for 5 hours, wait for the material to cool naturally, separate the solid material by centrifugation, wash the solid material, and vacuum dry to obtain a composite antibacterial agent.
[0044] The intermediate material and the composite antimicrobial agent were analyzed by infrared spectroscopy using a Vertex 70 Fourier transform infrared spectrometer produced by Bruker, Germany. The analysis results are shown in Figure 1 ,Depend on Figure 1 It can be seen that in the infrared spectrum of the intermediate material, 3285cm -1 The absorption peak of hydroxyl group OH appears at 1346 cm -1 The absorption peak of CN appears at 3421cm -1 The absorption peak of NH appears at 1020cm -1 The absorption peak of Si-O appears at 1759cm -1 The absorption peak of the ester group C=O appears at 1350cm -1 The absorption peak of CN appears at 3410 cm -1 The absorption peak of NH appears at 1025cm -1 The absorption peak of Si-O appears at
[0045] It can be inferred that the principle of the above scheme is: use sodium hydroxide solution to remove the stratum corneum of porous shell powder to obtain pretreated porous shell powder, under the action of ultrasound, copper ions interact with porous shell powder, and copper ions will flow into the pores of shell powder, and at the same time, water is used as the medium to prepare copper-loaded porous shell powder by immersion exchange method, and then under the action of tetrabutylammonium bromide, the active groups in the copper-loaded porous shell powder can react with the epoxy groups in the terminal epoxy silicone oil structure to undergo a ring-opening reaction, thereby introducing active hydroxyl groups produced by the ring-opening reaction into the copper-loaded porous shell powder to obtain an intermediate material, and under the action of p-toluenesulfonic acid, the active hydroxyl groups in the intermediate material structure can react with the carboxyl groups in the alginate structure to obtain a composite antibacterial agent.
[0046] Example 1
[0047] Step 1: Preparation of the first glaze
[0048] S1: 25g of quartz, 15g of potassium feldspar, 8g of calcite, 8g of kaolin, 5g of dolomite, 4g of pyrophyllite, 3g of barium carbonate, 4g of borax, and 5g of alumina are added to a pool furnace. The temperature of the pool furnace is 1000°C and the sintering time is 3h. The sintered material is drained into a water pool through a pipeline and crushed into particles by water flow. The temperature of the water flow is controlled at 20°C to obtain a composite material.
[0049] S2: Add the composite material into the ball mill for ball milling. During the ball milling process, the mass ratio of the composite material, ball and water is 1:2:0.4, the ball milling speed is 400rpm, the ball milling time is 5h, and after ball milling, it is passed through a 400-mesh sieve, and then water is added to adjust the specific gravity to 1.75g / cm 3 , obtaining a first glaze;
[0050] Step 2: Preparation of the second glaze
[0051] 8g of composite antibacterial agent and 40g of frit were added to the ball mill and milled for 20min, then water was added to adjust the specific gravity to 1.2g / cm 3 , continue ball milling until the slurry can all pass through a 100-mesh sieve to obtain a second glaze;
[0052] Step 3: Preparation of ceramic glaze
[0053] SS1: The first glaze and the second glaze are placed in a sand mill and fully ground until the glaze can pass through a sieve of 800 meshes, thereby obtaining a compound glaze, wherein the weight percentage of the second glaze in the compound glaze is 15%;
[0054] SS2: The compound glaze and sodium humate are stirred and mixed, wherein the addition amount of the sodium humate is 0.13% of the solid mass in the compound glaze, and then aged at 35° C. for 15 days to obtain an aged glaze;
[0055] SS3: Add water to the aged glaze and adjust the specific gravity to 1.6g / cm 3 , and then add methyl cellulose, wherein the amount of methyl cellulose added is 0.04% of the solid mass in the aged glaze, and stir evenly to obtain a ceramic glaze.
[0056] Example 2
[0057] Step 1: Preparation of the first glaze
[0058] S1: 30g quartz, 20g potassium feldspar, 10g calcite, 9g kaolin, 7g dolomite, 5g pyrophyllite, 4g barium carbonate, 4.5g borax, and 6g alumina are added to a pool furnace. The temperature of the pool furnace is 1100°C and the sintering time is 4h. The sintered material is drained into a water pool through a pipeline and crushed into particles by water flow. The temperature of the water flow is controlled at 35°C to obtain a composite material.
[0059] S2: Add the composite material into the ball mill for ball milling. During the ball milling process, the mass ratio of the composite material, ball and water is 1:2.5:0.5, the ball milling speed is 500rpm, the ball milling time is 8h, and after ball milling, it is passed through a 500-mesh sieve, and then water is added to adjust the specific gravity to 1.8g / cm 3 , obtaining a first glaze;
[0060] Step 2: Preparation of the second glaze
[0061] Add 10g of the composite antibacterial agent and 45g of the frit into the ball mill, mill for 30min, and then add water to adjust the specific gravity to 1.4g / cm 3 , continue ball milling until the slurry can all pass through a 150-mesh sieve to obtain a second glaze;
[0062] Step 3: Preparation of ceramic glaze
[0063] SS1: The first glaze and the second glaze are placed in a sand mill and fully ground until the glaze can pass through a 900-mesh sieve to obtain a compound glaze, wherein the weight percentage of the second glaze in the compound glaze is 18%;
[0064] SS2: The compound glaze and sodium humate are stirred and mixed, wherein the addition amount of the sodium humate is 0.14% of the solid mass in the compound glaze, and then aged at 40° C. for 20 days to obtain an aged glaze;
[0065] SS3: Add water to the aged glaze and adjust the specific gravity to 1.7g / cm 3 , and then add methyl cellulose, wherein the amount of methyl cellulose added is 0.05% of the solid mass in the aged glaze, and after stirring evenly, a ceramic glaze is obtained.
[0066] Example 3
[0067] Step 1: Preparation of the first glaze
[0068] S1: 35g of quartz, 25g of potassium feldspar, 12g of calcite, 10g of kaolin, 8g of dolomite, 6g of pyrophyllite, 5g of barium carbonate, 5g of borax, and 7g of alumina are added to a pool furnace. The temperature of the pool furnace is 1200°C and the sintering time is 5h. The sintered material is drained into a water pool through a pipeline and crushed into particles by water flow. The temperature of the water flow is controlled at 50°C to obtain a composite material.
[0069] S2: Add the composite material into the ball mill for ball milling. During the ball milling process, the mass ratio of the composite material, ball and water is 1:3:0.7, the ball milling speed is 600rpm, the ball milling time is 10h, and after ball milling, it is passed through a 600-mesh sieve, and then water is added to adjust the specific gravity to 1.85g / cm 3 , obtaining a first glaze;
[0070] Step 2: Preparation of the second glaze
[0071] Add 12g of composite antibacterial agent and 50g of frit into the ball mill, mill for 40min, then add water to adjust the specific gravity to 1.6g / cm 3 , continue ball milling until the slurry can all pass through a 200-mesh sieve to obtain a second glaze;
[0072] Step 3: Preparation of ceramic glaze
[0073] SS1: The first glaze and the second glaze are placed in a sand mill and fully ground until the glaze can pass through a 1000-mesh sieve to obtain a compound glaze, wherein the weight percentage of the second glaze in the compound glaze is 20%;
[0074] SS2: The compound glaze and sodium humate are stirred and mixed, wherein the addition amount of the sodium humate is 0.15% of the solid mass in the compound glaze, and then aged at 45° C. for 25 days to obtain an aged glaze;
[0075] SS3: Add water to the aged glaze and adjust the specific gravity to 1.8g / cm 3 , and then add methyl cellulose, wherein the amount of methyl cellulose added is 0.06% of the solid mass in the aged glaze, and after stirring evenly, a ceramic glaze is obtained.
[0076] Comparative Example 1
[0077] Step 1: Preparation of the first glaze
[0078] S1: 30g quartz, 20g potassium feldspar, 10g calcite, 9g kaolin, 7g dolomite, 5g pyrophyllite, 4g barium carbonate, 4.5g borax, 6g alumina, 10g nano copper oxide, and 45g frit are added to a pool furnace. The temperature of the pool furnace is 1100°C and the sintering time is 4h. The sintered material is drained into a water pool through a pipeline and crushed into particles by water flow. The temperature of the water flow is controlled at 35°C to obtain a composite material.
[0079] S2: Add the composite material into the ball mill for ball milling. During the ball milling process, the mass ratio of the composite material, ball and water is 1:2.5:0.5, the ball milling speed is 500rpm, the ball milling time is 8h, and after ball milling, it is passed through a 500-mesh sieve, and then water is added to adjust the specific gravity to 1.8g / cm 3 , obtaining a first glaze;
[0080] Step 2: Preparation of ceramic glaze
[0081] SS1: Place the first glaze in a sand mill and grind it thoroughly until the glaze can pass through a 900-mesh sieve to obtain a compound glaze;
[0082] SS2: The compound glaze and sodium humate are stirred and mixed, wherein the addition amount of the sodium humate is 0.14% of the solid mass in the compound glaze, and then aged at 40° C. for 20 days to obtain an aged glaze;
[0083] SS3: Add water to the aged glaze and adjust the specific gravity to 1.7g / cm 3 , and then add methyl cellulose, wherein the amount of methyl cellulose added is 0.05% of the solid mass in the aged glaze, and after stirring evenly, a ceramic glaze is obtained.
[0084] Performance testing:
[0085] A ceramic body of 15 cm×15 cm×8 mm was placed in a kiln, calcined at 700°C for 4 hours, and cooled. The ceramic glazes prepared in Examples 1 to 3 of the present invention and Comparative Example 1 were then evenly coated on the surface of the calcined ceramic body to obtain a glazed body. The glazed body was calcined at 1300°C for 5 hours, and a ceramic sample was obtained after cooling.
[0086] According to JC / T 897-2014 "Antibacterial Performance of Antibacterial Ceramic Products", the antibacterial performance of ceramic samples was tested, and the test bacteria were Escherichia coli and Staphylococcus aureus; the water contact angle of the ceramic sample surface was tested using a JC2000D4 contact angle meter to determine the antifouling performance of the ceramic sample. The specific test results are shown in the table below:
[0087]
[0088] From the test results in the above table, it can be seen that the antibacterial rates of the ceramic samples prepared in Examples 1 to 3 against Escherichia coli and Staphylococcus aureus are greater than 99%, and the water contact angles are greater than 120°, so they all have good antibacterial and anti-fouling properties; the ceramic sample prepared in Comparative Example 1 is coated on the surface of the ceramic embryo only by directly adding the first glaze of nano-copper oxide. Compared with the examples, the antibacterial and anti-fouling properties of the ceramic sample are poor.
[0089] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing a nano antibacterial ceramic glaze, characterized in that: The following steps are involved: SS1: Place the first glaze and the second glaze in a sand mill and grind them thoroughly until the glaze can pass through a sieve of 800-1000 meshes to obtain a compound glaze; SS2: The compound glaze and sodium humate are stirred and mixed, and then aged at 35 to 45° C. for 15 to 25 days to obtain an aged glaze; SS3: Add water to the aged glaze and adjust the specific gravity to 1.6-1.8 g / cm 3 , then add methyl cellulose and stir evenly to obtain ceramic glaze; The first glaze comprises the following raw materials in parts by weight: 25 to 35 parts of quartz, 15 to 25 parts of potassium feldspar, 8 to 12 parts of calcite, 8 to 10 parts of kaolin, 5 to 8 parts of dolomite, 4 to 6 parts of pyrophyllite, 3 to 5 parts of barium carbonate, 4 to 5 parts of borax, and 5 to 7 parts of aluminum oxide; The second glaze comprises the following raw materials in parts by weight: 8 to 12 parts of a composite antibacterial agent and 40 to 50 parts of a frit; The composite antibacterial agent is prepared by coating silicone oil and alginic acid on the surface of copper-carrying porous shell powder.
2. The method for preparing a nano antibacterial ceramic glaze according to claim 1, characterized in that: In step SS1, the weight percentage of the second glaze in the compound glaze is 15-20%.
3. The method for preparing a nano antibacterial ceramic glaze according to claim 1, characterized in that: The preparation method of the first glaze comprises the following steps: S1: adding quartz, potassium feldspar, calcite, kaolin, dolomite, pyrophyllite, barium carbonate, borax and alumina into a pool furnace, the temperature of the pool furnace is 1000-1200°C, the sintering time is 3-5h, the sintered materials are drained into a water pool through a pipeline, and crushed into particles by water flow, the temperature of the water flow is controlled at 20-50°C, and a composite material is obtained; S2: Add the composite material into the ball mill for ball milling. After ball milling, pass through a 400-600 mesh screen, and then add water to adjust the specific gravity to 1.75-1.85 g / cm 3 , and obtain the first glaze.
4. The method for preparing a nano antibacterial ceramic glaze according to claim 3, characterized in that: In step S2, during the ball milling process, the mass ratio of the composite material, the ball and the water is 1:2-3:0.4-0.7, the ball milling speed is 400-600 rpm, and the ball milling time is 5-10 hours.
5. The method for preparing a nano antibacterial ceramic glaze according to claim 1, characterized in that: The preparation method of the second glaze comprises the following steps: Add the composite antibacterial agent and frit into the ball mill, mill for 20-40 minutes, then add water to adjust the specific gravity to 1.2-1.6 g / cm 3 , continue ball milling until the slurry can all pass through the 100-200 mesh sieve to obtain the second glaze.
6. The method for preparing a nano antibacterial ceramic glaze according to claim 1, characterized in that: The preparation method of the composite antibacterial agent comprises the following steps: Ⅰ: treating the porous shell powder with an alkali solution to obtain a pretreated porous shell powder; II: Disperse the copper salt in deionized water, add the pretreated porous shell powder under stirring at 60-70°C, act with ultrasound for 20-40 minutes, soak for 15-25 hours, discharge the material, and obtain the copper-loaded porous shell powder; III: Under the action of tetrabutylammonium bromide, copper-loaded porous shell powder and end-epoxy silicone oil are added to dimethyl sulfoxide solution, ultrasonically dispersed for 20 to 30 minutes, the system temperature is raised to 60 to 70°C, kept warm for 4 to 8 hours, and the solid material is separated by filtration to obtain the intermediate material; IV: Add the intermediate material, alginate and N,N-dimethylformamide into the reaction kettle, stir evenly, then add p-toluenesulfonic acid, keep stirring at 90-110°C for 3-6 hours, discharge the material, and obtain the composite antibacterial agent.
7. The method for preparing a nano antibacterial ceramic glaze according to claim 6, characterized in that: In step I, the alkali solution is any one of sodium hydroxide solution, calcium hydroxide solution or sodium hypochlorite solution.
8. The method for preparing a nano antibacterial ceramic glaze according to claim 6, characterized in that: In step II, the copper salt is any one of copper sulfate, copper nitrate or copper chloride.
9. The method for preparing a nano antibacterial ceramic glaze according to claim 6, characterized in that: In step III, the epoxy value of the epoxy-terminated silicone oil is 0.15 to 0.25 mol / 100 g.
10. A nano antibacterial ceramic glaze, characterized in that: The method is as claimed in claim 1.
Citation Information
Patent Citations
Antifouling and antibacterial ceramic glaze and its preparation method
CN109970341B
Scale-inhibition function sanitary ceramics and preparation method thereof
CN105669252A
High-heat resistant antibacterial glaze powder and preparation method thereof
CN107188419A
Slow-release chlorine dioxide composite antibacterial material and preparation method of composite antibacterial material
CN111528223A
High-biocompatibility coating liquid and hydrophobic antibacterial gauze dressing
CN115957367A
Cited By
Efficient antibacterial ceramic glaze and preparation process thereof
CN118851570A
A high-efficiency antibacterial ceramic glaze and its preparation process