Butterfly-shaped trinuclear Schiff base rare earth metal catalyst, preparation method and application
By preparing a butterfly-shaped trinuclear Schiff base rare earth metal catalyst, the synergistic catalytic effect of rare earth metal ions and Schiff base ligands was utilized to solve the problems of harsh catalytic conditions and low efficiency in the existing technology, and a high-conversion carbon dioxide cycloaddition reaction with epoxides was achieved, which is suitable for the synthesis of cyclic carbonates.
Patent Information
- Application Number
- CN202411160646.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-22
AI Technical Summary
In the existing technology, tetradentate pyridyl Schiff base metal complex catalysts have harsh catalytic conditions, low catalytic efficiency, and low conversion rate, making it difficult to efficiently catalyze the cycloaddition reaction of carbon dioxide and epoxides under mild conditions.
A butterfly-shaped trinuclear Schiff base rare earth metal catalyst is used, which utilizes rare earth metal ions as active centers and Schiff base ligands as flexible frameworks. The reaction is promoted by acid-base synergistic catalysis. The preparation method is mild and the catalyst structure is stable. It is suitable for the cycloaddition reaction of carbon dioxide and epoxides.
It achieves efficient catalytic reaction of carbon dioxide and epoxide under mild conditions, with a conversion rate of 99%. The catalyst has good stability, low cost, and is suitable for industrial application.
Smart Images

Figure CN119039328A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of multifunctional new materials, and in particular to a butterfly-shaped trinuclear Schiff base rare earth metal catalyst, a preparation method and application thereof. Background Art
[0002] Carbon dioxide is the most widely distributed and abundant carbon resource on the earth. It is not only non-toxic, harmless, widely available, and inexpensive, but also a sustainable carbon source. Therefore, converting carbon dioxide into chemicals with high added value is one of the most effective ways to utilize resources. CO2 can react with a variety of organic compounds to produce high value-added chemicals, such as polycarbonates, carboxylic acids, esters, cyclic carbonates, formamides, methylamines, carbamates, oxazolidinone derivatives, etc. Among them, the method of combining carbon dioxide with epoxides to produce cyclic carbonates is an atom-economic reaction with 100% atomic utilization, which has attracted the attention of more and more scholars. However, since both carbon dioxide and epoxides are highly stable, they are not easy to activate during the reaction, resulting in a low conversion rate, and catalysts are often required.
[0003] In order to improve the reaction activity of carbon dioxide and epoxide cycloaddition reaction, the prior art is committed to developing catalysts with higher catalytic activity. For example, the disclosed heterogeneous catalysts include metal oxides, modified molecular sieves and clays, polymers, etc. Heterogeneous catalysts are easier to remove from the product, but they have problems such as low catalytic activity, low selectivity, long reaction time and harsh reaction conditions. In order to realize the cycloaddition reaction of carbon dioxide and epoxide under milder conditions, the prior art has developed homogeneous catalysts, such as metal complexes, especially tetradentate Schiff base metal complexes with cobalt, chromium, etc. as active centers, which show higher catalytic activity under milder reaction conditions, but their selectivity is low, and there will be the generation of byproducts such as polycarbonate in the cycloaddition reaction product.
[0004] The Chinese invention patent with the authorization publication number CN103447091 B discloses a tetradentate pyridyl Schiff base metal complex, a preparation method thereof and a method for preparing a cyclic carbonate. A tetradentate pyridyl Schiff base metal complex is prepared, which includes zinc, magnesium, manganese or iron metal elements as the active center of the tetradentate pyridyl Schiff base metal complex and a special structure outside the active center. When performing a catalytic reaction, the tetradentate pyridyl Schiff base metal complex is used as a main catalyst and a quaternary ammonium salt is used as a co-catalyst to achieve a cycloaddition reaction of carbon dioxide and epoxide with good selectivity. However, since the catalyst has a rigid skeleton structure, during the catalytic carbon dioxide cycloaddition reaction of the catalyst, not only the purity of the carbon dioxide is required to be high, the reaction conditions are harsh, the catalytic synthesis time is long, and there is a problem of low conversion rate. Summary of the invention
[0005] In view of the problems in the prior art that tetradentate pyridyl Schiff base metal complexes have harsh catalytic conditions, low catalytic efficiency and low conversion rate as catalysts, the present invention provides a butterfly-shaped trinuclear Schiff base rare earth metal catalyst, a preparation method and application.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention provides a butterfly-shaped trinuclear Schiff base rare earth metal catalyst, whose molecular structure is: Among them, M1~M3 are rare earth metal ions.
[0008] Furthermore, the rare earth metal ion is Sc 3+ , Y 3+ 、Ce 3+ 、Nd 3+ 、Sm 3+ , Gd 3+ 、Eu 3+ , Tb 3+ 、Dy 3+ , Er 3+ 、Ho 3+ 、Tm 3+ or Yb 3+ .
[0009] The present invention provides a method for preparing a butterfly-shaped trinuclear Schiff base rare earth metal catalyst, comprising:
[0010] preparing Schiff base ligands;
[0011] A butterfly-shaped trinuclear Schiff base rare earth metal catalyst is prepared by using a Schiff base ligand and a rare earth metal chloride. The molecular structure of the butterfly-shaped trinuclear Schiff base rare earth metal catalyst is: Among them, M1~M3 are rare earth metal ions.
[0012] Furthermore, the molecular structure of the Schiff base ligand is:
[0013] Furthermore, the rare earth metal chloride is ScCl3·6H2O, YCl3·6H2O, CeCl3·6H2O, NdCl3·6H2O, SmCl3·6H2O, GdCl3·6H2O, EuCl3·6H2O, TbCl3·6H2O, DyCl3·6H2O, ErCl3·6H2O, HoCl3·6H2O, TmCl3·6H2O or YbCl3·6H2O.
[0014] Furthermore, the method for preparing the Schiff base ligand is:
[0015] Reacting 1,3-propylenediamine and 3-amino-2-hydroxyacetophenone to obtain an intermediate;
[0016] The intermediate is reacted with o-vanillin to obtain the Schiff base ligand.
[0017] Furthermore, the method for preparing a butterfly-shaped trinuclear Schiff base rare earth metal catalyst using a Schiff base ligand and a rare earth metal chloride is:
[0018] The Schiff base ligand and the rare earth metal chloride are dissolved in a solvent, triethylamine is added, and a butterfly-shaped trinuclear Schiff base rare earth metal catalyst is obtained by reaction under room temperature.
[0019] A butterfly-shaped trinuclear Schiff base rare earth metal catalyst is prepared by the method.
[0020] The application of the butterfly-shaped trinuclear Schiff base rare earth metal catalyst in the preparation of cyclic carbonates.
[0021] Furthermore, a butterfly-shaped trinuclear Schiff base rare earth metal catalyst is used as a catalyst, tetrabutylammonium bromide is used as a co-catalyst, and epoxide and carbon dioxide are used as reaction substrates to carry out a cycloaddition reaction to obtain a cyclic carbonate; the epoxide is epichlorohydrin, allyl glycidyl ether, styrene oxide, butyl glycidyl ether or phenyl glycidyl ether; the cycloaddition reaction time is 1 to 3 hours, the reaction temperature is 60°C to 120°C, the conversion rate is 99%, and the molar ratio of epoxide, catalyst and co-catalyst is 1000:(0.4-1):(2-8).
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The present invention discloses a butterfly-shaped trinuclear Schiff base rare earth metal catalyst. Its molecular structure is: Among them, M1 to M3 are rare earth metal ions. The catalyst uses rare earth metal ions as active centers and butterfly-shaped ligands as flexible skeletons. Rare earth metal ions have high Lewis acidity and oxophilicity, which can promote the activation of epoxides, thereby promoting the reaction through acid-base synergistic catalysis. The butterfly-shaped ligand as a flexible skeleton is not only easier to coordinate with rare earth metal ions, but also the -C=N- group in the skeleton shows Lewis basicity, which helps to fix carbon dioxide in the target substrate. The addition of hydroxyl groups and -C=N- groups synergistically enrich the coordination sites of the butterfly-shaped ligands, thereby constructing a special energy level structure of a new Schiff base complex for catalytic conversion of carbon dioxide, so that the catalyst can still maintain structural stability under high temperature conditions. During catalysis, the reaction is not affected by additional moisture and air, the reaction conditions are mild, the catalytic cost is low, the catalytic efficiency is high, and the conversion rate is high.
[0024] The present invention provides a method for preparing a butterfly-shaped trinuclear Schiff base rare earth metal catalyst, which is prepared by preparing Schiff base ligands; using Schiff base ligands and rare earth metal chlorides to prepare butterfly-shaped trinuclear Schiff base rare earth metal catalysts; the method uses Schiff base ligands and rare earth metal chlorides as raw materials, has mild reaction conditions, does not require harsh reaction environments and equipment, has a wide source of raw materials and low costs, and has a short reaction time and high yield, is suitable for industrialization, effectively controls production input costs, and improves production efficiency and yield. The produced rare earth metal catalyst has better stability and higher catalytic efficiency.
[0025] A butterfly-shaped trinuclear Schiff base rare earth metal catalyst is prepared by the above method. The minimum structural unit of the catalyst includes one Schiff base ligand and three rare earth metal ions. The complex is a symmetrical structure, belongs to the monoclinic system, and has a C2 / c space group. In the complex, M1 and M2 have the same coordination environment, and both form an eight-coordinate structure with the O of two phenolic hydroxyl groups and the N of the imine group on the Schiff base ligand, the O of the methanol molecule, the O of two H2O molecules, and the O of two hydroxyl groups. M3 forms an eight-coordinate structure with the O of two phenolic hydroxyl groups, the O of two methoxy groups, the O of two hydroxyl groups, and the O of two water molecules on the Schiff base ligand. The catalyst has good catalytic stability. It has the characteristics of high catalytic efficiency and conversion rate and low catalytic cost.
[0026] For example, the application of the butterfly-shaped trinuclear Schiff base rare earth metal catalyst in the preparation of cyclic carbonates. Using the butterfly-shaped trinuclear Schiff base rare earth metal catalyst as a catalyst, tetrabutylammonium bromide as a co-catalyst, and epoxide and carbon dioxide as reaction substrates for cycloaddition reaction can quickly and stably realize the catalytic synthesis of cyclic carbonates. The cycloaddition reaction time is short, the efficiency is high, the conversion rate can be as high as 99%, and the catalyst can be recycled, the cost is low, and the economic efficiency of synthesizing cyclic carbonates is improved, which has very good application and promotion value. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The figure is a schematic diagram of the crystal structure of a butterfly-shaped trinuclear Schiff base rare earth metal catalyst of the present invention.
[0028] Figure 2 This is a schematic diagram of the catalytic mechanism of a butterfly-shaped trinuclear Schiff base rare earth metal catalyst of the present invention.
[0029] Figure 3 The present invention is a flow chart of a method for preparing a butterfly-shaped trinuclear Schiff base rare earth metal catalyst.
[0030] Figure 4 The present invention provides a synthetic route for a butterfly-shaped trinuclear Schiff base rare earth metal catalyst.
[0031] Figure 5The present invention provides a synthetic route for the Schiff base ligand H4L in the synthetic route of the butterfly-shaped trinuclear Schiff base rare earth metal catalyst.
[0032] Figure 6 It is an infrared curve diagram of the Schiff base ligand H4L in the synthesis path of a butterfly-shaped trinuclear Schiff base rare earth metal catalyst of the present invention.
[0033] Figure 7 The invention discloses a butterfly-shaped trinuclear Schiff base rare earth metal catalyst synthesis path of the Schiff base ligand 13 CNMR spectrum.
[0034] Figure 8 The invention discloses a butterfly-shaped trinuclear Schiff base rare earth metal catalyst synthesis path of the Schiff base ligand 1 HNMR spectrum.
[0035] Fig. 9 This is an infrared comparison image of a butterfly-shaped trinuclear Schiff base rare earth metal catalyst of the present invention and the Schiff base ligand H4L in the synthesis route.
[0036] Fig.10 This is a thermogravimetric comparison diagram of different butterfly-shaped trinuclear Schiff base rare earth metal catalysts of the present invention.
[0037] Fig.11 The invention discloses a butterfly-shaped trinuclear Schiff base rare earth metal catalyst for catalyzing the conversion of styrene oxide into a crude product. 1 HNMR spectrum.
[0038] Fig.12 The invention discloses a butterfly-shaped trinuclear Schiff base rare earth metal catalyst for catalyzing the conversion of n-butyl glycidyl ether into a crude product. 1 HNMR spectrum.
[0039] Fig.13 The invention discloses a butterfly-shaped trinuclear Schiff base rare earth metal catalyst for catalyzing the conversion of epoxypropyl phenyl ether into a crude product. 1 HNMR spectrum.
[0040] Fig.14 The invention discloses a butterfly-shaped trinuclear Schiff base rare earth metal catalyst for catalyzing the conversion of allyl glycidyl ether into a crude product. 1 HNMR spectrum. DETAILED DESCRIPTION
[0041] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0042] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0043] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0044] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0045] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0046] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0047] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0048] The present invention is further described in detail below in conjunction with specific embodiments, which are intended to explain the present invention rather than to limit it.
[0049] The present invention discloses a butterfly-shaped trinuclear Schiff base rare earth metal catalyst, the molecular structure of which is: Wherein, M1-M3 are rare earth metal ions. Preferably, the rare earth metal ions are Sc 3+ , Y 3+ 、Ce 3+ 、Nd 3+ 、Sm 3+ , Gd 3+ 、Eu 3+ , Tb 3+ 、Dy 3+ , Er 3+ 、Ho 3+ 、Tm 3+ or Yb 3+ .
[0050] See also Figure 1 Taking the rare earth element Er as an example, it should be noted that the coordinated anions and solvent molecules are omitted in this structure. Analysis of its crystal structure shows that the smallest structural unit of the catalyst includes one Schiff base ligand H4L and three rare earth metal ions. The complex is a symmetrical structure, belongs to the monoclinic system, and has a C2 / c space group. In the complex, the coordination environment of the rare earth metal ions Er1 and Er2 is the same, and both form an octa-coordinate structure with the O of the two phenolic hydroxyl groups and the N of the imine group on the ligand H4L, the O of the methanol molecule, the O of two H2O molecules, and the O of two hydroxyl groups. Er3 forms an octa-coordinate structure with the O of the two phenolic hydroxyl groups, the O of the two methoxy groups, the O of the two hydroxyl groups, and the O of the two water molecules on the ligand H4L. Among them, the Er-O bond length is 2.235(3)-2.479(4) Within the range, Er 3+ The bond angles formed with N and O are in the range of 67.63 (13)-153.19 (11). In subsequent catalytic experiments, the uncoordinated N atoms contained in the ligand can serve as active sites to promote acid-base synergistic catalysis and thus improve the conversion efficiency. The main crystal structure data are shown in Table 1 below:
[0051] Table 1 Crystal structure data of catalysts
[0052]
[0053]
[0054] See also Figure 2The catalytic principle of the butterfly-shaped trinuclear Schiff base rare earth metal catalyst is as follows: the complex generated by the coordination self-assembly of the Schiff base ligand H4L and the rare earth metal ions contains a large coordination cavity, which can adsorb carbon dioxide and thus improve the reaction conversion rate.
[0055] See also Figures 3 to 5 The present invention also provides a method for preparing a butterfly-shaped trinuclear Schiff base rare earth metal catalyst, comprising:
[0056] S1: Prepare Schiff base ligand, the specific method is as follows:
[0057] 1,3-propylenediamine and 3-amino-2-hydroxyacetophenone are uniformly dispersed in methanol or acetonitrile at a molar ratio of 1:2, reacted at 50°C to 60°C for 4 to 6 hours, filtered, washed, and dried to obtain an intermediate, denoted as M. The structural formula of the intermediate is:
[0058]
[0059] The intermediate M and o-vanillin are uniformly dispersed in methanol or acetonitrile at a molar ratio of 1:2, reacted at 55°C to 65°C for 4 to 6 hours, filtered, washed, and dried to obtain a Schiff base ligand, denoted as H4L. The structural formula of the Schiff base ligand is:
[0060] The intermediate is reacted with o-vanillin to obtain the Schiff base ligand.
[0061] S2: A butterfly-shaped trinuclear Schiff base rare earth metal catalyst is prepared by using Schiff base ligand and rare earth metal chloride. The Schiff base ligand is dissolved in methanol or acetonitrile solvent, triethylamine is added until the solution turns orange-red, rare earth metal chloride is added, and the solution turns from orange-red to orange-yellow. The solution evaporates at room temperature, is sealed and allowed to stand, and yellow crystals precipitate from the solution. The solution is filtered and dried to obtain a rare earth metal catalyst. The molar ratio of the Schiff base ligand to the rare earth metal chloride is 1:4, and the amount of triethylamine added is based on the color change of the solution, and its main function is deprotonation. The rare earth chloride salt is ScCl3·6H2O, YCl3·6H2O, CeCl3·6H2O, NdCl3·6H2O, SmCl3·6H2O, GdCl3·6H2O, EuCl3·6H2O, TbCl3·6H2O, DyCl3·6H2O, ErCl3·6H2O, HoCl3·6H2O, TmCl3·6H2O or YbCl3·6H2O, and the molecular structure of the butterfly-shaped trinuclear Schiff base rare earth metal catalyst is: Among them, M1~M3 are rare earth metal ions.
[0062] Example 1
[0063] Add 3.023g (0.02mol) 3-amino-2-hydroxyacetophenone to a round-bottom flask, add 80mL methanol solution, then add 0.743g (0.01mol) 1,3-propylenediamine, mix well, heat and reflux in a 55℃ oil bath for 5h, the solution turns from black to yellow. Cool and filter to obtain a yellow solid, i.e., the intermediate, with a calculated yield of 85%.
[0064] Take 1.7g (0.005mol) of the intermediate and add it to a round-bottom flask, add 1.521g (0.01mol) of o-vanillin, add an appropriate amount of methanol solution, mix well, and heat under reflux at 60°C for 6h. A red solution is obtained, cooled, and filtered to obtain a red solid, which is the Schiff base ligand, recorded as H4L, with a calculated yield of 90%.
[0065] Take 0.03g (0.05mmol) of Schiff base ligand and put it into a 10mL sample bottle, add 2mL of methanol solution and 2mL of acetonitrile solution, then add 0.076g (0.2mmol) of ErCl3·6H2O, and then add 40μL of triethylamine solution, and mix well. Seal with plastic wrap, poke holes, evaporate at room temperature for one week, and pale yellow crystal particles will precipitate in the bottle. Filter, wash, and dry to obtain complex crystals, with a calculated yield of about 86%. EA (%) C 37 H 52 N4O 18 Er3.Calc:C, 29.93; H, 3.50; N, 3.77; Found: C, 30.18; H, 3.58; N, 3.69.IR (KBr, ν, cm -1 ), 1599(s), 1553(m), 1455(m), 1391(w), 1298(s), 741(s).
[0066] Example 2
[0067] Add 3.023g (0.02mol) 3-amino-2-hydroxyacetophenone to a round-bottom flask, add 80mL methanol solution, then add 0.743g (0.01mol) 1,3-propylenediamine, mix well, heat and reflux in a 55℃ oil bath for 5h, the solution turns from black to yellow. Cool and filter to obtain a yellow solid, i.e., the intermediate, with a calculated yield of 85%.
[0068] Take 1.7g (0.005mol) of the intermediate and add it to a round-bottom flask, add 1.521g (0.01mol) of o-vanillin, add an appropriate amount of methanol solution, mix well, and heat under reflux at 60°C for 6h. A red solution is obtained, cooled, and filtered to obtain a red solid, which is the Schiff base ligand, recorded as H4L, with a calculated yield of 90%.
[0069] Take 0.03g (0.05mmol) of Schiff base ligand H4L and put it into a 10mL sample bottle, add 2mL of methanol solution and 2mL of acetonitrile solution, then add 0.078g (0.2mmol) of YbCl3·6H2O, and then add 40μL of triethylamine solution, and mix well. Seal with plastic wrap, poke holes, evaporate at room temperature for one week, and pale yellow crystal particles will precipitate in the bottle. Filter, wash, and dry to obtain complex crystals, with a calculated yield of about 90%. EA (%) C 37 H 58 N4O 19 Yb3. Calc: C, 29.15; H, 3.81; N, 3.67; Found: C, 29.30; H, 3.68; N, 3.76. IR (KBr, ν, cm -1 ), 1599(s), 1553(m), 1455(m), 1391(w), 1298(s), 741(s).
[0070] Example 3
[0071] Add 3.023g (0.02mol) 3-amino-2-hydroxyacetophenone to a round-bottom flask, add 80mL methanol solution, then add 0.743g (0.01mol) 1,3-propylenediamine, mix well, heat and reflux in a 55℃ oil bath for 5h, the solution turns from black to yellow. Cool and filter to obtain a yellow solid, namely intermediate M, with a calculated yield of 85%.
[0072] Take 1.7g (0.005mol) of the intermediate and add it to a round-bottom flask, add 1.521g (0.01mol) of o-vanillin, add an appropriate amount of methanol solution, mix well, and heat under reflux at 60°C for 6h. A red solution is obtained, cooled, and filtered to obtain a red solid, namely the Schiff base ligand H4L, with a calculated yield of 90%.
[0073] Take 0.03g (0.05mmol) of ligand H4L and put it into a 10mL sample bottle, add 2mL of methanol solution and 2mL of acetonitrile solution, then add 0.061g (0.2mmol) of YCl3·6H2O, and then add 40μL of triethylamine solution, and mix well. Seal with plastic wrap, poke holes, evaporate at room temperature for one week, and pale yellow crystal particles will precipitate in the bottle. Filter, wash, and dry to obtain complex crystals, with a calculated yield of about 82%. EA (%) C 37 H 58 N4O 18 Y3. Calc: C, 35.39; H, 4.62; N, 4.46; Found: C, 35.46; H, 4.43; N, 4.57. IR (KBr, ν, cm -1), 1599(s), 1553(m), 1455(m), 1391(w), 1298(s), 741(s).
[0074] Example 4
[0075] Add 3.023g (0.02mol) 3-amino-2-hydroxyacetophenone to a round-bottom flask, add 80mL methanol solution, then add 0.743g (0.01mol) 1,3-propylenediamine, mix well, heat and reflux in a 55℃ oil bath for 5h, the solution turns from black to yellow. Cool and filter to obtain a yellow solid, namely intermediate M, with a calculated yield of 85%.
[0076] Take 1.7g (0.005mol) of the intermediate and add it to a round-bottom flask, add 1.521g (0.01mol) of o-vanillin, add an appropriate amount of methanol solution, mix well, and heat under reflux at 60°C for 6h. A red solution is obtained, cooled, and filtered to obtain a red solid, namely the Schiff base ligand H4L, with a calculated yield of 90%.
[0077] Take 0.03g (0.05mmol) of Schiff base ligand H4L and put it into a 10mL sample bottle, add 2mL of methanol solution and 2mL of acetonitrile solution, then add 0.074g (0.2mmol) of GdCl3·6H2O, and then add 40μL of triethylamine solution, mix well. Seal with plastic wrap, poke holes, evaporate at room temperature for one week, and pale yellow crystal particles will precipitate in the bottle, filter, wash, and dry to obtain a rare earth metal catalyst.
[0078] Example 5
[0079] Add 3.023g (0.02mol) 3-amino-2-hydroxyacetophenone to a round-bottom flask, add 80mL methanol solution, then add 0.743g (0.01mol) 1,3-propylenediamine, mix well, heat and reflux in a 55℃ oil bath for 5h, the solution turns from black to yellow. Cool and filter to obtain a yellow solid, namely intermediate M, with a calculated yield of 85%.
[0080] Take 1.7 g (0.005 mol) of the yellow solid obtained from the intermediate and add it to a round-bottom flask, add 1.521 g (0.01 mol) of o-vanillin, add an appropriate amount of methanol solution, mix well, and heat under reflux at 60°C for 6 hours to obtain a red solution, cool it, and filter it to obtain a red solid, which is the Schiff base ligand H4L, with a calculated yield of 90%.
[0081] Take 0.03g (0.05mmol) of Schiff base ligand H4L and put it into a 10mL sample bottle, add 2mL of methanol solution and 2mL of acetonitrile solution, then add 0.075g (0.2mmol) of DyCl3·6H2O, and then add 40μL of triethylamine solution, mix well. Seal with plastic wrap, poke holes, evaporate at room temperature for one week, and pale yellow crystal particles will precipitate in the bottle, filter, wash, and dry to obtain a rare earth metal catalyst.
[0082] Example 6
[0083] Add 3.023g (0.02mol) 3-amino-2-hydroxyacetophenone to a round-bottom flask, add 80mL methanol solution, then add 0.743g (0.01mol) 1,3-propylenediamine, mix well, heat and reflux in a 55℃ oil bath for 5h, the solution turns from black to yellow. Cool and filter to obtain a yellow solid, namely intermediate M, with a calculated yield of 85%.
[0084] Take 1.7g (0.005mol) of the intermediate and add it to a round-bottom flask, add 1.521g (0.01mol) of o-vanillin, add an appropriate amount of methanol solution, mix well, and heat under reflux at 60°C for 6h. A red solution is obtained, cooled, and filtered to obtain a red solid, namely the Schiff base ligand H4L, with a calculated yield of 90%.
[0085] Take 0.03g (0.05mmol) of Schiff base ligand H4L and put it into a 10mL sample bottle, add 2mL of methanol solution and 2mL of acetonitrile solution, then add 0.074g (0.2mmol) of TbCl3·6H2O, and then add 40μL of triethylamine solution, mix well. Seal with plastic wrap, poke holes, evaporate at room temperature for one week, and pale yellow crystal particles will precipitate in the bottle, filter, wash, and dry to obtain a rare earth metal catalyst.
[0086] Example 7
[0087] Add 3.023g (0.02mol) 3-amino-2-hydroxyacetophenone to a round-bottom flask, add 80mL methanol solution, then add 0.743g (0.01mol) 1,3-propylenediamine, mix well, heat and reflux in a 55℃ oil bath for 5h, the solution turns from black to yellow. Cool and filter to obtain a yellow solid, namely intermediate M, with a calculated yield of 85%.
[0088] Take 1.7g (0.005mol) of the intermediate and add it to a round-bottom flask, add 1.521g (0.01mol) of o-vanillin, add an appropriate amount of methanol solution, mix well, and heat under reflux at 60°C for 6h. A red solution is obtained, cooled, and filtered to obtain a red solid, namely the Schiff base ligand H4L, with a calculated yield of 90%.
[0089] Take 0.03g (0.05mmol) of Schiff base ligand H4L and put it into a 10mL sample bottle, add 2mL of methanol solution and 2mL of acetonitrile solution, then add 0.073g (0.2mmol) of EuCl3·6H2O, and then add 40μL of triethylamine solution, mix well. Seal with plastic wrap, poke holes, evaporate at room temperature for one week, and pale yellow crystal particles will precipitate in the bottle, filter, wash, and dry to obtain a rare earth metal catalyst.
[0090] See also Figure 6 The Schiff base ligand H4L prepared in Example 1 was tested by infrared spectroscopy at 3000 cm -1 The peaks on the left and right are the CH stretching vibration absorption peaks on the benzene ring, 1604 cm -1 The stretching vibration of the characteristic group C=N of Schiff base, 1520cm -1 and 1453cm -1 The peak at 1349 cm is the vibration peak of the C=C skeleton on the benzene ring. -1 The characteristic peak of CN is 1245cm -1 The stretching vibration peak of Ar-O on aromatic ether is 1071 cm -1 OC stretching vibration peak of aromatic ether, 838 cm -1 The out-of-plane bending vibration peak of CH on the benzene ring is 730cm -1 It is the out-of-plane bending vibration absorption peak of phenolic hydroxyl group, indicating that the Schiff base ligand was successfully synthesized.
[0091] See also Figure 7 and Figure 8 , the Schiff base ligand prepared in Example 1 was subjected to H spectrum, C spectrum and NMR detection, and the H NMR spectrum can be interpreted as: 1 HNMR (400MHz, DMSO-d6) δ (ppm): 10.22 (s, 1H, Ar-OH), 9.11 (s, 1H, CN=CH), 6.62-7.56 (m, 6H, Ar-CH), 3.73-3.80 (m, 3H, -CH3), 2.47 (m, 3H, O=C-CH3); the carbon nuclear magnetic resonance spectrum can be interpreted as: 13CNMR (100MHz, DMSO) δ175.17, 174.39, 163.28, 161.17, 154.31, 152.80, 14 8.98, 138.85, 136.25, 128.53, 124.28, 124.16, 123.64, 119.55, 119.32, 11 8.82, 118.60, 117.69, 117.01, 116.48, 116.05, 115.42, 114.55, 69.54, 69. 13, 62.65, 56.27, 51.65, 40.65, 40.35, 40.14, 39.72, 39.51, 39.30, 15.24. Furthermore, it was determined that the Schiff base ligand H4L was successfully synthesized.
[0092] See also Fig. 9 Infrared spectrometry was performed on different rare earth metal catalysts and Schiff base ligands in Examples 1 to 3. In the figure, H4L represents the Schiff base ligand, 1 represents the rare earth metal catalyst prepared by ErCl3·6H2O as the rare earth metal chloride, 2 represents the rare earth metal catalyst prepared by YbCl3·6H2O as the rare earth metal chloride, and 3 represents the rare earth metal catalyst prepared by YCl3·6H2O as the rare earth metal chloride. The results show that their infrared spectra are basically the same, which indicates that their coordination structures are the same. Compared with the infrared spectra of the catalyst and the Schiff base ligand H4L, at a wavelength of 1599cm -1 The peak at 1298 cm-1 may be caused by the coordination between the C=N group on the Schiff base ligand H4L and the metal ion, resulting in a blue shift. -1 The peak at 741 cm is the stretching vibration peak of Ar-O on aromatic ether. -1 The peak at 1553cm is the bending vibration peak of the phenolic hydroxyl group. Compared with the peak position of H4L, it has a red shift, indicating that the O on the phenolic hydroxyl group of H4L is coordinated with the metal ion. -1 and 1455cm -1 The peak at 1391 cm is the vibration peak of the C=C skeleton on the benzene ring. -1 The peak at is the characteristic peak of CN.
[0093] See also Fig.10, thermogravimetric experiments were performed on different rare earth metal catalysts in Examples 1 to 3 to evaluate thermal stability. In the figure: 1 represents a rare earth metal catalyst prepared by ErCl3·6H2O as a rare earth metal chloride, 2 represents a rare earth metal catalyst prepared by YbCl3·6H2O as a rare earth metal chloride, and 3 represents a rare earth metal catalyst prepared by YCl3·6H2O as a rare earth metal chloride; it can be seen that in the thermogravimetric curve within 30°C to 800°C, the mass of the complex decreases by 5.79% at 60°C to 100°C, which is caused by the vaporization of free methanol molecules in the crystal due to the increase in temperature. When the temperature rises to 180°C, the mass decreases again, which is attributed to the loss of free water molecules in the complex. When the temperature rises from 480°C to 700°C, the mass decreases by 12%, which may be caused by the decomposition of the coordinated methanol molecules and water molecules in the complex. Finally, the remainder should be ligands and metal ions. It can be inferred that the structure of the complex does not change before heating to 200°C, indicating that this type of catalyst has high thermal stability and great potential for use as a catalyst.
[0094] A butterfly-shaped trinuclear Schiff base rare earth metal catalyst is prepared by the above method. The minimum structural unit of the catalyst includes one Schiff base ligand and three rare earth metal ions. The complex is a symmetrical structure, belongs to the monoclinic system, and has a C2 / c space group. In the complex, M1 and M2 have the same coordination environment, and both form an eight-coordinate structure with the O of two phenolic hydroxyl groups and the N of the imine group on the Schiff base ligand, the O of the methanol molecule, the O of two H2O molecules, and the O of two hydroxyl groups. M3 forms an eight-coordinate structure with the O of two phenolic hydroxyl groups, the O of two methoxy groups, the O of two hydroxyl groups, and the O of two water molecules on the Schiff base ligand. The catalyst has good catalytic stability. It has the characteristics of high catalytic efficiency and conversion rate and low catalytic cost.
[0095] The application of the butterfly-shaped trinuclear Schiff base in the catalytic synthesis of cyclic carbonates as mentioned above. A butterfly-shaped trinuclear Schiff base rare earth metal catalyst is used as a catalyst, tetrabutylammonium bromide is used as a co-catalyst, and epoxide and carbon dioxide are used as reaction substrates for a cycloaddition reaction to obtain a cyclic carbonate; the epoxide is epichlorohydrin, allyl glycidyl ether, styrene oxide, butyl glycidyl ether or phenyl glycidyl ether; the cycloaddition reaction time is 1 to 3 hours, the reaction temperature is 60°C to 120°C, the conversion rate is 99%, and the molar ratio of epoxide, catalyst and co-catalyst is 1000:(0.4 to 1):(2 to 8).
[0096] Example 8
[0097] To explore the effect of different metal ions on catalytic efficiency. Taking the cycloaddition reaction of styrene oxide and carbon dioxide as an example, 10mmol of styrene oxide, 0.1mol% of rare earth metal catalyst and 0.8mol% of co-catalyst tetrabutylammonium bromide (TBAB) were added to the autoclave, and the gas in the autoclave was circulated for 3 times to eliminate the interference of other gases, and then the reaction was carried out at 120℃ and 1.0MPaCO2 for 2h.
[0098] The catalytic effects are shown in the following table:
[0099] Catalytic efficiency of the catalyst for the reaction of CO2 and styrene oxide
[0100]
[0101] It can be seen that the catalytic conversion rates of the catalysts are 89%, 88%, 89%, and the TOF values are 445h -1 , 440h -1 , 445h -1 , the catalytic activity is not much different. Therefore, the catalytic efficiency of different types of rare earth metal complexes for the cycloaddition reaction of carbon dioxide and styrene oxide is similar. In the table, 1 represents a rare earth metal catalyst prepared by ErCl3·6H2O as the rare earth metal chloride, 2 represents a rare earth metal catalyst prepared by YbCl3·6H2O as the rare earth metal chloride, and 3 represents a rare earth metal catalyst prepared by YCl3·6H2O as the rare earth metal chloride.
[0102] Example 9: To investigate the effects of temperature, pressure, reaction time, catalyst dosage, co-catalyst dosage, water, and air on the catalytic effect in the reaction, the following experiment was conducted.
[0103] Catalytic Performance of Rare Earth Metal Catalyst 1 in the Cycloaddition of Carbon Dioxide and Styrene Oxide
[0104]
[0105]
[0106] It can be seen from the experimental data in the table that 10mmol styrene oxide and 1MPa CO2 reacted at 80℃ for 4h. When only the catalyst was added, the experimental conversion rate was almost 0, and when only the co-catalyst was added, the conversion rate was 19%. When the catalyst and the co-catalyst co-existed, the conversion rate increased to 99%, which shows that the synergistic catalysis of the catalyst and the co-catalyst can effectively promote the reaction. Other conditions remain unchanged, and the reaction was carried out at a temperature of 120℃ for 2h, and the experimental conversion rate was 94%. As the temperature dropped from 100℃ to 80℃, the conversion rate decreased from 89% to 85%. When the reaction temperature was 60℃, the conversion rate decreased significantly to 70%. Therefore, the optimal reaction temperature was selected as 80℃. When the pressure dropped from 1MPa to 0.4MPa, the conversion rate also dropped from 85% to 52%, indicating that the pressure had a great influence on the catalytic effect of the reaction. When the reaction time increases from 1h to 4h with a gradient of 1h, the conversion rate increases from 68% to 99%, wherein the conversion rates of 3h and 4h are not much different, 98% and 99% respectively, so the optimal reaction time is selected to be 3h. When the catalyst dosage is 0.01mmol, the reaction conversion rate is the highest, which is 98%. When the co-catalyst TBAB is at a low loading (0.04mmol, 0.02mmol), the conversion rates are 60% and 42% respectively. In addition, when additional water is added to the reaction system or the air in the reaction system is not excluded, there is no obvious effect on the conversion rate of the reaction, indicating that the catalytic system prepared by the present invention has good tolerance.
[0107] Based on the above experimental results and the concept of high efficiency and energy saving, the conditions selected were: temperature 80°C, pressure 1MPa, time 3h, catalyst dosage 0.01mmol, and co-catalyst dosage 0.08mmol, to explore the effect of the catalyst on the catalytic efficiency of the cycloaddition reaction of carbon dioxide and epoxide.
[0108] Example 10
[0109] The universality of the catalytic system in the cycloaddition reaction of different epoxides and carbon dioxide was explored. Four epoxides with different substituents were selected as substrates, and the catalytic experiment was carried out under the reaction conditions of temperature 80℃, pressure 1MPa, reaction time 3h, and catalyst and co-catalyst dosages of 0.01 and 0.08mmol respectively. Figures 11 to 14 The product was tested by nuclear magnetic resonance hydrogen spectrum, which showed that the rare earth metal catalyst had a good catalytic effect and improved the efficiency of product synthesis.
[0110] In summary, the present invention provides a butterfly-shaped trinuclear Schiff base rare earth metal catalyst, a preparation method and an application thereof. The method uses Schiff base ligand and rare earth metal chloride as raw materials, reacts at room temperature, and adds triethylamine to obtain a butterfly-shaped trinuclear Schiff base rare earth metal catalyst. The reaction conditions are mild, and harsh reaction environment and equipment are not required. The raw material sources are wide and the cost is low. The reaction time is short, the yield is high, and the catalyst is suitable for industrialization. The production input cost is effectively controlled, and the production efficiency and yield are improved. The rare earth metal catalyst produced has better stability, higher catalytic efficiency, and the catalytic process is not affected by additional moisture and air. The catalyst has good tolerance, and the conditions for the catalytic reaction can be greatly reduced, thereby reducing the catalytic cost.
[0111] The above description is only a preferred embodiment of the present invention and is not intended to impose any limitation on the technical solution of the present invention. Those skilled in the art should understand that, without departing from the spirit and principles of the present invention, the technical solution can also be subjected to several simple modifications and substitutions, and these modifications and substitutions are also within the scope of protection covered by the claims.
Claims
1. A butterfly-shaped trinuclear Schiff base rare earth metal catalyst, characterized in that: Its molecular structure is: Among them, M1~M3 are rare earth metal ions.
2. The butterfly-shaped trinuclear Schiff base rare earth metal catalyst according to claim 1, characterized in that: The rare earth metal ion is Sc 3+ , Y 3+ 、Ce 3+ 、Nd 3+ 、Sm 3+ , Gd 3+ 、Eu 3+ , Tb 3+ 、Dy 3+ , Er 3+ 、Ho 3+ 、Tm 3+ or Yb 3+ .
3. A method for preparing a butterfly-shaped trinuclear Schiff base rare earth metal catalyst, characterized in that: include: preparing Schiff base ligands; A butterfly-shaped trinuclear Schiff base rare earth metal catalyst is prepared by using a Schiff base ligand and a rare earth metal chloride. The molecular structure of the butterfly-shaped trinuclear Schiff base rare earth metal catalyst is: Among them, M1~M3 are rare earth metal ions.
4. The method for preparing the butterfly-shaped trinuclear Schiff base rare earth metal catalyst according to claim 3, characterized in that: The molecular structural formula of the Schiff base ligand is:
5. The method for preparing the butterfly-shaped trinuclear Schiff base rare earth metal catalyst according to claim 3, characterized in that: The rare earth metal chloride is ScCl3·6H2O, YCl3·6H2O, CeCl3·6H2O, NdCl3·6H2O, SmCl3·6H2O, GdCl3·6H2O, EuCl3·6H2O, TbCl3·6H2O, DyCl3·6H2O, ErCl3·6H2O, HoCl3·6H2O, TmCl3·6H2O or YbCl3·6H2O.
6. The method for preparing the butterfly-shaped trinuclear Schiff base rare earth metal catalyst according to claim 3, characterized in that: The method for preparing the Schiff base ligand is: Reacting 1,3-propylenediamine and 3-amino-2-hydroxyacetophenone to obtain an intermediate; The intermediate is reacted with o-vanillin to obtain the Schiff base ligand.
7. The method for preparing the butterfly-shaped trinuclear Schiff base rare earth metal catalyst according to claim 3, characterized in that: The method for preparing a butterfly-shaped trinuclear Schiff base rare earth metal catalyst by using a Schiff base ligand and a rare earth metal chloride is as follows: The Schiff base ligand and the rare earth metal chloride are dissolved in a solvent, triethylamine is added, and a butterfly-shaped trinuclear Schiff base rare earth metal catalyst is obtained by reaction under room temperature.
8. A butterfly-shaped trinuclear Schiff base rare earth metal catalyst, characterized in that: Prepared by the method according to any one of claims 3 to 7.
9. Use of the butterfly-shaped trinuclear Schiff base rare earth metal catalyst as claimed in claim 8 in the preparation of cyclic carbonates.
10. The use of the butterfly-shaped trinuclear Schiff base rare earth metal catalyst in the preparation of cyclic carbonate according to claim 9, characterized in that: A butterfly-shaped trinuclear Schiff base rare earth metal catalyst is used as a catalyst, tetrabutylammonium bromide is used as a co-catalyst, and epoxide and carbon dioxide are used as reaction substrates to carry out a cycloaddition reaction to obtain a cyclic carbonate; the epoxide is epichlorohydrin, allyl glycidyl ether, styrene oxide, butyl glycidyl ether or phenyl glycidyl ether; the cycloaddition reaction time is 1 to 3 hours, the reaction temperature is 60°C to 120°C, the conversion rate reaches 99%, and the molar ratio of epoxide, catalyst and co-catalyst is 1000:(0.4-1):(2-8).
Citation Information
Patent Citations
Trinuclear dysprosium single-molecular magnet based on acylhydrazone Schiff base and preparation method of trinuclear dysprosium single-molecular magnet
CN118206572A
Method for preparing cyclic carbonate
US20210355094A1