Dimethylene pyridine bridged amino bisphenol oxygen alkali metal complex as well as preparation method and application thereof
By designing dimethylene pyridine-bridged bisamophenoloxy alkali metal complex, the problem of highly toxic ligands in existing alkali metal catalysts is solved, and high activity and high controllability lactide polymerization is achieved, suitable for Industrialized production.
Patent Information
- Application Number
- CN202411143775.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-20
Smart Images

Figure CN119039215A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a type of dimethylene pyridine-bridged bisaminophenoloxy alkali metal complex and application of the complex in lactone polymerization. Background Art
[0002] In order to solve the problem of fossil energy shortage, people hope to use suitable substitutes to replace petroleum-derived plastics. Because polylactide (PLA, also known as polylactic acid) has excellent biodegradability and biocompatibility, and because it has similar physical and mechanical properties to some polyolefin products, it has been widely studied and applied in various fields such as biomedicine in the past two decades. Used polylactide products can be remelted, recycled and reused, or composted, and degraded by nature into carbon dioxide and water that are non-toxic and harmless to the environment. Compared with petroleum-based polyolefin products, it has significant advantages in sustainable production and post-processing.
[0003] The performance of polylactide is determined by its microstructure. The ring-opening polymerization of different types of lactide monomers such as levorotatory lactide (L-LA), dextrorotatory lactide (D-LA), meso-lactide (meso-LA) and racemic lactide (rac-LA) catalyzed by metal complexes can obtain polylactides with various microstructures. Random polylactide is amorphous, brittle, non-stretchable, and degrades quickly; isotactic polylactide or isotactic block polylactide is a semi-crystalline material with a high melting point, good thermodynamic properties and stretchability. Therefore, the development of new metal complex catalysts to achieve high-activity and high-controllability synthesis of polylactides with different microstructures has become the main research direction in this field.
[0004] Among the metal complex catalysts studied so far, alkali metal complexes have attracted attention due to their high catalytic activity for the polymerization of lactide. In 2011, the Mountford group synthesized a [OOO]-type tridentate bisphenoloxy potassium complex, which has high activity and controllability for the ring-opening polymerization of rac-LA. At room temperature, dichloromethane, and the addition of 1 equivalent of benzyl alcohol, 300 equivalents of rac-LA can be catalyzed to polymerize for 5 minutes to completely convert the monomer (Inorg. Chem., 2011, 50, 3589–3595). In 2015, the Francesca group synthesized a tetranuclear alkali metal complex, which can catalyze the polymerization of 250 equivalents of rac-LA for 3 minutes at room temperature, tetrahydrofuran, and the addition of 1 equivalent of benzyl alcohol to completely convert the monomer, and the polymerization has good controllability (Dalton Trans., 2015, 44, 20216-20231). In 2015, the Cano group synthesized iminophenoloxy alkali metal complexes, among which the potassium complex showed high catalytic activity for the ring-opening polymerization of rac-LA. At room temperature, 1 equivalent of benzyl alcohol was added as an initiator to catalyze the polymerization of 100 equivalents of rac-LA, and the monomer conversion rate reached 99% in 30 seconds. Under the same conditions, the lithium complex was less active, and it took 45 minutes to completely convert 100 equivalents of monomers (Organometallics, 2015, 34, 477–487). In 2014, the Wu group synthesized purine monophenoloxy sodium and potassium complexes containing crown ether structures. This type of complex has high catalytic activity for the polymerization of racemic lactide. At room temperature, 10 equivalents of benzyl alcohol were added to catalyze the polymerization of 500 equivalents of rac-LA, and the conversion was complete in just 2 minutes (Macromolecules, 2014, 47, 7789-7796). In 2015, Wu's group synthesized a trityl-substituted phenoloxy potassium complex with a crown ether structure as an auxiliary ligand, which has high catalytic activity for rac-LA polymerization. In toluene at room temperature, 10 equivalents of benzyl alcohol were added to catalyze the polymerization of 1000 equivalents of rac-LA, and the polymerization was completely converted in just 1 minute, and the polymerization was well controlled (Catal. Sci. Technol., 2016, 6, 515–520). In 2017, Wang's group synthesized an iminophenoloxy crown ether potassium complex, which has high catalytic activity at room temperature. In toluene at room temperature, 1 equivalent of benzyl alcohol was added to catalyze the polymerization of 100 equivalents of rac-LA, and the monomers were completely converted in 1 minute (RSC Adv., 2017, 7, 24055–24063).
[0005] People have made some breakthroughs in the field of lactide polymerization research. By effectively designing the structure of metal complex catalysts, polylactide with a certain degree of regularity has been obtained. Most alkali metal complexes with high activity for lactide ring-opening polymerization contain crown ethers as auxiliary ligands, but crown ethers are toxic and not suitable for industrial production. Therefore, the development of highly active and biocompatible alkali metal complexes is of great significance for the industrial application of lactide ring-opening polymerization. Summary of the invention
[0006] One of the purposes of the present invention is to disclose a type of dimethylene pyridine-bridged bisaminophenoloxy alkali metal complex.
[0007] The second object of the present invention is to disclose a method for preparing a type of dimethylene pyridine-bridged bisaminophenoloxy alkali metal complex.
[0008] The third object of the present invention is to disclose the application of a type of dimethylene pyridine-bridged bisaminophenoloxy alkali metal complex in lactone polymerization.
[0009] The technical concept of the present invention is as follows: Salan-type aminobisphenol ligands have the characteristics of easy raw material availability, simple synthesis, and adjustable structure. By changing the substituents to adjust the electronic effect and steric effect, the catalytic activity and stereoselectivity of the metal complex can be effectively regulated. However, it has only four coordination sites, and the small number of coordination sites in alkali metal catalysts is not conducive to stabilizing the metal center. The present invention contemplates introducing a pyridine group on the basis of the Salan ligand, utilizing its five chelating coordination sites to stabilize the alkali metal center and applying it to the polymerization of lactide. By changing the substituents in the ligand, the Lewis acidity of the metal center and the steric hindrance around the metal center can be adjusted, so as to achieve high activity and high controllability of the alkali metal complex to catalyze the ring-opening polymerization of racemic lactide.
[0010] The present invention provides a dimethylenepyridine-bridged bisaminophenol ligand (I) and an alkali metal complex (II) thereof, characterized in that they have the following general formula:
[0011]
[0012] In formula (I) and (II):
[0013] R 1 ~R 2 Represents C 1 ~C 20 Straight chain, branched chain or cyclic alkyl group, C 7 ~C 30 a mono- or poly-aryl-substituted alkyl group, or a halogen;
[0014] R 3 Represents C 1 ~C20 Straight chain, branched chain or cyclic alkyl group, C 7 ~C 30 A mono- or poly-aryl-substituted alkyl group, C 6 ~C 18 The aromatic group;
[0015] n is 0 or 1;
[0016] M represents Na and K.
[0017] More specifically, in formula (I) and (II), R 1 ~R 2 Preferably C 1 ~C 8 Straight chain, branched chain or cyclic alkyl group, C 7 ~C 20 mono- or poly-aryl-substituted alkyl, or halogen; R 3 Preferably C 1 ~C 8 Straight chain, branched chain or cyclic alkyl group, C 7 ~C 20 A mono- or poly-aryl-substituted alkyl group, C 6 ~C 12 The aromatic group.
[0018] Preferably, in formula (I) and (II), R 1 ~R 2 are methyl, isopropyl, tert-butyl, cumyl, and trityl; R 3 It is methyl, ethyl, tert-butyl, n-butyl, cyclopentyl, cyclohexyl, benzyl, and phenyl.
[0019] The preferred structure of the dimethylene pyridine-bridged bisaminophenol ligand is:
[0020]
[0021]
[0022] The preferred structure of the dimethylene pyridine bridged bisaminophenoloxy alkali metal complex is:
[0023]
[0024]
[0025] The method for preparing the dimethylenepyridine-bridged bisaminophenol ligand (I) and its alkali metal complex (II) of the present invention comprises the following steps:
[0026]
[0027] The 2-bromomethyl-4,6-disubstituted phenol represented by formula (III) and the 2,6-di(substituted aminomethyl)pyridine represented by formula (IV) are reacted in an organic medium in the presence of an alkylamine at a reaction temperature of 0 to 90° C. for a reaction time of 2 to 72 hours, and then a dimethylenepyridine-bridged bisaminophenol ligand compound (I) is collected from the reaction product;
[0028] Optionally, a dimethylpyridine-bridged bisaminophenol ligand compound represented by formula (I) is reacted with a metal hydride in an organic medium at a reaction temperature of 0 to 100° C. for a reaction time of 2 to 24 hours, and then a dimethylpyridine-bridged bisaminophenoloxy alkali metal complex (II) is collected from the reaction product;
[0029] In the above preparation method, the substituent R 1 ~R 3 The groups are consistent with the corresponding groups of the dimethylenepyridine-bridged bisaminophenol ligand (I) and its alkali metal complex (II) as described in the present invention;
[0030] The alkylamine is triethylamine, tributylamine or triisopropylamine;
[0031] Metal hydrides MH are NaH, KH;
[0032] The molar ratio of the dimethylpyridine-bridged bisaminophenol ligand compound (I) to the metal hydride is 1:2.0 to 4.0; preferably 1:2.2 to 2.5;
[0033] The organic medium is selected from one or more of tetrahydrofuran, ether, toluene, benzene, petroleum ether and n-hexane.
[0034] In the preparation method of the dimethylenepyridine-bridged bisaminophenol ligand (I) of the present invention, the synthesis of 2-bromomethyl-4,6-disubstituted phenol shown in formula (III) can be obtained by reacting 2,4-substituted phenol with paraformaldehyde in 33% hydrogen bromide acetic acid solution according to the following route (Inorg. Chem., 2002, 41, 3656; J. Org. Chem., 1994, 59, 1939):
[0035]
[0036] In the preparation method of the dimethylenepyridine bridged bisaminophenol ligand (I) of the present invention, the synthesis of 2,6-di(substituted aminomethyl)pyridine shown in formula (IV) can be carried out according to the following route, namely, 2,6-pyridinedicarboxaldehyde is obtained by oxidation of 2,6-pyridine dimethanol, and then reacted with a primary amine R 3 NH 2Reaction, reduction with a reducing agent to obtain:
[0037]
[0038] The synthesis of 2,6-di(substituted aminomethyl)pyridine shown in formula (IV) can also be carried out according to the following method (Nat. Commun., 2021, 12, 1572), that is, 2,6-pyridine dimethanol is reacted with hydrogen bromide to obtain 2,6-dibromomethylpyridine, which is then reacted with a primary amine R 3 NH 2 Reaction, reduction with a reducing agent to obtain:
[0039]
[0040] In the above preparation method, the reducing agent is a reducing agent commonly used in organic reactions, such as sodium borohydride and lithium aluminum hydride.
[0041] The dimethylene pyridine-bridged bisaminophenoloxy alkali metal complex of the present invention is a highly efficient lactone polymerization catalyst and can be used for the polymerization reaction of L-lactide, D-lactide, rac-lactide and meso-lactide, and the polymerization mode is solution polymerization and melt polymerization.
[0042] Using the dimethylene pyridine-bridged bisaminophenoloxy alkali metal complex of the present invention as a catalyst, lactide is polymerized at -70 to 250°C, preferably -70 to 180°C, and most preferably -70 to 140°C; during the polymerization, the molar ratio of the catalyst to the monomer is 1:1 to 10000, preferably 1:20 to 5000, and most preferably 1:100 to 3000.
[0043] The dimethylene pyridine bridged bisaminophenoloxy alkali metal complex of the present invention is used as a catalyst. When catalyzing the polymerization of lactone, a certain amount of alcohol can be added as a chain transfer agent to control the molecular weight of the obtained polymer. During the polymerization, the molar ratio of the catalyst to the alcohol and the lactide monomer is 1:1-50:1-10000, preferably 1:1-20:20-5000, and most preferably 1:1-10:100-3000; the alcohol is C 1 ~C 10 Alkyl alcohols with straight chain, branched chain or cyclic structure, C 7 ~C 20 The mono- or poly-aryl-substituted alkyl alcohol is preferably isopropanol or benzyl alcohol.
[0044] When the dimethylenepyridine-bridged bisaminophenoloxy alkali metal complex of the present invention is used as a catalyst to catalyze the polymerization of lactone, a solvent may also be included. The solvent is preferably one or more of toluene, tetrahydrofuran, dichloromethane, n-hexane, petroleum ether, m-xylene, o-xylene, mesitylene, and trichlorobenzene. Specifically, the solvent may be one, two, three, four, or five.
[0045] The catalyst provided by the present invention is easy to prepare and has stable properties; at the same time, the catalyst provided by the present invention has high catalytic activity and controllability in the process of catalyzing the ring-opening polymerization of lactide, and highly controllable polymerization can be achieved by regulating the ligand structure and polymerization conditions. The present invention is further described below through specific embodiments, but the present invention is not limited thereto. DETAILED DESCRIPTION
[0046] Example 1
[0047] Ligand L 1 H 2 Synthesis
[0048] (1) Synthesis of 2,6-pyridinedicarboxaldehyde
[0049]
[0050] Under argon protection, 2,6-pyridine dimethanol (5.40 g, 38.8 mmol), 40 mL of 1,4-dioxane and selenium dioxide (4.44 g, 43.5 mmol) were added to the bottle in sequence, and heated to 110 ° C for 5 h. The reaction mixture was filtered to obtain a yellow solution, which was concentrated to slightly turbidity, and 15 mL of petroleum ether was slowly added and placed in a refrigerator for crystallization. The obtained solid was vacuum-evacuated to dryness to obtain a light brown 2,6-pyridine dicarboxaldehyde solid (4.83 g, 90%).
[0051] 1 H NMR (400 MHz, CDCl 3 ):δ10.15(s,2H,-CHO),8.17(d, 3 J=7.6Hz,2H,PyH),8.08(t, 3 J = 7.6 Hz, 1H, PyH).
[0052] (2) Synthesis of 2,6-bis(benzylaminomethyl)pyridine
[0053]
[0054] Add 2,6-pyridinedicarboxaldehyde (1.35 g, 10.0 mmol) and 30 mL of methanol to a 100 mL round-bottom flask, add benzylamine (2.2 mL, 20 mmol), and heat under reflux for 12 hours. After cooling, slowly add NaBH4 (1.51 g, 40.0 mmol). The temperature was raised to 70°C and the reaction was continued for 12 h. Methanol was removed in vacuo, and a saturated potassium carbonate solution was added to quench the reaction. The mixture was poured into a separatory funnel, extracted with dichloromethane, dried over anhydrous sodium sulfate, filtered, and the solvent was removed from the filtrate to obtain 2,6-bis(benzylaminomethyl)pyridine (3.11 g, 98%).
[0055] 1 H NMR (400 MHz, CDCl 3 ):δ7.61(t, 3 J=7.6Hz,1H,Py-H),7.40–7.30(m,8H,Ar-Hand Ph-H),7.25(tt, 3 J=7.0Hz, 4 J=1.5Hz,2H,Ar-H),7.19(d, 3 J=7.6Hz,2H,Py-H),3.93(s,4H,Py-CH 2 -),3.86(s,4H,Ph-CH 2 -),2.39(br s,2H,-NH-).
[0056] (3) Ligand L 1 H 2 Synthesis
[0057]
[0058] Add 2,6-di(benzylaminomethyl)pyridine (3.11 g, about 9.82 mmol) and 60 mL of dichloromethane to a 100 mL round-bottom flask, and then add 11 mL of triethylamine. Add 2-bromomethyl-4,6-di-tert-butylphenol (6.00 g, 20.0 mmol) to form a yellow reaction solution. React for 24 hours. After completion, pour the reaction solution into 50 mL of water, shake and separate the liquids, extract with dichloromethane, combine the organic phases and wash with water, add anhydrous sodium sulfate to dry, filter, and drain to obtain a yellow oil. Recrystallize from dichloromethane / methanol to obtain 5.89 g of a light yellow solid with a yield of 78%.
[0059] 1 H NMR (400 MHz, CDCl 3 ):δ10.77(br s,2H,ArOH),7.60(t, 3 J=7.7Hz,1H,Py-H),7.35(d, 3 J=7.3Hz,4H,Ph-H),7.29(t, 3 J=7.3Hz,4H,Ph-H),7.23(t, 3J=7.3Hz,2H,Ph-H),7.21(d, 4 J=2.3Hz,2H,Ar-H),7.18(d, 3 J=7.7Hz,2H,Py-H),6.87(d, 4 J=2.3Hz,2H,Ar-H),3.84(s,4H,Py-CH 2 -),3.79(s,4H,Ar-CH 2 -),3.72(s,4H,Ph-CH 2 -),1.48(s,18H,-C(CH 3 ) 3 ),1.28(s,18H,-C(CH 3 ) 3 ). 13 C{ 1 H}NMR (100MHz, CDCl 3 ,298K): δ157.62,153.99,140.61,137.53,137.30,137.08,135.63,129.96,129.66,128. 68,128.36,127.63,127.28,124.43,124.19,123.24,122.94,122.24,121.94,121.67(All Ar-C),58.92(Py-CH 2 ),58.51(Ar-CH 2 ),58.10(Ph-CH 2 ),35.09(C(CH 3 ) 3 ),34.26(C(CH 3 ) 3 ),31.89,31.77,29.80(all C(CH 3 ) 3 ).ESI-HRMS calcd.for C 51 H 67 N 3 O 2 +H + [M+H]:754.5307; found:754.5309.
[0060] Example 2
[0061] Ligand L 2 H 2 Synthesis
[0062] (1) Synthesis of 2,6-bis(cyclohexylaminomethyl)pyridine
[0063]
[0064] The raw materials used were cyclohexylamine (4.00 g, 40.3 mmol), 2,6-pyridinedicarboxaldehyde (2.70 g, 20.0 mmol) and NaBH 4 Except for the addition of 2,6-di(benzylaminomethyl)pyridine (3.20 g, 80.0 mmol), the other reaction conditions were the same as those for synthesizing 2,6-di(benzylaminomethyl)pyridine to give 2,6-di(cyclohexylaminomethyl)pyridine (4.49 g, 75%).
[0065] 1 H NMR (400 MHz, CDCl 3 ):δ7.53(t, 3 J=7.7Hz,1H,Py-H),7.10(d, 3 J=7.7Hz,2H,Py-H),3.87(s,4H,-CH 2 -),2.45(tt, 3 J=10.1,3.8Hz,2H,CH of cyclohexyl),2.32(br s,2H,-NH-),1.90(br d, 3 J=11.5Hz,4H,CH 2 of cyclohexyl),1.74–1.65(m,4H,CH 2 ofcyclohexyl),1.62–1.53(m,2H,CH 2 of cyclohexyl),1.28-1.04(m,10H,CH 2 ofcyclohexyl).
[0066] (2) Ligand L 2 H 2 Synthesis
[0067]
[0068] Except that the raw materials used were 2,6-bis(cyclohexylaminomethyl)pyridine (3.01 g, 10.0 mmol) and 2-bromomethyl-4,6-di-tert-butylphenol (6.00 g, 20.0 mmol), the reaction process was the same as that of L 1 H 2 The same reaction was performed, and a yellow solid (4.52 g, 61%) was finally obtained.
[0069] 1 H NMR (400 MHz, CDCl 3):δ11.17(br s,2H,Ar-OH),7.56(t, 3 J=7.7Hz,1H,Py-H),7.21-7.16(m,4H,Ar-H&Py-H),6.84(d, 4 J=2.4Hz,2H,Ar-H),3.85(s,4H,Py-CH 2 ),3.81(s,4H,Ar-CH 2 ),2.63(tt, 3 J=11.5,3.0Hz,2H,CH 2 of cyclohexyl),1.94(br d, 3 J=11.5Hz,4H,CH 2 of cyclohexyl),1.77(br d, 3 J=12.0Hz,4H,CH 2 of cyclohexyl),1.59(br d, 3 J=10.6Hz,2H,CH of cyclohexyl),1.42(s,18H,Ar-C(CH 3 ) 3 )1.46-1.38(m,2H,CH 2 ofcyclohexyl),1.27(s,Ar-C(CH 3 ) 3 ),1.31-1.22(m,2H,CH 2 of cyclohexyl),1.19-1.01(m,6H,CH 2 of cyclohexyl). 13 C{ 1 H}NMR(100MHz,CDCl 3 ,298K):δ158.47,154.47,140.39,137.27,136.99,136.47,124.05,123.81,122.90,122.60,121.89,121.70,121.40(all Ar-C),58.88,58.68(Py-CH 2 N-),55.72(-NCH 2 Ar),54.48(-NCH-),34.97,34.24(C(CH 3 ) 3 ),31.91,31.77,29.75,29.69(all C(CH 3 )3 ),28.22,28.11,26.05(all-CH 2 -of cyclohexyl).ESI-HRMS calcd.for C 49 H 75 N 3 O 2 +H + [M+H]:738.5933; found:738.5940.
[0070] Example 3
[0071] Ligand L 3 H 2 Synthesis
[0072] (1) Synthesis of 2,6-bis(bromomethyl)pyridine
[0073]
[0074] Add 6.4 mL of 33 wt% hydrogen bromide in acetic acid solution and 26 mL of glacial acetic acid to a 100 mL eggplant-shaped bottle. Add 2,6-pyridine dimethanol (1.82 g, 13.1 mmol) under stirring and heat under reflux for 8 h. After the reaction is completed, cool down. Under ice-water cooling, slowly add sodium hydroxide solution to adjust pH to 9, and an off-white solid precipitates. Filter to obtain 2,6-bis(bromomethyl)pyridine as a white solid (2.20 g, 63%).
[0075] 1 H NMR (400 MHz, CDCl 3 ):δ7.71(t, 3 J=7.8Hz,1H,Py-H),7.38(d, 3 J=7.8Hz,2H,Py-H),4.54(s,4H,Py-CH 2 -).
[0076] (2) Synthesis of 2,6-di(tert-butylaminomethyl)pyridine
[0077]
[0078] Add tert-butylamine (12.7 mL, 120 mmol) and potassium carbonate (3.317 g, 240 mmol) to a 100 mL eggplant-shaped bottle for later use. Dissolve 2,6-di(bromomethyl)pyridine (2.65 g, 10.0 mmol) in 20 mL DMF and slowly drop it into the aforementioned eggplant-shaped bottle to react for 8 h. Add 50 mL of water to quench the reaction, extract with 100 mL of DCM, and dry with anhydrous sodium sulfate. After filtering to remove the desiccant, the filtrate is vacuum-evacuated to remove the solvent to obtain a light yellow transparent liquid (2.02 g, 80%).
[0079] 1 H NMR (400 MHz, CDCl 3 ):δ7.51(t, 3 J=2.7Hz,1H,Py-H),7.12(d, 3 J=2.7Hz,2H,Py-H),5.25(s,2H,-NH-),3.81(s,4H,Py-CH 2 -),1.14(s,18H,-C(CH 3 ) 3 ).
[0080] (3) Ligand L 3 H 2 Synthesis
[0081]
[0082] Except that 2,6-di(tert-butylaminomethyl)pyridine (2.02 g, 8.10 mmol) and 2-bromomethyl-4,6-di-tert-butylphenol (4.85 g, 16.2 mmol) were used as the starting materials, the other operations were the same as those of ligand L. 1 H 2 The synthesis of is the same as that of . Recrystallization from dichloromethane / petroleum ether gave a white solid (3.84 g, yield 56%).
[0083] 1 H NMR (400 MHz, CDCl 3 ): δ10.91(br s,2H,Ar-OH),7.31(t, 3 J=7.7Hz,1H,Py-H),7.12(d, 4 J=2.4Hz,2H,Ar-H),7.09(d, 3 J=7.7Hz,2H,Py-H),6.81(d, 4 J=2.4Hz,2H,Ar-H),3.91(s,4H,Py-CH 2 -),3.81(s,4H,Ar-CH 2-),1.38(s,18H,Ar-C(CH 3 ) 3 ),1.25(s,18H,Ar-C(CH 3 ) 3 ),1.19(s,18H,NC(CH 3 ) 3 ). 13 C{ 1 H}NMR (100MHz, CDCl 3 ,298K): δδ159.69,154.18,140.61,136.52,136.20,135.57,123.67,123.45,123.01,122.80,122.52,121.37,121.03(all Ar-C),56.99(Py-CH 2 N-),56.24(-NCH 2 Ar),54.77(NC(CH 3 ) 3 ),34.87,34.22(C(CH 3 ) 3 ),31.90,31.76,29.73,29.65(all C(CH 3 ) 3 ),27.12,26.96(NC(CH 3 ) 3 ).ESI-HRMS calcd.forC 45 H 71 N 3 O 2 +H + [M+H]:686.5620; found:686.5626.
[0084] Example 4
[0085] Synthesis of Alkali Metal Complex Na1
[0086]
[0087] Weighing L 1 H 2 (377 mg, 0.500 mmol) was placed in a 50 mL Schlenk bottle, 200 nml tetrahydrofuran was added to dissolve the solid, NaH (36 mg, 1.5 mmol) was added thereto, and the reaction was stirred for 8 h. After the reaction was completed, the remaining NaH and a small amount of solid impurities were filtered out. The clear liquid was concentrated in vacuo until the solution was slightly viscous, and n-hexane was added thereto until slightly mixed and recrystallized to obtain a light yellow solid (212 mg, 56%).
[0088] 1 H NMR(400MHz,C 6 D 6 ):δ7.61(d, 4 J=2.3Hz,2H,Ar-H),7.19(d, 4 J=2.3Hz,2H,Ar-H),6.91(d, 3 J=7.1Hz,4H,Ph-H),6.85–6.75(m,6H,Ph-H),6.58(t, 3 J=7.6Hz,1H,Py-H),6.04(d, 3 J=7.6Hz,2H,Py-H),4.68(d, 2 J=9.8Hz,2H,Py-CH 2 -),4.13(d, 2 J=16.1Hz,2H,Ar-CH 2 -),3.86(d, 2 J=12.3Hz,2H,Ph-CH 2 -),3.56-3.47(m,10H,2THF and 2H of Ph-CH 2 -),3.40(d, 2 J=9.8Hz,2H,Py-CH 2 -),3.02(d, 2 J=16.1Hz,2H,Ar-CH 2 -),1.75(s,18H,Ar-C(CH 3 ) 3 ),1.48(s,18H,Ar-C(CH 3 ) 3 ),1.38–1.24(m,8H,2THF). 13 C{ 1 H}NMR(100MHz,C 6 D 6 ):δ167.64,159.32,136.33,136.15,135.99,131.18,130.75,128.96,128.85,127.07,124.56,124.09,123.99,119.28,119.16(All Ar-C of),68.19(THF),61.68(-NCH 2 Py),55.06(-NCH 2 Ar),54.92(-NCH 2Ph),35.73(C(CH 3 ) 3 ),34.09(C(CH 3 ) 3 ),32.59(C(CH 3 ) 3 ),30.73(C(CH 3 ) 3 ),30.66(C(CH 3 ) 3 ),25.57(THF).Anal.Calcd.for C 59 H 81 N 3 Na 2 O 4 :C,75.20;H,8.66;N,4.46%. Found:C,74.92;H,8.69;N,4.54%.
[0089] Example 5
[0090] Synthesis of Alkali Metal Complex Na2
[0091]
[0092] Except for raw materials, L 2 H 2 The operation steps were the same as those for Na1 except for the addition of 2-nitropropene (369 mg, 0.599 mmol) and NaH (36 mg, 1.5 mmol), and a white solid (495 mg, 50% yield) was finally obtained.
[0093] 1 H NMR (400 MHz, C 6 D 6 ): δ7.52(br s,2H,Ar-H),7.19(br s,2H,Ar-H),6.83(t, 3 J=7.6Hz,1H,Py-H),6.38(d, 3 J=7.7Hz,2H,Py-H),4.30(br s,2H,Py-CH 2 N-), 3.99(br s,2H,Ar-CH 2 N-),3.75-3.28(m,12H,2THF,2H of Ar-CH 2 N-&2H of Py-CH 2 N-),2.58(t, 3 J=11.2Hz,2H,CH 2of cyclohexyl),2.00(br s,2H,CH 2 of cyclohexyl),1.68(br s,20H,CH 2 of cyclohexyl and Ar-C(CH 3 ) 3 ),1.49(br s,22H,4H of CH 2 of cyclohexyl and 18H ofAr-C(CH 3 ) 3 ),1.37-1.26(m,12H,CH 2 of cyclohexyl and 2THF),1.01(br s,4H,CH 2 ofcyclohexyl),0.88(br s,4H,CH 2 of cyclohexyl). 13 C{ 1 H}NMR(100MHz,C 6 D 6 ):δ167.07,161.31,137.06,136.49,135.89,130.82,128.70,124.57,123.44,119.96(All Ar-C),68.04(THF),61.91(Py-CH 2 N-),57.52(-NCH 2 Ar),53.36(-NCH-),35.41(C(CH 3 ) 3 ),34.02(C(CH 3 ) 3 ),32.60(C(CH 3 ) 3 ),30.70(C(CH 3 ) 3 ),27.93(-CH 2 -),27.00(-CH 2 -),26.67(-CH 2 -),25.57(THF).Anal.Calcd.for C 57 H 89 N 3 Na 2 O 4 :C,73.91;H,9.68;N,4.54%.Found:C,74.13;H,9.85;N,4.41%.
[0094] Example 6
[0095] Synthesis of Alkali Metal Complex Na3
[0096]
[0097] Except for raw materials, L 3 H 2 The operation steps were the same as Na1 except for the addition of 2-nitropropene (343 mg, 0.500 mmol) and NaH (36 mg, 1.5 mmol), and finally a light yellow solid (579 mg, yield 66%) was obtained.
[0098] 1 H NMR (400 MHz, C 6 D 6 )::δ7.53(br s,1H,Ar-H),7.26(br s,1H,Ar-H),7.11(br s,2H,Ar-H),6.83(t, 3 J=7.5Hz,1H,Py-H),6.25(d, 3 J=7.5Hz,2H,Py-H),4.67(br s,1H,PyCH 2 N-), 4.35(br s,1H,PyCH 2 N-), 3.91-3.44(m,5H,PyCH 2 N-),3.43-3.33(m,8H,THF),3.24(br s,1H,ArCH 2 N-),1.75(s,9H,Ar-C(CH 3 ) 3 ),1.54(s,9H,Ar-C(CH 3 ) 3 ),1.48(s,18H,Ar-C(CH 3 ) 3 ),1.35-1.22(m,17H,THF and NC(CH 3 ) 3 ),0.98(s,9H,NC(CH 3 ) 3 ). 13 C{ 1 H}NMR (100MHz, C 6 D 6): δ166.63,160.18,136.15,135.90,131.18,130.18,128.39,124.55,122.87,118.68,116.81(All Ar-C),68.01(THF),62.21(Py-CH 2 N-),58.49(-NCH 2 Ar), 56.75(Py-CH 2 N-),55.67(-NCH 2 Ar),54.42(NC(CH 3 ) 3 ),53.67(NC(CH 3 ) 3 ),35.65(C(CH 3 ) 3 ),35.30(C(CH 3 ) 3 ),34.03(C(CH 3 ) 3 ),32.69(C(CH 3 ) 3 ),30.94(C(CH 3 ) 3 ),27.45(C(CH 3 ) 3 ),27.09(C(CH 3 ) 3 ),25.48(THF).Anal.Calcd.for C 53 H 85 N 3 Na 2 O 4 :C,72.81;H,9.80;N,4.81%. Found:C,72.64;H,9.68;N,4.70%.
[0099] Example 7
[0100] Synthesis of Alkali Metal Complex K1
[0101]
[0102] Except for raw materials, L 1 H 2 The operation steps were the same as Na1 except for the addition of 2-nitropropene (377 mg, 0.500 mmol) and KH (60 mg, 1.5 mmol). Finally, a light yellow solid (533 mg, yield 64%) was obtained.
[0103] 1H NMR(400MHz,C 6 D 6 ):δ7.60(d, 4 J=2.8Hz,4H,Ar-H),7.26(d, 4 J=2.8Hz,4H,Ar-H),7.00-6.80(m,18H,Ph-H and Py-H),6.74(t, 3 J=7.0Hz,4H,Ph-H),6.61(d, 3 J=7.8Hz,4H,Py-H),3.65(br s,8H,NCH 2 Py),3.44(br s,8H,NCH 2 Ar),3.27(br s,8H,NCH 2 Ph),1.73(s,36H,C(CH 3 ) 3 ),1.52(s,36H,C(CH 3 ) 3 ). 13 C{ 1 H}NMR(100MHz,C 6 D 6 ):δ167.34,159.62,140.36,136.73,136.25,130.37,129.77,128.97,128.80,128.35,127.03,123.90,123.72,122.25(All Ar-C),67.83(THF),62.39(Py-CH 2 N-),61.14(Ar-CH 2 N-),59.27(-NCH 2 Ph),35.51(C(CH 3 ) 3 ),34.06(C(CH 3 ) 3 ),32.63(C(CH 3 ) 3 ),30.55(C(CH 3 ) 3 ),25.81(THF).Anal.Calcd.for C 102 H 130 K 4 N 6 O 4 ·C 4 H 8O:C,73.48;H,8.03;N,4.85%. Found:C 73.23;H7.99;N 5.00%.
[0104] Example 8
[0105] Under argon protection, add racemic lactide (0.144 g, 1.0 mmol) to the polymerization bottle, dissolve it with 0.3 mL of toluene, and then add 0.2 mL of benzyl alcohol toluene solution. Measure 0.5 mL of catalyst Na3 toluene solution and add it to the polymerization bottle. [rac-LA] 0 =1.0M, [Na] 0 =0.002M, [BnOH] 0 =0.004M, [rac-LA] 0 :[Na] 0 :[BnOH] 0 =500:1:2. Control the reaction temperature at 25±1°C, react for 1 min, and add petroleum ether to terminate the reaction. Remove the solvent, dissolve the residue with dichloromethane, and add methanol to precipitate the polymer. Vacuum dry for 24 h. Conversion rate 94%, M n =4.56×10 4 g / mol, molecular weight distribution PDI = 1.43, isotacticity P m =0.56.
[0106] Example 9
[0107] Under argon protection, add racemic lactide (0.144 g, 1.0 mmol) to the polymerization bottle, dissolve it with 0.1 mL of toluene, and then add 0.4 mL of toluene solution of benzyl alcohol. Measure 0.5 mL of toluene solution of catalyst Na3 and add it to the polymerization bottle. [rac-LA] 0 =1.0M, [Na] 0 =0.002M, [BnOH] 0 =0.008M, [rac-LA] 0 :[Na] 0 :[BnOH] 0 =500:1:4. Control the reaction temperature at 25±1°C, react for 35 seconds, and add petroleum ether to terminate the reaction. Remove the solvent, dissolve the residue with dichloromethane, and add methanol to precipitate the polymer. Vacuum dry for 24 hours. Conversion rate 90%, M n =1.96×10 4 g / mol, molecular weight distribution PDI = 1.41, isotacticity P m =0.54.
[0108] Example 10
[0109] Except that the temperature was changed to -50±1°C, other operations were the same as in Example 8. After 29 minutes of reaction, the conversion rate was 85%, M n =2.33×10 4 g / mol, molecular weight distribution PDI = 1.26, isotacticity P m =0.62.
[0110] Embodiment 11
[0111] Under argon protection, add racemic lactide (0.144 g, 1.0 mmol) to the polymerization bottle, dissolve it with 0.4 mL of toluene, and then add 0.1 mL of toluene solution of benzyl alcohol. Measure 0.5 mL of toluene solution of catalyst Na1 and add it to the polymerization bottle. [rac-LA] 0 =1.0M, [Na] 0 =0.002M, [BnOH] 0 =0.002M, [rac-LA] 0 :[Na] 0 :[BnOH] 0 =500:1:1. Control the reaction temperature at 25±1°C, react for 150 seconds, and add petroleum ether to terminate the reaction. Remove the solvent, dissolve the residue with dichloromethane, and add methanol to precipitate the polymer. Vacuum dry for 24 hours. Conversion rate 90%, M n =4.31×10 4 g / mol, molecular weight distribution PDI = 1.64, isotacticity P m =0.54.
[0112] Example 12
[0113] Except that the catalyst was replaced with Na1, the other operations were the same as in Example 8. After 66 seconds of reaction, the conversion rate was 85%, and M n =3.50×10 4 g / mol, molecular weight distribution PDI = 1.44, isotacticity P m =0.57.
[0114] Example 13
[0115] Under argon protection, add racemic lactide (0.144 g, 1.0 mmol) to the polymerization bottle, dissolve it with 0.2 mL of toluene, and then add 0.3 mL of toluene solution of benzyl alcohol. Measure 0.5 mL of toluene solution of catalyst Na1 and add it to the polymerization bottle. [rac-LA] 0 =1.0M, [Na] 0 =0.002M, [BnOH] 0 =0.002M, [rac-LA] 0 :[Na] 0:[BnOH] 0 =500:1:3. Control the reaction temperature at 25±1°C, react for 50 seconds, and add petroleum ether to terminate the reaction. Remove the solvent, dissolve the residue with dichloromethane, and add methanol to precipitate the polymer. Vacuum dry for 24 hours. Conversion rate 92%, M n =2.67×10 4 g / mol, molecular weight distribution PDI = 1.41, isotacticity P m =0.57.
[0116] Embodiment 14
[0117] Except that the catalyst was replaced with Na1, the other operations were the same as in Example 9. After 250 seconds of reaction, the conversion rate was 90%, and M n =1.91×10 4 g / mol, molecular weight distribution PDI = 1.39, isotacticity P m =0.53.
[0118] Embodiment 15
[0119] Except that the catalyst was replaced with Na1 and the temperature was changed to -50±1℃, the other operations were the same as in Example 8. After 28 minutes of reaction, the conversion rate was 61%, and M n =2.21×10 4 g / mol, molecular weight distribution PDI = 1.21, isotacticity P m =0.65.
[0120] Example 16
[0121] Except that the temperature was changed to -50±1℃, other operations were the same as Example 13. After 25 minutes of reaction, the conversion rate was 75%, M n =1.48×10 4 g / mol, molecular weight distribution PDI = 1.13, isotacticity P m =0.63.
[0122] Embodiment 17
[0123] Under argon protection, add racemic lactide (0.144 g, 1.0 mmol) to the polymerization bottle, dissolve it with 0.3 mL of tetrahydrofuran, and then add 0.2 mL of benzyl alcohol in tetrahydrofuran. Measure 0.5 mL of catalyst Na1 in tetrahydrofuran and add it to the polymerization bottle. [rac-LA] 0 =1.0M, [Na] 0 =0.002M, [BnOH] 0 =0.004M, [rac-LA] 0 :[Na] 0 :[BnOH] 0=500:1:2. Control the reaction temperature at 25±1°C, react for 18 min, and add petroleum ether to terminate the reaction. Remove the solvent, dissolve the residue with dichloromethane, and add methanol to precipitate the polymer. Vacuum dry for 24 h. Conversion rate 97%, M n =3.89×10 4 g / mol, molecular weight distribution PDI = 1.62, isotacticity P m =0.62.
[0124] Embodiment 18
[0125] Under argon protection, add racemic lactide (0.576 g, 4.0 mmol) to the polymerization bottle, dissolve it with 0.3 mL of toluene, and then add 0.2 mL of benzyl alcohol toluene solution. Measure 0.5 mL of catalyst Na1 toluene solution and add it to the polymerization bottle. [rac-LA] 0 =1.0M, [Na] 0 =0.002M, [BnOH] 0 =0.004M, [rac-LA] 0 :[Na] 0 :[BnOH] 0 =2000:1:2, control the reaction temperature at -50±1°C, react for 47 minutes, add petroleum ether to terminate the reaction. Remove the solvent, dissolve the residue with dichloromethane, add methanol to precipitate the polymer. Vacuum dry for 24h. Conversion rate 37%, M n =4.81×10 5 g / mol, molecular weight distribution PDI = 1.48, isotacticity P m =0.63.
[0126] Embodiment 19
[0127] Except that the catalyst was replaced with Na2, the other operations were the same as in Example 8. After 90 seconds of reaction, the conversion rate was 90%, and M n =5.21×10 4 g / mol, molecular weight distribution PDI = 1.36, isotacticity P m =0.52.
[0128] Embodiment 20
[0129] Except that the catalyst was replaced with Na2, the other operations were the same as in Example 9. After 50 seconds of reaction, the conversion rate was 95%, and M n =2.74×10 4 g / mol, molecular weight distribution PDI = 1.53, isotacticity P m =0.51.
[0130] Embodiment 21
[0131] Except that the catalyst was replaced with Na2 and the temperature was changed to -50±1℃, the other operations were the same as in Example 8. After 136 minutes of reaction, the conversion rate was 90%, and M n =6.66×10 4 g / mol, molecular weight distribution PDI = 1.45, isotacticity P m =0.63.
[0132] Embodiment 22
[0133] Except that the catalyst was replaced with K1, the other operations were the same as in Example 8. After 78 seconds of reaction, the conversion rate was 95%, and M n =6.31×10 4 g / mol, molecular weight distribution PDI = 1.49, isotacticity P m =0.54.
[0134] Embodiment 23
[0135] Except that the catalyst was replaced with K1, the other operations were the same as in Example 9. After 54 seconds of reaction, the conversion rate was 90%, and M n =2.79×10 4 g / mol, molecular weight distribution PDI = 1.47, isotacticity P m =0.53.
[0136] Embodiment 24
[0137] Except that the catalyst was replaced with K1 and the temperature was changed to -50±1℃, the other operations were the same as in Example 8. After 46 minutes of reaction, the conversion rate was 91%, and M n =4.11×10 4 g / mol, molecular weight distribution PDI = 1.51, isotacticity P m =0.62.
[0138] Embodiment 25
[0139] Under argon protection, add L-lactide (0.144 g, 1.0 mmol) to the polymerization bottle, dissolve it with 0.3 mL of tetrahydrofuran, and then add 0.2 mL of benzyl alcohol in tetrahydrofuran. Measure 0.5 mL of catalyst Na1 in tetrahydrofuran and add it to the polymerization bottle. [rac-LA] 0 =1.0M, [Na] 0 =0.002M, [BnOH] 0 =0.004M, [rac-LA] 0 :[Na] 0 :[BnOH] 0=500:1:2. Control the reaction temperature at 25±1°C, react for 42 seconds, and add petroleum ether to terminate the reaction. Remove the solvent, dissolve the residue with dichloromethane, and add methanol to precipitate the polymer. Vacuum dry for 24 hours. Conversion rate 95%, M n =4.89×10 4 g / mol, molecular weight distribution PDI = 1.46, isotacticity P m =1.
[0140] Embodiment 26
[0141] Under argon protection, add racemic lactide (0.144 g, 1.0 mmol) to the polymerization bottle, dissolve it with 0.5 mL of toluene, and add 0.5 mL of toluene solution of catalyst Na1 to the polymerization bottle. [rac-LA] 0 =1.0M, [Na] 0 =0.002M, [rac-LA] 0 :[Na] 0 =500:1. Control the reaction temperature at 25±1°C, react for 120 min, and add petroleum ether to terminate the reaction. Remove the solvent, dissolve the residue with dichloromethane, and add methanol to precipitate the polymer. Vacuum dry for 24 h. Conversion rate 90%, M n =1.13×10 4 g / mol, molecular weight distribution PDI=1.38.
Claims
1. A dimethylenepyridine-bridged bisaminophenol ligand (I) and an alkali metal complex (II) thereof, characterized in that: Has the following general formula: In formula (I) and (II): R 1 ~R 2 Represents C1~C 20 Straight chain, branched chain or cyclic alkyl group, C7~C 30 a mono- or poly-aryl-substituted alkyl group, or a halogen; R 3 Represents C1~C 20 Straight chain, branched chain or cyclic alkyl group, C7~C 30 Mono- or poly-aryl-substituted alkyl, C6~C 18 The aromatic group; n is 0 or 1; M represents Na and K.
2. The dimethylenepyridine-bridged bisaminophenol ligand (I) and its alkali metal complex (II) according to claim 1, characterized in that: R 1 ~R 2 Respectively represent C1~C8 straight chain, branched or cyclic alkyl groups, C7~C 20 mono- or poly-aryl-substituted alkyl, or halogen; R 3 It is a C1-C8 straight chain, branched chain or cyclic alkyl group, C7-C 20 Mono- or poly-aryl-substituted alkyl, C6~C 12 The aromatic group.
3. The dimethylenepyridine-bridged bisaminophenol ligand (I) and its alkali metal complex (II) according to claim 1, characterized in that: R 1 ~R 2 is methyl, isopropyl, tert-butyl, cumyl, trityl; R 3 It is methyl, ethyl, tert-butyl, n-butyl, cyclopentyl, cyclohexyl, benzyl, and phenyl.
4. A method for preparing the dimethylenepyridine-bridged bisaminophenol ligand (I) and its alkali metal complex (II) according to any one of claims 1 to 3, comprising the following steps: The 2-bromomethyl-4,6-disubstituted phenol represented by formula (III) and the 2,6-di(substituted aminomethyl)pyridine represented by formula (IV) are reacted in an organic medium in the presence of an alkylamine at a reaction temperature of 0 to 90° C. for a reaction time of 2 to 72 hours, and then a dimethylenepyridine-bridged bisaminophenol ligand compound (I) is collected from the reaction product; Optionally, a dimethylpyridine-bridged bisaminophenol ligand compound represented by formula (I) is reacted with a metal hydride in an organic medium at a reaction temperature of 0 to 100° C. for a reaction time of 2 to 24 hours, and then a dimethylpyridine-bridged bisaminophenoloxy alkali metal complex (II) is collected from the reaction product; In the above preparation method, the substituent R 1 ~R 3 The corresponding groups of the dimethylenepyridine-bridged bisaminophenol ligand (I) and its alkali metal complex (II) as described in any one of claims 1 to 3 are consistent; The alkylamine is triethylamine, tributylamine or triisopropylamine; Metal hydrides MH are NaH and KH.
5. The method according to claim 4, wherein the molar ratio of the dimethylpyridine-bridged bisaminophenol ligand compound (I) to the metal hydride is 1:2.0-4.0; and the organic medium is selected from one or more of tetrahydrofuran, ether, toluene, benzene, petroleum ether and n-hexane.
6. Use of the dimethylene pyridine-bridged bisaminophenoloxy alkali metal complex (I) according to any one of claims 1 to 3, characterized in that: Used for the ring-opening polymerization of lactones.
7. The use according to claim 6, characterized in that: The lactone is selected from L-lactide, D-lactide, rac-lactide, meso-lactide.
8. The use according to claim 6, characterized in that: The dimethylene pyridine-bridged bisaminophenoloxy alkali metal complex according to any one of claims 1 to 3 is used as a catalyst to polymerize lactide, and the molar ratio of the catalyst to the monomer during the polymerization is 1:1 to 10000.
9. The use according to claim 6, characterized in that: Using the dimethylene pyridine bridged bisaminophenoloxy alkali metal complex as described in any one of claims 1 to 3 as a catalyst, in the presence of an alcohol, lactide is polymerized, and the molar ratio of the catalyst to the alcohol and lactide during the polymerization is 1:1 to 50:1 to 10000; the alcohol is C1 to C 10 Alkyl alcohols with straight chain, branched chain or cyclic structure, C7~C 20 Mono- or polyaryl-substituted alkyl alcohols.
10. The use according to claim 1, characterized in that: Using the dimethylene pyridine bridged bisaminophenoloxy alkali metal complex as described in any one of claims 1 to 3 as a catalyst, in the presence of an alcohol, lactide is polymerized at -70 to 250°C, and the molar ratio of the catalyst to the alcohol and lactide during the polymerization is 1:1 to 50:1 to 10000; the alcohol is C1 to C 10 Alkyl alcohols with straight chain, branched chain or cyclic structure, C7~C 20 Mono- or polyaryl-substituted alkyl alcohols.
Citation Information
Patent Citations
Ethylene bridged amino bisphenol oxygroup alkali metal complex as well as preparation method and application thereof
CN116854712A
Anion-cation pair type amino bisphenol oxygroup alkali metal complex as well as preparation method and application thereof
CN116874414A
Cited By
Crown ether-like phenoloxy potassium complex as well as preparation method and application thereof
CN121318769A